Fumed aluminium oxide as Anti-settling agent in polymer-based thermally conductive mixtures

Fumed aluminum oxide with a specific BET surface area and low content addresses sedimentation issues in thermally conductive compositions, maintaining thermal conductivity and processability.

JP2024137785APending Publication Date: 2024-10-07EVONIK OPERATIONS GMBH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024036942
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-22
Filing Date
2024-03-11
Publication Date
2024-10-07

Smart Images

  • Figure 2024137785000001
    Figure 2024137785000001
  • Figure 2024137785000002
    Figure 2024137785000002
  • Figure 2024137785000003
    Figure 2024137785000003
Patent Text Reader

Abstract

To provide an anti-settling substance for thermally conductive compositions, which works both efficiently and specifically, whereby particularly in the case of low to moderate proportions of thermally conductive particles, the sedimentation of the particles should be reduced or completely prevented.SOLUTION: The present invention provides a composition comprising at least one prepolymer, thermally conductive particles and particles of fumed aluminium oxide having a BET surface area of 15 m2 / g to 200 m2 / g. The invention further provides a method for producing a thermally conductive composition comprising the step of adding fumed aluminium oxide having the BET surface area to the composition. The present invention also provides the use of fumed aluminium oxide having a BET surface area of 15 m2 / g to 200 m2 / g to reduce sedimentation of thermally conductive particles in polymer compositions.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to At least one prepolymer, thermally conductive particles, and a BET surface area of ​​15 m 2 / g~200m 2 and fumed aluminum oxide particles having a BET surface area of ​​15 m. 2 / g~200m 2 The present invention also relates to a method for making a thermally conductive polymer composition comprising the step of adding fumed aluminum oxide having a BET surface area of ​​15 m to the composition to reduce settling of the thermally conductive particles in the polymer composition. 2 / g~200m 2 / g of fumed aluminum oxide. [Background technology]

[0002] Thermally conductive plastics are used in many technical fields where efficient heat transfer is required. These include, in particular, coatings for electronic components and electrical insulators, which generate large amounts of heat in a minimum of space. To ensure the functional reliability and sufficient service life of these components, the generated heat must be efficiently dissipated. For optimal heat dissipation, the composites and adhesives or fillers used to manufacture said coatings and components must also be thermally conductive. Such components are therefore often manufactured from plastics that contain one or more prepolymers, which, together with various additives and fillers, are mixed with each other in a liquid or viscous state and then cured to become the finished polymer material.

[0003] It is known from the prior art that the thermal conductivity increases with the proportion of thermally conductive fillers in the composition. In the case of formulations that are easily free-flowing at low to moderate loadings, the settling is particularly pronounced. This is due to the significant difference in the density of the filler, on the one hand, and the density of the prepolymer, on the other hand. For example, aluminium oxide, known from the prior art for its thermal conductivity, has a density of 3.5-4 g / cm 3whereas the density of the prepolymers used to manufacture thermally conductive plastics is approximately 0.8 g / cm 3 ~2g / cm 3 That's all.

[0004] However, settling is undesirable, as it can lead to uneven heat transfer in the finished product, which can damage it during operation or reduce the overall efficiency of heat transfer, which in turn can impair the functional reliability and service life of the entire technical system in which the part is installed.

[0005] The use of fumed silica in thermally conductive compositions to reduce sedimentation behavior is known from the prior art. However, this additive has the drawback of adversely affecting the thermal conductivity of the finished product. Other anti-settling substances are known, for example, from CN 104693806. This document discloses a series of anti-settling substances, but does not indicate the particularly advantageous properties of the individual anti-settling substances, or the specific features of these anti-settling substances that would be particularly relevant for the intended application.

[0006] A further disadvantage of anti-settling substances known in the prior art is that they adversely affect the rheology of the composition before curing. The addition of known anti-settling substances can increase the viscosity at high shear rates to such an extent that metering is impaired. Poor metering makes the production of the desired end product more complicated and reduces the resource and cost efficiency of the production of each product. Furthermore, high viscosity impairs the flow behavior when applying the composition to a surface or when injecting the composition into a mold or gap, so that a uniform distribution of the composition before curing is not ensured. Non-uniform distribution of the composition leads to insufficient or no heat dissipation. WO 2009 / 032212 discloses compositions having a high proportion of fumed aluminum oxide (at least 5% to 80% by weight). This reference is specifically directed to achieving high filler loadings, and the disclosure is not directed to properties of the compositions with respect to settling.

[0007] Therefore, there is a need for efficient and specific anti-settling substances. Such substances are efficient if they provide a strong effect by adding a small amount of additive, and therefore are more cost-effective and resource-saving. Such substances are specific if they specifically reduce or completely prevent settling without compromising the processability, meterability and thermal conductivity of the formulation, as compared to the use of anti-settling substances known in the prior art, such as fumed silica. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] International Publication No. 2009 / 032212 Brochure Summary of the Invention [Problem to be solved by the invention]

[0009] It was therefore an object of the present invention to provide an anti-settling agent for thermally conductive compositions that acts efficiently and specifically to reduce or completely prevent the settling of thermally conductive particles, especially when the proportion of said particles is low to moderate. [Means for solving the problem]

[0010] overview Surprisingly, this objective was achieved with a BET surface area of ​​15 m 2 / g~200m 2 It has been found that this can be achieved by incorporating into the composition fumed aluminum oxide in a proportion of less than 5% by weight of the composition, with the composition having a viscosity of 100 .mu.m / g.

[0011] The present invention therefore relates to a composition comprising thermally conductive particles, the composition having a BET surface area of ​​15 m 2 / g~200m 2 / g and further comprising less than 5% by weight of the composition of fumed aluminum oxide.

[0012] The present invention further relates to a method for producing a thermally conductive polymer composition, the method comprising: 2 / g~200m 2 / g to the composition in an amount of less than 5% by weight of the composition.

[0013] The present invention also provides a method for reducing settling of thermally conductive particles in a polymer composition, comprising: 2 / g~200m 2 The present invention also relates to the use of fumed aluminum oxide, wherein the fumed aluminum oxide has a molecular weight of 1.0 to 1.0 g / g.

[0014] Detailed Description Unless otherwise stated, the numerical parameters and ranges set forth in the following description and the appended claims are approximate. Thus, unless otherwise stated, all numerical values ​​expressing values, ranges, amounts, or percentages may be read as being prefixed with the word "approximately", even if the term is not explicitly prefixed. Notwithstanding the fact that the numerical ranges and parameters describing the broad scope of the invention are approximate, the numerical values ​​of the specific experimental examples are described as precisely as possible. However, all numerical values ​​contain errors necessarily resulting from the standard deviation of their measurements.

[0015] Each numerical range recited herein includes all subranges contained therein. For example, a range of "1 to 10" is intended to include all subranges between and including the stated minimum value of 1 and the stated maximum value of 10, i.e., all subranges beginning with a minimum value of 1 or more and ending with a maximum value of 10 or less, e.g., 1 to 6.3, or 5.5 to 10, or 2.7 to 6.1. In the context of this disclosure, all endpoints of the ranges and / or values ​​within these ranges may be combined.

[0016] As used herein, the term "comprising" is understood to be open-ended and not to exclude the presence of additional components, materials, components, process steps, etc., not delineated or mentioned. The terms "including," "containing," "formed from," and similar terms are understood to be synonymous with "comprising." As used herein, the term "consisting of" excludes the presence of unspecified elements, components, process steps, etc. Although the present disclosure is described in terms of "comprising," "consisting of" or "consisting essentially of" are also within the scope of the present disclosure.

[0017] In the context of the present disclosure, the phrases "consisting essentially of" and "essentially formed from" a material mean that the corresponding component is primarily formed from the specified material, with other materials present in small amounts at most. The other materials are usually not intentionally added, and if present, result from, for example, impurities or incomplete separation. The other materials are usually present in such small amounts that they do not significantly affect the properties of the target component. For example, "consisting essentially of" and "essentially formed from" in this specification can mean that each component, such as each aggregate, particle, or prepolymer, is formed from or contains only the target material to the extent of 95% by weight or more, preferably 99% by weight or more, more preferably 99.5% by weight or more, and particularly preferably 99.9% by weight or more.

[0018] Unless the context clearly dictates otherwise, the singular forms "one" and "the" include the plural.

[0019] The amounts disclosed herein are specified in weight percent of the components of the compositions of the present invention and, unless otherwise specified, refer to the total weight of the composition.

[0020] The term "polymer" as used herein is understood to include both homopolymers, i.e. polymers derived from one type of monomer, and copolymers, i.e. polymers derived from two or more different types of monomers. In this context, the term "prepolymer" refers to a polymer that can be crosslinked and thus cured, for example chemically, thermally or by irradiation, optionally using catalysts and / or crosslinking agents. In the context of this specification, it is preferred that the prepolymer is liquid or free-flowing. This means that a free-flowing prepolymer has a viscosity of 10 mPa·s to 100,000 mPa·s (at 25°C and a shear rate of 10 s -1 This means that the viscosity of the polymer may also include medium to high viscosity polymers having a viscosity of 100 .mu.m or less (measured at 100 .mu.m).

[0021] The specific surface area or BET surface area dimensions listed herein refer to specific surface area on a mass basis and are in g / m unless otherwise specified. 2 All specific surface areas disclosed herein were determined by BET analysis, the technical details of which are known to those skilled in the art, inter alia, from DIN ISO 9277.

[0022] The thixotropy index referred to in this specification is given by the formula TI=η(γlow) / η(γhigh), where η(γlow) is the viscosity at low shear rate and η(γhigh) is the viscosity at high shear rate. All thixotropy data in this specification are based on the 1 s -1 at a low shear rate of 100 s -1 Each viscosity is based on a high shear rate of 1000 rpm. ... 2 / g~200m 2 / g of fumed aluminum oxide. Viscosity is measured as described in the Experimental Examples.

[0023] In the context of this specification, a thermally conductive substance or material, in particular a thermally conductive particle, may be a substance or material having a thermal conductivity of at least 1.0 W / mK, preferably at least 1.5 W / mK, more preferably at least 1.8 W / mK. Methods for measuring the thermal conductivity of a substance are known to those skilled in the art. Thermal conductivity can be measured, inter alia, by heat flow calorimetry.

[0024] The particles and aggregates described herein may also be described by D50, D10 and / or D90 particle size. The D50 particle size, also called the median, indicates the particle size of the volumetric particle size distribution below or above which 50% of all particles lie. The D10 particle size accordingly indicates the particle size of the volumetric particle size distribution below which 10% of all particles lie. The D90 particle size accordingly indicates the particle size of the volumetric particle size distribution below which 90% of all particles lie. The particle size and aggregate size mentioned herein refer to the D50 value of the particle size distribution and aggregate size distribution, respectively, unless otherwise stated, which was measured by laser diffraction in accordance with ISO22412:2017.

[0025] The composition according to the present invention comprises at least one prepolymer. It may be a prepolymer selected from silicone, polyether, polyepoxide, polyurethane, polyacrylate, polymethacrylate, silane-modified polymer, and combinations thereof. At least one prepolymer is preferably selected from silicone. At least one prepolymer may be modified, in particular end-modified. That is, at least one prepolymer has a reactive functional group at at least one position, preferably at least two positions. This functional group can react either with a crosslinking agent or with another functional group of the prepolymer. Depending on the chemical nature of the crosslinking, this may require a catalyst or an external energy supply.

[0026] Thus, the composition can be cured by at least one crosslinking agent, at least one catalyst, heating, and / or irradiation.The curing agent or method used in each case depends on the prepolymer selected, and two or more of the above curing agents or methods can be used simultaneously.For example, silicone prepolymer can be terminally modified with vinyl groups, which react with SiH crosslinking agent at high temperature in the presence of platinum catalyst to cure the composition.

[0027] Thus, the total amount of at least one prepolymer may contain one or more components depending on the prepolymer used or the curing method used. For example, a prepolymer to be cured by a crosslinker and a catalyst may contain two components. The first component may contain a portion of the prepolymer and a crosslinker dissolved or dispersed therein, and the second component may contain another portion of the prepolymer and a catalyst dissolved or dispersed therein.

[0028] The at least one prepolymer may be present in the composition of the present invention in a total amount of from 1% to 75% by weight, preferably from 5% to 50% by weight.

[0029] The second component of the composition according to the invention is thermally conductive particles. These thermally conductive particles include graphene, quartz, aluminum nitride, boron nitride, silicon carbide, and zeolites having a BET surface area of ​​0.01 m. 2 / g~20m 2 Particularly preferred are aluminum oxides having a BET surface area of ​​0.01 m / g, and combinations thereof. 2 / g to 20 m2 / g, and particularly preferably aluminum oxide having a BET surface area of ​​0.05 m 2 / g~15m 2 / g of aluminum oxide. This aluminum oxide fraction, if present, is distinct from the fraction of fumed aluminum oxide according to the invention, which acts as an anti-settling agent. When the thermally conductive particles are aluminum oxide particles, two different aluminum oxide fractions are present in the composition. In particular, when fumed aluminum oxide and aluminum oxide are present in the composition as thermally conductive materials, they differ in terms of their BET surface area. Furthermore, the two aluminum oxide fractions may differ in terms of average particle size or particle shape.

[0030] The thermally conductive particles may preferably be present in the form of spherical particles. The spherical particles are particularly suitable for thermally conductive plastic applications due to their dense spherical packing. These particles may have a size between 0.1 μm and 200 μm, preferably between 0.5 μm and 150 μm. The thermally conductive particles particularly advantageously comprise at least a first and a second fraction of thermally conductive particles. The first fraction comprises thermally conductive particles having a D50 size at least 5 times, preferably at least 10 times, more preferably at least 15 times smaller than the D50 size of the particles of the second thermally conductive particle fraction. This ensures a particularly dense packing of the thermally conductive particles, which improves the thermal conductivity of the cured composition. To achieve a particularly dense packing, it is preferred that the first and second fractions of thermally conductive particles are present in a ratio of 7:3 to 3:7, preferably 6:4 to 4:6.

[0031] The thermally conductive particles may be present in the composition in a total amount of from 30% to 95% by weight, preferably from 50% to 95% by weight.

[0032] As already mentioned, the above objectives are achieved according to the invention by providing a ferroelectric material having a BET surface area of ​​15 m 2 / g~200m 2 / g, which can be achieved by adding fumed aluminum oxide to the composition in a proportion of less than 5% by weight of the composition.

[0033] The fumed aluminum oxide is preferably present in the form of aggregates. Such aggregates are known to those skilled in the art to be primary particles held together and preserved by sintering. These primary particles should preferably be small in relation to the aggregates. The size of the primary particles forming the aggregates is therefore preferably at least 10 times, particularly preferably 25 times, smaller than the size of the aggregates. Furthermore, the average size of the aggregates is preferably between 50 nm and 1 μm, preferably between 100 and 800 nm. If the aggregates are too small, the viscosity at low shear rates is adversely affected. However, if the aggregates are larger than 1 μm, they tend to settle out of their own accord. The BET surface area of ​​the fumed aluminum oxide is 15 m 2 / g~200m 2 / g, preferably 25m 2 / g~200m 2 / g.

[0034] The ratio of BET surface area to aggregate size of fumed aluminum oxide can also be expressed by the efficiency index, which is the product of aggregate size and the BET surface area of ​​the aggregate (dAgg × BET), expressed in mm 3 In order to inhibit the settling of the thermally conductive particles in the composition particularly efficiently, the efficiency index of the fumed aluminum oxide is preferably 3 mm 3 / kg~100mm 3 / kg.

[0035] The fumed aluminum oxide according to the present invention may be hydrophobically modified. The hydrophobically modified improves the compatibility of the anti-settling agent with the prepolymer matrix, thus improving the incorporation and dispersibility compared to unmodified fumed aluminum oxide. The fumed aluminum oxide may be modified with, for example, silicone oil, octamethylcyclotetrasiloxane, hexamethyldisilazane, dimethyldichlorosilane, or a combination thereof.

[0036] The fumed aluminum oxide may be present in the composition according to the invention in a total amount of 0.05% to 5% by weight, preferably 0.1% to 4% by weight, particularly preferably 0.3% to 3% by weight, based on the composition.

[0037] The compositions according to the invention may advantageously be characterized by a thixotropy index TI between 6 and 80, preferably between 10 and 50. Such a thixotropy index is favorable in that even small additions of the fumed aluminum oxide according to the invention can significantly increase the viscosity of the composition at low shear rates, greatly reducing or ideally completely preventing settling of the thermally conductive particles during storage of the composition. Furthermore, the viscosity increases only slightly even at high shear rates, which allows the composition to be easily metered and processed.

[0038] In addition to the above, the composition according to the invention may also contain further components as additives. The additives used may be, for example, organic and inorganic pigments, dyes, pH adjusters, flame retardants, susceptors, stabilizers, processing aids, or mixtures and combinations thereof. Examples of pigments are titanium dioxide, ferrites, zirconium dioxide, and carbon black. Suitable stabilizers are phenols, in particular sterically hindered phenols. One additive or a mixture of two or more additives may be present in the powder according to the invention. The suitable additives are in each case used in an amount suitable for the desired purpose. The typical amounts used are known to those skilled in the art. The total amount of additives relative to the total weight of the composition may be, for example, at most 10% by weight, at most 6% by weight, at most 3% by weight, at most 2% by weight, at most 1% by weight, at most 0.5% by weight, at most 0.25% by weight, at most 0.2% by weight, at most 0.1% by weight, or at most 0.05% by weight. In a preferred embodiment of the invention, the composition according to the invention is essentially free of additives. That is, if additives are present in the composition, they are present only as impurities. In a further preferred embodiment of the present invention, the composition according to the present invention does not contain any additives.

[0039] The present invention further relates to a method for producing a thermally conductive composition, the method comprising the steps of: 2 / g~200m 2 / g to the composition in an amount of less than 5% by weight of the composition.

[0040] The fumed aluminum oxide may be incorporated into the composition before, after or in parallel with the thermally conductive particles. Thus, the method according to the invention may comprise a step of first dosing or adding the fumed aluminum oxide to the thermally conductive particles. The fumed aluminum oxide is preferably mixed homogeneously with the thermally conductive particles. For this purpose, dry mixing processes known to those skilled in the art may be used. The fumed aluminum oxide and / or the thermally conductive particles may be incorporated by standard mixing techniques for (free-flowing) solid and liquid or viscous polymeric materials, such as compounding.

[0041] Depending on the prepolymer used, the compositions according to the invention can be used in a variety of technical applications, including, among others, adhesives, fillers, sealants, and thermally conductive articles and parts.

[0042] For this purpose, the composition according to the invention may be shaped into an article or part and cured at the same time by conventional techniques such as pressing, (injection) casting or moulding, optionally at high temperature and / or pressure. Alternatively, the composition according to the invention in the uncured state may be applied to at least a part of the surface of an article or part and then subjected to a curing process as described above.

[0043] The following examples are intended to illustrate compositions according to the invention and their uses according to the invention, without limiting the invention thereto. EXAMPLES

[0044] Working Example Preparation of Formulations Composition 1 (basic formulation) (non-inventive) - 8.12% by weight of silicone polymer VS200 (Evonik) - 86% by weight of spherical aluminum oxide particles BAK-40 (40 μm) / BAK-2 (2 μm) 60 / 40 (manufactured by Bestry) - 3.52% by weight of the inhibitor mixture 1-ethynyl-1-cyclohexanol (Aldrich) (as a 2% mixture in silicone polymer VS200) - 0.6 wt% KAT511 platinum catalyst (Evonik) (as a 10% mixture in silicone polymer VS200) - 1.76% by weight of SiH crosslinker Crosslinker 100 (manufactured by Momentive)

[0045] Composition 2 (Inventive) - 6.12% by weight of silicone polymer VS200 (Evonik) - 86% by weight of spherical aluminum oxide particles BAK-40 (40 μm) / BAK-2 (2 μm) 60 / 40 (manufactured by Bestry) - 2% by weight of aluminum oxide particles (AEROXIDE® Alu C 805 or Alu 45, Evonik Industries). AEROXIDE® Alu C 805 corresponds to the surface-modified fumed aluminum oxide mentioned above, AEROXIDE® Alu 45 is unmodified. - 3.52% by weight of the inhibitor mixture 1-ethynyl-1-cyclohexanol (Aldrich) (as a 2% mixture in silicone polymer VS200) - 0.6 wt% KAT511 platinum catalyst (Evonik) (as a 10% mixture in silicone polymer VS200) - 1.76% by weight of SiH crosslinker Crosslinker 100 (manufactured by Momentive)

[0046] Dry mixing of fillers The fillers (BAK-40 / BAK-2 60 / 40 or BAK-40 / BAK-2 60 / 40 + aluminum oxide particles) are premixed using a dry mix process in a Hauschild Speedmixer. The fillers are weighed into the Speedmixer beaker and mixed for 2000 minutes. -1 Homogenize for 4 minutes at 35°C. Homogenize in up to 5 steps as needed for heating.

[0047] Preparation of compounds First, 6.12 wt% of the silicone polymer VS200, 3.52 wt% of the inhibitor mixture 1-ethynyl-1-cyclohexanol, and 0.6 wt% of the KAT511 platinum catalyst were mixed in a Hauschild Speedmixer for 2000 min. -1 Then, the filler mixture from the dry mix process (BAK-40 / BAK-2 60 / 40 or BAK-40 / BAK-2 60 / 40 + aluminum oxide particles) is added at 2000°C for 15 seconds. -1 Disperse the mixture in water for 60 seconds four times. Then, add 1.76% by weight of the SiH crosslinker Crosslinker 100 for 2000 minutes. -1 Mix twice for 30 seconds at RT.

[0048] Specimen preparation Crosslinking of test pieces of the compound with a thickness of 6 mm and a diameter of 55 mm is carried out in a hot press at a pressure of 100 bar and a temperature of 120° C. for 10 minutes. The test pieces are then post-crosslinked in an oven at 200° C. for 4 hours.

[0049] Measurement of thixotropy index Determination of the rheological properties of liquid silicone with aluminum oxide as filler. Viscosity [Pa s] describes the property of a substance to flow and deform irreversibly under the influence of stress. The shear rate is a function of the speed of the measuring cone [m / s] and the distance between the measuring cone and the plate [m].

[0050] The filled liquid silicone sample must be kept in the measurement room for at least 4 hours to reach ambient temperature before the viscosity measurement. A Haake RheoStress1 rheometer from Thermo Scientific is used with the RheoWin control program. The measurements are performed at a rate of 1 s -1 ~100 seconds -1 The shear rate is controlled by a measurement geometry of C20 / 2°Ti cone and measurement plate attachment MPC35 with a cone-plate separation distance of 0.105 m.

[0051] Thermal Conductivity Measurement The thermal conductivity of the cross-linked specimens was measured according to ASTM D7984 using a measurement technique based on the unsteady plane heat source method for measuring thermal conductivity.

[0052] Aggregate size measurement To measure the hydrophilic aggregates of, for example, AEROXIDE® Alu 45, a 1 wt.% aqueous dispersion is prepared. First, 0.2 g of hydrophilic material is placed in a 20 mL sonication vessel to which 19.8 g of demineralized water is added. Dispersion is performed using a commercial ultrasonic finger. The dispersion finger is immersed 1.5 cm into the dispersion. The sample is sonicated for 5 minutes at half the power of the device.

[0053] To measure the hydrophobic aggregates of, for example, AEROXIDE® Alu C 805, a 1 wt% dispersion in ethanol is prepared. First, 0.2 g of hydrophobic material is placed in a 20 mL sonication vessel. To this, 20 g of ethanol and 40 g of high molecular weight wetting additive are added. Disperse using a commercial ultrasonic finger. Immerse the dispersion finger 1.5 cm into the dispersion. Sonicate the sample for 5 minutes at half the power of the instrument.

[0054] Depending on the optical density, place 500-2500 mg of the dispersion in a cuvette and fill to 2500 mg with the dispersion medium. This cuvette is then used to measure the size distribution. For the measurement, use a dynamic light scattering instrument that complies with ISO22412:2017.

[0055] [Table 1-1]

[0056] [Table 1-2]

[0057] result From the table it can be seen that products containing fumed aluminum oxide having a BET surface area within the range of the present invention have particularly high efficiency even at low loadings without reducing the thermal conductivity of the finished product, especially when the product is further hydrophobized.

Claims

1. At least one prepolymer and at least one fraction of thermally conductive particles, the BET surface area being greater than or equal to 15 m. 2 / g to 200m 2 / g (DIN ISO 9277), The composition, wherein the fumed aluminum oxide is present in an amount of less than 5% by weight based on the composition.

2. 2. The composition of claim 1, wherein the fumed aluminum oxide has an aggregate size of 50 nm to 1 μm (laser diffraction according to ISO 22412:2017), preferably 100 nm to 800 nm.

3. The efficiency index of the fumed aluminum oxide is 3 mm 3 / kg to 100mm 3 3. The composition of claim 1 or claim 2, wherein the efficiency index is the product of aggregate size and BET surface area.

4. - from 1% to 75% by weight, preferably from 5% to 50% by weight, of at least one prepolymer, - 30% to 95% by weight, preferably 50% to 95% by weight, of thermally conductive particles, and / or - 0.05% to 5% by weight, preferably 0.1% to 4% by weight of fumed aluminum oxide. The composition according to any one of claims 1 to 3, comprising:

5. The composition according to any one of claims 1 to 4, wherein the prepolymer is selected from silicones, polyethers, polyepoxides, polyurethanes, poly(meth)acrylates, silane-modified polymers, and combinations thereof, preferably selected from silicones.

6. The thermally conductive particles are graphene, quartz, aluminum nitride, boron nitride, silicon carbide, and have a BET surface area of ​​0.01 m 2 / g to 20m 2 / g aluminum oxide, and combinations thereof.

7. The thermally conductive particles have a BET surface area of ​​0.01 m 2 / g to 20m 2 / g, preferably 0.05m 2 / g to 15m 2 7. The composition of claim 6, wherein the aluminum oxide is selected from the group consisting of 0.1 to 1.0 g of aluminum oxide.

8. The composition according to any one of claims 1 to 7, wherein the thermally conductive particles are in the form of spherical particles.

9. The composition according to claim 8, wherein the size of said spherical particles is between 0.1 μm and 200 μm, preferably between 0.5 μm and 150 μm.

10. The composition of any one of claims 1 to 9, wherein the fumed aluminum oxide is hydrophobically modified.

11. 11. The composition of claim 10, wherein the fumed aluminum oxide is modified with silicone oil, octamethylcyclotetrasiloxane, hexamethyldisilazane, dimethyldichlorosilane, or combinations thereof.

12. 12. The composition according to any one of claims 1 to 11, wherein the thermally conductive particles comprise at least one first and a second thermally conductive particle fraction, the particle size D50 of the first fraction being at least 5 times, preferably at least 10 times, more preferably at least 15 times smaller than the particle size D50 of the second fraction.

13. The composition according to any one of claims 1 to 12, which is cured by means of at least one crosslinking agent, at least one catalyst, heat and / or radiation.

14. A method for producing a thermally conductive polymer composition, comprising: BET surface area is 15m 2 / g to 200m 2 / g to said composition in an amount of less than 5% by weight based on said composition.

15. A polymer composition having a BET surface area of ​​15 m to reduce settling of thermally conductive particles in the polymer composition. 2 / g to 200m 2 / g of fumed aluminum oxide.

Citation Information

Patent Citations

  • Thermal interface materials

    WO2009032212A1