Ferrite-austenite duplex stainless steel plate
A ferritic-austenitic duplex stainless steel sheet with a controlled composition and structure addresses the challenges of high strength, smoothness, and flatness, enabling stable performance in precision parts for electronic and precision equipment.
Patent Information
- Application Number
- JP2023048349
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-04
AI Technical Summary
Conventional stainless steel sheets face challenges in stably ensuring high strength, excellent etched surface smoothness, and flatness before and after etching processing, which are crucial for the miniaturization and weight reduction of parts in electronic and precision equipment.
A ferritic-austenitic duplex stainless steel sheet with a specific chemical composition and controlled metallographic structure, including a grain size of 2.0 μm or less and a ferrite phase ratio of 20 to 80%, is developed, allowing for high Vickers hardness of 400HV or higher and a radius of curvature after half etching of 150 mm or more.
The solution provides a stainless steel sheet with stable strength, smooth etched surface, and excellent flatness before and after etching, suitable for precision parts in electronic and precision equipment.
Smart Images

Figure 2024137012000001 
Figure 2024137012000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a ferritic-austenitic duplex stainless steel sheet, and in particular to a ferritic-austenitic duplex stainless steel sheet suitable as a material for parts of electronic devices and precision machines that are manufactured with etching. [Background technology]
[0002] The parts used in electronic and precision equipment are required to be smaller and lighter, and to have high dimensional accuracy. For this reason, the materials for these parts tend to be thinner, and they also need to have a good balance between strength and elongation, specifically, high strength while maintaining the same level of workability as before (hereinafter simply referred to as high strength).
[0003] In addition, when manufacturing the above-mentioned parts, a method of partially thinning the plate thickness by etching is often used as one of the means for obtaining a predetermined shape with high precision. Therefore, the material of the above-mentioned parts is required to have small shape change and no plate warping after etching, that is, excellent flatness before and after etching and smoothness of the etched surface.
[0004] Sheet warpage refers to the deformation of the entire steel sheet after partial etching (herein referred to as "half etching") of the steel sheet surface. The warpage of the steel sheet after half etching is caused by the residual stress of the steel sheet. Therefore, this warpage can be reduced by carrying out a heat treatment for the purpose of relieving stress after temper rolling, that is, a so-called stress relief heat treatment.
[0005] Furthermore, the material used for the above-mentioned parts is generally austenitic stainless steel, which has an excellent balance between strength and elongation among stainless steels and has had its strength increased by temper rolling, etc. In particular, metastable austenitic stainless steels such as SUS301 and SUS304 are used, which combine high strength associated with deformation-induced martensitic transformation with excellent workability due to the TRIP effect and which, among the austenitic stainless steels, can relatively easily obtain high strength.
[0006] The austenitic stainless steel sheet, the strength of which has been increased by temper rolling or the like, is further subjected to shape correction using a tension leveler, distortion relief heat treatment for the purpose of reducing residual stress, and the like. This is to make the steel sheet shaped and flat in response to the precision machining of the above-mentioned parts. In addition, when small pieces corresponding to parts are taken out from a material manufactured from a relatively large steel sheet or steel strip by pressing, etching, or the like, or when the thickness of a part of the small pieces is reduced by further etching, as described above, deformation due to residual stress occurs. Furthermore, the more excellent the smoothness of the processed surface, particularly the etched surface (hereinafter also referred to as the etched surface), the more precise parts with higher dimensional accuracy can be manufactured from the material.
[0007] Patent Document 1 discloses a stainless steel sheet for photoetching in which the average crystal grain size is refined so as to obtain a smooth etched surface, and which is further subjected to a distortion relief heat treatment.
[0008] Patent Document 2 discloses a method for manufacturing an austenitic stainless steel sheet in which cold rolling conditions and straightening conditions using a tension leveler are adjusted, and further a tension equivalent to 0.2% yield strength or less of the cold-rolled material is applied to perform a strain relief heat treatment. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2005-320587 A [Patent Document 2] JP 2001-226718 A Summary of the Invention [Problem to be solved by the invention]
[0010] However, with conventional stainless steel sheets, it was difficult to consistently ensure all of the properties required for the material of precision parts with high dimensional accuracy, namely, high strength, excellent smoothness of the etched surface, and flatness before and after etching.
[0011] The object of the present invention is to provide a ferritic-austenitic duplex stainless steel sheet that is excellent in all respects, including strength, smoothness of the etched surface, and flatness before and after etching, and which can stably obtain these properties, thereby enabling the demand for further miniaturization and weight reduction of parts used in electronic and precision instruments. [Means for solving the problem]
[0012] In order to solve the above problems, the inventors carried out prototype tests using a large number of stainless steels and conducted intensive research based on the results obtained. As a result, they found that by applying a ferritic-austenitic duplex stainless steel consisting of a specified composition, it is possible to stably achieve a finer average crystal grain size even when the stress relief heat treatment is performed at a high temperature, and that it is possible to stably ensure high strength and smoothness of the etched surface. Furthermore, they found that by increasing the temperature of the stress relief heat treatment, it is possible to perform stronger shape correction, thereby improving the shape of the steel sheet, efficiently reducing increased residual stress, and achieving excellent flatness before and after processing such as etching. They completed the present invention by clarifying the chemical composition and metal structure characteristics of the steel sheet that can achieve these effects.
[0013] The present invention has been made based on the above findings and further studies, and the gist of the present invention, which has the object of solving the above problems, is as follows.
[0014] [1] Chemical composition, by mass%, C: 0.08% or less, Si: 0.1 to 1.0%, Mn: 1.0-5.0%, Cr: 20.0-28.0%, Ni: 1.0-7.0%, Mo: 0.1-2.0%, N: 0.10-0.30%, Cu: 0-2.0%, Nb: 0-0.50%, Ti: 0 to 0.50%, V: 0 to 0.50%, W: 0 to 0.50%, Co: 0-0.50%, B: 0 to 0.0050%, Sn: 0-0.50%, Al: 0-0.50%, Mg: 0 to 0.010%, Ca: 0 to 0.0100%, Ta: 0 to 0.050%, Ga: 0 to 0.050%, Zr: 0 to 0.50%, and Rare earth elements: 0~0.010% with the remainder being Fe and impurities, The average crystal grain size is 2.0 μm or less, A ferritic-austenitic duplex stainless steel plate characterized by a Vickers hardness of 400HV or more. [2] The ferritic-austenitic duplex stainless steel sheet according to [1] above, characterized in that in the metal structure, the ferritic phase ratio is 20 to 80%. [3] A ferritic-austenitic duplex stainless steel sheet according to [1] or [2] above, characterized in that the radius of curvature after half-etching is 150 mm or more. [4] A ferritic-austenitic duplex stainless steel sheet according to [1] or [2] above, characterized in that it is used for parts of electronic devices or precision instruments. [5] A ferritic-austenitic duplex stainless steel sheet according to the above [3], characterized in that it is used for parts of electronic devices or precision instruments. Effect of the Invention
[0015] According to the present invention, it is possible to provide a ferritic-austenitic duplex stainless steel sheet which is excellent in all respects, including strength, smoothness of the etched surface, and flatness before and after etching, and which can stably obtain all of these properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, a ferritic-austenitic duplex stainless steel sheet according to an embodiment of the present invention (hereinafter, also referred to as "duplex stainless steel sheet", "stainless steel sheet" or "steel sheet") will be described in detail.
[0017] (chemical composition) First, the chemical composition of the duplex stainless steel sheet according to this embodiment will be described in detail. The austenite phase (γ phase) constituting the duplex stainless steel sheet according to this embodiment is composed of a stable γ phase that does not exhibit deformation-induced transformation. In other words, the chemical composition of the duplex stainless steel sheet according to this embodiment is a component system that does not exhibit deformation-induced transformation. The specific chemical composition will be described below. Note that, unless otherwise noted, % for element content in this specification means mass %.
[0018] C: 0.08% or less Carbon (C) is an element that acts as a stabilizing element for the austenite phase. If the C content exceeds 0.08%, Cr carbides are generated during cooling after the finish annealing and stress relief heat treatment (particularly, stress relief heat treatment), which may reduce the corrosion resistance of the steel sheet. Therefore, the C content is set to 0.08% or less. It is preferably 0.06% or less, and more preferably 0.04% or less. There is no particular lower limit for the C content. However, if the C content is reduced excessively, the manufacturing cost increases. From this viewpoint, the C content is preferably 0.005% or more.
[0019] Si: 0.1 to 1.0% Silicon (Si) is an element that acts as a stabilizing element for the ferrite phase. If the Si content is less than 0.1%, it will lead to an increase in manufacturing costs. Therefore, the Si content is set to 0.1% or more. It is preferably 0.2% or more, and more preferably 0.3% or more. On the other hand, if the Si content exceeds 1.0%, it will promote cracking during manufacturing. Therefore, the Si content is set to 1.0% or less. It is preferably 0.9% or less, more preferably 0.8% or less, and even more preferably 0.7% or less.
[0020] Mn: 1.0-5.0% Mn is an element that acts as a stabilizing element for the austenite phase. Mn is also effective as an element that suppresses the decrease in strength due to strain relief heat treatment. If the Mn content is less than 1.0%, the effect of suppressing the decrease in strength during strain relief heat treatment may not be obtained. Therefore, the Mn content is set to 1.0% or more. It is preferably 1.1% or more, more preferably 1.2% or more, and further preferably 1.5% or more. On the other hand, if the Mn content exceeds 5.0%, it will lead to an increase in manufacturing costs. Therefore, the Mn content is set to 5.0% or less. It is preferably 4.7% or less, and more preferably 4.5% or less.
[0021] Cr: 20.0~28.0% Chromium (Cr) is an element that acts on the phase ratio as a stabilizing element of the ferrite phase. Cr is also an element that effectively acts on corrosion resistance. If the Cr content is less than 20.0%, the corrosion resistance may be insufficient. Therefore, the Cr content is set to 20.0% or more. It is preferably 21.0% or more, and more preferably 22.0% or more. On the other hand, if the Cr content exceeds 28.0%, it may lead to a decrease in manufacturability. Therefore, the Cr content is set to 28.0% or less. It is preferably 27.0% or less, and more preferably 25.0% or less.
[0022] Ni: 1.0-7.0% Nickel (Ni) is an element that acts as a stabilizing element for the austenite phase. Ni is also effective as an element that suppresses the decrease in strength during strain relief heat treatment. If the Ni content is less than 1.0%, the effect of suppressing the decrease in strength during strain relief heat treatment may not be obtained. Therefore, the Ni content is set to 1.0% or more. It is preferably 1.3% or more, and more preferably 1.6% or more. On the other hand, if the Ni content exceeds 7.0%, it may lead to an increase in alloy cost and an impairment of manufacturability. Therefore, the Ni content is set to 7.0% or less. It is preferably 6.0% or less, more preferably 5.7% or less, and even more preferably 5.4% or less.
[0023] Mo: 0.1-2.0% Molybdenum (Mo) is an element that acts as a stabilizing element for the ferrite phase. It is also an element that effectively acts on corrosion resistance. If the Mo content is less than 0.1%, the corrosion resistance may be insufficient. Therefore, the Mo content is set to 0.1% or more. It is preferably 0.3% or more, and more preferably 0.6% or more. On the other hand, Mo is also an expensive element. Therefore, if the Mo content exceeds 2.0%, there is a risk of an increase in manufacturing costs. Therefore, the Mo content is set to 2.0% or less. It is preferably 1.7% or less, and more preferably 1.4% or less.
[0024] N: 0.10~0.30% Nitrogen (N), like C, is an element that acts as a stabilizing element for the austenite phase. It is also an element that effectively acts on corrosion resistance. If the N content is less than 0.10%, corrosion resistance may not be ensured. Therefore, the N content is set to 0.10% or more. It is preferably 0.12% or more, and more preferably 0.14% or more. On the other hand, even if the N content exceeds 0.30%, the effect is saturated. Therefore, the N content is set to 0.30% or less. It is preferably 0.28% or less, and more preferably 0.26% or less.
[0025] The above is the basic chemical composition of the ferritic-austenitic stainless steel sheet of this embodiment, with the remainder being iron (Fe) and impurities. Furthermore, the ferritic-austenitic stainless steel sheet of this embodiment may optionally contain one or more of Cu, Nb, Ti, V, W, Co, B, and Sn in order to further improve workability, corrosion resistance, and hot workability. The lower limit of these elements is 0% or more, and preferably more than 0%.
[0026] Cu:2.0% or less Copper (Cu) is an austenite stabilizing element, and also has the effect of improving corrosion resistance by suppressing the precipitation of nitrides. Therefore, the Cu content may be 0.10% or more. However, if the Cu content exceeds 2.0%, it may increase the raw material cost and deteriorate the hot workability. Therefore, the Cu content is preferably 2.0% or less, and more preferably 1.8% or less.
[0027] Nb: 0.50% or less Niobium (Nb) forms nitrides (NbN) and carbides (NbC) and has the effect of improving workability. Therefore, the Nb content may be 0.01% or more. However, if the Nb content exceeds 0.50%, there is a risk of reducing ductility, so the Nb content is preferably 0.50% or less. The Nb content is more preferably 0.30% or less, and even more preferably 0.20% or less.
[0028] Ti: 0.50% or less Titanium (Ti), like Nb, forms nitrides (TiN) and carbides (TiC) and has the effect of improving workability. Therefore, the Ti content may be 0.01% or more. However, if the Ti content exceeds 0.50%, there is a risk of reducing ductility, so the Ti content is preferably 0.50% or less. The Ti content is more preferably 0.30% or less, and even more preferably 0.20% or less.
[0029] V: 0.50% or less Vanadium (V) forms nitrides and has the effect of improving workability. Therefore, the V content may be 0.01% or more. However, if the V content exceeds 0.50%, there is a risk of reducing ductility and hot workability, so the V content is preferably 0.50% or less, and more preferably 0.40% or less.
[0030] W: 0.50% or less Tungsten (W) is an element that improves corrosion resistance, and in order to exert this effect, the W content is preferably 0.05% or more. However, if the W content exceeds 0.50%, there is a risk of reducing workability, so the W content is preferably 0.50% or less, and more preferably 0.40% or less.
[0031] Co:0.50% or less Cobalt (Co) has the effect of increasing high-temperature strength and improving hot workability. Therefore, the Co content is preferably 0.01% or more. However, if the Co content exceeds 0.50%, there is a risk of reducing toughness, so the Co content is preferably 0.50% or less, and more preferably 0.30% or less.
[0032] B: 0.0050% or less Boron (B) is an element that segregates to grain boundaries and improves hot workability. To achieve this effect, the B content is preferably 0.0002% or more. However, if the B content exceeds 0.0050%, the corrosion resistance may be significantly deteriorated, so the B content is preferably 0.0050% or less, and more preferably 0.0030% or less.
[0033] Sn: 0.50% or less Tin (Sn) is an element that can improve corrosion resistance. To achieve this effect, the Sn content is preferably 0.01% or more, and more preferably 0.03% or more. However, if the Sn content exceeds 0.50%, there is a risk of deteriorating hot workability, so the Sn content is preferably 0.50% or less, and more preferably 0.4% or less.
[0034] Furthermore, the ferritic-austenitic stainless steel sheet of this embodiment may optionally contain one or more of Al, Ca, Mg, Ta, Ga, Zr, and rare earth elements for deoxidization and desulfurization during refining. The lower limit of these elements is 0% or more, preferably more than 0%.
[0035] Al: 0.50% or less Aluminum (Al) may be contained in small amounts for desulfurization and deoxidation. The above effects are exhibited when the Al content is 0.01%, so the Al content is preferably 0.01% or more. However, when the Al content exceeds 0.50%, there is a risk of increasing manufacturing defects and increasing raw material costs, so the Al content is preferably 0.50% or less.
[0036] Mg: 0.010% or less Magnesium (Mg) not only deoxidizes but also has the effect of refining the solidified structure. To achieve these effects, the Mg content is preferably 0.0002% or more. However, if the Mg content exceeds 0.010%, it will increase the cost of the steelmaking process, so the Mg content should be 0.010% or less.
[0037] Ca:0.0100% or less A small amount of calcium (Ca) may be contained for desulfurization and deoxidization. The above effects are exhibited when the Ca content is 0.0001% or more, so the Ca content is preferably 0.0001% or more. However, if the Ca content exceeds 0.0100%, there is a risk of hot work cracking and a decrease in corrosion resistance, so the Ca content is preferably 0.0100% or less, and more preferably 0.0050% or less.
[0038] Ta: 0.050% or less Tantalum (Ta) is an element that improves corrosion resistance by modifying inclusions, and may be contained as necessary. In order to exert this effect, the Ta content is preferably 0.0002% or more. However, if the Ta content exceeds 0.050%, there is a risk of causing a decrease in room temperature ductility and toughness, so the Ta content is preferably 0.050% or less, more preferably 0.030% or less.
[0039] Ga: 0.050% or less Gallium (Ga) is an element that improves corrosion resistance and suppresses hydrogen embrittlement, and may be contained as necessary. In order to exert this effect, the Ga content is preferably 0.0002% or more. However, if the Ga content exceeds 0.050%, there is a risk of causing a decrease in workability, so the Ga content is preferably 0.050% or less, and more preferably 0.030% or less.
[0040] Zr: 0.50% or less Zirconium (Zr) has a similar effect to Nb and Ti, and is also an element that improves oxidation resistance. To achieve these effects, the Zr content is preferably 0.01% or more. However, if the Zr content exceeds 0.50%, it will lead to an increase in raw material costs, so the Zr content is preferably 0.50% or less, and more preferably 0.30% or less.
[0041] Rare earth elements: 0.010% or less Rare earth elements (REM) are elements that improve hot workability. The above effects are achieved when the total content of rare earth elements is 0.0002% or more, so the content of rare earth elements may be 0.0002% or more. However, if the total content of rare earth elements exceeds 0.010%, manufacturability is impaired and costs increase, so the upper limit of rare earth elements is preferably 0.010%. A more preferable content range of rare earth elements is 0.0005 to 0.008%.
[0042] Here, rare earth elements (REM) refer to two elements, scandium (Sc) and yttrium (Y), and 15 elements (lanthanoids) from lanthanum (La) to lutetium (Lu). In this specification, "rare earth elements" refers to one or more elements selected from these rare earth elements, and "content of rare earth elements" refers to the total amount of rare earth elements.
[0043] The stainless steel sheet of this embodiment contains, in addition to the elements described above, Fe and impurities (including unavoidable impurities). However, in addition to the elements described above, other elements can also be contained within a range that does not impair the effects of the present invention.
[0044] In addition, scrap materials are often used in the manufacture of stainless steel sheets. Therefore, various impurity elements are often inevitably mixed into the stainless steel sheets, and it is difficult to determine the content of the impurity elements uniquely. Therefore, the impurities in this embodiment refer to elements contained in an amount that does not impair the effects of the present invention.
[0045] (Metal structure) In the metal structure of the ferritic-austenitic duplex stainless steel sheet of this embodiment, when the ferritic phase ratio is within a predetermined range, the average crystal grain size of the metal structure can be easily refined. The ferritic phase ratio is preferably 20% or more and 80% or less. When the ferritic phase ratio is within this range, the ferritic phase and the austenitic phase inhibit each other's grain growth, and the crystal grains can be further refined. It is more preferably 25% or more and 75% or less, and even more preferably 30% or more and 70% or less. From the viewpoint of the above-mentioned grain growth inhibition effect, the ferritic phase ratio is most preferably 50%.
[0046] <Average grain size> In order to achieve high strength of the steel sheet and obtain excellent smoothness of the etched surface, it is effective to make the average crystal grain size of the metal structure 2.0 μm or less. If the average crystal grain size exceeds 2.0 μm, the etched surface becomes rough, and good smoothness of the etched surface cannot be obtained. The average crystal grain size is preferably 1.5 μm or less, and more preferably 1.0 μm or less. The lower limit of the average crystal grain size is not particularly limited, but may be 0.4 μm or more for practical purposes.
[0047] (Vickers hardness) As a material that can respond to the trend toward smaller and lighter electronic devices and precision machinery, and the associated trend toward thinner materials, it is effective for the steel plate to have a Vickers hardness (hereinafter also simply referred to as "hardness") of 400 HV or more. The hardness is preferably 410 HV or more, and more preferably 420 HV or more. There is no particular upper limit to the hardness, but it is set to 440 HV or less in consideration of the processability during part molding. On the other hand, if the hardness is less than 400 HV, the strength required as a material for the parts cannot be ensured.
[0048] Hardness and strength are considered to be proportional to each other, and a 400HV steel plate can be said to have a 0.2% yield strength of 1200MPa or more. Furthermore, the total elongation (elongation at break) at that time is about 5%.
[0049] (Radius of curvature after half etching) In order to obtain flatness of the steel sheet before and after etching, it is effective that the radius of curvature after half etching is 150 mm or more. The radius of curvature after half etching is preferably 175 mm or more, and more preferably 200 mm or more. The upper limit of the radius of curvature before and after etching is desirably ∞ (infinity), i.e., no warping, and is not particularly limited. However, in addition, the value after half etching may be 400 mm or less in practical use. On the other hand, if the radius of curvature after half etching is less than 150 mm, the flatness before and after etching required for the material of the part cannot be ensured.
[0050] The term "half etching" used here refers to etching one of the rolled surfaces of a steel sheet in the sheet thickness direction until the sheet thickness is reduced to half. Half etching is performed by coating the rolled surface with nail polish and immersing it in an etching solution such as ferric chloride.
[0051] (Thickness) The thickness of the duplex stainless steel plate according to this embodiment is not particularly limited, but may be 3.0 to 0.05 mm. It is preferably 0.08 mm or more. Furthermore, by making the thickness 1.5 mm or less, it becomes easy to refine the metal structure, and the above-mentioned metal structure can be easily ensured. Therefore, the thickness may be 1.0 mm or less. It is preferably 0.5 mm or less.
[0052] (Manufacturing method) A method for manufacturing the ferritic-austenitic duplex stainless steel sheet of this embodiment will now be described. The ferritic-austenitic duplex stainless steel sheet according to this embodiment can achieve the above-mentioned effects as long as it has the above-mentioned characteristics, regardless of the manufacturing method. However, in order to achieve both strength, smoothness of the etched surface, and flatness before and after etching, it is necessary to control the metal structure (particularly the average crystal grain size) and hardness as described above. The above-mentioned metal structure and hardness can be achieved by combining the chemical composition of the steel with appropriate manufacturing conditions. A preferred manufacturing method for obtaining the ferritic-austenitic duplex stainless steel sheet of this embodiment will be described below.
[0053] First, a steel slab having the above-mentioned chemical composition, which is produced by continuous casting or ingot casting after melting, is hot-rolled into a steel sheet (hot rolling process). Then, a hot-rolled sheet annealing process, a pickling process, and a cold rolling process are performed to obtain a cold-rolled sheet having a predetermined thickness. The hot-rolled sheet annealing may be performed as necessary, and may be omitted. Each of the above processes may be a general manufacturing method for ferritic-austenitic duplex stainless steel sheet.
[0054] (Finish annealing process) Finish annealing is performed on the cold-rolled steel sheet controlled to a predetermined thickness in the cold rolling process. The finish annealing temperature is 850°C or more and 1050°C or less. If the finish annealing temperature is less than 850°C, the metal structure will be a mixture of recrystallized grains and non-recrystallized grains, resulting in a state in which the hardness between the crystal grains varies. If the hardness varies between the crystal grains, good flatness cannot be obtained after shape correction by a tension leveler. On the other hand, if the finish annealing temperature exceeds 1050°C, the average crystal grain size after the finish annealing will become coarse, and the average crystal grain size after the distortion relief heat treatment will also become coarse. Therefore, the finish annealing temperature is 850°C or more and 1050°C or less. The annealing time (holding time) in the finish annealing process can be set appropriately. Typically, it is 600 seconds or less. It is preferably 400 seconds or less, more preferably 150 seconds or less. From the viewpoint of recrystallization, the lower limit of the annealing time in the final annealing step may be set to 5 seconds or more.
[0055] After the finish annealing process, the steel sheet is cooled to room temperature (around 25°C). The average cooling rate during cooling may be 1°C / sec to 100°C / sec. If the average cooling rate is less than 1°C / sec, Cr carbides may be generated during the cooling process, which may result in a decrease in corrosion resistance. In addition, considering productivity and pickling properties, the average cooling rate is preferably 5 to 50°C / sec. Here, the "average cooling rate" is defined as the value obtained by dividing the temperature drop of the steel sheet from the start of cooling (end of holding) to room temperature by the time required to cool from the start of cooling to room temperature.
[0056] (Temper rolling process) After the finish annealing process, temper rolling is performed (temper rolling process). Temper rolling is a process for improving the strength of the material (steel plate). The temper rolling in this embodiment may be a common manufacturing method in stainless steel manufacturing, and the temper rolling reduction ratio may be adjusted according to the desired strength. For example, the temper rolling ratio may be 40 to 70%. Note that the austenite phase of the ferritic-austenitic duplex stainless steel in this embodiment is in a stable state, and deformation-induced martensite is not generated during temper rolling.
[0057] (shape correction process) The steel sheet after the temper rolling is repeatedly bent while applying a tension of 0.5 to 3.0% elongation by a tension leveler, thereby performing shape correction (shape correction process). Shape correction by a tension leveler is a process for ensuring the flatness of the steel sheet, and is usually controlled by the elongation. The shape correction process in this embodiment can be performed under general conditions in the production of ferritic-austenitic duplex stainless steel sheets, but it is preferable to set the elongation to 0.5 to 3.0%. If the elongation is less than 0.5%, warping after half etching may become large. On the other hand, if the elongation exceeds 3.0%, hardening may occur in the production line. From the viewpoint of stable production, the elongation is preferably in the range of 0.5% to 1.5%.
[0058] (Distortion heat treatment process) The steel sheet after the shape correction by the tension leveler is subjected to a stress relief heat treatment at a temperature range of 700°C to 800°C (strain relief heat treatment process). The stress relief heat treatment is a process for reducing residual stress caused by temper rolling and shape correction by the tension leveler. The reason why the ferritic-austenitic duplex stainless steel sheet of this embodiment can stably secure strength even when the stress relief heat treatment is performed at a high temperature is not clear, but it is presumed that the strain introduced during the temper rolling is easily uniformly accumulated in the metal structure by containing a predetermined chemical composition, and the recovery during the stress relief heat treatment is suppressed. That is, according to this embodiment, since the steel sheet has a predetermined chemical composition, the stress relief heat treatment temperature can be increased without worrying about a decrease in strength, so that the residual stress in the steel sheet can be sufficiently reduced, and as a result, both strength and excellent flatness before and after the etching process can be achieved. If the temperature of the stress relief heat treatment is less than 700°C, the removal of residual stress is insufficient, and flatness before and after the etching process cannot be secured. On the other hand, if the temperature of the distortion heat treatment exceeds 800°C, the hardness significantly decreases, and the necessary strength cannot be ensured. Therefore, the temperature of the distortion heat treatment is set to 700°C or higher and 800°C or lower.
[0059] The process described above makes it possible to manufacture the ferritic-austenitic duplex stainless steel sheet according to this embodiment. EXAMPLES
[0060] In order to confirm the effects of the present invention in detail, the following experiment was carried out. Note that this example shows one embodiment of the present invention, and the present invention is not limited to the following configuration.
[0061] Steel having the chemical composition shown in Table 1 was melted to obtain an ingot having a thickness of 100 mm. The ingot was then heated to 1230°C, and hot-rolled to obtain a hot-rolled sheet having a thickness of 5.0 mm. The hot-rolled sheet was then annealed (annealing temperature: 1080°C, annealing time: 60 seconds), and cold-rolled with intermediate annealing repeatedly performed to obtain a cold-rolled sheet having a thickness of 0.22 mm to 0.50 mm. The cold-rolled sheet was heated at the finish annealing temperature in Table 2 for 60 seconds, and then cooled to room temperature to obtain a finish annealed sheet. Furthermore, the finish annealed sheet was subjected to temper rolling at the temper rolling rate and tension leveler elongation (TL elongation) shown in Table 2, and shape correction was performed with a tension leveler (TL) to obtain a steel sheet having a thickness of 0.10 mm. Then, a distortion relief heat treatment was performed for 60 seconds under the conditions shown in Table 2 to obtain a duplex stainless steel sheet. The resulting duplex stainless steel sheets were subjected to the following various evaluation tests.
[0062] (Method of measuring average crystal grain size) The average crystal grain size was determined as follows: The L-section (plane including the rolling direction and the sheet thickness direction) of the steel sheet prepared by electrolytic polishing was measured by electron backscatter diffraction (EBSD). The measurement area was 100 μm × 300 μmL at the center of the sheet thickness, and the measurement step size was 0.1 μm. Using the analysis software "OIM-Analysis" made by TSL Solutions, plot data with a Confidence Index value of more than 0.1 was extracted from the measured data, and the average grain size was calculated by quadrature. If the crystal orientation difference between adjacent plot data was less than 15°, they were considered to be the same grain, and if the orientation difference was 15° or more, they were treated as different grains. In addition, no distinction was made between the ferrite phase and the austenite phase when calculating the average grain size.
[0063] (Hardness measurement method) The hardness of the steel plate surface was measured using a Vickers hardness tester in accordance with JIS Z 2244:2009. The steel plate surface was measured 10 times with a load of 0.5 kgf, and the average value was calculated and used as the representative value. If the hardness was 400 HV or more, it was deemed to have the necessary strength and passed the test.
[0064] (Method of measuring ferrite phase ratio) The measurement of the ferrite phase ratio was specified as follows: A number of test pieces measuring t×40 mm were cut out from the steel plate, stacked to a total thickness of 2 mm or more, and then measured using a ferrite meter. The measurement was carried out five times, and the average value was taken as the ferrite phase ratio of the steel plate.
[0065] (Evaluation test of smoothness of etched surface) One surface of a test piece cut from a steel plate with a thickness of 0.1 mm x 50 mm x 50 mm was etched by spraying an aqueous solution of ferric chloride with a specific gravity of 1.35 heated to 50°C for 4 minutes. The smoothness of the etched surface was measured using a contact surface roughness meter to measure the arithmetic mean roughness Ra along the direction perpendicular to the rolling direction. A Ra of 0.6 μm or less was considered to be acceptable.
[0066] (Evaluation test of flatness before and after etching) A test piece measuring 0.1 mm thick x 12 mm wide x 100 mm wide was cut from the steel plate, which was then half-etched in an aqueous solution of ferric chloride. The radius of curvature of the test piece was measured when the thickness had been reduced by half. If the radius of curvature after half-etching was 150 mm or more, the test piece was deemed to have passed the test, as it had the necessary flatness before and after etching.
[0067] The results of the various evaluation tests are shown in Table 2. Note that the underlines in Tables 1 and 2 indicate that the results are outside the scope of the present invention, or outside the scope of the preferred manufacturing conditions and properties of the present invention. Inventive examples Nos. 1 to 16 and 30 to 38, in which the chemical composition, hardness, average crystal grain size, and radius of curvature after half-etching were within the prescribed ranges, all satisfied the strength, smoothness of the etched surface, and flatness before and after etching. In addition, in these inventive examples as well as the comparative examples described below, the radius of curvature of the steel sheet before half-etching was almost ∞ (infinity), and the steel sheet was adjusted to a flat shape without warping.
[0068] No. 17 had insufficient strength because the temperature for stress relief heat treatment was too high, and No. 18 had insufficient flatness before and after etching because the temperature for stress relief heat treatment was too low.
[0069] Nos. 19 and 20 are ferrite-austenite dual phases that are outside the chemical composition range of the present invention. No. 19 had insufficient strength due to an insufficient Mn content. No. 20 had insufficient strength due to an insufficient Ni content.
[0070] No. 21 and No. 22 are metastable austenitic stainless steels. No. 21 did not have a two-phase ferrite-austenite structure, and therefore had insufficient strength. No. 22 had a higher finish annealing temperature and a lower stress relief heat treatment temperature than No. 21, and therefore had a large average grain size and insufficient smoothness and flatness. In addition, No. 22 was made using steel type S and stress relief was performed at 700°C, so the processing-induced martensite formed during temper rolling did not reverse transform to austenite, and some of it remained. As a result, the ferrite phase ratio was 25%.
[0071] No. 23 and No. 24 are stable austenitic stainless steels. No. 23 was not strong because it did not have a two-phase ferrite-austenite structure. No. 24 was not flat enough before and after etching because the temperature of the stress relief heat treatment was too low compared to No. 23.
[0072] No. 25 and 26 are stable austenitic stainless steels with nitrogen added to increase strength. No. 25 does not have a ferrite-austenite two-phase structure, so it had insufficient strength despite having a relatively high N content. No. 26 had insufficient flatness before and after etching because the temperature of the stress relief heat treatment was too low compared to No. 25.
[0073] No. 27 is a ferritic stainless steel. Grain growth during finish annealing was rapid, resulting in coarsening of the average crystal grain size, and therefore the smoothness of the etched surface was insufficient. The strength was also insufficient.
[0074] For No. 28, the temperature of the final annealing was too high, which resulted in coarsening of the average crystal grain size and insufficient strength. For No. 29, the temperature of the final annealing was too low, which resulted in a metal structure with a mixture of recrystallized and non-recrystallized grains, resulting in variation in hardness between the crystal grains. As a result, good flatness could not be obtained after shape correction using a tension leveler, and as a result, half-etching tests could not be performed.
[0075] [Table 1]
[0076] [Table 2] [Industrial Applicability]
[0077] The ferritic-austenitic duplex stainless steel sheet of the present invention is stable in all respects: strength, flatness before and after etching, and smoothness of the etched surface. In other words, by using the ferritic-austenitic duplex stainless steel sheet of the present invention as a component material, it is expected that, for example, electronic devices and precision machinery that are etched during component manufacturing will become lighter and more compact.
Claims
1. Chemical composition, in mass%, C: 0.08% or less, Si: 0.1-1.0%, Mn: 1.0 to 5.0%, Cr: 20.0-28.0%, Ni: 1.0 to 7.0%, Mo: 0.1-2.0%, N: 0.10-0.30%, Cu: 0-2.0%, Nb: 0 to 0.50%, Ti: 0 to 0.50%, V: 0 to 0.50%, W: 0 to 0.50%, Co: 0 to 0.50%, B: 0 to 0.0050%, Sn: 0 to 0.50%, Al: 0-0.50%, Mg: 0 to 0.010%, Ca: 0-0.0100%, Ta: 0 to 0.050%, Ga: 0 to 0.050%, Zr: 0 to 0.50%, and Rare earth elements: 0-0.010% with the remainder being Fe and impurities, The average crystal grain size is 2.0 μm or less, A ferritic-austenitic duplex stainless steel sheet characterized by having a Vickers hardness of 400 HV or more.
2. 2. The ferritic-austenitic duplex stainless steel sheet according to claim 1, characterized in that in the metal structure, the ferritic phase ratio is 20 to 80%.
3. 3. The ferritic-austenitic duplex stainless steel sheet according to claim 1, wherein the radius of curvature after half etching is 150 mm or more.
4. 3. The ferritic-austenitic duplex stainless steel sheet according to claim 1 or 2, which is used for parts of electronic devices or precision devices.
5. The ferritic-austenitic duplex stainless steel sheet according to claim 3, which is used for parts of electronic devices or precision instruments.
Citation Information
Patent Citations
Dual-phase anti-corrosion stainless steel and corrosion resistance optimizing treatment process thereof
CN105385958A
Ferritic-austenitic stainless steel sheet having excellent press formability, and method for producing the same
JP2011184792A
Two phase stainless steel for ozone-containing water
JP2016191149A
Stainless steel
JP2019151901A
Ferritic-austenitic two-phase stainless steel material and method for manufacturing same
WO2017141907A1
Cited By
Economical duplex stainless steel for low-temperature storage tank and manufacturing method of middle plate of economical duplex stainless steel
CN120249809A