Thick steel plate and method for producing the same
A chemically optimized thick steel plate with a controlled surface oxidation layer and manufacturing process addresses both laser cuttability and machinability issues, ensuring defect-free cutting and extended tool life.
Patent Information
- Application Number
- JP2024024776
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2024-02-21
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2044-02-21
AI Technical Summary
Existing thick steel plates face challenges in laser cuttability and machinability, particularly for plates thicker than 20 mm, with issues such as cutting defects, dross adhesion, and poor automation, and existing solutions do not adequately address both properties simultaneously.
A thick steel plate composition with controlled chemical elements and a surface oxidation layer, including specific ranges of C, Sb, Si, Mn, P, Al, N, B, and optional elements like Cu, Ni, Cr, Mo, W, V, Nb, Ti, REM, Ca, Mg, and Sn, combined with a manufacturing process involving hot rolling and descaling to achieve uniform scale adhesion and machinability.
The steel plate achieves excellent laser cutting performance with no cutting defects, reduced tool wear, and improved machinability, enhancing manufacturing efficiency and cutting quality.
Smart Images

Figure 2024137745000001 
Figure 2024137745000002 
Figure 2024137745000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a thick steel plate and a manufacturing method thereof, and more particularly to a thick steel plate having excellent laser cuttability and machinability and a manufacturing method thereof. [Background technology]
[0002] When thick hot-rolled steel plates are used for components such as dies and machine parts, they are generally cut or machined into the desired shape before assembly. The proportion of cutting and machining work in the machining process of steel structures is high, and there is a high demand for high efficiency and low cost of work. In addition, the shapes of steel structures are becoming more complex from the perspective of design, and the cut surface shapes are becoming more complex due to the omission of processes after cutting, so high precision is required for the cut surfaces. In addition, in the cutting process, it is required to process parts with the specified shape, precision, and roughness from the specified work material as cheaply as possible, including the replacement life of cutting tools and labor costs.
[0003] Conventionally, gas cutting and plasma cutting have been used as methods for cutting thick steel plates. Gas cutting is the most widely used method because it requires the lowest equipment installation costs and can cut even very thick steel plates. However, it is difficult to automate the control and monitoring of the gas flame, and the cutting speed is slow, making it less user-friendly.
[0004] Plasma cutting is capable of high-speed cutting up to a maximum thickness of about 50 mmt, but the torch has a life of only a few hours and requires frequent cutting, making it difficult to automate.
[0005] On the other hand, laser cutting is also being applied to cutting thick steel plates due to the high output and low cost of laser oscillators. The advantages of laser cutting are that it is easy to fully automate, the cutting heat input is small and the thermal impact is small, and the quality of the cut surface is good.
[0006] However, with the current laser output, the cutting stability drops sharply when the plate thickness is 20 mm or more. Although efforts are being made to improve cutting performance by further increasing the output of laser cutting machines, studies have been made on the laser cutting performance of the steel plate itself, i.e., how to prevent cutting defects.
[0007] Patent Document 1 describes a steel sheet with excellent laser cuttability, which has a specific chemical composition, a scale layer with an average thickness of 10 μm or less, and in which the scale layer contains 60 mass % or more of magnetite.
[0008] Patent Document 2 describes a thick steel plate with excellent laser cuttability in which the amounts of alloy elements such as Al, Cu, Ni, and Cr are controlled and the surface scale layer has an Al2O3-containing layer at the interface with the base steel.
[0009] Patent Document 3 describes a manufacturing method for thick steel plate with excellent laser cuttability, in which scale is removed by descaling at the start of rolling and the rolling end temperature is controlled to reduce the sum of the porosity in the scale and the peeling rate at the interface between the scale and the base steel to 15% or less.
[0010] Patent Document 4 describes a thick steel plate that contains a predetermined amount of Sb, has a surface oxide layer with a thickness of 15 μm or more and 50 μm or less, and has excellent laser cuttability.
[0011] Moreover, MnS free-cutting steel is known as an example of a steel material with excellent machinability (Non-Patent Document 1). [Prior art documents] [Patent documents]
[0012] [Patent Document 1] JP 2012-87339 A [Patent Document 2] Japanese Patent Application Publication No. 11-323478 [Patent Document 3] JP 2004-169093 A [Patent Document 4] Patent Publication No. 2022-054486 [Non-patent literature]
[0013] [Non-Patent Document 1] Chubu Kohan Co., Ltd. website, "Machinability improved steel plate," searched February 1, 2023, Internet,<URL:https: / / www.chubukohan.co.jp / product / standard / info / > Summary of the Invention [Problem to be solved by the invention]
[0014] In Patent Document 1, strict temperature control during rolling is required to obtain a thin scale containing 60 mass% or more of magnetite, and stable production is lacking. In Patent Document 2, adjustment of the amount of alloy elements is required to improve laser cuttability. In Patent Document 3, problems such as dross adhesion occur when laser cutting a plate thickness of 25 mm or more. In Patent Documents 1 to 3, machinability is not taken into consideration. In Patent Document 4, only improvement of laser cuttability is described, and machinability is not considered. In Non-Patent Document 1, although improvement of machinability is described, laser cuttability is lacking.
[0015] The present invention has been made in view of these circumstances, and has an object to provide a thick steel plate having excellent laser cuttability and machinability, and a method for manufacturing the same. [Means for solving the problem]
[0016] In order to achieve the above-mentioned object, the inventors have conducted extensive research into the influence of the steel plate's chemical composition, manufacturing method, and the thickness and adhesion of a surface oxide layer (hereinafter sometimes simply referred to as "scale") on laser cutting in order to ensure excellent laser cuttability of thick steel plate, and have obtained the following findings.
[0017] (1) When high-density energy is applied to thick steel plates by laser irradiation, thermal stress is generated, which destroys the surface scale and makes cutting defects more likely to occur. To prevent this, it is necessary to improve the adhesion of the scale.
[0018] (2) When a predetermined amount of Sb is contained to improve the adhesion of the scale, Sb is concentrated at the interface between the scale and the base steel. Although the inclusion of Si, Cu, and Ni is said to be effective in improving the adhesion of the scale, these elements are rather undesirable for the uniformity of the scale. Since Si, Cu, and Ni are locally concentrated at specific positions such as grain boundaries and cause differences in the growth rate of the scale, the scale becomes non-uniform when Si, Cu, and Ni are contained in excess. In the present invention, by setting the contents of Si, Cu, and Ni to a predetermined amount or less and containing a predetermined amount of Sb, Sb is concentrated at the interface between the scale and the base steel, and a scale with excellent adhesion and uniformity can be formed.
[0019] (3) By setting the thickness of the scale to 15 μm or more and 60 μm or less, cutting defects during laser cutting can be suppressed, the cut surface can be made smooth, and adhesion of dross can also be suppressed.
[0020] Furthermore, in order to ensure excellent machinability for thick steel plate, the inventors have conducted extensive research into the effects of the component composition and manufacturing method of the steel plate on machinability, and have obtained the following findings: Note that machinability is obtained by a comprehensive evaluation of tool wear, chip disposal, cutting resistance, cutting temperature, and adhesion, but when each individual evaluation item is excellent, it can naturally be said that the machinability is good.
[0021] (4) To reduce friction between the tool and the chip, it would be necessary to supply lubricant to the contact surface between the tool and the chip, but lubricant cannot be supplied to the contact surface because the contact surface is subject to high temperature and pressure. By adding B and N, or Ca and N in combination to the steel plate, it is possible to suppress tool wear and improve machinability by acting as a solid film that prevents direct contact between the tool and the back surface of the chip even under high temperature and pressure conditions.
[0022] The present invention was made based on the above findings and further investigations, and the gist of the present invention is as follows.
[0023] [1] In mass percent, C: more than 0.03% and less than 0.20%, Sb: 0.003 to 0.050%, Si: 0.60% or less, Mn: 0.10-2.50%, P:0.030% or less, S: 0.030% or less, Al: 0.150% or less, N: 0.02% or less, and B: More than 0.0030% and less than 0.0100% The remainder of the composition is Fe and unavoidable impurities. A thick steel plate having a surface oxide layer with a thickness of 15 μm to 60 μm. [2] The composition further includes, in mass%, Cu: 1.00% or less, Ni: 1.00% or less, Cr: 0.01 to 1.00%, Mo: 0.01 to 1.00%, W: 0.01 to 1.00%, V: 0.003~0.100%, Nb: 0.003 to 0.030%, Ti: 0.003 to 0.050%, REM: 0.0001~0.0030%, Ca: 0.0001 to 0.0030%, Mg: 0.0001 to 0.0030%, and Sn: 0.001 to 0.030% The steel plate according to [1], containing one or more selected from the following: [3] In mass percent, C: more than 0.03% and less than 0.20%, Sb: 0.003 to 0.050%, Si: 0.60% or less, Mn: 0.10-2.50%, P:0.030% or less, S: 0.030% or less, Al: 0.150% or less, N: 0.02% or less, and Ca: more than 0.0030% and less than 0.0100% The remainder of the composition is Fe and unavoidable impurities. A thick steel plate having a surface oxide layer with a thickness of 15 μm to 60 μm. [4] The composition further comprises, in mass%, Cu: 1.00% or less, Ni: 1.00% or less, Cr: 0.01 to 1.00%, Mo: 0.01 to 1.00%, W: 0.01 to 1.00%, V: 0.003~0.100%, Nb: 0.003 to 0.030%, Ti: 0.003 to 0.050%, REM: 0.0001~0.0030%, B: 0.0001~0.0030%, Mg: 0.0001 to 0.0030%, and Sn: 0.001 to 0.030% The steel plate according to [3], containing one or more selected from the following: [5] The steel plate according to any one of [1] to [4], wherein the standard deviation of the thickness of the surface oxide layer is 5.0 μm or less. [6] A method for producing a thick steel plate, comprising heating a steel material having a chemical composition according to any one of [1] to [4] above to 1000 to 1200°C, and then performing hot rolling at a rolling end temperature of 700 to 1000°C, in which descaling is performed five or more times by spraying water onto at least one side of the steel plate during a rolling pass in a temperature range from (rolling end temperature + 100°C) to the rolling end temperature. Effect of the Invention
[0024] According to the present invention, it is possible to provide a thick steel plate having excellent laser cuttability and machinability.
[0025] The thick steel plate of the present invention provides excellent workability and cutting quality when laser cut, and further provides excellent machinability and tool life in cutting. Specifically, it has excellent cutting properties, such as no cutting defects such as notches on the cross section of the steel plate after laser cutting and no dross adhesion on the back surface of the steel plate, and it has excellent machinability, such that the workpiece (thick steel plate) is easy to cut during cutting processing, the cutting tool is less likely to wear, and the cutting chips are easy to dispose of. Use of the steel plate of the present invention contributes greatly to improving the manufacturing efficiency when manufacturing steel structures, and provides significant industrial benefits. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] The present invention will be described in detail below. Note that the following description shows examples of preferred embodiments of the present invention, and the present invention is not limited thereto.
[0027] The steel plate (base steel of the steel plate) of the present invention has a chemical composition according to the first or second embodiment shown below. The reasons for limiting each chemical composition will be explained below. Note that "%" in relation to the chemical composition means "mass %" unless otherwise specified.
[0028] [Component composition of the first embodiment] The steel plate according to the first embodiment of the present invention has a composition containing, in mass%, C: more than 0.03% and not more than 0.20%, Sb: 0.003 to 0.050%, Si: 0.60% or less, Mn: 0.10 to 2.50%, P: 0.030% or less, S: 0.030% or less, Al: 0.150% or less, N: 0.02% or less, and B: more than 0.0030% and not more than 0.0100%, with the balance being Fe and unavoidable impurities.
[0029] The composition may further contain, in mass%, one or more selected from Cu: 1.00% or less, Ni: 1.00% or less, Cr: 0.01 to 1.00%, Mo: 0.01 to 1.00%, W: 0.01 to 1.00%, V: 0.003 to 0.100%, Nb: 0.003 to 0.030%, Ti: 0.003 to 0.050%, REM: 0.0001 to 0.0030%, Ca: 0.0001 to 0.0030%, Mg: 0.0001 to 0.0030%, and Sn: 0.001 to 0.030%.
[0030] C: More than 0.03% and less than 0.20% C is an element necessary for increasing the strength of steel and ensuring the strength required for a thick steel plate. To obtain this effect, it is necessary to contain C in an amount of more than 0.03%. The C content is preferably 0.04% or more, and more preferably 0.10% or more. On the other hand, if the C content exceeds 0.20%, the toughness is deteriorated and the weldability is reduced. For this reason, the C content is set to 0.20% or less. The C content is preferably 0.18% or less.
[0031] Sb: 0.003 to 0.050% Sb is an element necessary for improving scale adhesion. Sb diffuses to the surface during the steel material heating to hot rolling, and is uniformly concentrated at the interface between the scale (surface oxide layer) and the base steel. This concentrated layer makes the scale less likely to peel off. Furthermore, by uniformly concentrating, there is no local difference in the scale growth rate, and the uniformity of the scale is not hindered. As a result, the desired laser cuttability is obtained. In order to obtain this effect, it is necessary to contain Sb at 0.003% or more. The Sb content is preferably 0.005% or more. On the other hand, if the Sb content exceeds 0.050%, scratches are likely to occur on the surface of the thick steel plate, deteriorating the laser cuttability. Therefore, the Sb content is 0.050% or less. The Sb content is preferably less than 0.030%, and more preferably 0.020% or less.
[0032] Si:0.60% or less Silicon is an element that acts as a deoxidizer. However, if the silicon content exceeds 0.60%, the toughness of the base material and the cold cracking resistance of the welded portion may be significantly deteriorated. For this reason, the silicon content is set to 0.60% or less. The silicon content is preferably set to 0.40% or less. The lower limit of the silicon content is not particularly limited, but the silicon content is preferably 0.01% or more.
[0033] Mn: 0.10-2.50% Mn has the effect of increasing the hardenability of steel, and is contained at 0.10% or more in order to ensure the strength of the base material. The Mn content is preferably 0.20% or more, and more preferably 1.30% or more. On the other hand, if the Mn content exceeds 2.50%, the toughness, ductility, and weldability of the base material may be significantly deteriorated. For this reason, the Mn content is set to 2.50% or less. The Mn content is preferably set to 2.00% or less.
[0034] P:0.030% or less P exists in steel as an impurity, and by segregating at grain boundaries, it may have adverse effects such as deteriorating the low-temperature toughness and ductility of the base material. For this reason, it is desirable to keep the P content as low as possible, but 0.030% or less is acceptable. Therefore, the P content is set to 0.030% or less. There is no particular lower limit for the P content, but reducing it to less than 0.001% is difficult in industrial-scale production. For this reason, from the viewpoint of productivity, it is preferable to set the P content to 0.001% or more.
[0035] S: 0.030% or less S is present in steel as sulfide-based inclusions such as MnS, and may have adverse effects such as deteriorating the low-temperature toughness and ductility of the base material, so it is desirable to reduce the S content as much as possible. On the other hand, when a certain amount of S is contained, MnS present in the steel is softer than the base material at high temperatures, and is stretched during deformation in the shear region, acting as a stress concentration point, which reduces the deformation resistance in the shear deformation region of the tool cutting edge and the workpiece material, thereby improving machinability. However, the toughness in the C direction decreases with an increase in the S content. In consideration of the above, the S content is set to 0.030% or less. The lower limit of the S content is not particularly limited, but it is difficult to reduce it to less than 0.001% in industrial-scale production. For this reason, from the viewpoint of productivity, it is preferable to set the S content to 0.001% or more.
[0036] Al: 0.150% or less Al acts as a deoxidizer and fixes N in steel as AlN, which contributes to improving the toughness of the base material and welded parts. In cutting, Al acts to prevent diffusion and adhesion between the tool and the back side of the chip in the workpiece, and at the same time, it has the property of firmly adhering to the tool surface as a film during cutting. However, if the Al content exceeds 0.150%, the toughness of the base material may decrease. Therefore, the Al content is set to 0.150% or less. The Al content is preferably set to 0.110% or less. The lower limit of the Al content is not particularly limited, but the Al content is preferably 0.015% or more.
[0037] N: 0.02% or less N is an element that exists in steel as an impurity. If the N content exceeds 0.02%, the toughness of the base material may be significantly reduced. On the other hand, N in steel is fixed as AlN by Al and contributes to improving machinability, so it is preferable to include an appropriate amount. For this reason, the N content is set to 0.02% or less. In addition, the N content is preferably 0.001% or more.
[0038] B: More than 0.0030% and less than 0.0100% At high temperatures such as during cutting, Al and BN in steel generate AlN, and the presence of an AlN film on the tool wear surface suppresses the diffusion reaction between the tool and the workpiece, reducing tool wear. This effect is greater as the B content is greater. In addition, B is an element that acts to increase the strength of steel through improving hardenability. In order to obtain these effects, the B content is made to exceed 0.0030%. Preferably, the B content is made to exceed 0.0050%, and more preferably, to be 0.0055% or more. On the other hand, if the B content exceeds 0.0100%, the hardenability is significantly increased, and the toughness and ductility of the base material are deteriorated. In addition, if the B content exceeds 0.0100% and the ratio of the N content to the B content (N / B ratio) becomes small, the B that exists in a free state in the steel remains, and the machinability is deteriorated. For this reason, the B content is made to be 0.0100% or less. The B content is preferably made to be 0.0080% or less.
[0039] The steel plate according to the first embodiment of the present invention may have the above-mentioned components as the basic components, with the balance being Fe and unavoidable impurities.
[0040] The chemical composition of the steel plate according to the first embodiment of the present invention may further contain, in addition to the above-mentioned chemical composition, one or more of Cu, Ni, Cr, Mo, W, V, Nb, Ti, REM, Ca, Mg and Sn, each in the following content ranges.
[0041] Cu: 1.00% or less Cu is an element that contributes to improving the strength of thick steel plate. In order to obtain this effect, when Cu is contained, the Cu content is preferably 0.01% or more. On the other hand, when the Cu content exceeds 1.00%, hot brittleness may occur and the surface properties of the steel plate may be significantly deteriorated. Therefore, when Cu is contained, the Cu content is preferably 1.00% or less.
[0042] Ni: 1.00% or less Ni is an element that contributes to improving the strength of thick steel plate. In order to obtain this effect, when Ni is contained, the Ni content is preferably 0.01% or more. On the other hand, when the Ni content exceeds 1.00%, the scale thickness becomes significantly non-uniform, and the laser cuttability deteriorates. For this reason, when Ni is contained, the Ni content is preferably 1.00% or less.
[0043] Cr: 0.01~1.00% Cr is an element that contributes to improving the strength of thick steel plate. In order to obtain this effect, when Cr is contained, the Cr content is preferably 0.01% or more. On the other hand, when Cr is contained in excess of 1.00%, the toughness, ductility, and weldability of the base material may be significantly deteriorated. For this reason, when Cr is contained, the Cr content is preferably 1.00% or less.
[0044] Mo: 0.01 to 1.00% Mo is an element that contributes to improving the strength of thick steel plate. In order to obtain this effect, when Mo is contained, the Mo content is preferably 0.01% or more. On the other hand, if the Mo content exceeds 1.00%, it may have an adverse effect on the base material toughness, ductility, and weld crack resistance. Therefore, when Mo is contained, the Mo content is preferably 1.00% or less.
[0045] W: 0.01 to 1.00% W is an element that contributes to improving the strength of thick steel plate. In order to obtain this effect, when W is contained, the W content is preferably 0.01% or more. On the other hand, when the W content exceeds 1.00%, it may have an adverse effect on the base material toughness, ductility, and weld crack resistance. For this reason, when W is contained, the W content is preferably 1.00% or less.
[0046] V: 0.003~0.100% V is an element that greatly contributes to improving the strength of thick steel plate. In order to obtain this effect, when V is contained, the V content is preferably 0.003% or more. On the other hand, when the V content exceeds 0.100%, there is a risk of deteriorating the toughness and ductility of the base material. For this reason, when V is contained, the V content is preferably 0.100% or less.
[0047] Nb: 0.003 to 0.030% Nb is an element that greatly contributes to improving the strength of thick steel plate. In order to obtain this effect, when Nb is contained, the Nb content is preferably 0.003% or more. The Nb content is preferably 0.005% or more. On the other hand, when the Nb content exceeds 0.030%, the base material toughness and ductility are deteriorated. Therefore, when Nb is contained, the Nb content is preferably 0.030% or less.
[0048] Ti: 0.003~0.050% Ti is an element that has a strong affinity with N and precipitates as TiN during solidification, suppressing the coarsening of austenite grains in the heat-affected zone of welding, thereby contributing to high toughness. In order to obtain this effect, when Ti is contained, the Ti content is preferably 0.003% or more. On the other hand, when the Ti content exceeds 0.050%, the TiN particles may coarsen, deteriorating the toughness of the base material and the welded zone. Therefore, when Ti is contained, the Ti content is preferably 0.050% or less.
[0049] REM:0.0001~0.0030%, Mg:0.0001~0.0030% Both REM and Mg combine with S to control the morphology of sulfides, thereby contributing to improving the toughness of steel. In order to obtain this effect, when these elements are contained, it is preferable that each content is 0.0001% or more. On the other hand, even if each of these elements is contained in an amount exceeding 0.0030%, the effect is saturated. Therefore, when these elements are contained, it is preferable that each content is 0.0030% or less. Here, REM (rare earth metal) is a general term for a total of 17 elements, including Sc, Y, and lanthanoid elements. One or more of these 17 elements can be contained in steel, and the REM content means the total content of these elements.
[0050] Ca: 0.0001 to 0.0030% Ca combines with S to control the morphology of sulfides, thereby contributing to improving the toughness of steel. In order to obtain this effect, when Ca is contained, the Ca content is preferably 0.0001% or more. On the other hand, even if the Ca content exceeds 0.0030%, the effect saturates. Therefore, when Ca is contained, the Ca content is preferably 0.0030% or less.
[0051] Sn: 0.001 to 0.030% Sn contributes to improving corrosion resistance. In order to obtain this effect, when Sn is contained, the Sn content is preferably 0.001% or more. On the other hand, when the Sn content exceeds 0.030%, there is a risk of deteriorating toughness. Therefore, when Sn is contained, the Sn content is preferably 0.030% or less.
[0052] In addition, when the content of Cu, Ni, Cr, Mo, W, V, Nb, Ti, REM, Ca, Mg, or Sn described above as optional components is less than the lower limit (however, in the case of Cu and Ni, when the content is less than 0.01%), the component is considered to be included as an unavoidable impurity.
[0053] [Component composition of the second embodiment] The steel plate according to the second embodiment of the present invention has a composition containing, in mass%, C: more than 0.03% and not more than 0.20%, Sb: 0.003 to 0.050%, Si: 0.60% or less, Mn: 0.10 to 2.50%, P: 0.030% or less, S: 0.030% or less, Al: 0.150% or less, N: 0.02% or less, and Ca: more than 0.0030% and not more than 0.0100%, with the balance being Fe and unavoidable impurities.
[0054] The composition may further contain, in mass%, one or more selected from Cu: 1.00% or less, Ni: 1.00% or less, Cr: 0.01 to 1.00%, Mo: 0.01 to 1.00%, W: 0.01 to 1.00%, V: 0.003 to 0.100%, Nb: 0.003 to 0.030%, Ti: 0.003 to 0.050%, REM: 0.0001 to 0.0030%, B: 0.0001 to 0.0030%, Mg: 0.0001 to 0.0030%, and Sn: 0.001 to 0.030%.
[0055] The reasons for limiting the composition of the steel plate according to the second embodiment of the present invention to C: more than 0.03% and not more than 0.20%, Sb: 0.003 to 0.050%, Si: 0.60% or less, Mn: 0.10 to 2.50%, P: 0.030% or less, S: 0.030% or less, Al: 0.150% or less, and N: 0.02% or less are the same as those for the first embodiment described above.
[0056] Ca: more than 0.0030% and less than 0.0100% Ca combines with S to control the morphology of sulfides, thereby contributing to improving the toughness of steel. It also acts as a deoxidizer, and when the Ca content is 0.0020% or more and the Al content is 0.150% or less, a protective film (Belaag) is formed on the tool surface, reducing tool wear. On the other hand, even if the Ca content exceeds 0.0100%, the effect of reducing tool wear tends to saturate, so the upper limit of the Ca content is set to 0.0100%. Furthermore, if the Ca content exceeds 0.0100%, the proportion of CaS, which has a higher melting point than MnS, increases, reducing machinability. Therefore, the Ca content is set to 0.0100% or less. Also, if the Ca content is too low, the effect of reducing tool wear is low, so the Ca content is set to more than 0.0030%.
[0057] The steel plate according to the second embodiment of the present invention may have the above-mentioned components as the basic components, with the balance being Fe and unavoidable impurities.
[0058] The chemical composition of the steel plate according to the second embodiment of the present invention may further contain, in addition to the above-mentioned chemical composition, one or more of Cu, Ni, Cr, Mo, W, V, Nb, Ti, REM, B, Mg and Sn, each in the following content ranges.
[0059] In the chemical composition of the steel plate according to the second embodiment of the present invention, when one or more selected from Cu: 1.00% or less, Ni: 1.00% or less, Cr: 0.01 to 1.00%, Mo: 0.01 to 1.00%, W: 0.01 to 1.00%, V: 0.003 to 0.100%, Nb: 0.003 to 0.030%, Ti: 0.003 to 0.050%, REM: 0.0001 to 0.0030%, Mg: 0.0001 to 0.0030%, and Sn: 0.001 to 0.030% are contained, the reasons for limiting the content of each of the above-mentioned components are the same as those for the first embodiment described above.
[0060] B: 0.0001 to 0.0030% B is an element that has the effect of increasing the strength of steel by improving hardenability. In order to obtain this effect, when B is contained, the B content is preferably 0.0001% or more. On the other hand, even if the B content exceeds 0.0030%, the effect is saturated. Therefore, when B is contained, the B content is preferably 0.0030% or less.
[0061] In addition, when the content of Cu, Ni, Cr, Mo, W, V, Nb, Ti, REM, B, Mg, or Sn described above as optional components is less than the lower limit (however, in the case of Cu and Ni, when the content is less than 0.01%), the component is considered to be included as an unavoidable impurity.
[0062] [Preferable ranges for Si, Cu, and Ni] In the thick steel plate according to the present invention, the contents of Si, Cu, and Ni are preferably set to Si: 0.10% or less, Cu: 0.03% or less, and Ni: 0.03% or less, respectively. In addition to the effect of adding Sb, by strictly controlling the contents of Si, Cu, and Ni to be equal to or less than a predetermined amount, the standard deviation of the thickness of the surface oxide layer can be set to 5.0 μm or less, as described below. This makes it possible to further uniformize the thickness of the surface oxide layer. As a result, the laser cuttability can be further improved.
[0063] Si: 0.10% or less (preferable range) Since Si is an easily oxidized element and is easily incorporated into the scale, it is desirable to keep the Si content as low as possible in order to make the scale uniform. From this perspective, a Si content of 0.10% or less is acceptable. From the viewpoint of deoxidization, a Si content of 0.01% or more is preferable. In addition, the melting point (around 1700°C) of SiO2 (silicon oxide) formed by the oxidation of Si is higher than the melting point of iron (1536°C), and the generation of SiO2 reduces the fluidity of the molten metal during laser cutting, increasing the roughness of the cut surface, which is thought to be one of the factors that develop into burning. Considering this point, a low Si content is preferable.
[0064] Cu: 0.03% or less (preferable range), Ni: 0.03% or less (preferable range) As with Si, it is desirable to keep the Cu and Ni contents as low as possible in order to make the scale uniform. From this point of view, when Cu and Ni are contained, the Cu and Ni contents are each permissible if they are 0.03% or less. From this point of view, the Cu and Ni contents may be 0%.
[0065] [Surface oxide layer] The surface oxide layer (scale) of the thick steel plate of the present invention is an oxide layer formed by oxidizing the surface of the thick steel plate during the manufacturing of the thick steel plate. The surface oxide layer has a higher absorption rate of laser light than the Fe of the base material (base steel), and also serves as a source of oxygen required during cutting, so it is a necessary layer for laser cutting. In order to increase the absorption energy of the laser light and improve the cutting efficiency, the thickness of the surface oxide layer is set to 15 μm or more. The thicker the surface oxide layer is, the higher the laser absorption energy is. However, if the surface oxide layer is too thick, it is likely to peel off at the interface between the surface oxide layer and the base steel, and the thickness of the surface oxide layer is likely to become uneven, deteriorating the laser cuttability. For this reason, the thickness of the surface oxide layer is set to 60 μm or less.
[0066] In order to ensure stable laser cutting performance, it is preferable to make the standard deviation of the thickness of the surface oxide layer 5.0 μm or less in order to make the thickness of the surface oxide layer uniform. In order to make the standard deviation of the thickness of the surface oxide layer 5.0 μm or less, as described above, the contents of Si, Cu, and Ni are controlled to predetermined values. Here, ensuring stable laser cutting performance means, for example, that there is no notch or dross attached to the cut surface, and cutting is possible even when the laser cutting speed is high.
[0067] The thickness and standard deviation of the surface oxide layer can be measured by the method shown in the Examples.
[0068] Plate Thickness The thickness of the thick steel plate of the present invention is not particularly limited and can be any thickness. As an example, the thickness of the thick steel plate of the present invention is 4.5 mm or more. As another example, the thickness of the thick steel plate of the present invention is 32 mm or less. In the present invention, the thickness of the thick steel plate is preferably 4.5 to 32 mm, since excellent cutting quality can be obtained, particularly when cutting with a laser, for a thick steel plate having a thickness of 4.5 to 32 mm.
[0069] [Manufacturing method] Next, a manufacturing method of the thick steel plate of the present invention will be described. The thick steel plate of the present invention can be manufactured by heating a steel material having the composition of the first or second embodiment described above, and performing descaling under predetermined conditions on the surface oxide layer generated during hot rolling. Specifically, in a manufacturing method of one embodiment of the thick steel plate of the present invention, a steel material having the above composition is heated to 1000 to 1200°C, and then hot rolling is performed at a rolling end temperature of 700 to 1000°C, and descaling is performed five or more times by spraying water on at least one side of the steel plate during a rolling pass in a temperature range of (rolling end temperature + 100°C) to the rolling end temperature. In the following description, the indication of "°C" regarding temperature means the temperature of the surface layer of the thick steel plate. The temperature can be measured by a surface thermometer or the like.
[0070] Heating temperature of steel material: 1000~1200℃ If the heating temperature of the steel material is less than 1000°C, the deformation resistance in hot rolling is high, and the reduction amount per pass cannot be large. As a result, the number of rolling passes increases, which leads to a decrease in rolling efficiency and the casting defects in the steel material (slab) cannot be pressed. On the other hand, if the heating temperature exceeds 1200°C, surface defects are likely to occur due to excessive high-temperature scale generated during heating, the maintenance load after rolling increases, and the crystal grains become coarse, deteriorating the brittleness and ductility of the base material. For this reason, the heating temperature of the steel material is set to a range of 1000 to 1200°C. In addition, the present invention can adopt a conventional method in which the steel material is cooled to room temperature after production and then heated again. In addition to this, the steel material is charged into the heating furnace as a hot piece without being cooled to room temperature, or direct rolling in which the steel material is immediately rolled after a short period of heat retention can also be applied.
[0071] Rolling end temperature: 700~1000℃ If the rolling end temperature of hot rolling exceeds 1000°C, not only will blisters occur in the surface oxide layer, but the surface oxide layer will grow excessively during the cooling process after the rolling is completed. As a result, the surface oxide layer of the desired thickness cannot be obtained. In addition, the structure will become coarse, resulting in deterioration of toughness. On the other hand, if the rolling end temperature is lower than 700°C, the deformation resistance will be too high, the rolling load will increase, and the burden on the rolling machine will become large. In addition, in order to lower the rolling temperature, it is necessary to wait in the middle of rolling, which not only significantly impedes productivity, but also because the steel plate temperature is low, the surface oxide layer will not grow and will become thin, and the surface oxide layer of the desired thickness cannot be obtained. Furthermore, since the strain accumulated in the thick steel plate will increase, the thick steel plate will deform during laser cutting, causing problems such as a decrease in cutting accuracy and cutting stopping midway. For this reason, the rolling end temperature is set to the range of 700 to 1000°C.
[0072] Descaling during rolling passes in the temperature range from (rolling end temperature + 100°C) to the rolling end temperature: 5 times or more In the present invention, in order to stably generate a surface oxide layer of the desired thickness, it is important to strictly control the number of descalings during rolling. In the present invention, the number of descalings is set to 5 or more during a rolling pass in the temperature range from (rolling end temperature + 100°C) to the rolling end temperature. If the number of descalings in the above temperature range is less than 5, the surface oxide layer that is generated and grows during rolling is not sufficiently peeled off, and the surface oxide layer grows excessively. Furthermore, the surface oxide layer peels off locally, which increases the variation in thickness of the surface oxide layer.
[0073] Descaling can be performed by spraying water on at least one surface of the steel plate. When descaling is performed, descaling is usually performed once before or after one rolling pass or during rolling. Descaling is preferably performed with a water spray pressure of 10 MPa or more. EXAMPLES
[0074] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the following examples.
[0075] Steel materials (steel slabs) prepared to various component compositions shown in Tables 1 and 2 using the converter-ladle refining-continuous casting process were made into 25 mm thick steel plates using various hot rolling conditions shown in Tables 3 to 5. Descaling was performed on both sides of the steel plates with a water injection pressure of 15 MPa. Note that blanks in Tables 1 and 2 indicate that the element was not intentionally added, and include not only cases where the element is not contained (0%) but also cases where the element is unavoidably contained.
[0076] Six samples of 20 mm × 20 mm × plate thickness were taken from the positions 500 mm from the leading end, center, and tail end of the obtained steel plate in the longitudinal direction, respectively at the 1 / 4 and 1 / 2 positions in the plate width direction, one for each steel type. Each sample was embedded in carbon resin so that the cross section parallel to the rolling direction was the observation surface, and polished to a mirror finish. Five optical microscope photographs were taken at 400 times magnification of the area including the base steel and the surface oxide layer, and the thickness of the surface oxide layer (scale thickness) was measured at 10 arbitrary points on each photograph using an image analyzer. The average value of the measurements for all six samples was taken as the thickness of the surface oxide layer. The standard deviation of the measurements for all six samples was taken as the standard deviation of the thickness of the surface oxide layer. The presence or absence of an Sb-enriched layer was evaluated by performing Sb mapping analysis using an electron beam microanalyzer (accelerating voltage 15 kV) on the above cross-sectional sample in an area of 20 μm × 30 μm including the interface between the surface oxide layer and the base steel. Specifically, the presence of Sb at the interface was judged to indicate the presence of an Sb-enriched layer.
[0077] Regarding the tensile properties, in accordance with JIS Z2241:2022, one JIS No. 1A test piece was taken from the C direction (perpendicular to the rolling direction) of the thick steel plate, and a tensile test was carried out to determine the yield strength and tensile strength. The tensile strength is preferably 400 MPa or more.
[0078] Regarding toughness, in accordance with JIS Z 2242:2018, three test pieces were taken from the 1 / 4 position of the plate thickness (t) so that the notch direction was in the L direction (parallel to the rolling direction) (test piece: 2 mm V notch, size: 10 mm x 10 mm), and a Charpy impact test was performed. The absorbed energy vE0℃ at the test temperature of 0℃ was obtained to evaluate the impact properties. vE0℃ is preferably 27 J or more. The absorbed energy value was the average value of the three test pieces.
[0079] The laser cuttability was evaluated by cutting a thick steel plate using a 6kW carbon dioxide laser, and visually checking the presence or absence of a notch on the cross section of the thick steel plate after cutting, and the presence or absence of dross on the back surface of the thick steel plate. The cutting test conditions were an oxygen pressure of 0.3kgf / cm 2The evaluation was performed with a cutting length of 500 mm and cutting speeds of 750 mm / min and 900 mm / min. "Cuttable" was determined based on whether the plate could be separated regardless of the state of the cut surface. Specifically, plates that could not be separated due to reasons such as the cutting being stopped midway were deemed "uncuttable." The results are shown in Tables 3 to 5. In this test, plates that could be cut at a cutting speed of 750 mm / min, had no notches on the cross section of the thick steel plate after cutting, and had no dross attached to the back surface of the thick steel plate were evaluated as having excellent laser cuttability (good) and were deemed to have passed.
[0080] Machinability was evaluated by conducting a cutting (peripheral turning) test. The tool material was carbide tool P20, and the cutting conditions were feed 0.20 mm / rev, depth of cut 2.0 mm, cutting speed 150 m / min, no lubrication. Tool life was evaluated as the cutting time at which the flank wear width VB = 0.2 mm. In this test, a tool life of 20 min or more was evaluated as excellent (good) machinability and was deemed to have passed. The results are shown in Tables 3 to 5.
[0081] All of the examples of the present invention were excellent in laser cuttability and machinability. Furthermore, all of the examples of the present invention had excellent strength with a tensile strength of 400 MPa or more and excellent toughness with a vE0℃ of 27 J or more. Furthermore, those with a standard deviation of scale thickness of 5.0 μm or less could be cut even under conditions of a cutting speed of 900 mm / min, ensuring stable laser cuttability, and having no notches on the cross section of the thick steel plate after cutting and no dross adhesion on the back surface of the thick steel plate, showing particularly excellent laser cuttability.
[0082] [Table 1]
[0083] [Table 2]
[0084] [Table 3]
[0085]
Table 4
[0086]
Table 5
Claims
1. In mass percent, C: more than 0.03% and less than 0.20%, Sb: 0.003 to 0.050%, Si: 0.60% or less, Mn: 0.10 to 2.50%, P: 0.030% or less, S: 0.030% or less, Al: 0.150% or less, N: 0.02% or less, and B: More than 0.0030% and less than 0.0100% The balance is Fe and unavoidable impurities, A thick steel plate having a surface oxide layer having a thickness of 15 μm or more and 60 μm or less.
2. The composition further includes, in mass%, Cu: 1.00% or less, Ni: 1.00% or less, Cr: 0.01-1.00%, Mo: 0.01-1.00%, W: 0.01-1.00%, V: 0.003-0.100%, Nb: 0.003 to 0.030%, Ti: 0.003 to 0.050%, REM: 0.0001-0.0030%, Ca: 0.0001-0.0030%, Mg: 0.0001 to 0.0030%, and Sn: 0.001-0.030% The steel plate according to claim 1, comprising one or more selected from the following:
3. In mass percent, C: more than 0.03% and less than 0.20%, Sb: 0.003 to 0.050%, Si: 0.60% or less, Mn: 0.10 to 2.50%, P: 0.030% or less, S: 0.030% or less, Al: 0.150% or less, N: 0.02% or less, and Ca: more than 0.0030% and less than 0.0100% The balance is Fe and unavoidable impurities, A thick steel plate having a surface oxide layer having a thickness of 15 μm or more and 60 μm or less.
4. The composition further includes, in mass%, Cu: 1.00% or less, Ni: 1.00% or less, Cr: 0.01-1.00%, Mo: 0.01-1.00%, W: 0.01-1.00%, V: 0.003-0.100%, Nb: 0.003 to 0.030%, Ti: 0.003 to 0.050%, REM: 0.0001-0.0030%, B: 0.0001 to 0.0030%, Mg: 0.0001 to 0.0030%, and Sn: 0.001-0.030% The steel plate according to claim 3, comprising one or more selected from the following:
5. The steel plate according to any one of claims 1 to 4, wherein the standard deviation of the thickness of the surface oxide layer is 5.0 µm or less.
6. A method for producing a thick steel plate, comprising heating a steel material having a component composition according to any one of claims 1 to 4 to 1000 to 1200°C, and then performing hot rolling at a rolling end temperature of 700 to 1000°C, and performing descaling five or more times by spraying water onto at least one surface of the steel plate during a rolling pass in a temperature range from (rolling end temperature + 100°C) to the rolling end temperature.
Citation Information
Patent Citations
Steel sheet for laser gas cutting
JP1998017996A
Steel for machine structure having excellent machinability
JP2010242123A
Hot rolled steel sheet excellent in scale adhesion and manufacturing method therefor
JP2019183267A
Thick steel plate and method for producing the same
JP2022054486A
Thick steel plate and method for manufacturing the same
JP2023128426A