Heat prevention and insulation / wave transmission integrated nanopore silicon resin-based composite material as well as preparation method and application thereof

By introducing nanopore structures and fiber prefabricated bodies into resin-based wave-transmissive materials, the problem of insufficient insulation performance of resin-based wave-transmissive materials at high temperatures is solved, and efficient heat insulation and wave-transmissive performance is achieved, suitable for aircraft Radar equipment and other fields.

CN118931205AActive Publication Date: 2024-11-12EAST CHINA UNIV OF SCI & TECH

Patent Information

Application Number
CN202411253965.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-12
Estimated Expiration
2044-09-09

AI Technical Summary

Technical Problem

The existing resin-based wave-transmissive materials have insufficient thermal insulation performance at high temperatures, which limits their application in radar equipment and other fields, and the molding process is complex and costly.

Method used

Develop an integrated thermal insulation/wave-transmissive nanopore silicone resin-based composite material, and form an organic-inorganic with nanopore structure by using raw materials such as polysiloxane, silane monomer/silane prepolymer and alkaline catalyst. The resin matrix and combined with the fiber preforms, a material with excellent heat insulation and wave transmissive properties was prepared through a sol-gel reaction and drying process.

Benefits of technology

It realizes materials that have both heat insulation and wave transmission functions under a single structure, reduces the transmission loss of electromagnetic waves, improves wave transmission performance and ablation resistance at high temperatures, and is suitable for aircraft radar radomes and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931205A_ABST
    Figure CN118931205A_ABST
Patent Text Reader

Abstract

The invention relates to a heat insulation / wave transmission integrated nanopore silicon resin-based composite material and a preparation method and application thereof, the composite material comprises a matrix and a reinforcing phase, the matrix comprises nanopore silicon resin, and the reinforcing phase comprises a fiber preform; the nanopore silicon resin is prepared from the following raw materials: polysiloxane, a silane monomer / silane prepolymer and a basic catalyst. Compared with the prior art, the composite material is endowed with excellent ablation resistance, heat insulation and low dielectric properties by utilizing the nanopore silicon resin. The composite material can be subjected to molecular-scale in-situ ceramization reaction at a high temperature, so that the formation of a continuous carbon pathway is effectively hindered, and the composite material has the wave transmission rate of 90% or above at the room temperature of 1200 DEG C below zero and within the wave band of 2-18 GHz, and can be used as a high-temperature heat prevention and insulation / wave transmission integrated material in the fields of aircraft radomes, antenna windows and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of heat-insulating materials, and in particular to a heat-insulating / wave-transmitting integrated nanoporous silicone resin-based composite material and a preparation method and application thereof. Background Art

[0002] Electromagnetic wave communication equipment, mainly represented by radar, plays an increasingly important role in modern warfare and is an indispensable detection tool. The detection capability of radar equipment is not only related to the performance of its own electromagnetic wave transmitting and receiving devices, but also to the working environment of its internal precision components. Therefore, the shell material needs to protect the normal operation of the aircraft's communication, telemetry, guidance, detonation and other systems in harsh environments, which puts forward the requirements for light weight, high temperature resistance, ablation resistance and high efficiency heat insulation for wave-transmitting materials.

[0003] At present, the commonly used wave-transparent materials can be divided into two categories: ceramic-based wave-transparent materials and resin-based wave-transparent materials. The dielectric loss of ceramic-based wave-transparent materials at high temperatures will increase significantly due to the conductivity generated by vacancy ionization, and the molding process is complex and the preparation cost is high. In comparison, resin-based composite materials have better dielectric stability, better mechanical and thermal insulation properties, relatively simple molding process, short production cycle and relatively low cost. They have been widely used in various wave-transparent materials. Among them, silicone resin, due to its low dielectric constant and dielectric loss, can accommodate a larger wall thickness to improve the strength of the antenna wave-transparent cover, and has excellent thermal stability. It is one of the current research hotspots of resin-based wave-transparent materials. However, silicone resin has poor thermal insulation performance and wave transmission performance needs to be improved, which limits its application.

[0004] Therefore, developing an integrated heat-insulating / wave-transparent silicone-based composite material is an urgent need in the current field. Summary of the invention

[0005] The purpose of the present invention is to provide a heat-proof / wave-transmitting integrated nanoporous silicone resin-based composite material and a preparation method and application thereof, wherein the material has heat-proof and wave-transmitting functions.

[0006] The object of the present invention can be achieved by the following technical scheme: an integrated heat-insulating / wave-transmitting nanoporous silicone resin-based composite material, comprising a matrix and a reinforcing phase, wherein the components of the matrix include nanoporous silicone resin, and the reinforcing phase includes a fiber preform;

[0007] The raw materials of the nanoporous silicone resin include polysiloxane, silane monomer / silane prepolymer and alkaline catalyst.

[0008] The silicone resin matrix of the composite material of the present invention is composed of organic-inorganic resin composed of polysiloxane, silane monomer / silane prepolymer and catalyst, and the reinforcing phase is a fiber preform of different types, densities and structural forms.

[0009] Preferably, the polysiloxane has a long chain structure, the main chain is composed of Si-O-Si, and the side chain groups include organic groups and reactive groups.

[0010] Further preferably, the organic group includes -CH 3 , -C 6 H 5 .

[0011] Further preferably, the reactive groups include Si-OH, -OCH 3 、-OC 2 H 5 .

[0012] Further preferably, the molecular weight of the polysiloxane is 2000-5000, and the reactive groups Si-OH, -OCH 3 、-OC 2 H 5 The content is 10-25wt%. Silicone itself has good antioxidant properties. By adjusting the molecular weight and the content of reactive groups, the crosslinking degree of the sol-gel reaction can be effectively controlled, thereby regulating the average pore size and pore structure of the silicone resin matrix. If the crosslinking degree is too low, the resulting silicone resin matrix lacks a complete skeleton structure, and the material is difficult to form; if the crosslinking degree is too high, the pore size structure is small, and the capillary force is large during drying, resulting in shrinkage and cracking. The molecular weight and active group content of the polysiloxane control a moderate degree of crosslinking, which gives the material a relatively complete pore structure and air insulation layer, with an average pore size of 20-70nm, which can effectively reduce gas-phase and solid-phase heat conduction, so the anti-insulation performance of the composite material is improved. In addition, the size of the nanopores is much smaller than the wavelength of electromagnetic waves in the communication frequency band, which can reduce the reflection and scattering of electromagnetic waves inside the material, reduce the material's dissipation of electromagnetic waves, and improve wave transmission performance.

[0013] Preferably, the silane monomers include all di- and tri-functional silane monomers.

[0014] Preferably, the silane prepolymer includes one or more of a silane monomer polymer obtained by polymerizing a difunctional or trifunctional silane monomer and other silane prepolymers.

[0015] More preferably, the other silane prepolymers include polyhedral oligomeric silsesquioxane (POSS) and low molecular weight silicone resin.

[0016] More preferably, the silane monomer / silane prepolymer is not limited to one kind thereof, and one or more silane monomers, silane monomer polymers, POSS, and low molecular weight silicone resins can be added into the silicone resin matrix as silicon sources.

[0017] More preferably, the POSS is an inorganic core composed of a silicon-oxygen skeleton alternately connected by Si-O, with a molecular weight of 530-1300, and its top corner groups include Si-OH, -OCH 3 、-CH 3 and -C 6 H 5 POSS can provide a large free volume, which reduces the number of polar molecules per unit volume and can effectively reduce the dielectric constant of the composite material.

[0018] More preferably, the low molecular weight silicone resin also has Si-O-Si as the main chain, a molecular weight of 500-1000, and its side chain groups include -CH 3 , -C 6 H 5 Organic groups such as Si-OH, -OCH 3 、-OC 2 H 5 As a capping agent.

[0019] Further preferably, the method for preparing the silane monomer polymer comprises the following steps: dissolving the silane monomer and the surfactant in an alcohol solvent, adjusting the pH, and performing reduced pressure distillation after the silane reaction is complete to obtain the silane monomer polymer.

[0020] More preferably, the mass ratio of the surfactant to the silane monomer is (0.1-0.3):(1-3).

[0021] More preferably, the surfactant includes hexadecyltrimethylammonium bromide and hexadecyltrimethylammonium chloride.

[0022] More preferably, the alcohol solvent includes methanol, ethanol, and isopropanol. Methanol, ethanol, isopropanol, etc. are organic solvents with low surface tension and boiling points of about 80°C. This characteristic promotes the volatilization of the alcohol solvent during aging and drying to form a nanoporous structure, which is beneficial to improving the heat insulation performance of the composite material.

[0023] More preferably, a TMOH (tetramethylammonium hydroxide) solution is used to adjust the pH to 8-9, and after the silane monomer reacts completely, the mixture is distilled under reduced pressure.

[0024] More preferably, the silane monomer polymer is polymerized from one or more difunctional or trifunctional silane monomers, with Si-O-Si as the main chain and -CH 3, -C 6 H 5 The main organic groups are -OCH 3 、-OC 2 H 5 As a capping agent.

[0025] Further preferably, the silane monomers include all di- and tri-functional silane monomers, and some containing specific groups such as phenyl and fluorine-containing groups are more preferred, that is, the silane monomers are preferably phenyl-containing silanes and fluorine-containing group silanes. The introduction of phenyl groups can effectively avoid the degradation of the side chain groups of the silicone resin under high temperature conditions and improve the thermal stability of the silicone resin. The 2s and 2d orbitals of the fluorine atom can reduce the electric effect of the external electric field and reduce the polarizability of the resin matrix. At the same time, the free volume of the fluorine-containing group is large, and the number of polar molecules per unit volume is reduced. The above characteristics of the fluorine-containing group are conducive to reducing the dielectric constant of the resin matrix, thereby improving the wave transmission performance.

[0026] More preferably, the di- or tri-functional silane monomers include methylphenyldimethoxysilane, diphenyldimethoxysilane, phenyltrimethoxysilane, methylphenyldiethoxysilane, diphenyldiethoxysilane, phenyltriethoxysilane, trifluoromethyltrimethoxysilane and the like.

[0027] Preferably, the alkaline catalyst comprises tetramethylammonium hydroxide (TMOH), ammonia (NH 3 ·H 2 O), urea (CO (NH 2 ) 2 ). The alkaline catalyst can catalyze the dehydration condensation between Si-OH without introducing other organic / inorganic groups.

[0028] Preferably, the fiber preform is woven from at least one of inorganic fibers having wave-transmitting properties.

[0029] Further preferably, the inorganic fiber includes quartz fiber, boron nitride fiber, silicon nitride fiber, alumina fiber or basalt fiber. The common feature of the above fibers is that they have a lower dielectric constant and loss, which is beneficial to reducing the transmission loss of electromagnetic waves.

[0030] Preferably, the fiber preform structure comprises acupuncture, stitching, 2.5D, 3D and orthogonal three-dimensional.

[0031] A method for preparing the above-mentioned integrated heat-insulating / wave-transmitting nanoporous silicone resin-based composite material comprises the following steps:

[0032] (1) Preparation of organic silica sol: silane monomer / silane monomer polymer, other silane prepolymers, polysiloxane and water are mixed in an alcohol solvent, stirred in an ice-water bath until completely hydrolyzed, an alkaline catalyst is added, and stirring in an ice-water bath is continued until the solution is clear to obtain a uniform organic silica sol;

[0033] (2) Pouring of organosilicon sol: placing the fiber preform in a mold, and pouring the prepared organosilicon sol into the mold, repeatedly until the fiber preform is completely impregnated with the organosilicon sol, and closing the injection port to seal the mold;

[0034] (3) Reaction gelation and aging: placing the mold in a high temperature environment to allow the organosilicon sol to undergo a gelation reaction and further age to obtain a wet gel composite material;

[0035] (4) Drying: Drying the wet gel composite material at high temperature to obtain a heat-insulating / wave-transmitting integrated nanoporous silicone resin-based composite material.

[0036] Preferably, the preparation of the organic silica sol comprises the following steps: mixing silane monomer / silane monomer polymer (i.e., silane monomer or silane monomer polymer) with other silane prepolymers, adding polysiloxane and water in batches, continuing to stir in an ice-water bath until completely hydrolyzed, and finally adding an alkaline catalyst, continuing to stir in an ice-water bath until the solution is clear, to obtain a uniform organic silica sol.

[0037] Preferably, the mass ratio of the silane monomer / silane monomer polymer, other silane prepolymers, water and polysiloxane in step (1) is (1-3): (0.4-0.7): (0.2-1): (1-9).

[0038] Preferably, when the silane monomer is used as the raw material in step (1), the silane monomer, the surfactant and other silane prepolymers are mixed, and then the polysiloxane and water are added in batches.

[0039] More preferably, the mass ratio of the silane monomer, other silane prepolymers, surfactant, water and polysiloxane is (1-3): (0.4-0.7): (0.1-0.3): (0.2-1): (1-9).

[0040] Further preferably, the surfactant includes hexadecyltrimethylammonium bromide and hexadecyltrimethylammonium chloride.

[0041] Preferably, in the organic silica sol of step (1), the mass fraction of the alkaline catalyst is 0.1%-0.5%.

[0042] Preferably, the polysiloxane in step (1) is added in batches at intervals of 5-20 minutes. By gradually adding the polysiloxane in batches, the polysiloxane can be fully contacted with the active sites of the silane monomer / silane prepolymer, thereby enhancing the reaction activity of the subsequent sol-gel.

[0043] Preferably, the ice water bath in step (1) needs to be in 0° C. circulating water, the purpose of which is to prevent the organic silicon sol from solidifying at room temperature after the catalyst is added.

[0044] Preferably, the percentage (solid content) of silicon precursor in the organosilicon sol in step (1) to the total mass of silicon precursor and alcohol solvent is 30%-50%. The silicon precursor includes silicon-containing substances such as polysiloxane, silane monomer, silane monomer polymer, and other silane prepolymers.

[0045] Preferably, the pouring of the organic silicon sol in step (2) comprises the following steps: laying the fiber preform flat in a mold, pouring the prepared organic silicon sol into the mold using a circulating injection tank, repeating the process until the fiber preform is completely impregnated with the organic silicon sol, and closing the injection port to seal the mold.

[0046] Preferably, in the injection process of step (2), the silica sol can be injected into the mold by gravity or pressure. Depending on the density of the fiber preform, the pressure of the pressurized injection is 0.5-5 bar.

[0047] Preferably, the perfusion process of the organic silica sol in step (2) needs to be repeated 2-10 times.

[0048] Preferably, the temperature of the reaction gel and aging in step (3) is 60-120° C. and the time is 6-48 h.

[0049] Further preferably, the reaction gel and aging temperature in step (3) is 80-100° C. and the time is 24-48 h.

[0050] More preferably, the reaction gelation and aging process in step (3) can adopt gradient gelation, first placing the mold in an 80°C environment for 10-14 hours, preferably 12 hours, and then raising the temperature to 100°C, which is beneficial to improve the degree of gelation and obtain a wet gel composite material with a more complete skeleton.

[0051] Preferably, the drying temperature in step (4) is 60-120° C. and the drying time is 12-48 hours.

[0052] Further preferably, the process of step (4) adopts gradient drying, and the wet gel composite material is dried at 60° C. and 120° C. for 12-24 hours respectively.

[0053] Preferably, the density of the integrated heat-insulating / wave-transmitting nanoporous silicone resin-based composite material is 0.3-1.3 g / cm 3 The pore size of silicone resin is 20-70nm, the porosity is 50-80%, the room temperature thermal conductivity is 0.035-0.09W / m·K, the dielectric constant is 1.5-2.5, and the loss tangent value is 0.004-0.01.

[0054] An application of the above-mentioned heat-insulating / wave-transmitting integrated nanoporous silicone resin-based composite material is to use the composite material as a high-temperature wave-transmitting material for aircraft.

[0055] Preferably, the composite material is used for aircraft radar radome and antenna window materials.

[0056] The composite material of the present invention is mainly composed of a matrix and a reinforcement phase, wherein the matrix mainly comprises nanoporous silicone resin, the raw materials of which include polysiloxane, silane monomer / silane prepolymer and alkaline catalyst, and the reinforcement phase comprises a fiber preform.

[0057] Compared with the prior art, the present invention has the following beneficial effects:

[0058] 1. The material of the present invention can realize multiple functions such as heat insulation and wave transmission under a single structure, and can be applied to radar antenna covers and antenna window materials of high-speed aircraft.

[0059] 2. The present invention adopts nanoporous silicone resin as the resin matrix, which reduces the overall density of the composite material and effectively reduces the transmission loss of electromagnetic waves caused by the resin used in traditional high-density, low-porosity wave-transmitting materials.

[0060] 3. The present invention introduces polysiloxane and silane monomer / silane prepolymer as silicon sources, and the two are cross-linked through active sites under the condition of alkaline catalyst, and have an interpenetrating double network structure, which effectively overcomes the shortcomings of low intermolecular force and poor thermal stability of general organic silicone resins. At the same time, the nanoporous structure gives the composite material a lower dielectric constant and better heat insulation performance.

[0061] 4. The organic silicon resin matrix used in the present invention contains organic-inorganic hybrid components, which undergo organic-inorganic transformation at high temperatures to generate a dense ceramic structure, which can effectively improve the ablation resistance and heat insulation performance of the material. At the same time, the generated Si-OC ceramic structure can hinder the formation of connected carbon pathways at high temperatures, reduce the conductivity loss of the material, and greatly improve the high-temperature wave transmission performance of the material. After carbonization, the dielectric constant and loss are within an acceptable range, and the wave transmittance is more than 90% at room temperature -1200°C.

[0062] 5. The present invention uses nanoporous silicone resin to give the composite material excellent ablation resistance, heat insulation and low dielectric properties. The composite material will undergo an in-situ ceramic reaction at a molecular scale at high temperature, effectively hindering the formation of continuous carbon pathways, so that the composite material has a wave transmittance of more than 90% in the room temperature-1200°C and 2-18GHz band, and can be used as a high-temperature heat-insulating / wave-transmitting integrated material in the fields of aircraft radomes, antenna windows, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0063] Figure 1 is a surface photograph of the composite material in Example 1;

[0064] Figure 2 is a scanning electron microscope image of the nanoporous silicone resin matrix in Example 1;

[0065] Figure 3 The back temperature rise curve of the samples of Example 1 and Example 3 heated at 800°C for 600s in a single-sided muffle furnace;

[0066] Figure 4 This is the curve of wave transmittance variation with frequency of the sample in Example 7, with a test frequency of 2-18 GHz. DETAILED DESCRIPTION

[0067] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.

[0068] A heat-insulating / wave-transmitting integrated nanoporous silicone resin-based composite material and a preparation method thereof, the method comprising the following steps:

[0069] S1 (optional): select one or more of the silane monomers and surfactants to be miscible in an alcohol solvent, adjust the pH to a slightly alkaline solution, mix and stir at room temperature for 20-40 minutes until the silane monomers are substantially reacted, and perform reduced pressure distillation on the resulting solution to obtain a polymer of the silane monomers.

[0070] S2: Mix the silane monomer or the obtained silane monomer polymer with other silane prepolymers in an alcohol solvent, add the polysiloxane to the silane prepolymer in three batches under an ice-water bath, and the three batches account for 30%, 30% and 40% of the total mass of the silicone oil respectively in the order of addition, with an interval of 5-20 minutes. Add water as a hydrolysis raw material in batches according to the same mass ratio, and continue to stir until the polysiloxane and the silane monomer / silane prepolymer are completely hydrolyzed. Finally, add 25% tetramethylammonium hydroxide as an alkaline catalyst, stir in an ice-water bath for 10-20 minutes, and obtain an organic silica sol.

[0071] S3: placing the fiber preform in a mold, injecting the organosilicon sol prepared in step S2 into the mold, repeating the process 2-10 times based on the density of the fiber preform and the viscosity of the organosilicon sol, and closing the injection port and sealing the mold after the organosilicon sol completely impregnates the fiber preform.

[0072] S4: The mold is transferred to a high temperature oven for reaction gelation and aging, wherein the gel aging temperature and time are 60-120° C. and 12-48 h, respectively. The mold is opened to take out the obtained wet gel composite material.

[0073] S5: Drying the wet gel composite material obtained in step (4) at 60-120° C. for 12-24 hours, controlling the humidity not to be too high, thereby preparing a heat-insulating / wave-transmitting integrated nanoporous silicone resin-based composite material.

[0074] The following describes it in detail with reference to specific embodiments.

[0075] Unless otherwise specified, the reagents, methods, instruments and equipment used in the present invention are conventional reagents, methods, instruments and equipment in the art. Unless otherwise specified, the reagents and materials used in the following examples are commercially available.

[0076] Example 1

[0077] Step 1. Select methylphenyldimethoxysilane, phenyltrimethoxysilane, trifluoromethyltrimethoxysilane as silane monomers, hexadecyltrimethylammonium bromide as a surfactant, and ethanol as an alcohol solvent, add them into a flask in a molar ratio of 1:2:1:0.3:5, adjust the pH of the solution to slightly alkaline after hydrolysis to provide reaction conditions for silane monomer polymerization, react at room temperature for 30 minutes, and obtain a polymer of the silane monomer after reduced pressure distillation.

[0078] Step 2. Select POSS (vertex groups contain Si-OH, -CH 3 and -C 6 H 5) is other silane prepolymer, POSS is mixed with the polymer of silane monomer and stirred, and ethanol is added to form a uniform silane prepolymer mixture. Polysiloxane is added to the silane prepolymer in 3 batches under an ice-water bath, and the 3 batches account for 30%, 30% and 40% of the total mass of polysiloxane respectively in the order of addition, and the interval time is 10min. Water is added in batches as a hydrolysis raw material according to the same mass ratio, and stirring is continued for 10min until the polysiloxane and silane prepolymer are completely hydrolyzed. Finally, 25% of tetramethylammonium hydroxide is added as an alkaline catalyst, and stirred for 10min under an ice-water bath to obtain a prepared organic silicon sol. Among them, the mass ratio of polysiloxane, silane monomer polymer, POSS, hexadecyltrimethylammonium bromide, ethanol, water, and tetramethylammonium hydroxide is 5:1:0.5:0.19:15:0.5:0.2, and the mass of polysiloxane and silane prepolymer accounts for 30% of the total mass of silicon precursor and ethanol (solid content).

[0079] Step 3. Select the size of 220mm*220mm*10mm and the density of 0.27g / cm 3 The needle-punched quartz fiber preform is used as the reinforcement phase, and the fiber preform is laid in a stainless steel mold. The organic silicon sol prepared according to step (2) is injected into the mold by a pressure-assisted injection method, with an injection pressure of 1 bar, and the process is repeated 3 times. After the organic silicon sol completely impregnates the fiber preform and no bubbles emerge from the glue outlet, the injection port is closed and the mold is sealed.

[0080] Step 4. The mold was transferred to an oven at 80°C for reaction gelation and aging for 12 hours. The temperature was raised to 100°C and aging was continued for 12 hours. The mold was then opened to take out the obtained wet gel composite material.

[0081] Step 5. The wet gel composite material obtained in step (4) was placed in an oven at 60°C and 120°C and dried for 12 hours respectively, thereby obtaining Figure 1 The heat-insulating / wave-transmitting integrated nanoporous silicone resin-based composite material is shown in Table 1. The density and room temperature thermal conductivity test results thereof are shown in Table 1.

[0082] Figure 2 This is a scanning electron microscope image of the nanoporous silicone resin matrix in Example 1, showing that it has a regular nanoporous structure with a pore size of 20-50 nm.

[0083] Example 2

[0084] Example 2 is basically the same as Example 1, except that the size of the sample is 220 mm*220 mm*2 mm and the density is 0.27 g / cm 3The needle-punched quartz fiber preform is used as the reinforcement phase. Its density, average dielectric constant and loss tangent value before and after carbonization at 800℃ at a frequency of 2-18GHz are shown in Table 2.

[0085] Example 3

[0086] Step 1. Select methylphenyldimethoxysilane, phenyltrimethoxysilane, trifluoromethyltrimethoxysilane as silane monomers, hexadecyltrimethylammonium bromide as a surfactant, and ethanol as an alcohol solvent, add them into a flask in a molar ratio of 1:2:1:0.3:5, adjust the pH of the solution to slightly alkaline after hydrolysis to provide reaction conditions for silane monomer polymerization, react at room temperature for 30 minutes, and obtain a polymer of the silane monomer after reduced pressure distillation.

[0087] Step 2. Select POSS (vertex groups contain Si-OH, -CH 3 and -C 6 H 5 ) is other silane prepolymer, POSS is mixed with the polymer of silane monomer and stirred, and ethanol is added to form a uniform silane prepolymer mixture. Polysiloxane is added to the silane prepolymer in 3 batches under an ice-water bath, and the 3 batches account for 30%, 30% and 40% of the total mass of polysiloxane respectively in the order of addition, and the interval time is 10min. Water is added in batches as a hydrolysis raw material according to the same mass ratio, and stirring is continued for 10min until the polysiloxane and silane prepolymer are completely hydrolyzed. Finally, 25% tetramethylammonium hydroxide is added as an alkaline catalyst, and stirred for 10min under an ice-water bath to obtain a prepared organosilicon sol. Among them, the mass ratio of polysiloxane, silane monomer polymer, POSS, hexadecyltrimethylammonium bromide, ethanol, water, and tetramethylammonium hydroxide is 5:1:0.5:0.19:12:0.4:0.2, and the mass of polysiloxane and silane prepolymer accounts for 35% of the total mass of silicon precursor and ethanol (solid content).

[0088] Step 3. Select the size of 220mm*220mm*10mm and the density of 0.27g / cm 3 The needle-punched quartz fiber preform is used as the reinforcement phase, and the fiber preform is laid in a stainless steel mold. The organic silicon sol prepared according to step (2) is injected into the mold by a pressure-assisted injection method, with an injection pressure of 1 bar, and the process is repeated 3 times. After the organic silicon sol completely impregnates the fiber preform and no bubbles emerge from the glue outlet, the injection port is closed and the mold is sealed.

[0089] Step 4. The mold was transferred to an oven at 80°C for reaction gelation and aging for 12 hours. The temperature was raised to 100°C and aging was continued for 12 hours. The mold was then opened to take out the obtained wet gel composite material.

[0090] Step 5. The wet gel composite material obtained in step (4) was placed in an oven at 60°C and 120°C for drying for 12 hours respectively, thereby obtaining an integrated heat-insulating / wave-transmitting nanoporous silicone resin-based composite material. The test results of its density and room temperature thermal conductivity are shown in Table 1.

[0091] A single-sided muffle furnace was used to perform a static aerobic environment thermal test on Example 1 and Example 3, with a test temperature of 800° C. and a test time of 600 s. Figure 3 This is the back temperature rise curve. After heating, the back temperature is 240℃-270℃, and the mass loss is 3.8%-4.7%, which meets the needs of composite materials for heat insulation.

[0092] Example 4

[0093] Example 4 is basically the same as Example 3, except that the size of the sample is 220 mm*220 mm*2 mm and the density is 0.27 g / cm 3 The needle-punched quartz fiber preform is used as the reinforcement phase. Its density, average dielectric constant and loss tangent value before and after carbonization at 800℃ at a frequency of 2-18GHz are shown in Table 2.

[0094] Example 5

[0095] Step 1. Select difunctional methylphenyldimethoxysilane and trifunctional phenyltrimethoxysilane as silane monomers, hexadecyltrimethylammonium bromide as surfactant, ethanol as alcohol solvent, and mix them in a molar ratio of 1:2:0.3:5. Select POSS (vertex groups include Si-OH, -CH 3 and -C 6 H 5 ) is a silane prepolymer, and POSS is directly mixed with silane monomer and ethanol to form a uniform silane prepolymer mixture. Polysiloxane is added to the silane prepolymer in three batches under an ice-water bath, and the three batches account for 30%, 30% and 40% of the total mass of polysiloxane respectively in the order of addition, and the interval time is 10min. Water is added in batches as a hydrolysis raw material according to the same mass ratio, and stirring is continued for 10min until the polysiloxane and silane prepolymer are completely hydrolyzed. Finally, 25% of tetramethylammonium hydroxide is added as an alkaline catalyst, and stirred for 10min under an ice-water bath to obtain a prepared organic silicon sol. Among them, the mass ratio of polysiloxane, silane monomer, POSS, hexadecyltrimethylammonium bromide, ethanol, water, and tetramethylammonium hydroxide is 5:1:0.5:0.19:12:0.4:0.2, and the mass of polysiloxane and silane prepolymer accounts for 35% of the total mass of silicon precursor and ethanol (solid content).

[0096] Step 2. Select the size of 220mm*220mm*10mm and the density of 0.27g / cm 3The needle-punched quartz fiber preform is used as the reinforcement phase, and the fiber preform is laid in a stainless steel mold. The organic silicon sol prepared according to step (1) is injected into the mold by a pressure-assisted injection method, with an injection pressure of 1 bar, and the process is repeated 3 times. After the organic silicon sol completely impregnates the fiber preform and no bubbles emerge from the glue outlet, the injection port is closed and the mold is sealed.

[0097] Step 3. The mold was transferred to an oven at 80°C for reaction gelation and aging for 12 hours. The temperature was raised to 100°C and aging was continued for 12 hours. The mold was then opened to take out the obtained wet gel composite material.

[0098] Step 4. The wet gel composite material obtained in step (3) was placed in an oven at 60°C and 120°C for drying for 12 hours respectively, thereby obtaining an integrated heat-insulating / wave-transmitting nanoporous silicone resin-based composite material. The test results of its density and room temperature thermal conductivity are shown in Table 1.

[0099] Example 6

[0100] Example 6 is basically the same as Example 5, except that the size of the sample is 220 mm*220 mm*2 mm and the density is 0.27 g / cm 3 The needle-punched quartz fiber preform is used as the reinforcement phase. Its density, average dielectric constant and loss tangent value before and after carbonization at 800℃ at a frequency of 2-18GHz are shown in Table 2.

[0101] Example 7

[0102] Example 7 is basically the same as Example 3, except that the size of the sample is 300 mm*300 mm*10 mm and the density is 0.27 g / cm 3 The needle-punched structured quartz fiber preform is used as the reinforcement phase. According to the national standard GJB 7954-2012 method, the wave transmittance of the composite material was tested using the focusing lens test method, with a test frequency of 2-18GHz and a test temperature of room temperature to 1200℃. The test results are as follows Figure 4 It can be seen that the overall wave transmittance is above 90%, and at higher temperatures (>800°C), the wave transmittance in higher frequency bands decreases slightly.

[0103] Density is measured according to the national standard GB / T 1463-2005; room temperature thermal conductivity is measured according to GB / T 10294-1988; dielectric constant and loss are measured according to the national standard GB / T 5597-1999;

[0104] Table 1

[0105] Material <![CDATA[Density g / cm 3 > Room temperature thermal conductivity W / m·K Example 1 0.52 0.041 Example 3 0.57 0.047 Example 5 0.56 0.049

[0106] Table 2

[0107]

[0108] Comparing Example 1 and Example 3, the main difference is that the percentage (solid content) of the mass of polysiloxane and silane prepolymer to the total mass of silicon precursor and ethanol is different. As the solid content increases, the density of the composite material increases, and the room temperature thermal conductivity and static aerobic thermal test back temperature increase. The increase in solid content is not conducive to maintaining good thermal insulation performance.

[0109] The main difference between Example 3 and Example 5 and Example 4 and Example 6 is that the polymer of silane monomer is used and the silane monomer is directly used to participate in the sol-gel reaction. The latter has a slightly increased room temperature thermal conductivity when the density is similar, and its dielectric constant is slightly increased.

[0110] Comparing Example 2 with Example 4, the main change is that the solid content changes while the precursor ratio remains unchanged, and thus the material density changes. The dielectric constant increases slightly with the increase of the density of the composite material. After carbonization, the dielectric constant of the material does not change much, and the loss increases significantly.

[0111] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A nanoporous silicone resin-based composite material with integrated heat insulation and wave transmission, It is characterized in that It comprises a matrix and a reinforcement phase, wherein the matrix comprises nanoporous silicone resin and the reinforcement phase comprises a fiber preform; The raw materials of the nanoporous silicone resin include polysiloxane, silane monomer / silane prepolymer and alkaline catalyst.

2. The heat-insulating / wave-transmitting integrated nanoporous silicone resin-based composite material according to claim 1, It is characterized in that The main chain of the polysiloxane is composed of Si-O-Si, and the side chain groups include organic groups and reactive groups.

3. The heat-insulating / wave-transmitting integrated nanoporous silicone resin-based composite material according to claim 2, It is characterized in that The organic group includes -CH 3 , -C 6 H 5 , reactive groups include Si-OH, -OCH 3 、-OC 2 H 5 .

4. The heat-insulating / wave-transmitting integrated nanoporous silicone resin-based composite material according to claim 1, It is characterized in that The silane monomers include silane monomers with di- and tri-functionality; The silane prepolymer includes one or more of a silane monomer polymer obtained by polymerizing a difunctional or trifunctional silane monomer and other silane prepolymers; The other silane prepolymers include polyhedral oligomeric silsesquioxane and small molecular weight silicone resin.

5. The heat-insulating / wave-transmitting integrated nanoporous silicone resin-based composite material according to claim 4, It is characterized in that The silane monomers include methylphenyldimethoxysilane, diphenyldimethoxysilane, phenyltrimethoxysilane, methylphenyldiethoxysilane, diphenyldiethoxysilane, phenyltriethoxysilane, and trifluoromethyltrimethoxysilane.

6. The heat-insulating / wave-transmitting integrated nanoporous silicone resin-based composite material according to claim 1, It is characterized in that The alkaline catalyst includes tetramethylammonium hydroxide, ammonia water and urea.

7. The heat-insulating / wave-transmitting integrated nanoporous silicone resin-based composite material according to claim 1, It is characterized in that The fiber preform includes inorganic fibers with wave-transmitting properties, and the inorganic fibers include quartz fibers, boron nitride fibers, silicon nitride fibers, alumina fibers or basalt fibers; The fiber preform structure includes needle punching, stitching, 2.5D, 3D and orthogonal three-dimensional.

8. A method for preparing the heat-insulating / wave-transmitting integrated nanoporous silicone resin-based composite material according to any one of claims 1 to 7, It is characterized in that The following steps are involved: Preparation of organic silica sol: Mix silane monomer / silane monomer polymer, other silane prepolymers, polysiloxane and water in an alcohol solvent, stir in an ice-water bath until completely hydrolyzed, add an alkaline catalyst, continue stirring in an ice-water bath until the solution is clear, and obtain a uniform organic silica sol; Pouring of organosilicon sol: placing the fiber preform in a mold, and pouring the prepared organosilicon sol into the mold, repeating the process until the fiber preform is completely impregnated with the organosilicon sol, and closing the injection port to seal the mold; Reaction gelation and aging: placing the mold in a high temperature environment to cause the organosilicon sol to undergo a gelation reaction and further age to obtain a wet gel composite material; Drying: Drying the wet gel composite material at high temperature to obtain a heat-insulating / wave-transmitting integrated nanoporous silicone resin-based composite material.

9. The method for preparing the heat-insulating / wave-transmitting integrated nanoporous silicone resin-based composite material according to claim 8, It is characterized in that The mass ratio of the silane monomer / silane monomer polymer, other silane prepolymers, water and polysiloxane is (1-3): (0.4-0.7): (0.2-1): (1-9).

10. An application of the heat-insulating / wave-transmitting integrated nanoporous silicone resin-based composite material according to any one of claims 1 to 7, It is characterized in that The composite material is used as a high-temperature wave-transparent material for aircraft.

Citation Information

Patent Citations

  • Organic silicon resin-based heat-resisting wave-penetrating composite material and preparation method thereof

    CN101891957A

  • High-strength ablation-resistant nanopore organic silicon aerogel composite material as well as preparation method and application thereof

    CN116239817A

  • Ceramic-hybrid resin based gradient heat prevention and insulation integrated composite material and preparation method thereof

    CN117510228A

  • Nano-pore hybrid resin-based heat prevention and insulation material capable of being repeatedly used for limited times and preparation method of nano-pore hybrid resin-based heat prevention and insulation material

    CN117866440A

  • Composites and methods of forming composites having an increased volume of oxidation resistant ceramic particles

    US20230382810A1

Cited By

  • Organosilicon composite material for improving high-temperature wave-transparent performance through in-situ oxygen release and carbon removal and preparation method thereof

    CN120590795A

  • Wave-absorbing, heat-preventing and heat-insulating composite material based on impedance gradient structure as well as preparation method and application thereof

    CN121379172A

  • Impedance gradient structure-based wave-absorbing and heat-proof composite material, preparation method and application thereof

    CN121379172B

  • Wave-absorbing composite material as well as preparation method and application thereof