Positive electrode material for sodium battery and manufacturing method thereof

A sodium iron manganese titanium silicate-based positive electrode material with a carbon coating addresses the conductivity limitations of sodium iron silicate, enhancing capacity and cycle life in sodium batteries through a tailored manufacturing process.

JP2024137719AActive Publication Date: 2024-10-07HUBEI WANRUN NEW ENERGY TECH CO LTD

Patent Information

Application Number
JP2024012945
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-21
Filing Date
2024-01-31
Publication Date
2024-10-07
Estimated Expiration
2044-01-31

AI Technical Summary

Technical Problem

Current polyanion type positive electrodes for sodium batteries face challenges in realizing multi-electron reactions due to low intrinsic electronic conductivity, leading to limited energy output and slow charge exchange processes, with sodium iron silicate (Na2FeSiO4) having a theoretical capacity that is not fully realized in practice.

Method used

A positive electrode material composed of sodium iron manganese titanium silicate coated with a carbon layer, with a specific molecular formula NaqFexMny(TiO2)z(SiO4)m, is developed, where q, x, y, z, and m are within specified ranges, and a manufacturing process involving mixing, calcination, and vapor phase deposition of carbon is used to enhance conductivity and uniformity.

Benefits of technology

The solution results in a positive electrode material with improved specific capacity, enhanced ionic conductivity, and uniform carbon coating, facilitating a complete two-electron reaction and prolonged cycle life, suitable for sodium batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137719000004
    Figure 2024137719000004
  • Figure 2024137719000005
    Figure 2024137719000005
  • Figure 2024137719000006
    Figure 2024137719000006
Patent Text Reader

Abstract

To provide a positive electrode material for a sodium battery and a manufacturing method thereof, which can facilitate processing and at the same time improve battery capacity.SOLUTION: A cathode material is sodium iron manganese titanium silicate coated with a carbon layer, and the molecular formula of sodium iron manganese titanium silicate is NaqFexMny(TiO2)z(SiO4)m, where 1.5≤q≤2.5, 0.7≤x≤0.8, 0.2≤y≤0.3, 0.07≤z≤0.5, and 0.5≤m≤1.5 are satisfied. A method for manufacturing the cathode material includes a step (1) of mixing and calcining an iron source, a manganese source, a sodium source, and a solvent to obtain a precursor, and a step (2) of mixing the precursor with a silicate ester, a titanate, and an organic solvent to obtain a mixture, and calcining the mixture in the presence of an organic substance to obtain a sodium battery cathode material.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims priority to a Chinese patent application having application number 202310280551.7, filed on March 21, 2023, the entire contents of which are incorporated herein by reference.

[0002] The present invention relates to the technical field of positive electrode materials for sodium batteries, and more particularly to positive electrode materials for sodium batteries and methods for producing the same. [Background technology]

[0003] In recent years, sodium ion batteries have been attracting a lot of attention due to their abundant sodium resource reserves and similar working principle to lithium ion batteries, and are one of the new energy storage technologies that are expected to promote the low-cost application and sustainable development of energy storage technology. Polyanionic compounds are high-performance and high-safety positive electrode materials that have been widely studied, and the strong covalent bonds in their structures are favorable for stabilizing the structural frame, which can effectively improve the safety of the electrode during the charge and discharge process.

[0004] However, the currently reported polyanion-type positive electrodes have difficulty in realizing multi-electron reactions under the condition of a single polyanion group, and their energy exertion is significantly limited. Taking sodium iron silicate (Na2FeSiO4) as an example, it can theoretically realize two-electron reactions and has a high theoretical capacity of 276mAh / g, but due to the low intrinsic electronic conductivity of Na2FeSiO4, the charge exchange process in the electrode is slow, and within the safe voltage window of the electrolyte, the Na2FeSiO4 positive electrode cannot realize multi-electron reactions, so its actual capacity is much lower than the theoretical capacity.

[0005] Professor Jiang Yinzhu of Zhejiang University and his team designed the structural framework of sodium iron silicate and selected fluorine ions as a modifier to substitute oxygen sites. Kinetics-wise, fluorine ions can break the local charge balance in the Na2FeSiO4 structure and increase the electron transfer paths, thus promoting charge transfer. Thermodynamics-wise, the introduction of fluorine can increase the charge transfer rate of Fe 4+ To stabilize the intermediate phase containing Fe 3+ / Fe 4+ This is the first time that it has been proven that the redox reaction can be promoted. The specific capacity of the resulting fluorine-substituted sodium iron silicate positive electrode (NFSF) is as high as 271mAh / g, which allows a complete and reversible two-electron reaction to be realized. However, the manufacturing process in the above paper is relatively complicated, making it difficult to realize industrialization. Summary of the Invention

[0006] In view of this, the present invention aims to provide a cathode material for sodium batteries and a manufacturing method thereof, which is doped with titanium and manganese and coated with carbon, which can facilitate processing and at the same time improve the capacity of subsequent batteries.

[0007] To achieve the above objectives, the present invention uses the following technical solutions:

[0008] A sodium battery cathode material which is a sodium iron manganese titanium silicate coated with a carbon layer, the molecular formula of which is Na q Fe x Mn y( TiO2) z (SiO4) m where 1.5≦q≦2.5, 0.7≦x≦0.8, 0.2≦y≦0.3, 0.07≦z≦0.5, and 0.5≦m≦1.5.

[0009] The specific surface area of ​​the positive electrode material for sodium batteries of the present invention is 15-25 m 2 / g, preferably 19.75m 2 / g, the resistivity of the powder is 8-12 Ω cm, preferably 9.5 Ω cm, the D50 particle size of the sodium battery positive electrode material is 7-10 μm, preferably 7.8 μm, and the D90 particle size of the sodium battery positive electrode material is 20-30 μm, preferably 25.3 μm.

[0010] The tap density of the sodium battery positive electrode material of the present invention is 1-2 g / mL, preferably 0.95 g / mL;

[0011] The compressed density is 1-3 g / mL, preferably 2.15 g / mL; The thickness of the carbon layer is 2-3 nm, preferably 2.5 nm.

[0012] The molecular formula of the sodium iron manganese titanium silicate of the present invention is Na q Fe x Mn y Ti z (SiO4) m wherein 1.5≦q≦2.5, 0.7≦x≦0.8, 0.2≦y≦0.3, 0.07≦z≦0.5, 0.5≦m≦1.5, and preferably 1.8≦q≦2.0, 0.095≦z≦0.285, and 0.665≦m≦0.855.

[0013] The molecular formula of the sodium battery positive electrode material of the present invention is Na q Fe x Mn y( TiO2) z (SiO4) m / C, where 1.5≦q≦2.5, 0.7≦x≦0.8, 0.2≦y≦0.3, 0.07≦z≦0.5, and 0.5≦m≦1.5, and preferably 1.8≦q≦2.0, 0.095≦z≦0.285, and 0.665≦m≦0.855.

[0014] In one embodiment of the present invention, the molecular formula of sodium iron manganese titanium silicate is Na 1.97 Fe 0.77 Mn 0.25( TiO2) 0.25 (SiO4) 0.77The molecular formula of the positive electrode material for sodium batteries is Na 1.97 Fe 0.77 Mn 0.25( TiO2) 0.25 (SiO4) 0.77 / C.

[0015] The present invention further provides a method for producing a cathode material for a sodium battery, the method comprising the steps of: (1) mixing an iron source, a manganese source, a sodium source, and a solvent and calcining the mixture to obtain a precursor; and (2) mixing the precursor with a silicate ester, a titanate, and an organic solvent to obtain a mixture, and calcining the mixture in the presence of an organic substance to obtain a positive electrode material for a sodium battery.

[0016] In the present invention, the molar ratio of the iron source, manganese source, and sodium source is 1:(0.1-1):(5-10), preferably 1:(0.1-0.5):(7-10), and more preferably 1:0.45:7.

[0017] The mass ratio of the total mass of the iron source, manganese source and sodium source to the solvent is 1:(5-10), preferably 1:(4-8), and more preferably 1:6.

[0018] In the present invention, the molar ratio of sodium in the precursor, silicon in the silicate ester, and titanium in the titanate is 2:(0.7-0.9):(0.1-0.3), preferably 2:0.8:0.25, and the mass ratio of the precursor to the organic solvent is 1:(1-10), preferably 1:(3-5), more preferably 1:4.

[0019] In the step (2), the mass ratio of the organic material to the mixture is 1:(0.02-0.05), the organic material preferably participates in the calcination process in the form of gas, and the organic material is preferably n-propyl alcohol gas. The vapor deposition method can coat the surface of sodium iron manganese titanium silicate with carbon more uniformly.

[0020] In step (1) of the present invention, the precursor, the silicate ester, the titanate and the organic solvent are mixed to obtain a mixture, and the mixture is preferably pulverized, the pulverization method is pulverization, and the pulverization is performed until the particle size is 130 nm, and the pulverization temperature is ≦45° C.

[0021] Before carrying out the calcination, it is preferable to dry the mixture obtained by mixing the iron source, the manganese source, the sodium source, and the solvent, and the drying is preferably spray drying.

[0022] The sodium source is one or more of sodium nitrate, sodium hydroxide, sodium carbonate, sodium oxalate, sodium nitrite, disodium hydrogen phosphate, sodium bicarbonate, sodium citrate, anhydrous sodium sulfate, sodium stearate, sodium oleate, sodium tartrate, sodium alginate, sodium carboxymethylcellulose or sodium lactate, preferably sodium nitrate.

[0023] The iron source is one or more of ferrous nitrate, ferrous citrate, ferrous stearate, ferrous oleate, ferrous tartrate, ferrous alginate, ferrous carboxymethylcellulose or ferrous lactate, preferably ferrous nitrate.

[0024] The manganese source is one or more of manganese nitrate, manganese citrate, manganese stearate, manganese oleate, manganese tartrate, manganese alginate, manganese carboxymethylcellulose or manganese lactate, preferably manganese nitrate.

[0025] The silicate ester is one or more of isopropyl orthosilicate, ethyl orthosilicate or trimethylsiloxysilicate, preferably isopropyl orthosilicate.

[0026] The phthalate ester is one or more of tetraisopropyl titanate, tetrabutyl titanate, or tetraethyl titanate, preferably tetraisopropyl titanate.

[0027] Nitrates have the property of being easily decomposable, and can significantly lower the reaction temperature and shorten the reaction time, thereby making it possible to obtain particles with a small primary particle size and improve the subsequent reaction activity.

[0028] In the step (1) of the present invention, the calcination temperature is 650-750°C, preferably 700°C, the time is 4-6h, preferably 5h, after the calcination is completed, it is preferable to cool the material temperature to ≦80°C and then discharge the material, and the calcination temperature increase rate is preferably 2.5°C / h.

[0029] The exhaust gases generated during the calcination process are preferably absorbed with a sodium hydroxide solution to obtain a sodium nitrate solution, which can be reused.

[0030] In the step (2) of the present invention, the calcination temperature is 620° C. and the calcination time is 10-15 h; The calcination is divided into a heating stage, a temperature-holding stage and a temperature-lowering stage. During the heating process, the oxygen content in the furnace is maintained at less than 5 ppm, preferably by introducing nitrogen gas to maintain the oxygen content in the furnace at less than 5 ppm. The heating rate in the heating stage is 1.0-2.5 ° C. / h. In the incubation stage, organic gas was introduced into the system, and the incubation time was 11-14 h. In the cooling stage, the cooling rate is 1-1.5°C / h, and after the material temperature is lowered to ≦60°C, the cooling is stopped and then the material is discharged.

[0031] In one embodiment of the present invention, the organic gas is gaseous n-propyl alcohol, which is preheated to a vapor state.

[0032] In the present invention, the solvent is one or more of water, ethanol, and acetone, preferably water, and the organic solvent is one or more of ethanol, propanol, ethylene glycol, and acetone, preferably ethanol.

[0033] In the step (2) of the present invention, the mixture is dried to obtain a dried product; The drying is carried out in the presence of an inert gas, the inert gas is preferably nitrogen gas, the temperature of the nitrogen gas is 330-350°C, the drying process is preferably spray drying, the spray drying is preferably pressure spray drying, the gas pressure of the spray drying is 8-12 atmospheres, and the intake volume per unit time is 800-2000 times the volume of the slurry introduced; After the spray drying is completed, the spray-dried material and organic gas are introduced into a cyclone dust collection tower for solid-gas separation, the solid matter is collected, the nitrogen gas and organic gas are filtered through a dust collection cloth bag and then condensed, the organic solvent is recovered, and the nitrogen gas is recycled.

[0034] In the present invention, the total mass of the organic gas introduced is 0.002-0.006 times the mass of the spray-dried material, preferably 0.04 times.

[0035] In the step (2) of the present invention, it is preferable to grind the mixture before drying, using zirconia balls as grinding media, lowering the temperature with cooling water during the grinding process, maintaining the temperature of the organic solvent below 45°C, grinding until the particle size of the slurry reaches 130 nm, and obtaining a ground product.

[0036] In the present invention, the manufacturing method further includes, in the step (2), mixing the calcined material with an adhesive and a diluent, and performing spray granulation to obtain a positive electrode material for a sodium battery; The crushed material is preferably sieved through a 80-150 mesh sieve, and the calcined material is crushed, after which the iron is removed by electromagnetism, and then mixed with the adhesive and diluent, and the iron is removed until the content of magnetic substances is less than 1 ppm, when the iron removal is stopped; The adhesive is a polyurethane and the diluent is one or more of ethyl acetate, toluene, dimethylformamide, glycol ethers, and glycol esters.

[0037] The sodium battery positive electrode material obtained by the manufacturing method of the present invention has a particle size of 5-15 μm, a core-shell structure, the inner core is sodium iron manganese titanium silicate, and the surface of the sodium iron manganese titanium silicate is uniformly coated with a carbon layer of 2-3 nm.

[0038] The present invention further provides a battery comprising the above-mentioned sodium battery positive electrode material.

[0039] The present invention does not have any special requirements for the raw materials and manufacturing methods of other materials such as the negative electrode of the battery, and conventional raw materials and methods in this field can be used.

[0040] The beneficial effects of the present invention are as follows:

[0041] 1. A precursor is obtained by using an iron source, a manganese source, and a sodium source to produce a material in which manganese, iron, and sodium are uniformly mixed. By using a solution method, the iron ions, sodium ions, and manganese ions can be mixed at the atomic level. The mixture is then dried by spray drying and calcined at high temperature. Since the size range involved in the mixing is relatively small, the ion migration distance can be greatly reduced.

[0042] 2. In the design of the positive electrode material for sodium batteries, the present invention introduces silicate and titanium. The introduction of titanium can realize the doping of titanium, so as to improve the ionic conductivity and thereby improve the capacity. The introduction of titanium can also effectively consume the free sodium remaining on the surface of the material. Titanium and free sodium ions can form sodium titanate, which can improve the processing performance and further improve the capacity of the subsequent battery.

[0043] 3. The present invention uses silicate ester and titanate as raw materials, and silicate ester and titanate can be completely dissolved in organic solvent. After mixing silicate ester and titanate with precursor, spray drying, the mixture of precursor, silicate ester and titanate will crystallize and precipitate, and the mixing will be more complete, making the subsequent reaction more complete. At the same time, the thermal decomposition of the alkyl group in the organic matter can generate carbon source, so that the particle growth can be effectively restricted and a material with a small primary particle size can be obtained. From the viewpoint of coating effect, compared with the aspect of introducing additional carbon source, the carbon coating rate can be improved, so that the coating effect is higher. At the same time, in the organic system, the dispersibility of iron manganese titanium sodium silicate is excellent, so that the primary particle size of the final product is more uniform.

[0044] 4. In the present invention, during the pre-calcination temperature-retention stage, organic gas is introduced into the system by vapor deposition, and when there are ferrous ions at the sites not covered with carbon, i.e., the ferrous ions are exposed to the outside, the organic gas is catalytically decomposed at these sites into carbon, and the carbon adheres to these sites, thereby further improving the uniformity of the carbon coating.

[0045] 5. In the spray drying stage, the present invention controls the particle size, and the final product is not crushed but directly sieved, so that it can achieve the granulation of spherical particles with a particle size of 5-15 μm. Spray drying can improve the solid content when homogenizing the slurry in the final processing process, so as to improve the processing performance and reduce costs, and at the same time, it can also improve the pole piece compression density of the product. [Brief description of the drawings]

[0046] [Figure 1] FIG. 2 is an SEM image of the unground precursor after sintering in step (1) of Example 1. [Diagram 2] FIG. 2 is an SEM image of the precursor after sintering and grinding in step (1) of Example 1. [Diagram 3] FIG. 2 is an SEM image of the positive electrode material for a sodium battery obtained in Example 1. [Figure 4] FIG. 2 is a transmission electron microscope image of the crushed sodium battery positive electrode material obtained in Example 1. [Diagram 5] 2 is a charge / discharge curve of the sodium battery positive electrode material obtained in Example 1. [Figure 6] 1 is a cycle curve of the positive electrode material for a sodium battery obtained in Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0047] The technical solutions of the present invention will be described clearly and completely below with reference to the embodiments of the present invention. Of course, the described embodiments are only a part of the embodiments of the present invention, and are not all of the embodiments. Based on the embodiments of the present invention, any other embodiments that a person skilled in the art can think of without any creative effort are all within the scope of protection of the present invention.

[0048] In order to further illustrate the present invention, the following examples are provided in more detail. All of the raw materials used in the following examples of the present invention are commercially available products.

[0049] Electrochemical performance test: The compounding ratio (mass ratio) of the pole pieces was electrode material: conductive graphite: PVDF = 87:8:5.

[0050] A CR2025 button battery is manufactured using metallic sodium as the reference electrode, the negative electrode is sodium flakes, and the electrolyte is sodium hexafluorophosphate. The button battery is left at room temperature (25°C) for 10 hours, and then the button battery is charged and discharged to activate it. Then, a charge and discharge cycle test is performed on the button battery manufactured above using a battery charge and discharge tester manufactured by Aiden.

[0051] First, at room temperature (25°C), one cycle is performed at a magnification of 0.1C, then one cycle at a magnification of 0.2C, then one cycle at a magnification of 0.5C, and then one cycle at a magnification of 1C, where the charge / discharge voltage range of the control battery is detected in a voltage window of 1.0-4.5V.

[0052] Other performance tests Method for measuring tap density: Take 50g of material and place it in a calibrated 100mL measuring cylinder. Then, set the amplitude to 2cm and the vibration frequency to 5000 times, and calculate the density to be the tap density.

[0053] Method for measuring compressed density: Use an electronic compressed density meter to take 1g of material, then put it into a mold and press it under 3T pressure for 30s, then calculate the density as the compressed density. EXAMPLES

[0054] Example 1

[0055] (1) Mix iron nitrate, manganese nitrate, and sodium nitrate in a mass ratio of 0.75:0.25:1.9, add pure water to dissolve, mix uniformly, the total mass ratio of iron nitrate, manganese nitrate, and sodium nitrate to pure water is 1:6, then spray dry to obtain the spray material, heat up to 700 ° C at a rate of 2.5 ° C / h, calcinate for 5 h, then cool to a material temperature ≦ 80 ° C, discharge the material, the exhaust gas generated in the calcination process is absorbed with sodium hydroxide solution to obtain sodium nitrate solution, which is used back, the precursor can be obtained by the method of step (1), the main component of the precursor is a mixture of iron nitrate, manganese nitrate, and sodium nitrate. The performance detection data of the precursor is as shown in Table 1. The SEM of the precursor before and after grinding is shown in Figure 1 and Figure 2, respectively.

[0056] [Table 1]

[0057] (2) Mix the precursor, isopropyl orthosilicate, and tetraisopropyl titanate, the molar ratio of sodium in the precursor, silicon in the silicate ester, and titanium in the titanate is 2:0.8:0.25, add ethanol solvent, and the mass ratio of the precursor to ethanol is 1:4. Put it into a sand grinder and grind it, using zirconia balls as the grinding medium, and cool it with cold water during the grinding process, and keep the temperature of the organic solvent below 45°C, grind it until the particle size of the slurry is 130 nm, and obtain a ground product.

[0058] (3) The ground material is pressure spray-dried. In the spray-drying, nitrogen gas is used as a heating medium, and the nitrogen gas is heated to 330°C. Then, the nitrogen gas is introduced into the spray-drying tower to dry the spray droplets and gasify the organic solvent. Then, the spray-dried material and the organic gas are introduced into the cyclone dust-collecting tower for solid-gas separation, and the solid matter is collected. The nitrogen gas and the organic gas are filtered through a dust-collecting cloth bag, and then condensed to recover the organic solvent. The nitrogen gas is cycled. In the spray-drying process, the gas pressure of the pressure spray-drying is 9 atmospheres, and the intake volume per unit time is 1500 times the volume of the slurry introduced. The spray-dried material is obtained by the above steps. The D50 particle size of the spray-dried material is 9.2 μm.

[0059] (4) The spray-dried material is placed in an atmospheric furnace and calcined. The calcination is divided into a heating stage, a temperature-keeping stage and a temperature-reducing stage. In the temperature-keeping stage of the calcination process, nitrogen gas is introduced to maintain the oxygen content in the furnace below 5 ppm. The heating rate in the heating stage is 1.3°C / h. Then the temperature is increased to 620°C, and calcination is performed at this temperature for 13 h. Then the temperature is reduced, and the temperature-reducing rate is 1.4°C / h. After the material temperature is reduced to ≦60°C, the cooling is stopped, and the material is discharged. In the temperature-keeping stage, n-propyl alcohol is introduced into the system, and n- The propyl alcohol is heated to a vapor state in advance, and the gas pipe of the organic gas is inserted into the bottom of the charging sagger in the atmosphere furnace. The total mass of the organic gas introduced is 0.04 times the mass of the spray-dried material. After the material is cooled, it is crushed and then sieved through a 125 mesh sieve. The iron removal is stopped until the content of magnetic substances is less than 0.87 ppm. Then, the polyurethane adhesive and ethyl acetate are mixed, and then directly spray-granulated without grinding to obtain a spherical carbon-coated sodium battery positive electrode material, which has the molecular formula Na 1.97 Fe 0.77 Mn 0.25( TiO2) 0.25 (SiO4) 0.77 The powdered sodium battery positive electrode material was examined by a transmission electron microscope, and the results are shown in FIG. 4. It can be seen that the surface of the sodium iron manganese titanium silicate is coated with a carbon layer of about 2.5 nm, and the carbon layer is uniformly coated.

[0060] The sodium battery positive electrode material of the present invention was assembled into a battery, and the charge / discharge curve was as shown in FIG. 5, and the cycle curve was as shown in FIG.

[0061] [Table 2]

[0062] The data shows that the materials of the present invention have very high capacity and long cycle life.

[0063] Comparison 1

[0064] Referring to the steps and condition parameters in Example 1, the precursor obtained in step (1) is mixed with silicon dioxide and titanium dioxide, and ethanol is added, and a subsequent test is carried out, in which the molar ratio of sodium in the precursor, silicon in the silicon dioxide and titanium dioxide, and titanium in the titanate is 2:0.8:0.25. The performance test of the product obtained in this comparative example is shown in Table 3 below. It can be seen that the positive electrode material for sodium ion batteries made from the raw materials not only has a significantly reduced initial discharge efficiency, but also has a significantly reduced capacity retention rate at -20°C and room temperature.

[0065] [Table 3]

[0066] The above description of the disclosed embodiments enables those skilled in the art to realize or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Thus, the present invention is not intended to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. The sodium iron manganese titanium silicate is coated with a carbon layer, and the molecular formula of the sodium iron manganese titanium silicate is Na q Fe x Mn y( TiO 2 ) z (SiO 4 ) m wherein 1.5≦q≦2.5, 0.7≦x≦0.8, 0.2≦y≦0.3, 0.07≦z≦0.5, and 0.5≦m≦1.

5.

2. The specific surface area is 15-25m 2 2. The positive electrode material for a sodium battery according to claim 1, characterized in that the powder resistivity is 8-12 Ω·cm, and the D50 particle size is 7-10 μm.

3. 2. The positive electrode material for sodium batteries according to claim 1, characterized in that the tap density is 1-2 g / mL, the pressed density is 1-3 g / mL, and the thickness of the carbon layer is 2-3 nm.

4. (1) mixing an iron source, a manganese source, a sodium source, and a solvent and calcining the mixture to obtain a precursor; and (2) mixing the precursor with a silicate ester, a titanate, and an organic solvent to obtain a mixture, and calcining the mixture in the presence of an organic substance to obtain a positive electrode material for a sodium battery.

5. 5. The method for producing a positive electrode material for a sodium battery according to claim 4, wherein the molar ratio of the iron source, the manganese source, and the sodium source is 1:(0.1-1):(5-10).

6. the molar ratio of sodium in the precursor, silicon in the silicate ester, and titanium in the titanate is 2:(0.7-0.9):(0.1-0.3); 5. The method for producing a positive electrode material for a sodium battery according to claim 4, wherein the mass ratio of the organic material to the mixture is 1:(0.02-0.05).

7. the sodium source being one or more of sodium nitrate, sodium nitrite, sodium citrate, sodium stearate, sodium oleate, sodium tartrate, sodium alginate, sodium carboxymethylcellulose, or sodium lactate; the iron source being one or more of iron nitrate, iron citrate, iron stearate, iron oleate, iron tartrate, iron alginate, iron carboxymethylcellulose, or iron lactate; the manganese source is one or more of manganese nitrate, manganese citrate, manganese stearate, manganese oleate, manganese tartrate, manganese alginate, manganese carboxymethylcellulose, or manganese lactate; the silicate ester is one or more of isopropyl orthosilicate, ethyl orthosilicate, or trimethylsiloxysilicate; 5. The method for producing a positive electrode material for a sodium battery according to claim 4, wherein the titanate is one or more of tetraisopropyl titanate, tetrabutyl titanate, and tetraethyl titanate.

8. 5. The method for producing a positive electrode material for a sodium battery according to claim 4, wherein in step (1), the temperature of calcination is 650-750°C and the time is 4-6h, and in step (2), the temperature of calcination is 620°C and the time is 10-15h.

9. 5. The method for producing a positive electrode material for a sodium battery according to claim 4, further comprising: mixing the calcined material with an adhesive and a diluent in step (2), followed by spray granulation to obtain a positive electrode material for a sodium battery.

10. A battery comprising the sodium battery positive electrode material according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • Positive electrode material for lithium secondary battery, positive electrode for lithium secondary battery, and lithium secondary battery

    JP2012248283A

Cited By

  • Method for producing positive electrode active material for sodium-ion secondary batteries

    WO2026127118A1