METHOD AND DEVICE FOR THERMAL POST-PROCESSING ON AT LEAST ONE SiC BULK SINGLE CRYSTAL

The method and apparatus address the inadequacy of existing thermal post-treatment by employing a radial thermal gradient through free thermal radiation, effectively reducing mechanical stresses and improving SiC substrate quality.

JP2024137753AActive Publication Date: 2024-10-07SICRYSTAL GMBH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024027533
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-23
Filing Date
2024-02-27
Publication Date
2024-10-07
Estimated Expiration
2044-02-27

AI Technical Summary

Technical Problem

Existing thermal post-treatment methods for SiC bulk single crystals fail to effectively relieve mechanical stresses and curvature/warping issues, particularly in larger diameters, due to insufficient consideration of radial thermal gradients and reliance on thermal conduction for heat exchange.

Method used

A method and apparatus that utilize a heterogeneous temperature profile with a continuously increasing radial thermal gradient, achieved through free thermal radiation at multiple interfaces, minimizing mechanical stress by allowing dislocations to migrate and reduce entropy in the crystal structure.

Benefits of technology

The method and apparatus significantly reduce mechanical stresses and improve the geometry of SiC substrates by enhancing stress relief, resulting in high-quality substrates with minimal curvature and warping.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137753000001_ABST
    Figure 2024137753000001_ABST
Patent Text Reader

Abstract

To provide a method and device for thermal post-processing on at least one SiC bulk single crystal.SOLUTION: A method targets thermal post-processing on at least one SiC bulk single crystal 2, having a substantially cylindrical basic shape, that has a crystal length measured in an axial direction, has a crystal diameter measured in a radial direction, and has a crystal center longitudinal axis 10 extending in the axial direction, and also comprises three boundary surfaces, namely, a bottom surface 11, a top surface 12 and an outer peripheral end surface 13. The SiC bulk single crystal is held at a post-processing temperature so as to reduce mechanical stress present in the SiC bulk single crystal after previous crystal breeding is completed. Here, a heterogeneous temperature profile having a radial heat gradient rising continuously from a crystal center vertical axis to the outer peripheral end surface is set in the SiC bulk single crystal, and heat exchange of the SiC bulk single crystal with a free space 4 surround it is carried out through free heat radiation on at least two of three boundary surfaces (11, 12 and 13).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This patent application claims priority to US Patent No. 6,399,633, the contents of which are incorporated herein by reference.

[0002] The present invention relates to a method for the thermal post-treatment of at least one bulk SiC single crystal, the bulk SiC single crystal having a crystal length measured in the axial direction, a crystal diameter measured in the radial direction, a central crystal longitudinal axis extending in the axial direction, and an essentially cylindrical basic shape with three boundary surfaces, namely a bottom surface, a top surface and a peripheral end surface. The present invention also relates to an apparatus for the thermal post-treatment of at least one such bulk SiC single crystal. [Background technology]

[0003] Due to its excellent physical, chemical, electrical and optical properties, the semiconductor material silicon carbide (SiC) is also used as the starting material for power electronic semiconductor components, high frequency components and special light emitting semiconductor components. These components require SiC substrates (=SiC wafers) with the largest possible substrate diameter and the highest possible quality. The basis for this is high-quality SiC bulk single crystals.

[0004] Such bulk SiC single crystals are usually produced by physical vapor deposition (PVT), for example by the sublimation method described in US Pat. No. 5,399,633. In this method, a single crystal SiC disk is introduced into a crystal growth crucible as a SiC seed together with a suitable source material. Under controlled temperature, pressure and gas conditions, the source material is sublimated and the gaseous seed (=SiC growth gas phase) is deposited on the SiC seed, growing a bulk SiC single crystal.

[0005] Disk-shaped monocrystalline SiC substrates are cut from these bulk SiC monocrystals and then provided with at least one epitaxial layer, in particular made of SiC, as part of the component manufacturing process, after a multi-stage polishing treatment of its surface. Generally, defects from the SiC substrate are inherited by the applied epitaxial layer, thus leading to a deterioration of the component properties. The quality of the component therefore depends to a great extent on the quality of the grown bulk SiC monocrystals and the SiC substrates obtained therefrom.

[0006] The geometry of the SiC substrates used is very important for the production of epitaxial layers of components. For example, in epitaxy reactors, good thermal bonding, which is very important for homogeneous and high-quality epitaxial layer growth, can essentially only be achieved with SiC substrates that do not have significant curvature. In contrast, SiC substrates with poor geometric properties, i.e., in particular SiC substrates with excessive curvature and / or warpage, inevitably lead to a reduced quality or yield from the epitaxy process.

[0007] Patent document 3 describes a method for thermal post-treatment of a bulk SiC single crystal in order to reduce thermal stresses in the bulk SiC single crystal and thus improve the crystal quality. After its crystal growth, the bulk SiC single crystal is tempered in a crucible during an additional processing step, where it is completely embedded in SiC powder. During the thermal post-treatment, the temperature field in the bulk SiC single crystal is as isothermal or homogeneous as possible. Preferably, the temperature difference measured in the direction of the central longitudinal axis (=axis) is set as low as possible, a maximum of 2 K, in favor of homogenization of the mechanical stress in the axial direction. However, such an isothermal temperature field can only have an overall effect on the stress field in the bulk SiC single crystal, so that the mechanical stresses present in the crystal structure are only partially relieved.

[0008] Patent document 4 describes a further method of thermal post-treatment of bulk SiC single crystals, which is intended to favorably influence the geometry of the SiC substrates obtained therefrom. During this post-treatment, the bulk SiC single crystal is subjected to an axial temperature gradient opposite to the axial temperature gradient set during crystal growth. The bulk SiC single crystal to be tempered can rest on a graphite intermediate piece.

[0009] Patent document 5 describes another method for thermal post-treatment of bulk SiC single crystals, in which the bulk SiC single crystals are completely embedded directly or indirectly in a powdered polycrystalline SiC source material. In the case of indirect embedding, the bulk SiC single crystal to be tempered is placed in a thin-walled container made of low-density porous graphite and then placed inside the polycrystalline SiC source material. The tempering should be performed at a temperature as uniform as possible. Both axial and radial temperature gradients are preferably minimized. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] European Patent Application Publication No. 23163761.2 [Patent Document 2] U.S. Patent No. 8,865,324B2 [Patent Document 3] DE 102009048868 B4 [Patent Document 4] U.S. Patent No. 8,449,671 B2 [Patent Document 5] U.S. Patent No. 7,767,022B1 Summary of the Invention [Problem to be solved by the invention]

[0011] It is therefore an object of the present invention to provide a further improved method as well as a further improved apparatus for the thermal post-treatment of bulk SiC single crystals.

[0012] To achieve the object of the method, a method according to the features of claim 1 is disclosed. In the method according to the invention, a bulk SiC single crystal is brought to a post-treatment temperature in order to reduce mechanical stresses present in the bulk SiC single crystal after completion of the prior crystal growth. Here, a non-homogeneous temperature profile is set in the bulk SiC single crystal with a radial thermal gradient that increases continuously from the crystal central axis towards the peripheral end face, and at least two of the three boundary faces, heat exchange of the bulk SiC single crystal with the free space surrounding it occurs by free thermal radiation.

[0013] The bottom surface of the SiC bulk single crystal is in particular essentially circular and preferably essentially flat. The bottom surface is preferably, but not necessarily, formed by the lower surface of the SiC seed crystal used for the growth of the SiC bulk single crystal. Alternatively, the SiC seed crystal can be separated from a part of the SiC bulk single crystal grown during a previous crystal growth prior to the thermal post-treatment. The top surface of the SiC bulk single crystal is opposite the bottom surface. It is in particular not flat, and is preferably cap-shaped or dome-shaped. The peripheral end surface is essentially in the form of a cylindrical surface. The SiC bulk single crystal grows axially during its growth. The term "axial" here refers to a direction parallel to or along the central longitudinal axis of the crystal, the term "radial" refers to a direction perpendicular thereto, and the term "tangential" refers to a circumferential direction extending around the central longitudinal axis of the crystal.

[0014] It has been recognized that the radial thermal gradients prevailing in the SiC bulk single crystals being tempered during thermal post-treatment are more important for reducing mechanical stresses in the crystal structure than the axial thermal gradients, which have been the main focus of known post-treatment processes so far, especially for larger crystal diameters. During sublimation growth of SiC bulk single crystals, the growth interface is defined by the isotherms of the temperature field. A curved growth interface is an important prerequisite for producing high-quality SiC bulk single crystals. Thus, during growth, SiC bulk single crystals grow in a curved temperature field. Different temperatures prevail at the curved growth interface. This applies in particular to the temperature comparison between the center and the edge regions of the growth interface. These temperature differences generate dislocations and mechanical stresses in the growing SiC bulk single crystal. The SiC substrate, which is later cut out from the SiC bulk single crystal, also has partial regions that were grown at different temperatures during the crystal growth. The mechanical stresses induced in the SiC substrate are one cause of the aforementioned curvature and / or warping. The curvature of the thermal field set during growth also expands to a considerable extent in the radial direction. [Means for solving the problem]

[0015] This is where the invention comes in. It has been found that a thermal gradient that starts from the crystal central longitudinal axis and increases continuously in the radial direction is a particularly effective thermal post-treatment method for achieving the desired stress reduction in the SiC bulk single crystal and thus positively influencing the geometry of the SiC substrate obtained from the SiC bulk single crystal. Such a continuously increasing radial thermal gradient advantageously leads to a reduction or preferably even a minimization of the stress balance in the crystal structure of the SiC bulk single crystal. In this context, stress should be understood in particular as frozen dislocations and / or other defects in the crystal lattice. During the thermal post-treatment, the SiC bulk single crystal is brought to a post-treatment temperature at which these dislocations are favorably mobile. They can then move within the crystal structure. The continuously increasing radial thermal gradient also defines the direction in which the dislocations that have become mobile are likely to move. In particular, the dislocations then move radially outward or dissolve. This also advantageously reduces the entropy in the SiC bulk single crystal.

[0016] It has also been recognized that this advantageous inhomogeneous temperature profile with a continuously increasing thermal gradient in the radial direction can be particularly well set by surrounding the SiC bulk single crystal with free space during the thermal after-treatment, in particular on more than 50% of its entire crystal surface, or by having more than 50% of its entire crystal surface adjacent to free space. In particular, the SiC bulk single crystal is non-contact at these times, i.e. it is not in mechanical contact with other objects, such as the inner wall of the after-treatment crucible or the holding surface of the crystal holder, or with other materials, such as SiC powder material. Advantageously, the heat exchange between the SiC bulk single crystal to be tempered and the free space at these non-contact points located on at least two of the three boundary surfaces of the SiC bulk single crystal is carried out by free heat radiation. In particular, the heat exchange in the non-contact areas, i.e. the contact points or areas of the SiC bulk single crystal, takes place mainly by heat conduction, but here the proportion of the entire crystal surface with free heat radiation preferably predominates over the proportion of the entire crystal surface with heat conduction. At the post-treatment temperature, heat is transferred to various extents by both mechanisms, but the thermal radiation mechanism is in particular better than the thermal conduction mechanism. The ratio of the percentage of the surface area with thermal conduction to the percentage of the surface area with free thermal radiation is a preferred parameter for setting up a non-homogeneous temperature profile, in particular with a thermal gradient that increases continuously in the radial direction.

[0017] In contrast to this, some of the thermal post-treatment methods known so far use an opposite temperature field. This applies in particular to post-treatment methods in which the SiC bulk single crystal is completely surrounded by SiC powder. This embedding is performed in particular to prevent non-stoichiometric dissolution of the SiC bulk single crystal, which may occur at high post-treatment temperatures. On the other hand, the complete embedding in the SiC powder reduces the heat transport by thermal radiation. Instead, the heat exchange with the environment takes place almost exclusively by thermal conduction. As a result, these post-treatment methods result in high-temperature homogeneity in the SiC bulk single crystal to be tempered. However, for this reason, due to the inhomogeneous temperature profile with a continuously increasing radial thermal gradient, it is not possible to achieve an equally favorable stress relief in the SiC bulk single crystal as in the post-treatment method according to the invention. Furthermore, the method according to the invention has further advantages over the known post-treatment methods of embedding the SiC bulk single crystal in SiC powder. Without such embedding, SiC can evaporate from the surface of the SiC bulk single crystal. However, this effect can be counteracted by adjusting, in particular increasing, the process pressure in the post-treatment crucible. On the other hand, forgoing embedding in the SiC powder offers the advantage that parasitic SiC does not grow uncontrollably on the SiC bulk single crystal to be tempered during the thermal post-treatment according to the invention. Such growth of parasitic SiC can cause renewed and / or additional mechanical stresses in the edge regions of the SiC bulk single crystal during cooling of the SiC bulk single crystal embedded in the SiC powder after completion of the thermal post-treatment, which can have a negative effect on the geometry of the SiC substrate generated from the SiC bulk single crystal, in particular due to the curvature and / or bowing caused by these stresses.

[0018] Advantageous embodiments of the method according to the invention result, inter alia, from the features of the claims dependent on claim 1.

[0019] In a preferred embodiment, the heat exchange of the SiC bulk single crystal with the surrounding free space is performed by free thermal radiation at all three interfaces. In particular, non-contact points or non-contact areas of the SiC bulk single crystal can be located at all three of its interfaces, where each interface can preferably be completely or only partially non-contact. Heat exchange by thermal radiation is particularly efficient. At non-non-contact points or areas of the SiC bulk single crystal, i.e., at those that are in contact, heat exchange occurs mainly by thermal conduction.

[0020] According to a further preferred embodiment, the heat exchange between the SiC bulk monocrystal and the surrounding free space is carried out by free thermal radiation at a radiating surface portion of the total surface area of ​​the SiC bulk monocrystal, where the total surface area is composed of the sum of the three boundary surfaces and the radiating surface portion is in the range of 63% to 83%, in particular 63% to 78%, of the total surface area. This allows a particularly good adjustment of the inhomogeneous temperature profile with a thermal gradient that rises continuously in the radial direction from the crystal central longitudinal axis. The radiating surface portion is in particular a portion of the total surface area that is not in contact with other objects or materials. Non-contact is therefore preferred.

[0021] According to another preferred embodiment, the radial thermal gradient is set to a value between 0.1 K / cm and 0.3 K / cm, in particular between 0.1 K / cm and 0.25 K / cm, in the central region of the SiC bulk monocrystal, which extends radially from the crystal central longitudinal axis to half the crystal diameter, which provides a particularly good stress relief in the crystal structure of the SiC bulk monocrystal.

[0022] According to a further preferred embodiment, the radial thermal gradient is set to have a value between 0.25 K / cm and 0.8 K / cm, in particular between 0.25 K / cm and 0.7 K / cm, in the end region of the SiC bulk single crystal extending in the radial direction from half the crystal diameter to the peripheral end face. This method also serves to relieve stress in the crystal structure of the SiC bulk single crystal.

[0023] According to another preferred embodiment, the temperature value of the post-treatment temperature is set higher than the growth temperature at which the SiC bulk single crystal was grown, in particular up to 500° C. higher, preferably up to 200° C. higher. In particular, a post-treatment temperature of more than 1950° C., preferably more than 2000° C., preferably more than 2200° C., is set, the upper limit of this temperature being in particular 2500° C., preferably 2450° C.

[0024] According to yet another preferred embodiment, a gas atmosphere is set up around the SiC bulk single crystal, and at least one silicon-free process gas is supplied for this purpose. Preferably, this at least one silicon-free process gas is a gas selected from the group of argon, helium, another noble gas and nitrogen, or a mixture of gases selected from this group. The thermal post-treatment of the SiC bulk single crystal is in particular carried out without the active addition of gaseous or solid silicon-containing components. In particular, no silicon-containing components, whether gaseous or solid, such as SiC powder, are introduced into the post-treatment crucible. The SiC bulk single crystal to be tempered is preferably not in direct contact with such silicon-containing components. Indirect contact, as can be achieved, for example, by inserting a barrier in the form of a porous separation element or a porous membrane, is in particular not present here. This prevents the formation of a silicon-containing atmosphere in the post-treatment crucible due to the active supply of silicon-containing components. Nevertheless, in particular if there is a small amount of silicon-containing gas content in the atmosphere, this is essentially attributable solely to the SiC bulk single crystal being tempered, for example due to evaporation of SiC from the surface of the SiC bulk single crystal.

[0025] According to a further preferred embodiment the process gas pressure is set in the range of 800 mbar to 1200 mbar, in particular in the range of 800 mbar to 1000 mbar.

[0026] According to another preferred embodiment, the crystal length is at most 50 mm, in particular at most 45 mm, preferably 25 mm to 30 mm. The lower limit of the crystal length is in particular 15 mm, preferably 25 mm, most preferably 30 mm.

[0027] According to yet another preferred embodiment, the crystal diameter is at least 150 mm, in particular at least 200 mm. The upper limit of the crystal diameter is in particular 450 mm, preferably 300 mm. As the crystal diameter increases, the possibility that the SiC substrate produced from the SiC bulk single crystal has a disordered curvature and / or warpage induced by thermally induced mechanical stresses in the crystal structure of the SiC bulk single crystal increases. In particular, this applies to SiC bulk single crystals with a crystal diameter of about 150 mm or more. The post-treatment method according to the invention is therefore particularly advantageous and efficient for SiC bulk single crystals with such large crystal diameters, since the increasingly increasing mechanical stresses in the crystal structure of the SiC bulk single crystal are relieved.

[0028] According to a further preferred embodiment, the aspect ratio, which is formed by dividing the crystal length by the crystal diameter, is in the range of 0.05 to 0.35, in particular in the range of 0.1 to 0.3. The crystal length of the SiC bulk single crystals that can be produced by physical vapor deposition (PVT) is in particular limited to a few centimeters and is almost independent of the crystal diameter. With increasing crystal diameter, the aspect ratio of the SiC bulk single crystal changes. It becomes smaller and smaller. With increasing crystal diameter, the radial thermal gradient becomes increasingly dominant for the properties of the growing SiC bulk single crystal compared to the axial thermal gradient. As a result, the stress in the growing SiC bulk single crystal and its influence on the geometry of the SiC substrate subsequently produced therefrom are increasingly determined by the radial thermal gradient prevailing during growth. It is recognized that when the aspect ratio is below a certain upper limit, the axial thermal gradient becomes less important. This applies both to the growth of the SiC bulk single crystal and to the thermal post-treatment. This upper limit for the aspect ratio is in particular in the range of 0.3 to 0.35. Instead, the decisive factor is to focus on the radial thermal gradient provided in the post-treatment method according to the invention in order to have the desired positive influence on the geometry of the SiC substrate produced from the SiC bulk monocrystal to be tempered.

[0029] According to another preferred embodiment, the at least one SiC bulk single crystal to be thermally post-treated is placed on a crystal holder arranged in a post-treatment crucible having a holding surface for holding the at least one SiC bulk single crystal in contact therewith, wherein the holding surface contacts the at least one SiC bulk single crystal to be post-treated only at the radial end regions of the SiC bulk single crystal.

[0030] According to yet another preferred embodiment, an inner diameter of the post-processing crucible is provided that is larger than the crystal diameter, so that when the SiC bulk single crystal is inserted into the post-processing crucible, a tangentially completely circumferentially free annular gap exists between the outer peripheral end face of the SiC bulk single crystal and the inner wall of the post-processing crucible.

[0031] According to a further preferred embodiment, the crystal holder is designed as an annular crystal support.

[0032] According to another preferred embodiment, a thickness of the crystal support, measured in the axial direction, in the range between 1 mm and 5 mm, in particular in the range between 1 mm and 3 mm, is provided.

[0033] According to yet another preferred embodiment, the holder material constituting the crystal holder or the holder material contained in the crystal holder is provided with a thermal conductivity lower than the thermal conductivity of the crucible material constituting the post-processing crucible or contained in the post-processing crucible.

[0034] According to a further preferred embodiment, the holder material constituting the crystal holder or the holder material contained in the crystal holder is provided with a porosity higher than the porosity of the crucible material constituting the post-processing crucible or contained in the post-processing crucible.

[0035] To achieve the object of the device, an apparatus according to the features of claim 10 is disclosed. The apparatus according to the invention comprises a thermal post-treatment crucible with a receiving space for at least one SiC bulk single crystal to be thermally post-treated, a heating device for heating the post-treatment crucible and the SiC bulk single crystal placed therein to a post-treatment temperature to reduce mechanical stresses present in the SiC bulk single crystal after completion of the preceding growth, and a crystal holder arranged in the post-treatment crucible with a holding surface for contacting and holding the at least one SiC bulk single crystal to be thermally post-treated. In this process, the holding surface contacts the at least one SiC bulk single crystal to be post-treated only in the radial end region of the SiC bulk single crystal, so that a non-homogeneous temperature profile with a radial thermal gradient is established in the at least one SiC bulk single crystal to be post-treated, which profile rises continuously from the crystal central axis to the peripheral end surface, and heat exchange of the at least one SiC bulk single crystal to be post-treated surrounded by a free space is performed by free thermal radiation at at least two of the three boundary surfaces, where the free space is a part of the receiving space.

[0036] The radial end region of the SiC bulk single crystal that is in contact with the holding surface of the crystal holder particularly includes the outer peripheral end surface and partial regions of the bottom surface and top surface adjacent to the outer peripheral end surface.

[0037] The device according to the invention and its embodiments offer essentially the same advantages as already explained in connection with the method according to the invention and its embodiments.

[0038] Advantageous embodiments of the device according to the invention result, inter alia, from the features of the claims dependent on claim 10.

[0039] A preferred embodiment is one in which the crystal holder is constructed such that heat exchange between the SiC bulk single crystal and the surrounding free space occurs by free thermal radiation at all three interfaces.

[0040] According to a further preferred embodiment, the crystal holder is designed such that heat exchange with the free space surrounding the SiC bulk monocrystal is performed by free thermal radiation on a radiating surface portion of the total surface area of ​​the SiC bulk monocrystal, the total surface area being composed of the sum of the three boundary surfaces and the radiating surface portion being in the range of 63% to 83%, in particular in the range of 63% to 78%, of the total surface area.

[0041] According to another preferred embodiment, contact of the at least one SiC bulk monocrystal by the holding surface is designed such that the radial thermal gradient in the central region of the SiC bulk monocrystal has a value between 0.1 K / cm and 0.3 K / cm, in particular between 0.1 K / cm and 0.25 K / cm, and the central region of the SiC bulk monocrystal extends radially from the crystal central longitudinal axis to half the crystal diameter.

[0042] According to yet another preferred embodiment, contact by the holding surface to at least one SiC bulk single crystal is designed such that the radial thermal gradient in the end region of the SiC bulk single crystal is between 0.25 K / cm and 0.8 K / cm, in particular 0.25 K / cm and 0.7 K / cm, and the end region of the SiC bulk single crystal extends radially from half the crystal diameter to the outer peripheral end face.

[0043] According to a further preferred embodiment, the post-treatment temperature is a temperature value higher than the growth temperature at which the SiC bulk single crystal was previously grown, in particular up to 500° C. higher, preferably up to 200° C. higher. In particular, the post-treatment temperature is higher than 1950° C., preferably higher than 2000° C., preferably higher than 2200° C., where the upper limit of this temperature is in particular 2500° C., preferably 2450° C.

[0044] According to another preferred embodiment, the inner diameter of the after-treatment crucible is larger than the crystal diameter, so that when the SiC bulk single crystal is inserted into the after-treatment crucible, a completely circumferentially free annular gap exists between the outer peripheral end surface of the SiC bulk single crystal and the inner wall of the after-treatment crucible in the tangential direction. As a result, heat exchange takes place on the peripheral surface of the SiC bulk single crystal by free thermal radiation with the free space that also extends into the free annular gap. The annular gap has a gap width in particular in the range between 5 mm and 20 mm, preferably in the range between 5 mm and 15 mm.

[0045] According to yet another preferred embodiment, the crystal holder is designed as an annular crystal support, which allows the essentially cylindrical SiC bulk single crystal to be very well supported, especially in the region of the peripheral edge and bottom surface, while the annular crystal support only contacts a small portion of the interface of the SiC bulk single crystal, so that a large portion of the interface is available for heat exchange by free thermal radiation.

[0046] According to a further preferred embodiment, the crystal support has a thickness, measured in the axial direction, in the range between 1 mm and 5 mm, in particular in the range between 1 mm and 3 mm. The thickness of the crystal support used can also preferably be used to control the heat conduction through the crystal support, which means that the radial heat gradient in the SiC bulk single crystal to be tempered can also be further adapted and / or adjusted. The thickness of the crystal support is in particular one of the means for adjusting or fine-tuning the ratio between heat conduction and heat radiation, i.e. the ratio between the two heat exchange mechanisms by which the SiC bulk single crystal placed on the crystal support exchanges heat with its environment, in particular with objects located in the environment or with the surrounding free space, during thermal post-treatment.

[0047] According to another preferred embodiment, the holder material constituting the crystal holder or the holder material contained in the crystal holder has a lower thermal conductivity than the crucible material constituting the post-treatment crucible or the crucible material contained in the post-treatment crucible. The thermal conductivity of the holder material can also be preferably used to control the heat conduction through the crystal support, which means that the radial thermal gradient in the SiC bulk single crystal to be tempered can be further adapted and / or adjusted. In particular, the thermal conductivity of the holder material is also one of the means to adjust or fine-tune the ratio of heat conduction and heat radiation between the SiC bulk single crystal to be tempered. The holder material can in particular be graphite. In particular, the crucible material can also be graphite.

[0048] According to yet another preferred embodiment, the holder material constituting the crystal holder or the holder material contained by the crystal holder has a higher porosity than the crucible material constituting the aftertreatment crucible or the crucible material contained by the aftertreatment crucible. A higher porosity leads in particular to a lower degree of heat conduction, since there are fewer direct heat bridges, i.e. fewer direct contact points. The porosity of the holder material can also be preferably used to control the heat conduction through the crystal support, which means that the radial heat gradient in the SiC bulk single crystal to be tempered can be further adapted and / or adjusted. In particular, the porosity of the holder material is also one of the means for adjusting or fine-tuning the ratio of heat conduction and heat radiation to and from the SiC bulk single crystal to be tempered. The holder material can in particular be porous graphite. In particular, the crucible material can also be graphite. Graphite is available in various variants. The graphite of the holder material is preferably more porous than the graphite of the crucible material. In particular, the crystal holder can be implemented as a two-layer or multi-layer structure, for example, containing a substrate made of a dense first holder material, for example dense graphite, and a substrate covering layer made of a second holder material, for example porous graphite, which is more porous than the first holder material.

[0049] According to a further preferred embodiment, the receiving space is designed to receive at least one bulk SiC single crystal to be thermally post-treated, the crystal length being at most 50 mm, in particular at most 45 mm. Preferably, the crystal length is between 25 mm and 30 mm. The lower limit of the crystal length is in particular 15 mm, preferably 25 mm, most preferably 30 mm.

[0050] According to another preferred embodiment, the receiving space is designed to receive at least one bulk SiC single crystal to be thermally post-treated, the crystal diameter being at least 150 mm, in particular at least 200 mm. The upper limit of the crystal diameter is in particular 450 mm, preferably 300 mm.

[0051] According to yet another preferred embodiment, the receiving space is designed to receive at least one SiC bulk single crystal to be thermally post-treated, the aspect ratio formed by dividing the crystal length by the crystal diameter being in the range of 0.05 to 0.35, in particular in the range of 0.1 to 0.3.

[0052] Further features, advantages and details of the invention are provided in the following description of embodiments with reference to the drawings. [Brief description of the drawings]

[0053] [Figure 1] 1 shows a first embodiment of an apparatus for thermal post-treatment of bulk SiC single crystals having a crystal holder in a post-treatment crucible. [Diagram 2] 2 shows an enlarged cross-sectional view of the apparatus according to FIG. 1, in which a bulk SiC single crystal to be tempered is placed on the crystal holder. [Diagram 3] 1 shows examples of embodiments of tempered bulk SiC single crystals with the same crystal length but different crystal diameters. [Figure 4] 1 shows examples of embodiments of tempered bulk SiC single crystals with the same crystal length but different crystal diameters. [Diagram 5] 1 shows examples of embodiments of tempered bulk SiC single crystals with the same crystal length but different crystal diameters. [Figure 6] 4 shows further example embodiments of the apparatus for thermal post-treatment using other heating devices. [Figure 7] 4 shows further example embodiments of the apparatus for thermal post-treatment using other heating devices. [Figure 8] 4 shows further example embodiments of the apparatus for thermal post-treatment using other heating devices.

[0054] Corresponding parts are provided with the same reference numerals in Figures 1 to 8. The details of the example embodiments described in more detail below may constitute an invention in their own right or form part of the subject matter of the invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0055] 1 and 2 show an example embodiment of an apparatus 1 for the thermal post-treatment of a bulk SiC single crystal 2. The apparatus 1 can also be called a tempering apparatus.

[0056] It contains a post-treatment crucible 3, the interior of which forms a receiving space 4 for a SiC bulk single crystal 2 to be thermally post-treated (=tempered). The post-treatment crucible 3 consists of a crucible material, which in the example embodiment is dense graphite. Alternatively, the crucible material may be tantalum (Ta), tungsten (W) or other refractory metals or metal carbides, such as tantalum carbide (TaC) or tungsten carbide (WC). The post-treatment crucible 3 is surrounded by a thermal insulation 5, which in the example embodiment shown is made of graphite felt. The thermal insulation 5 has two openings at the top and bottom, each in the form of a pyrometer channel 6, so that the temperature in the post-treatment crucible 3 can be measured using a pyrometer, not shown. The thermal insulation 5 is surrounded by an induction heating device in the form of a heating coil 7.

[0057] The crystal holder 8 is arranged in the receiving space 4 of the after-treatment crucible 3, which has a holding surface 9 on which the SiC bulk single crystal 2 rests during thermal after-treatment. The crystal holder 8 is configured as an annular crystal support and consists of a holder material that has a higher porosity and a lower thermal conductivity compared to the crucible material in the illustrated embodiment. In this embodiment, the holder material is porous graphite. However, there are also alternative embodiments in which the holder material has the same or at least similar porosity and thermal conductivity as the crucible material, where these two material properties are then not used or at most only to a very small extent used as parameters for the (fine)adjustment of the ratio of thermal conduction to thermal radiation. This adjustment is then almost exclusively carried out via the proportion of the non-contact area in the total surface area of ​​the SiC bulk single crystal 2 (see below).

[0058] The illustrated apparatus 1 is designed for the thermal post-treatment of only one SiC bulk single crystal 2. However, this is not a fundamental limitation: there are other apparatuses that are capable of tempering two or more SiC bulk single crystals together.

[0059] According to an enlarged view of the part of the apparatus 1 shown in Fig. 2 where the SiC bulk single crystal 2 to be tempered is located during the thermal post-treatment, the SiC bulk single crystal 2 to be tempered has an essentially cylindrical basic shape with a crystal central longitudinal axis 10 and three boundary surfaces, namely a flat circular bottom surface 11, a cap-shaped top surface 12 and a cylindrical peripheral end surface 13. The crystal central longitudinal axis 10 extends in the axial direction along which the SiC bulk single crystal 2 grew during its growth, along which the crystal length L of the SiC bulk single crystal 2 is also measured. In the perpendicular direction thereto, i.e. in the radial direction, the crystal diameter D of the SiC bulk single crystal 2 is measured.

[0060] During the growth process, mechanical stresses arise in the crystal structure of the growing SiC bulk monocrystal 2, which may have an unfavorable effect on the geometry and thus the quality of the SiC substrates subsequently produced from the SiC bulk monocrystal 2. For this reason, these stresses should be relieved by thermal post-treatment of the SiC bulk monocrystal 2.

[0061] The larger the crystal diameter D of the SiC bulk single crystal 2, the greater the effect of the radial temperature gradient (=thermal gradient) on the characteristics of the growing SiC bulk single crystal 2 during growth. At the same time, the effect of the axial temperature gradient becomes smaller.

[0062] This is also due to the fact that the physical vapor deposition techniques used for crystal growth allow the production of bulk SiC single crystals with increasingly larger crystal diameters D, but limit the achievable crystal length L in the axial direction to a few centimeters. Thus, the ratio of crystal length L to crystal diameter D, referred to here as the aspect ratio, changes with increasing crystal diameter D, i.e. becomes smaller.

[0063] The representations of Figures 3 to 5 illustrate this effect. Three SiC bulk single crystals 14, 15 and 16 are shown, each with the same crystal length L of 25 mm, but with different crystal diameters D. The SiC bulk single crystal 14 according to Figure 3 has a crystal diameter D of 76.2 mm, and therefore an aspect ratio L / D of 0.33. The SiC bulk single crystal 15 according to Figure 4 has a crystal diameter D of 150 mm, and therefore an aspect ratio L / D of 0.17. The SiC bulk single crystal 15 according to Figure 4 has a crystal diameter D of 150 mm, and therefore an aspect ratio L / D of 0.17. The SiC bulk single crystal 16 according to Figure 5 has a crystal diameter D of 200 mm, and therefore an aspect ratio L / D of 0.13.

[0064] The effect of the increasing radial ratio also influences the stresses leading to the growth of the SiC volumetric single crystal 2, which becomes increasingly determined by the radial temperature gradient as the crystal diameter D increases.

[0065] It has been recognized that this effect must also be taken into account during thermal post-treatment. In order to achieve as complete a stress relief as possible, special temperature conditions are provided in the radial direction of the SiC bulk monocrystal 2 during the post-treatment process. Advantageously, a non-homogeneous temperature profile is set up with a continuously increasing radial temperature gradient from the crystal central longitudinal axis to the peripheral end face.

[0066] This special inhomogeneous temperature profile inside the SiC bulk single crystal 2 to be tempered is not generated only by the external heating device of the apparatus 1. The external heating device in the form of a heating coil 7 essentially only directly influences the temperature in the crucible wall of the aftertreatment crucible 3. In the apparatus 1, the aftertreatment crucible 3 constitutes a kind of heater. It transports the heat supplied to it to the internal receiving chamber 4. In order to adjust the temperature profile with an inhomogeneous radial temperature gradient in the SiC bulk single crystal 2, further measures for influencing the temperature are provided in the apparatus 1.

[0067] This heat transport mechanism transfers heat from the crucible wall to the SiC bulk single crystal 2 inside the post-treatment crucible 3 , and also affects the temperature distribution inside the SiC bulk single crystal 2 .

[0068] For example, it has been shown that embedding a bulk SiC single crystal 2 in SiC powder prevents heat transfer by thermal radiation. Instead, thermal conduction is the determining factor for heat transfer. Furthermore, it has been shown that the SiC powder has a rather insulating and homogenizing effect on the temperature profile within the bulk SiC single crystal 2. An inhomogeneous temperature profile with a radially increasing temperature gradient cannot be set up.

[0069] An effect similar to complete embedding in SiC powder occurs when the entire bottom surface 11 of the SiC bulk single crystal 2 rests on the support surface. In the contact area between the bottom surface 11 and the support surface, heat is transported from the SiC bulk single crystal 2 to the SiC bulk single crystal 2 by thermal conduction.

[0070] According to another finding, in order to set a non-homogeneous temperature profile with a radially increasing temperature gradient in the SiC bulk single crystal 2, free thermal radiation should be the dominant mechanism for heat transfer to and from the SiC bulk single crystal 2. However, there is another mechanism of heat transfer, which is based on thermal conduction. The ratio of the proportion of thermal conduction in the heat transfer to the proportion of thermal radiation in the heat transfer can be used to advantageously set a non-homogeneous temperature profile with a radially increasing temperature gradient from the inside to the outside during thermal after-treatment. Thus, the SiC bulk single crystal 2 is supported or held in the receiving chamber 4 by the crystal holder 8 in such a way that the heat transfer to and from the SiC bulk single crystal 2 by free thermal radiation has a significant or dominant proportion. For this purpose, the crystal holder 8 is preferably designed so that the held SiC bulk single crystal 2 does not come into contact with another object, such as the inner wall of the after-treatment crucible 3 or the holding surface 9 of the crystal holder 8, in the maximum part of its total surface area, which is composed of three boundary surfaces, i.e. the bottom surface 11, the top surface 12 and the outer peripheral end surface 13. The heat exchange or transfer between the SiC bulk single crystal 2 to be tempered and the adjacent free space of the receiving chamber 4 then takes place in these non-contact areas of the entire surface of the SiC bulk single crystal 2 by free thermal radiation. These non-contact areas form a radiating surface portion, which in relation to the total surface area of ​​the SiC bulk single crystal 2 ranges in particular between 63% and 83%. Thus, in other areas of the total surface area of ​​the SiC bulk single crystal 2, the proportion of which in particular ranges from 17% to 37%, there is contact with other objects or components of the device 1, in particular the crystal holder 8, so that heat is transferred there mainly by thermal conduction.

[0071] Heat exchange of the SiC bulk single crystal 2 with the surrounding free space by free thermal radiation preferably takes place at least on two of the three boundary surfaces, and even on all three boundary surfaces, in the embodiment example shown in Figures 1 and 2. The central part of the bottom surface 11 is not in contact with the crystal holder 8 designed as an annular crystal support. The bottom surface 11 remains in non-contact in the region of the annular opening of the crystal holder, so that there is heat exchange by free thermal radiation with the adjacent free space. The top surface 12 and the peripheral end surface 13 are completely non-contact and are therefore fully available for heat exchange by free thermal radiation.

[0072] Since the inner diameter of the post-treatment crucible 3 is larger than the crystal diameter of the SiC bulk single crystal 2, the outer peripheral end face 13 is not in contact with the SiC bulk single crystal 2, and as a result, a completely circumferentially free annular gap 17 is present between the outer peripheral end face 2 of the inserted SiC bulk single crystal 2 and the inner wall of the post-treatment crucible 3 in the tangential direction. This annular gap 17 preferably has a gap width B of 5 mm to 20 mm (see FIG. 2).

[0073] Thanks to this heat exchange between the SiC bulk single crystal 2 and the surrounding free space by means of free thermal radiation, an advantageous inhomogeneous temperature profile having a radially increasing temperature gradient arises in the SiC bulk single crystal 2 during thermal post-treatment, leading to the desired reduction of mechanical stresses in the SiC bulk single crystal 2.

[0074] As an optional additional measure for further adaptation and adjustment of the radial temperature gradient, the thickness of the crystal holder 8, designed as an annular crystal support, can be varied and additionally or alternatively, a holder material with a correspondingly adapted thermal conductivity or porosity can be used for the crystal holder 8. In particular, a holder material with a low thermal conductivity and / or a high porosity can be selected.

[0075] Apart from the above mentioned components, the device 1 comprises further components, which are not shown in Figures 1 and 2 for clarity. Also, there is at least one exhaust system and a gas system for supplying a controlled gas flow of a process gas and maintaining the process gas atmosphere at an adjustable process gas pressure during the post-treatment process. The supplied process gas is argon (Ar), helium (He) or nitrogen (N) or a mixture of these gases.

[0076] The thermal post-treatment process is described in more detail below.

[0077] Before the actual post-treatment process begins, evacuation is performed to ensure a controlled atmosphere and minimize impurities. Prior to heating, a process gas pressure in the range of 800 mbar to 1200 mbar, preferably 800 mbar to 1000 mbar, is set to minimize surface evaporation of SiC material from the SiC bulk single crystal 2 to be tempered.

[0078] The after-treatment crucible 3 is then heated to the desired process temperature with the SiC bulk single crystal 2 placed therein. Here, after reaching a temperature range of 900°C to 1500°C, preferably 1000°C to 1200°C, a further temperature increase to the actual after-treatment temperature is performed with a temperature ramp of 1°C / h to 5°C / h to avoid the formation of additional stresses. The actual after-treatment temperature is up to 500°C, preferably up to 200°C, higher than the growth temperature at which the SiC bulk single crystal 2 is grown. The after-treatment temperature is therefore in the range of 1950°C to 2450°C.

[0079] After the start of the actual thermal post-treatment, the process conditions of pressure, atmospheric composition and temperature are kept as constant as possible for the subsequent process period of 5 h to 72 h, preferably 15 h to 50 h. The slight temperature fluctuations are less than 10° C., preferably less than 2° C. On the one hand, this provides sufficient time for the reduction of mechanical stresses in the crystal structure of the SiC bulk mono-crystal. On the other hand, the stress release is not hindered by fluctuations in the process parameters.

[0080] After the process time has elapsed, the SiC bulk single crystal 2 is slowly cooled down to a temperature range of 900°C-1500°C, preferably 1000°C-1200°C, with a temperature gradient of 0.5°C / h-3°C / h, preferably 0.5°C / h-2°C / h, to avoid the formation of new mechanical stresses due to temperature inhomogeneities that may be caused by heat transport mechanisms. After final cooling of the treated crucible 3 and the tempered SiC bulk single crystal 2 to approximately room temperature, the treated crucible 3 is filled with ambient atmosphere and the SiC bulk single crystal 2 is removed for further processing.

[0081] The apparatus 1 according to Fig. 1 and Fig. 2 has an induction heating device, which allows to adjust the overall temperature distribution inside the after-treatment crucible 3. However, the heating device does not necessarily have to be designed to be inductive. Fig. 6-8 show alternative tempering devices 18, 19 and 20 for the thermal after-treatment of SiC bulk single crystals 2, which are provided with resistance heaters instead of the heating coil 7. These resistance heaters can be used to adjust the overall temperature distribution inside the after-treatment crucible 3, similar to the induction heater of the apparatus 1. However, both heating concepts can only be used to adjust the temperature of the after-treatment crucible 3 itself. The additional temperature influencing means described above with reference to the apparatus 1 are advantageously used together with the tempering devices 18, 19, 20, but are not shown in Fig. 6-8, as are some other components of the tempering devices 18, 19, 20.

[0082] In the tempering apparatus 18 according to FIG. 6, a cylindrical resistance heating element 21 is arranged in the aftertreatment crucible 3 adjacent to or in contact with a tangentially surrounding cylindrical crucible side wall 22 .

[0083] 7, a cylindrical resistive heating element 23 and two circular resistive heating elements 24 and 25 are disposed outside the aftertreatment crucible 3 but inside the insulator 5. The resistive heating element 23 surrounds the cylindrical crucible side wall 22. The resistive heating elements 24 and 25 cover the upper and lower axial crucible end walls 26 and 27, respectively, of the aftertreatment crucible 3.

[0084] In the tempering apparatus 20 shown in Fig. 8, a cylindrical resistance heating element 28 surrounds the cylindrical crucible side wall 22 outside the aftertreatment crucible 3 and inside the insulator 5. The resistance heating element 28 corresponds to the resistance heating element 23 of the tempering apparatus 19. In contrast to the tempering apparatus 19, in the tempering apparatus 20, there are no resistance heating elements at the two axial end faces of the aftertreatment crucible 3.

[0085] The devices 1, 18, 19 and 20 each have a rotationally symmetric heating device. These are examples of embodiments. Other, in particular non-rotationally symmetric, structures and alternative arrangements of the heating devices or combinations of different heating devices are also possible.

[0086] Overall, all of the devices 1, 18, 19 and 20 allow a very advantageous thermal post-treatment, in which a non-homogeneous temperature profile with a radially increasing temperature gradient is set up in the SiC bulk monocrystal 2 to be tempered, corresponding to the stress balance inside the SiC bulk monocrystal 2. This results in a very good reduction of the existing mechanical stresses. High-quality SiC substrates with very low curvature and warpage can be produced from the SiC bulk monocrystal 2 thermally post-treated in this way.

Claims

1. 1. A method for thermal post-treatment of at least one SiC bulk single crystal (2) having a crystal length measured in an axial direction, a crystal diameter measured in a radial direction, a crystal central longitudinal axis (10) extending in an axial direction, and a substantially cylindrical basic shape with three boundary surfaces, namely a bottom surface (11), a top surface (12) and a peripheral end surface (13), comprising: a) a SiC bulk single crystal (2) is brought to a post-treatment temperature to reduce mechanical stresses present in said SiC bulk single crystal (2) after completion of a prior crystal growth, wherein: b) a non-homogeneous temperature profile is established within the SiC bulk single crystal (2) having a continuously increasing radial temperature gradient from the crystal central longitudinal axis (10) to the peripheral end surface (13); and c) heat exchange between the SiC bulk single crystal (2) and the free space (4) surrounding it is carried out by free thermal radiation on at least two of the three boundary surfaces (11, 12, 13); Thermal post-treatment methods.

2. 2. The method according to claim 1, characterized in that the heat exchange between the SiC bulk single crystal (2) and the surrounding free space (4) is performed by free thermal radiation at all three interface surfaces (11, 12, 13).

3. 3. The method according to claim 1 or 2, characterized in that heat exchange between the SiC bulk single crystal (2) and the free space (4) surrounding it occurs by free thermal radiation on a radial surface portion of the entire surface of the SiC bulk single crystal (2), wherein the total surface area is constituted by the sum of the three boundary surfaces (11, 12, 13) and the radial surface portion is in the range of 63% to 83% of the total surface area.

4. The method according to any one of claims 1 to 3, characterized in that the radial temperature gradient is set to have a value between 0.1 K / cm and 0.3 K / cm in a central region of the SiC bulk single crystal (2) extending radially from the crystal central longitudinal axis (10) to half the crystal diameter.

5. The method according to any one of claims 1 to 4, characterized in that the radial temperature gradient is set to have a value between 0.25 K / cm and 0.8 K / cm in an end region of the SiC bulk single crystal (2) extending from half the crystal diameter to the outer peripheral end face.

6. The method according to any one of claims 1 to 5, characterized in that a gas atmosphere is set up around the SiC bulk single crystal (2) and for that purpose at least one silicon-free process gas is supplied, in particular a gas selected from the group consisting of argon, helium, other noble gases and nitrogen or a mixture of gases from this group.

7. The method according to any one of claims 1 to 6, characterized in that the crystal length is 50 mm or less.

8. A method according to any one of claims 1 to 7, characterised in that the crystal diameter is at least 150 mm.

9. A method according to any one of claims 1 to 8, characterized in that the aspect ratio formed by dividing the crystal length by the crystal diameter is in the range of 0.05 to 0.

35.

10. An apparatus for the thermal post-treatment of at least one bulk SiC single crystal (2), the apparatus having a crystal length measured in the axial direction, a crystal diameter measured in the radial direction, a crystal central longitudinal axis (10) extending in the axial direction, and an essentially cylindrical basic shape with three boundary surfaces, namely a bottom surface (11), a top surface (12) and an outer peripheral end surface (13), a) a crucible (3) for thermal post-treatment, comprising a receiving space (4) for the at least one bulk SiC single crystal (2) to be thermally post-treated; b) a heating device (7; 21; 23, 24, 25; 28) for heating the post-treatment crucible (3) and the SiC bulk single crystal (2) placed therein to a post-treatment temperature to relieve mechanical stresses present in the SiC bulk single crystal (2) after completion of the preliminary crystal growth; and c) an apparatus having a crystal holder (8) arranged in the after-treatment crucible (2) with a holding surface (9) for holding in contact with the at least one single crystal (2) of SiC volume to be thermally after-treated, d) wherein the holding surface (9) is in contact with the at least one SiC bulk single crystal (2) to be post-treated only in the radial end region of the SiC bulk single crystal (2); d1) in the at least one SiC bulk single crystal (2) to be post-treated, a non-homogeneous temperature profile is established having a continuously increasing radial thermal gradient from the crystal central vertical axis (10) to the outer peripheral end surface (13); and d2) heat exchange with the free space surrounding the at least one SiC bulk single crystal (2) to be post-treated is carried out by free thermal radiation at at least two of the three boundary surfaces (11, 12, 13), where the free space is part of the receiving space (4); Device.

11. The apparatus according to claim 10, characterized in that the inner diameter of the post-treatment crucible (3) is larger than the crystal diameter, so that when the SiC bulk single crystal (2) is inserted into the post-treatment crucible (3), a tangentially completely circumferentially free annular gap (17) exists between the outer peripheral end surface (13) of the SiC bulk single crystal (2) and the inner wall of the post-treatment crucible (3).

12. 12. Apparatus according to claim 10 or 11, characterized in that the crystal holder (8) is designed as an annular crystal support.

13. Apparatus according to claim 12, characterized in that the crystal holder (8) has a thickness, measured axially, in the range of 1 mm to 5 mm.

14. The apparatus according to any one of claims 10 to 13, characterized in that the holder material constituting or contained in the crystal holder (8) has a lower thermal conductivity than the crucible material constituting or contained in the post-treatment crucible (3).

15. 15. The apparatus according to claim 10, wherein the holder material constituting or contained in the crystal holder (8) has a higher porosity than the crucible material constituting or contained in the post-treatment crucible (3).

Citation Information

Patent Citations

  • Secondary annealing method of silicon carbide crystal

    CN113564719A

  • Manufacturing process for a SiC volume single crystal using a thermal treatment and low-resistance single-crystal SiC substrate

    DE102009048868B4

  • Method and device for thermal post-treatment of at least one sic bulk crystal

    EP4435155A1

  • Method of annealing a sublimation grown crystal

    US7767022B1

  • Fabrication of SiC substrates with low warp and bow

    US8449671B2