Positive electrode active material and method of producing the same

By treating lithium transition metal composite oxides with sodium ions and boron compounds, the method addresses synthesis challenges in lithium-nickel composite oxides, enhancing cycle characteristics and charge/discharge performance in non-aqueous electrolyte secondary batteries.

JP2024138184AActive Publication Date: 2024-10-07NICHIA CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024124137
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-07-11
Filing Date
2024-07-31
Publication Date
2024-10-07
Estimated Expiration
2040-06-04

AI Technical Summary

Technical Problem

Lithium-nickel composite oxides used in non-aqueous electrolyte secondary batteries face challenges in synthesizing high charge/discharge capacity materials with unreacted alkaline components causing slurry thickening and gas generation, and conventional washing methods degrade cycle characteristics.

Method used

A method involving lithium transition metal composite oxides with a nickel-to-total metals ratio of 0.7 to less than 1, treated with a sodium ion solution, mixed with a boron compound, and heat-treated to form a positive electrode active material with sodium at grain boundaries and boron uniformly distributed, enhancing cycle characteristics.

Benefits of technology

The method results in a positive electrode active material with improved cycle characteristics and charge/discharge performance by reducing resistance and maintaining structural integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138184000001_ABST
    Figure 2024138184000001_ABST
Patent Text Reader

Abstract

To provide a method of producing a positive electrode active material with good cycle characteristics.SOLUTION: A method of producing a positive electrode active material includes: bringing first particles that contain a lithium transition metal composite oxide into contact with a solution containing sodium ions to obtain second particles containing the lithium transition metal composite oxide and sodium elements, the lithium transition metal composite oxide having a layered structure and having a composition ratio of a number of moles of nickel to a total number of moles of metals other than lithium in a range of from 0.7 or more to less than 1; mixing the second particles and a boron compound to obtain a mixture; and heat-treating the mixture at a temperature in a range of from 100°C or more to 450°C or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a positive electrode active material and a method for producing the same. [Background technology]

[0002] Lithium transition metal composite oxides such as lithium cobalt oxide, lithium nickel oxide, and lithium nickel cobalt manganese oxide are used as the positive electrode active material of non-aqueous electrolyte secondary batteries. Lithium nickel composite oxides, which have a higher ratio of nickel instead of cobalt, a scarce resource, have the advantage of having a high charge / discharge capacity per unit weight. However, lithium nickel composite oxides are difficult to synthesize, and unreacted raw materials may remain as alkaline components. Residual alkaline components may cause thickening of the slurry during electrode preparation and gas generation during charging. However, reducing the alkaline components by washing with water or the like may deteriorate the cycle characteristics.

[0003] In relation to the above, a technique has been proposed in which after washing with water, the material is brought into contact with an aqueous sulfate solution to cause sulfate to be present on the surfaces of the primary particles, thereby improving cycle characteristics (see, for example, Patent Document 1). Also, a technique has been proposed in which a lithium transition metal composite oxide based on lithium nickel oxide is washed with water, mixed with a boron compound, and heat-treated, thereby improving cycle characteristics (see, for example, Patent Document 2). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2011-124086 A [Patent Document 2] JP 2015-088343 A Summary of the Invention [Problem to be solved by the invention]

[0005] Positive electrode active materials for non-aqueous electrolyte secondary batteries are required to have further improved cycle characteristics. In view of this, an object of one aspect of the present disclosure is to provide a positive electrode active material having excellent cycle characteristics and a method for producing the same. [Means for solving the problem]

[0006] The first aspect is a method for producing a positive electrode active material, comprising: contacting first particles containing a lithium transition metal composite oxide having a layered structure, in which the ratio of the number of moles of nickel to the total number of moles of metals other than lithium in the composition is 0.7 or more and less than 1, with a solution containing sodium ions to obtain second particles containing the lithium transition metal composite oxide and elemental sodium; mixing the second particles with a boron compound to obtain a mixture; and heat-treating the mixture at a temperature of 100°C or more and 450°C or less.

[0007] The second aspect is a positive electrode active material which includes secondary particles formed by an aggregation of a plurality of primary particles which include a lithium transition metal composite oxide having a layered structure and in which the ratio of the number of moles of nickel to the total number of moles of metals other than lithium in the composition is 0.7 or more and less than 1, wherein a compound containing boron is attached to at least a portion of the surface of the primary particles and a compound containing sodium is present in at least a portion of the grain boundaries of the secondary particles, and the value obtained by dividing the standard deviation of the detected amount by the average amount of boron element in any three regions in a cross section of the secondary particles is less than 0.18.

[0008] A third aspect is a non-aqueous electrolyte secondary battery including the positive electrode active material in a positive electrode. A fourth aspect is a non-aqueous electrolyte secondary battery including a current collector and a positive electrode active material layer disposed on the current collector, the positive electrode active material layer including the positive electrode active material and having a density of 2.8 g / cm 3 More than 3.7g / cm 3 The following is an electrode for a non-aqueous electrolyte secondary battery. Effect of the Invention

[0009] According to one aspect of the present disclosure, it is possible to provide a positive electrode active material having excellent cycle characteristics and a method for producing the same. [Brief description of the drawings]

[0010] [Figure 1] FIG. 11 is a diagram showing an example of the boron element distribution in the lithium transition metal composite oxide of Example 5. [Diagram 2] FIG. 11 is a diagram showing an example of the boron element distribution in the lithium transition metal composite oxide of Comparative Example 5. [Diagram 3] FIG. 13 is a diagram showing an example of the boron element distribution in the lithium transition metal composite oxide of Comparative Example 6. [Figure 4] This is an equivalent circuit model for AC impedance measurement. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] In this specification, the term "step" refers not only to an independent step, but also to a step that cannot be clearly distinguished from other steps, as long as the intended purpose of the step is achieved. In addition, the content of each component in the composition means the total amount of the multiple substances present in the composition when multiple substances corresponding to each component are present in the composition, unless otherwise specified. Hereinafter, the embodiments of the present invention will be described in detail. However, the embodiments shown below are examples of positive electrode active materials and methods for producing the same for embodying the technical idea of ​​the present invention, and the present invention is not limited to the positive electrode active materials and methods for producing the same shown below.

[0012] [Method of manufacturing positive electrode active material] The method for producing a positive electrode active material includes a washing step of contacting first particles containing a lithium transition metal composite oxide having a layered structure and in which the ratio of the number of moles of nickel to the total number of moles of metals other than lithium in the composition is 0.7 or more and less than 1 with a solution containing sodium ions to obtain second particles containing the lithium transition metal composite oxide and elemental sodium, a mixing step of mixing the second particles with a boron compound to obtain a mixture, and a heat treatment step of heat treating the mixture at a temperature of 100° C. or more and 450° C. or less. In addition, other steps such as a preparation step of preparing the first particles may be included as necessary.

[0013] A positive electrode active material obtained by washing a lithium transition metal composite oxide having a nickel molar ratio of 0.7 or more and less than 1 with a sodium ion-containing aqueous solution and then heat-treating it together with a boron compound can achieve good cycle characteristics when applied to a non-aqueous electrolyte secondary battery. This is thought to be because, for example, the presence of sodium at the grain boundaries of the secondary particles containing the lithium transition metal composite oxide that constitutes the positive electrode active material allows boron to be uniformly distributed throughout the grain boundaries of the lithium transition metal composite oxide particles.

[0014] Preparation process In the preparation step, first particles containing a lithium transition metal composite oxide having a layered structure are prepared. The lithium transition metal composite oxide constituting the first particles contains nickel in its composition, and the ratio of the number of moles of nickel to the total number of moles of metals other than lithium is 0.7 or more and less than 1. The first particles may be prepared by appropriately selecting from commercially available products, or may be prepared by a preparation method described below.

[0015] The method for preparing the first particles may include, for example, a precursor preparation step of preparing a precursor, and a synthesis step of synthesizing the first particles containing a lithium transition metal composite oxide from the precursor and a lithium compound. The first particles may be configured as secondary particles composed of a plurality of primary particles containing a lithium transition metal composite oxide.

[0016] In the precursor preparation step, a precursor containing a composite oxide containing nickel is prepared. The precursor may be prepared by appropriately selecting from commercially available products, or may be prepared by preparing a nickel-containing composite oxide having a desired composition by a conventional method. Here, examples of the precursor include nickel-containing composite oxides, composite oxides containing nickel and metals other than nickel (e.g., Co, Mn, Al, Ti, Nb, etc.), and the like.

[0017] Methods for obtaining a nickel-containing composite oxide having a desired composition include a method in which raw material compounds (hydroxides, carbonates, etc.) are mixed according to the target composition and decomposed into a nickel-containing composite oxide by heat treatment, as well as a coprecipitation method in which a solution in which the raw material compounds are dissolved is prepared, a precursor precipitate having the target composition is obtained by adjusting the temperature, adjusting the pH, adding a complexing agent, etc., and the nickel-containing composite oxide is obtained by heat treating the precursor precipitate. An example of a method for producing a nickel-containing composite oxide (hereinafter also simply referred to as a composite oxide) will be described below.

[0018] The method for obtaining a composite oxide by coprecipitation can include a seed generation step of adjusting the pH of a mixed solution containing metal ions in a desired composition ratio to obtain seed crystals, a crystallization step of growing the generated seed crystals to obtain a composite hydroxide having desired properties, and a step of heat-treating the obtained composite hydroxide to obtain a composite oxide. For details of the method for obtaining such a composite oxide, reference can be made to, for example, JP 2003-292322 A and JP 2011-116580 A (US Patent Application Publication No. 2012 / 270107).

[0019] In the seed generation step, the pH of the mixed solution containing nickel ions at a desired composition ratio is adjusted to, for example, 11 to 13 to prepare a liquid medium containing seed crystals. The seed crystals may contain, for example, a hydroxide containing nickel at a desired ratio. The mixed solution may be prepared by dissolving nickel salts in water at a desired ratio. Examples of nickel salts include sulfates, nitrates, and hydrochlorides. In addition to nickel salts, the mixed solution may contain other metal salts at a desired composition ratio as necessary. The temperature in the seed generation step may be, for example, 40°C to 80°C. The atmosphere in the seed generation step may be a low oxidizing atmosphere, and for example, the oxygen concentration may be maintained at 10% by volume or less.

[0020] In the crystallization step, the generated seed crystals are grown to obtain a precursor precipitate containing nickel having desired properties. The seed crystals can be grown, for example, by adding a mixed solution containing nickel ions and, if necessary, other metal ions to a liquid medium containing the seed crystals while maintaining the pH of the medium in the range of, for example, 7 to 12.5, preferably 7.5 to 12. The time for adding the mixed solution is, for example, 1 hour to 24 hours, preferably 3 hours to 18 hours. The temperature in the crystallization step can be, for example, 40°C to 80°C. The atmosphere in the crystallization step is the same as that in the seed generation step.

[0021] The pH in the seed generation step and the crystallization step can be adjusted using an acidic aqueous solution such as an aqueous sulfuric acid solution or an aqueous nitric acid solution, or an alkaline aqueous solution such as an aqueous sodium hydroxide solution or an aqueous ammonia solution.

[0022] In the crystallization process, it is desirable to control the particle size of the precursor precipitate. The particle size of the precursor precipitate can be controlled by adjusting the temperature, pH, stirring speed, etc. of the reaction field. These conditions can be appropriately adjusted according to actual conditions such as the shape of the vessel that contains the reaction field, the starting material, and the introduction speed of the starting material into the reaction field. Furthermore, the particle size of the precursor precipitate can be controlled by the maturation time after the precipitation of the precursor precipitate begins, the stirring speed, etc. The conditions in this case may also be appropriately adjusted according to actual conditions, since the growth rate and shape of the particles differ depending on the shape of the reaction vessel.

[0023] In the step of obtaining a composite oxide, the composite hydroxide-containing precursor precipitate obtained in the crystallization step is heat-treated to obtain the composite oxide. The heat treatment may be performed by heating the composite hydroxide at a temperature of, for example, 500°C or less, preferably 350°C or less. The heat treatment temperature may be, for example, 100°C or more, preferably 200°C or more. The heat treatment time may be, for example, 0.5 to 48 hours, preferably 5 to 24 hours. The heat treatment atmosphere may be air or an atmosphere containing oxygen. The heat treatment may be performed using, for example, a box furnace, a rotary kiln furnace, a pusher furnace, a roller hearth kiln furnace, or the like.

[0024] The obtained composite oxide may contain other metal elements in addition to nickel. Examples of the other metals include Co, Mn, Al, Ti, Nb, etc., and at least one selected from the group consisting of these is preferable, and at least one selected from the group consisting of Co, Mn, and Al is preferable. When the composite oxide contains other metals, the mixed aqueous solution from which the precursor precipitate is obtained may contain other metal ions in a desired composition. In this way, the precursor precipitate is made to contain nickel and other metals, and the precursor precipitate is heat-treated to obtain a composite oxide having a desired composition.

[0025] The average particle size of the complex oxide is, for example, 2 μm to 30 μm, preferably 3 μm to 25 μm. The average particle size of the complex oxide is a volume average particle size, which is a value at which the volume integrated value from the small particle size side in the volume distribution obtained by the laser scattering method is 50%.

[0026] In the synthesis step of synthesizing the first particles containing a lithium transition metal composite oxide, a mixture containing lithium obtained by mixing the composite oxide with a lithium compound is heat-treated at a temperature of 550° C. to 1000° C. to obtain a heat-treated product. The heat-treated product has a layered structure and contains a lithium transition metal composite oxide containing nickel.

[0027] Examples of the lithium compound to be mixed with the composite oxide include lithium hydroxide, lithium carbonate, lithium oxide, etc. The particle size of the lithium compound used for mixing is, for example, 0.1 μm or more and 100 μm or less, preferably 2 μm or more and 20 μm or less, as a volume average particle size.

[0028] The ratio of the total moles of lithium to the total moles of metal elements constituting the composite oxide in the mixture may be, for example, 0.95 to 1.2. The composite oxide and the lithium compound can be mixed using, for example, a high-speed shear mixer.

[0029] The mixture may further contain other metal elements other than the metal elements constituting the lithium and composite oxide. Examples of the other metal elements include Al, Si, Zr, Ti, Mg, Ta, Nb, Mo, W, etc., and at least one selected from the group consisting of these is preferable. For example, when the mixture contains W, Nb, etc. as other metal elements, the output characteristics are improved. For example, when the mixture contains Al, Zr, etc., it is suitable for further improving the cycle characteristics. For example, when the mixture contains Ti, Si, etc., it is suitable for further improving the cycle characteristics under high voltage. When the mixture contains other metal elements, a mixture can be obtained by mixing a simple substance or a metal compound of the other metal element with the composite oxide and the lithium compound. Examples of metal compounds containing other metal elements include oxides, hydroxides, chlorides, nitrides, carbonates, sulfates, nitrates, acetates, oxalates, etc.

[0030] When the mixture contains other metal elements, the ratio of the total number of moles of the metal elements constituting the composite oxide to the total number of moles of the other metal elements may be, for example, 1:0.0001 to 1:0.1, and preferably 1:0.0005 to 1:0.03, or 1:0.001 to 1:0.01.

[0031] The heat treatment temperature of the mixture is, for example, 550°C or more and 1000°C or less, preferably 600°C or more and 950°C or less, and more preferably 700°C or more and 950°C or less. The heat treatment of the mixture may be performed at a single temperature, but is preferably performed at multiple temperatures in terms of discharge capacity at high voltage. When performing heat treatment at multiple temperatures, for example, it is desirable to hold the first temperature for a predetermined time, then further increase the temperature, and hold the second temperature for a predetermined time. The first temperature is, for example, 200°C or more and 600°C or less, preferably 400°C or more and 500°C or less, and the second temperature is, for example, 600°C or more and 900°C or less, preferably 650°C or more and 750°C or less. The heat treatment time is, for example, 0.5 hours to 48 hours, and when performing heat treatment at multiple temperatures, each can be 0.2 hours to 47 hours.

[0032] The heat treatment may be performed in an atmosphere containing oxygen or in the air, and may be performed using, for example, a box furnace, a rotary kiln furnace, a pusher furnace, a roller hearth kiln furnace, or the like.

[0033] The composition of the lithium transition metal composite oxide obtained above is such that the ratio of the number of moles of nickel to the total number of moles of metals other than lithium is 0.7 or more and less than 1, preferably 0.7 or more and 0.95 or less, more preferably 0.75 or more and 0.95 or less, and even more preferably 0.8 or more and 0.95 or less. The lithium transition metal composite oxide may contain cobalt. When the lithium transition metal composite oxide contains cobalt, the ratio of the number of moles of cobalt to the total number of moles of metals other than lithium may be, for example, greater than 0 and 0.3 or less, preferably 0.02 or more and 0.2 or less. The lithium transition metal composite oxide may contain manganese. When the lithium transition metal composite oxide contains manganese, the ratio of the number of moles of manganese to the total number of moles of metals other than lithium may be, for example, greater than 0 and 0.3 or less, preferably greater than 0 and 0.15 or less, and more preferably 0.01 or more and 0.15 or less. The lithium transition metal composite oxide may contain aluminum. When the lithium transition metal composite oxide contains aluminum, the ratio of the number of moles of aluminum to the total number of moles of metals other than lithium may be, for example, greater than 0 and less than 0.1, preferably greater than 0 and less than 0.05, and more preferably 0.01 or more and 0.04 or less. When the lithium transition metal composite oxide contains at least one of manganese and aluminum, the ratio of the number of moles of manganese and aluminum to the total number of moles of metals other than lithium may be, for example, greater than 0 and less than 0.3, preferably greater than 0 and less than 0.25, and more preferably 0.01 or more and 0.15 or less.

[0034] The lithium transition metal composite oxide may have a composition represented by the following formula (1), for example. Li (1+p) Ni (1-x-y-z-w) Co x Mn y Al z Mw O2(1) In the formula, -0.05 ≦ p ≦ 0.2, 0 < x + y + z + w ≦ 0.3, 0 ≦ x ≦ 0.3, 0 ≦ y ≦ 0.3, 0 ≦ z ≦ 0.1, and 0 ≦ w ≦ 0.03 are satisfied. M is at least one element selected from the group consisting of Zr, Ti, Mg, Ta, Nb, Mo, and W.

[0035] The volume average particle diameter of the first particles containing the lithium transition metal composite oxide is, for example, 2 μm or more and 30 μm or less, preferably 3 μm or more and 25 μm or less.

[0036] Washing step In the washing step, the first particles containing the lithium transition metal composite oxide are brought into contact with a solution containing sodium ions (hereinafter also referred to as the washing solution) to obtain second particles containing the lithium transition metal composite oxide and sodium element. After contact with the washing solution, dehydration treatment, drying treatment, etc. may be carried out on the treated product as necessary. The washing step is, for example, a step of removing at least a part of the alkaline component of the unreacted raw material present in the first particles.

[0037] The solution containing sodium ions only needs to contain at least sodium ions and water. The solution containing sodium ions can be prepared, for example, by dissolving a sodium salt in a solvent. Examples of the sodium salt include sodium sulfate, sodium hydroxide, etc., and at least one selected from the group consisting of these is preferable, and it is more preferable to contain at least sodium sulfate. The solvent may, for example, contain at least water, and may contain a water-soluble organic solvent such as alcohol as necessary in addition to water. The content rate of sodium ions in the washing solution is, for example, 0.01 mol / L or more and 2.0 mol / L or less, preferably 0.05 mol / L or more and 2.0 mol / L or less, more preferably 0.1 mol / L or more and 1.5 mol / L or less, still more preferably 0.15 mol / L or more and 1.0 mol / L or less, and particularly preferably 0.15 mol / L or more and 0.6 mol / L or less.

[0038] The cleaning solution may contain metal ions other than sodium as necessary. Examples of metal ions other than sodium include alkali metal ions such as lithium ions and potassium ions, and alkaline earth metal ions such as magnesium ions. When the cleaning solution contains metal ions other than sodium, the content of the metal ions is, for example, 0.1 mol / L or less, and preferably less than 0.01 mol / L.

[0039] The contact temperature between the first particles and the washing liquid is, for example, 5° C. to 60° C., and preferably 10° C. to 40° C. The contact time is, for example, 1 minute to 2 hours, and preferably 5 minutes to 30 minutes. The amount of the washing liquid used for the contact is, for example, 0.25 to 10 times, and preferably 0.5 to 4 times, the mass of the first particles.

[0040] The contact between the first particles and the washing liquid may be carried out by preparing a slurry by putting the first particles into the washing liquid. When the contact is carried out as a slurry, the solid content concentration of the first particles in the slurry is, for example, 10% by mass or more and 80% by mass or less, and preferably 20% by mass or more and 60% by mass or less. The contact may be carried out by passing the washing liquid through the first particles held on a filter, or by passing the washing liquid through a dehydrated cake obtained by washing the first particles with pure water or the like and dehydrating the first particles. When the washing liquid is passed through a dehydrated cake obtained by washing the first particles with pure water or the like and then dehydrating the first particles, the total amount of the pure water and the washing liquid used is preferably 0.25 times or more and 10 times or less, more preferably 0.5 times or more and 4 times or less, relative to the mass of the first particles. Note that a solution containing sodium ions (e.g., a sodium sulfate solution) has a higher solubility of residual alkali (e.g., lithium carbonate) than pure water, and is easy to remove residual alkali. Therefore, from the viewpoint of reducing damage to the lithium transition metal composite oxide, it is preferable to give priority to the contact with the washing liquid. It is also preferable not to wash with pure water.

[0041] The second particles obtained in the washing step contain a compound containing sodium in addition to the lithium transition metal composite oxide. The compound containing sodium may be present, for example, in the grain boundary of the secondary particles consisting of the primary particles containing the lithium transition metal composite oxide. The content of the compound containing sodium contained in the second particles is, for example, 100 ppm or more and 1400 ppm or less, preferably 150 ppm or more and 1300 ppm or less, more preferably 150 ppm or more and 1200 ppm or less, even more preferably 200 ppm or more and 1000 ppm or less, and particularly preferably 300 ppm or more and 1000 ppm or less, calculated as sodium element. When the content of the compound containing sodium is within the above range, the resistance component during charging and discharging is sufficiently reduced. The content of the compound containing sodium in the second particles can be adjusted, for example, by the sodium ion concentration of the washing liquid, the amount of water attached to the dehydrated cake, etc.

[0042] The second particles obtained in the washing step may be dried. The drying process may be performed by heating, air drying, or vacuum drying, as long as it can remove at least a part of the moisture attached to the second particles. The drying temperature in the case of heating and drying may be any temperature at which the moisture contained in the second particles is sufficiently removed. The drying temperature is, for example, 80°C or more and 300°C or less, and preferably 100°C or more and 250°C or less. When the drying temperature is within the above range, the dissolution of lithium into the attached water can be sufficiently suppressed. In addition, the collapse of the crystal structure on the particle surface can be suppressed, and the decrease in the charge / discharge capacity can be sufficiently suppressed. The drying time may be appropriately selected depending on the amount of moisture contained in the second particles. The drying time is, for example, 1 hour or more and 10 hours or less. The amount of moisture contained in the second particles after the drying process is, for example, 0.2 mass% or less, and preferably 0.1 mass% or less.

[0043] The degree of cleaning in the cleaning process can be confirmed by the lithium content, residual alkaline components, specific surface area, etc., of the second particles. In general, when the specific surface area of ​​the second particles is small, particle cracking, elution of elements constituting lithium and composite oxide, etc. can be sufficiently suppressed, and cycle characteristics tend to be improved. In addition, by making the specific surface area to a certain degree, the residual alkaline components can be sufficiently reduced. Since the solubility of lithium salts in sodium salt aqueous solutions such as sodium sulfate as a cleaning solution is higher than that in pure water, lithium salt aqueous solutions, etc., the amount of solution required for removing the alkali can be reduced. As a result, the specific surface area of ​​the second particles is reduced, and excessive elution of lithium from the second particles can be suppressed.

[0044] The specific surface area of ​​the second particles obtained in the washing step is, for example, 0.5 m 2 / g or more 4m 2 / g or less, preferably 1.0m 2 / g or more 3.0m 2 / g or less, more preferably 1.0m 2 / g or more 1.6m 2 / g or less, more preferably 1.0m 2 / g or more 1.4m 2 The specific surface area can be measured by the BET method.

[0045] Mixing process In the mixing step, the second particles and the boron compound are mixed to obtain a mixture. The mixing of the second particles and the boron compound may be performed in a dry manner or a wet manner. The mixing may be performed using, for example, a super mixer. In addition, in this mixing step, a simple substance, an alloy, or a metal compound of another metal element may be mixed in addition to the boron compound. Examples of the other metal element include Al, Si, Zr, Ti, Mg, Ta, Nb, Mo, W, etc., and at least one selected from the group consisting of these is preferable.

[0046] The boron compound may be at least one selected from the group consisting of boron oxide, boron oxoacids, and boron oxoacid salts. More specific examples of the boron compound include lithium tetraborate (Li2B4O7), ammonium pentaborate (NH4B5O8), orthoboric acid (H3BO3; so-called ordinary boric acid), lithium metaborate (LiBO2), boron oxide (B2O3), etc. At least one selected from the group consisting of these is preferred, and orthoboric acid is more preferred from the viewpoint of cost.

[0047] The boron compound may be mixed with the second particles in a solid state, or may be mixed with the second particles as a solution of the boron compound. When using a solid boron compound, the volume average particle size of the boron compound is, for example, 1 μm or more and 60 μm or less, preferably 10 μm or more and 30 μm or less.

[0048] The content of the boron compound in the mixture, expressed as the ratio of the number of moles of boron element to the total number of moles of metals other than lithium in the lithium transition metal composite oxide, is, for example, 0.1 mol% or more and 2 mol% or less, preferably 0.1 mol% or more and 1.5 mol% or less, and more preferably 0.1 mol% or more and 1.2 mol% or less.

[0049] Heat Treatment Process In the heat treatment step, the mixture is heat treated at a temperature of, for example, 100°C to 450°C to obtain a positive electrode active material. The heat treatment temperature may be 200°C to 400°C, preferably 220°C to 350°C, more preferably 250°C to 350°C. By increasing the heat treatment temperature higher than the drying treatment temperature, the charge / discharge capacity may be further improved. The heat treatment atmosphere may be an oxygen-containing atmosphere or air. The heat treatment time is, for example, 1 hour to 20 hours, preferably 5 hours to 10 hours. The heat-treated product obtained in the heat treatment step may be subjected to crushing treatment, classification treatment, etc. as necessary.

[0050] Lithium-deficient regions may be formed near the surfaces of the second particles after the washing step, and the lithium-deficient regions may inhibit the desorption and insertion of lithium ions. However, by mixing a boron compound with the second particles after the washing step and subjecting them to a heat treatment, it is believed that the lithium deficiency is compensated for, and the inhibition of the desorption and insertion of lithium ions is suppressed, thereby improving the charge / discharge characteristics and cycle characteristics.

[0051] [Cathode active material] The positive electrode active material has a layered structure and includes secondary particles formed by aggregating a plurality of primary particles including a lithium transition metal composite oxide in which the ratio of the number of moles of nickel to the total number of moles of metals other than lithium in the composition is 0.7 or more and less than 1. A compound containing boron is attached to at least a portion of the surface of the primary particles. A compound containing sodium is present in at least a portion of the grain boundary of the secondary particles. The coefficient of variation (CV), which is the value (σ1 / t1) obtained by dividing the standard deviation σ1 of the detected amount of boron element by the average value t1 of the detected amount of boron element in any three regions in the cross section of the secondary particles, is less than 0.18.

[0052] The positive electrode active material includes a lithium transition metal composite oxide and is configured to include secondary particles formed by aggregating a plurality of primary particles having a boron-containing compound attached to the surface, and thus the charge / discharge characteristics and cycle characteristics of a non-aqueous electrolyte secondary battery configured using the positive electrode active material are improved. In addition, the presence of a sodium-containing compound at the grain boundaries of the secondary particles is thought to distribute the boron-containing compound uniformly throughout the secondary particles, thereby achieving good charge / discharge characteristics and cycle characteristics. The positive electrode active material can be efficiently manufactured by the above-mentioned manufacturing method for the positive electrode active material.

[0053] The variation coefficient of the detected amount of boron element in the cross section of the positive electrode active material particle is preferably less than 0.18, more preferably 0.15 or less, even more preferably 0.14 or less, and particularly preferably 0.13 or less. The lower limit of the variation coefficient is, for example, 0.04 or more. The fact that the variation coefficient of the detected amount of boron element is a predetermined value or less is considered to indicate that the boron compound is uniformly distributed throughout the positive electrode active material particle.

[0054] The average value of the detected amount of boron element used to calculate the coefficient of variation is calculated as the arithmetic average of the detected amount in each of three selected regions in an arbitrary cross section of the secondary particle constituting the positive electrode active material. The standard deviation of the detected amount of boron element is calculated from the obtained average value and the detected amount in each region. The detected amount of boron element in the cross section of the positive electrode active material particle may be measured using, for example, a secondary ion mass spectrometry (SIMS).

[0055] The region where boron element is detected can be selected from, for example, a region near the surface (surface portion), a region near the center (center portion), and a region between the surface portion and the center (middle portion) in the cross section of the positive electrode active material particle. Alternatively, a plurality of regions may be selected from each of the surface portion, the middle portion, and the center portion, and the arithmetic average of the detection amounts in the plurality of regions may be taken as the detection amounts in the surface portion, the middle portion, and the center portion.

[0056] The ratio of the mole number of nickel to the total mole number of metals other than lithium in the composition of the lithium transition metal composite oxide constituting the primary particles is 0.7 or more and less than 1, preferably 0.7 or more and 0.95 or less, more preferably 0.8 or more and 0.95 or less, and even more preferably 0.9 or more and 0.95 or less. In a positive electrode active material containing a lithium transition metal composite oxide having a large mole number ratio of nickel, better charge / discharge characteristics and cycle characteristics are achieved. The composition of the lithium transition metal composite oxide can be measured, for example, by an inductively coupled plasma optical emission spectrometer.

[0057] The lithium transition metal composite oxide may contain cobalt in its composition. When the lithium transition metal composite oxide contains cobalt, the ratio of the number of moles of cobalt to the total number of moles of metals other than lithium is, for example, greater than 0 and not more than 0.3, preferably not less than 0.02 and not more than 0.2. The lithium transition metal composite oxide may contain manganese. When the lithium transition metal composite oxide contains manganese, the ratio of the number of moles of manganese to the total number of moles of metals other than lithium is, for example, greater than 0 and not more than 0.3, preferably greater than 0 and not more than 0.15. The lithium transition metal composite oxide may contain aluminum. When the lithium transition metal composite oxide contains aluminum, the ratio of the number of moles of aluminum to the total number of moles of metals other than lithium is, for example, greater than 0 and not more than 0.1, preferably greater than 0 and not more than 0.05, more preferably not less than 0.01 and not more than 0.04.

[0058] When the lithium transition metal composite oxide contains nickel, cobalt, and at least one of manganese and aluminum, the content ratio Ni / Co / (Mn + Al) of nickel, cobalt, manganese, and aluminum can be, for example, 8 / 1 / 1, 8 / 1 / (0.5 + 0.5), etc. on a molar basis.

[0059] The lithium transition metal composite oxide may have a composition represented by, for example, the following formula (1). Li (1+p) Ni 1-x-y-z-w Co x Mn y Al z M w O2(1) In the formula, -0.05 ≦ p ≦ 0.2, 0 < x + y + z + w ≦ 0.3, 0 ≦ x ≦ 0.3, 0 ≦ y ≦ 0.3, 0 ≦ z ≦ 0.1, 0 ≦ w ≦ 0.03 are satisfied. M is at least one selected from the group consisting of Zr, Ti, Mg, Ta, Nb, Mo, and W.

[0060] In formula (1), from the perspective of output characteristics, p is preferably -0.02 or more, or 0.02 or more. Also, p is preferably 0.12 or less, or 0.06 or less. x is preferably 0 < x ≤ 0.3, more preferably 0.02 ≤ x ≤ 0.2. y is preferably 0 < y ≤ 0.3, more preferably 0 < y ≤ 0.15. z is preferably 0 < z ≤ 0.1, more preferably 0 < z ≤ 0.05, and even more preferably 0.01 ≤ z ≤ 0.04.

[0061] On at least a part of the surface of the primary particles, a boron-containing compound is attached. Examples of the boron-containing compound include lithium metaborate (LiBO2) and the like. The boron-containing compound may form a complex with the lithium transition metal composite oxide. The content of the boron-containing compound in the positive electrode active material is, for example, 0.1 mol% or more and 2 mol% or less, preferably 0.1 mol% or more and 1.5 mol% or less, as the ratio of the number of moles of boron element to the total number of moles of metals other than lithium in the lithium transition metal composite oxide. The content of boron in the positive electrode active material can be measured, for example, by an inductively coupled plasma optical emission spectrometer.

[0062] In at least a part of the grain boundaries of the secondary particles, a sodium-containing compound exists. Examples of the sodium-containing compound include sodium sulfate (Na2SO4) and the like. The content of the sodium-containing compound in the positive electrode active material is, for example, 100 ppm or more and 1400 ppm or less in terms of sodium element, preferably 150 ppm or more and 1300 ppm or less, more preferably 150 ppm or more and 1200 ppm or less, even more preferably 200 ppm or more and 1000 ppm or less, and particularly preferably 300 ppm or more and 1000 ppm or less. The content of sodium element in the positive electrode active material can be measured, for example, by an inductively coupled plasma optical emission spectrometer.

[0063] The specific surface area of the positive electrode active material is, for example, 0.2 m 2 / g or more and 3.0 m 2 / g or less, preferably 0.3 m 2 / g or more 2.0m 2 The specific surface area of ​​the positive electrode active material is measured by the BET method.

[0064] The positive electrode active material can be used in the positive electrode of a nonaqueous electrolyte secondary battery to form a nonaqueous electrolyte secondary battery that can achieve excellent cycle characteristics. The positive electrode active material can be included in a positive electrode active material layer disposed on a current collector to form a positive electrode. That is, the present invention includes an electrode for a nonaqueous electrolyte secondary battery that includes the positive electrode active material, and a nonaqueous electrolyte secondary battery that includes the electrode.

[0065] [Nonaqueous electrolyte secondary battery electrode] The electrode for a non-aqueous electrolyte secondary battery includes a current collector and a positive electrode active material layer disposed on the current collector and containing the above-mentioned positive electrode active material or the positive electrode active material produced by the above-mentioned production method. A non-aqueous electrolyte secondary battery including such an electrode can achieve excellent cycle characteristics.

[0066] The density of the positive electrode active material layer is, for example, 2.6 g / cm 3 More than 3.9g / cm 3 or less, preferably 2.8 g / cm 3 More than 3.8g / cm 3 Less than or equal to 3.1 g / cm 3 More than 3.7g / cm 3 More preferably, 3.2 g / cm 3 More than 3.6g / cm 3 The density of the active material layer is calculated by dividing the mass of the active material layer by the volume of the active material layer. The density of the active material layer can be adjusted by applying pressure to the electrode composition described below after applying it to the current collector.

[0067] Examples of the material of the current collector include aluminum, nickel, stainless steel, etc. The positive electrode active material layer can be formed by applying an electrode composition obtained by mixing the above-mentioned positive electrode active material, conductive material, binder, etc. with a solvent onto the current collector, and then performing drying treatment, pressure treatment, etc. Examples of the conductive material include natural graphite, artificial graphite, acetylene black, etc. Examples of the binder include polyvinylidene fluoride, polytetrafluoroethylene, polyamide acrylic resin, etc. Examples of the solvent include N-methyl-2-pyrrolidone (NMP), etc.

[0068] [Nonaqueous electrolyte secondary battery] The non-aqueous electrolyte secondary battery comprises the above-mentioned electrode for non-aqueous electrolyte secondary battery. The non-aqueous electrolyte secondary battery comprises, in addition to the electrode for non-aqueous electrolyte secondary battery, a negative electrode for non-aqueous secondary battery, a non-aqueous electrolyte, a separator, etc. In the non-aqueous electrolyte secondary battery, the negative electrode, non-aqueous electrolyte, separator, etc., for example, those for non-aqueous electrolyte secondary batteries described in JP 2002-075367 A, JP 2011-146390 A, JP 2006-12433 A (the entire disclosures of which are incorporated herein by reference) can be appropriately used. EXAMPLES

[0069] Examples of the present invention will be described below, but the present invention is not limited to these examples. The volume average particle size was measured using a value where the volume cumulative value from the small particle size side in the volume distribution obtained by the laser scattering method was 50%. Specifically, the volume average particle size was measured using a laser diffraction type particle size distribution device (MALVERN Inst. MASTERSIZER 2000). The specific surface area was measured by a gas adsorption method (one-point method) using nitrogen gas using a BET specific surface area measurement device (Macsorb, manufactured by Mountec Co., Ltd.). The alkaline component was measured by adding the positive electrode active material to pure water, titrating the eluted lithium with sulfuric acid, and measuring up to the second neutralization point. The amount of the alkaline component neutralized with sulfuric acid was taken as the lithium hydroxide (LiOH) content. The composition was measured using an inductively coupled plasma atomic emission spectrometer (ICP-AES; manufactured by PerkinElmer Co., Ltd.). The amount of sulfuric acid was measured using an ICP-AES (manufactured by HITACHI Co., Ltd.). The amount of sodium (Na amount) was measured using an atomic absorption spectrometer (AAS; manufactured by HITACHI Co., Ltd.).

[0070] [Example 1] Precursor preparation process By coprecipitation, the volume average particle size of the secondary particles was 20 μm, and (Ni 0.95 Co 0.05 Composite oxide particles having a composition represented by the formula:

[0071] Synthesis process The obtained composite oxide particles, lithium hydroxide, and aluminum hydroxide were mixed in a molar ratio of Li:(Ni+Co):Al=1.10:0.97:0.03 to obtain a raw material mixture. The obtained raw material mixture was heat-treated in air. The heat treatment was performed at a first temperature of 450°C for 3 hours and at a second temperature of 680°C for 4 hours. After the heat treatment, the mixture was dispersed to obtain a lithium transition metal composite oxide with a composition of Li 1.03 Ni 0.92 Co 0.05 Al 0.03 We got the first particle which is O2.

[0072] Cleaning process The obtained first particles were added to an aqueous sodium sulfate solution prepared so that the sodium ion concentration was 0.469 mol / L to obtain a slurry with a solid concentration of 45 mass%. The solid concentration was calculated by mass of the first particles / (mass of the first particles+mass of the washing solution). After stirring the slurry for 30 minutes, it was dehydrated in a funnel and separated as a cake. The separated cake was dried at 150°C for 10 hours to obtain second particles as washed particles.

[0073] Mixing process Orthoboric acid was added in an amount such that the boron element accounted for 1 mol % relative to the total number of moles of metals other than lithium in the lithium transition metal composite oxide contained in the obtained second particles, and the mixture was mixed and stirred to obtain a mixture.

[0074] Heat Treatment Process The resulting mixture was heat-treated in air at 250° C. for 10 hours to obtain the target positive electrode active material E1 containing a lithium transition metal composite oxide.

[0075] [Example 2] A positive electrode active material E2 was obtained in the same manner as in Example 1, except that the concentration of the aqueous sodium sulfate solution in the washing step was adjusted so that the sodium ion concentration was 0.156 mol / L.

[0076] [Example 3] A positive electrode active material E3 was obtained in the same manner as in Example 1, except that the sodium sulfate aqueous solution in the washing step was changed to a sodium hydroxide aqueous solution.

[0077] [Comparative Example 1] A positive electrode active material C1 was obtained in the same manner as in Example 1, except that pure water was used instead of the aqueous sodium sulfate solution in the washing step, and the solid content concentration of the slurry was set to 42 mass %.

[0078] [Comparative Example 2] A positive electrode active material C2 was obtained in the same manner as in Example 1, except that in the washing step, a lithium sulfate aqueous solution prepared so as to have a lithium ion concentration of 0.469 mol / L was used instead of the sodium sulfate aqueous solution, and the solid content concentration of the slurry was set to 32 mass %.

[0079] [Cycle characteristics evaluation 1] The cycle characteristics of the positive electrode active materials obtained in Examples 1 to 3 and Comparative Examples 1 and 2 were evaluated as follows.

[0080] Preparation of the positive electrode 96.5 parts by mass of the positive electrode active material, 65 parts by mass of SUPER-C (manufactured by Timical Corporation), and 2 parts by mass of PVDF (polyvinylidene fluoride) were dispersed and dissolved in NMP (N-methyl-2-pyrrolidone) to prepare a positive electrode slurry. The obtained positive electrode slurry was applied to a current collector made of aluminum foil, dried, and then pressed with a roll press machine until the density of the positive electrode active material layer became 3.5 g / cm. 3 Compression molded to a size of 15cm 2 The positive electrode was obtained by cutting the positive electrode into pieces having a diameter of 10 mm and a thickness of 1 mm.

[0081] Preparation of non-aqueous electrolyte A mixed solvent was prepared by mixing EC (ethylene carbonate), DMC (dimethyl carbonate), and EMC (ethyl methyl carbonate) in a volume ratio of 3:4:3. Lithium hexafluorophosphate (LiPF6) was dissolved in the mixed solvent to a concentration of 1 mol / L to obtain a nonaqueous electrolyte.

[0082] Assembling the evaluation battery A lead electrode was attached to the positive electrode current collector, and then vacuum dried at 120°C. A separator made of porous polyethylene was placed on the positive electrode in a dry box, and the positive electrode was stored in a bag-shaped laminate pack. After storage, the positive electrode current collector was vacuum dried at 60°C to remove moisture adsorbed on each component. After vacuum drying, the Li foil adhered to a SUS plate in an argon box and the positive electrode current collector covered with the separator were placed opposite each other and inserted into the laminate pack. The aforementioned nonaqueous electrolyte was injected into the laminate pack, which was then sealed to obtain a laminate type nonaqueous electrolyte secondary battery as an evaluation battery.

[0083] aging The obtained evaluation battery was charged and discharged once, consisting of a constant-voltage constant-current charge at a charge voltage of 4.25 V (counter electrode Li) and a charge current of 0.2 C (1 C ≡ a current at which discharging is completed in 1 hour), and a constant-current discharge at a discharge voltage of 2.75 V (counter electrode Li) and a discharge current of 0.2 C.

[0084] Capacity retention rate measurement After aging, one cycle consisted of a constant-voltage constant-current charge at a charge voltage of 4.25 V (counter electrode Li) and a charge current of 0.3 C, and a constant-current discharge at a discharge voltage of 2.75 V (counter electrode Li) and a discharge current of 0.3 C. The discharge capacity after each cycle was measured at a constant temperature of 45°C. The ratio of the discharge capacity Ed(n) after n cycles to the discharge capacity Ed(1) after 1 cycle (≡Ed(n) / Ed(1)) was defined as the capacity retention rate Rs(n) after n cycles, and the number of cycles n was 30. The evaluation results are shown in Table 1.

[0085] [Table 1]

[0086] As shown in Table 1, the evaluation batteries constructed using the positive electrode active materials E1 to E3 of Examples 1 to 3, which were washed with a sodium salt aqueous solution, mixed with a boron compound, and heat-treated, had excellent cycle characteristics. The positive electrode active material C1 of Comparative Example 1 had a large specific surface area of ​​the second particles. This is thought to be due to, for example, washing with pure water. In addition, the evaluation battery constructed using the positive electrode active material C1 had a low capacity retention rate and poor battery performance. The positive electrode active material C2 of Comparative Example 2 had a small specific surface area of ​​the second particles compared to Comparative Example 1. This is thought to be due to, for example, washing with a lithium sulfate aqueous solution. In addition, the evaluation battery constructed using the positive electrode active material C2 had a low capacity retention rate and poor battery performance.

[0087] [Example 4] Precursor preparation process By coprecipitation, the volume average particle size was 18 μm, and (Ni 0.85 Co 0.15 Composite oxide particles having a composition represented by the formula:

[0088] Synthesis process The first particles were obtained in the same manner as in Example 1, except that the mixing ratio in the synthesis step was changed to Li:(Ni+Co):Al=1.10:0.96:0.04 and the second temperature was changed to 745°C.

[0089] Cleaning process Second particles were obtained in the same manner as in Example 1, except that the sodium sulfate aqueous solution in the washing step was adjusted to have a sodium ion concentration of 0.313 mol / L and a solid content concentration of 40 mass %.

[0090] Mixing process Positive electrode active material E4 was obtained in the same manner as in Example 1, except that the amount of boric acid added in the mixing step was 0.3 mol% in terms of boron element relative to the total number of moles of metals other than lithium in the lithium transition metal composite oxide contained in the second particles.

[0091] [Comparative Example 3] A positive electrode active material C3 was obtained in the same manner as in Example 4, except that pure water was used instead of the aqueous sodium sulfate solution in the washing step and the solid content concentration was set to 45 mass %.

[0092] [Comparative Example 4] A positive electrode active material C4 was obtained in the same manner as in Example 4, except that in the washing step, an aqueous lithium sulfate solution prepared so as to have a lithium ion concentration of 0.313 mol / L was used instead of the aqueous sodium sulfate solution.

[0093] The positive electrode active materials obtained in Example 4 and Comparative Examples 3 and 4 were evaluated in the same manner as in Cycle Characteristics Evaluation 1. The evaluation results are shown in Table 2.

[0094] [Table 2]

[0095] As shown in Table 2, the evaluation batteries constructed with the positive electrode active materials C3 and C4 of Comparative Examples 3 and 4 had lower capacity retention rates and inferior battery performance compared to the evaluation battery constructed with the positive electrode active material E4 of Example 4 that had been washed with a sodium salt aqueous solution.

[0096] [Example 5] Precursor preparation process By coprecipitation, the volume average particle size was 22 μm, and (Ni 0.88 Co 0.09 Mn 0.03 Composite oxide particles having a composition represented by the formula:

[0097] Synthesis process The first particles were obtained in the same manner as in Example 1, except that the mixing ratio in the synthesis step was changed to Li:(Ni+Co+Mn):Al=1.12:0.98:0.02 and the second temperature was changed to 730°C.

[0098] Cleaning process Similarly to Example 1, the first particles were washed with an aqueous sodium sulfate solution prepared so that the sodium ion concentration was 0.469 mol / L to obtain second particles.

[0099] Mixing process A mixture was obtained in the same manner as in Example 1, except that the amount of boric acid added in the mixing step was 0.5 mol % in terms of elemental boron relative to the total number of moles of metals other than lithium in the lithium transition metal composite oxide contained in the second particles, and tungsten oxide was added so as to be 0.3 mol % relative to the total number of moles of metals other than lithium in the lithium transition metal composite oxide contained in the second particles.

[0100] Heat Treatment Process The mixture was heat-treated in the same manner as in Example 1 to obtain a positive electrode active material E5.

[0101] [Comparative Example 5] A positive electrode active material C5 was obtained in the same manner as in Example 5, except that pure water was used instead of the aqueous sodium sulfate solution in the washing step, and the solid content concentration of the slurry was set to 37 mass %.

[0102] [Comparative Example 6] A positive electrode active material C6 was obtained in the same manner as in Example 5, except that in the washing step, a lithium sulfate aqueous solution prepared so as to have a lithium ion concentration of 0.469 mol / L was used instead of the sodium sulfate aqueous solution, and the solid content concentration of the slurry was set to 28 mass %.

[0103] [Cycle characteristics evaluation 2] The cycle characteristics of the positive electrode active materials obtained in Example 5 and Comparative Examples 5 and 6 were evaluated as follows.

[0104] Preparation of positive electrode active material The volume average particle size is 4.5 μm, and Li 1.03 Ni 0.835 Co 0.14 Al 0.025 A positive electrode active material A was prepared, which contained a lithium transition metal composite oxide having a composition represented by O2 and was obtained through a washing process using an aqueous sodium sulfate solution. The positive electrode active materials E5, C5, and C6 obtained in Example 5 and Comparative Examples 5 to 6 were mixed with the positive electrode active material A in a weight ratio of 7:3 to prepare mixed positive electrode active materials for evaluation.

[0105] Preparation of the positive electrode 92 parts by mass of the mixed positive electrode active material obtained above, 3 parts by mass of acetylene black, and 5 parts by mass of PVDF (polyvinylidene fluoride) were dispersed and dissolved in NMP (N-methyl-2-pyrrolidone) to prepare a positive electrode slurry. The obtained positive electrode slurry was applied to a current collector made of aluminum foil, dried, and then pressed with a roll press machine until the density of the positive electrode active material layer became 3.3 g / cm. 3 Compression molded to a size of 15cm 2 The positive electrode was obtained by cutting the positive electrode into pieces having a diameter of 10 mm and a thickness of 1 mm.

[0106] Preparation of the negative electrode A negative electrode slurry was prepared by dispersing 97.5 parts by mass of artificial graphite, 1.5 parts by mass of CMC (carboxymethyl cellulose), and 1.0 parts by mass of SBR (styrene butadiene rubber) in water. The obtained negative electrode slurry was applied to a copper foil, dried, and further compression molded to obtain a negative electrode.

[0107] Preparation of non-aqueous electrolyte EC (ethylene carbonate) and EMC (ethyl methyl carbonate) were mixed in a volume ratio of 3:7 to prepare a mixed solvent. Lithium hexafluorophosphate (LiPF6) was dissolved in the obtained mixed solvent to a concentration of 1 mol / L to obtain a nonaqueous electrolyte solution.

[0108] Assembling the evaluation battery The battery for evaluation was assembled in the same manner as in cycle characteristic evaluation 1. Specifically, lead electrodes were attached to the current collectors of the positive and negative electrodes, respectively, and then vacuum dried at 120°C. Next, the separator was placed between the positive and negative electrodes, and these were stored in a bag-shaped laminate pack. After storage, the pack was vacuum dried at 60°C to remove moisture adsorbed on each member. After vacuum drying, a nonaqueous electrolyte was injected into the laminate pack and sealed, to obtain a laminate-type nonaqueous electrolyte secondary battery as a battery for evaluation.

[0109] aging The obtained evaluation battery was charged and discharged once, consisting of a constant-voltage constant-current charge at a charge voltage of 4.2 V (counter electrode C) and a charge current of 0.1 C, and a constant-current discharge at a discharge voltage of 2.75 V (counter electrode C) and a discharge current of 0.2 C. Thereafter, the charge current was changed to 0.2 C and charge and discharge were performed twice to allow the positive electrode and negative electrode to become familiar with the nonaqueous electrolyte.

[0110] The discharge capacity retention rate was measured in the same manner as in Cycle Characteristics 1, except that the charge voltage was 4.2 V (counter electrode C), the discharge voltage was 2.75 V (counter electrode C), and the number of cycles was n = 100. The evaluation results are shown in Table 3.

[0111] [Table 3]

[0112] [Evaluation of boron element distribution] The distribution of boron element inside the particles was evaluated for the positive electrode active materials obtained in Example 5 and Comparative Examples 5 and 6. Specifically, a positive electrode was prepared in the same manner as above, and the obtained positive electrode was processed under vacuum conditions using an ion milling device IM400PLUS (manufactured by HITACHI Corporation) to obtain a cross-sectional sample of the positive electrode active material particle. An Ar beam was used for the processing, and the processing time was 1 hour. The amount of each element detected in the cross section of the positive electrode active material particle in the obtained cross-sectional sample was measured using a double focusing sector magnetic field type mass spectrometer (NanoSIMS 50L; manufactured by Cameca Corporation). The primary ion species was Cs + The primary acceleration voltage was set to 8 kV, -8 kV was applied to the sample stage, and the sample was charged with Cs + By irradiating the sample with BO, the secondary ions 2- A signal of (mass number 42.97) was measured. A cross-sectional image was created based on the intensity of the measured signal. 2- FIG. 1 shows an example of an image showing the distribution of BO in the positive electrode active material particles obtained in Comparative Example 5. 2- FIG. 2 shows an example of an image showing the distribution of BO in the positive electrode active material particles obtained in Comparative Example 6. 2- An example of an image showing the distribution of each is shown in FIG.

[0113] Using image analysis software (OpenMIMS ImageJ Plugin), the obtained image data was used to identify the BO in the area near the particle surface (surface area), the area in the middle layer of the particle (middle layer area), and the area near the center of the particle (center area). 2- The amount of detected ions was calculated by analysis. The analysis was performed on three positive electrode active material particles for each Example and Comparative Example by selecting two regions from each of the surface, middle layer, and center. Each region was selected on a straight line that crossed the cross section of the particle so as to be approximately symmetrical with respect to the center of the particle, and the area of ​​each region was approximately 1.5 × 10 -11 m 2 The two central regions were selected as one continuous region. 2-The amount of BO detected was calculated as the arithmetic average for each of the two regions. From the amount of BO detected, it was found that the amount of BO detected in the three regions of the surface, middle layer, and center of the positive electrode active material particles was 2- The arithmetic mean value t1, standard deviation σ1, and coefficient of variation (CV; σ1 / t1) of the amount of boron detected were calculated. At this time, the standard deviation σ1 was calculated using the STDEV.P function of EXCEL. Regarding the coefficient of variation CV, the arithmetic mean results of three particles for each of the examples and comparative examples are shown in Table 4, and these results were evaluated as the distribution of boron element.

[0114] [Table 4]

[0115] As shown in Tables 3 and 4, the positive electrode active materials obtained in Comparative Examples 5 and 6 had lower capacity retention rates and inferior battery performance compared to Example 5, which was washed with a sodium salt aqueous solution. In addition, compared to Example 5, the boron-containing compound was not uniformly distributed to the inside of the particles. This is thought to be due to, for example, the absence of sodium at the grain boundaries of the positive electrode active material particles.

[0116] [Example 6] Precursor preparation process By coprecipitation, the volume average particle size was 4 μm, and (Ni 0.885 Co 0.115 )O3 composite oxide particles were obtained.

[0117] Synthesis process The same procedure as in Example 1 was carried out except that the mixing ratio in the synthesis step was changed to Li:(Ni+Co):Al=1.10:0.97:0.03 and the second temperature was changed to 690° C., to obtain first particles.

[0118] Cleaning process Second particles were obtained in the same manner as in Example 1, except that the aqueous sodium sulfate solution in the washing step was adjusted so that the sodium ion concentration was 0.156 mol / L.

[0119] Mixing process Positive electrode active material E6 was obtained in the same manner as in Example 1, except that the amount of boric acid added in the mixing step was 0.1 mol% in terms of boron element relative to the total number of moles of metals other than lithium in the lithium transition metal composite oxide contained in the second particles.

[0120] [Comparative Example 7] A positive electrode active material C7 was obtained in the same manner as in Example 6, except that in the washing step, a lithium sulfate aqueous solution prepared so as to have a lithium ion concentration of 0.156 mol / L was used instead of the sodium sulfate aqueous solution, and the solid content concentration of the slurry was set to 30 mass %.

[0121] The cycle characteristics of the positive electrode active materials obtained in Example 6 and Comparative Example 7 were evaluated as follows.

[0122] The volume average particle size is 22 μm, and Li 1.03 Ni 0.86 Co 0.09 Mn 0.03 Al 0.02 A positive electrode active material B containing a lithium transition metal composite oxide having a composition represented by O2 and obtained through a washing process using a sodium sulfate aqueous solution was prepared. The positive electrode active materials E6 and C7 obtained in Example 6 and Comparative Example 7 were mixed with the positive electrode active material B in a weight ratio of 3:7 to obtain a mixed positive electrode active material for evaluation. Evaluation was performed in the same manner as in cycle characteristic evaluation 2. The evaluation results are shown in Table 5.

[0123] [Table 5]

[0124] As shown in Table 5, the positive electrode active material obtained in Comparative Example 7 had a lower capacity retention rate and was inferior in battery performance compared to Example 6.

[0125] [Resistant rate evaluation] For the positive electrodes containing the positive electrode active materials obtained by the same production methods as in Example 5 and Comparative Examples 5 and 6, the resistance increase rate was evaluated as follows.

[0126] [Example 7] Preparation of positive electrode active material A positive electrode active material for evaluation was prepared by the same manufacturing method as in Example 5.

[0127] Preparation of the positive electrode 92 parts by mass of the positive electrode active material obtained above, 3 parts by mass of acetylene black, and 5 parts by mass of PVDF (polyvinylidene fluoride) were dispersed and dissolved in NMP (N-methyl-2-pyrrolidone) to prepare a positive electrode slurry. The obtained positive electrode slurry was applied to a current collector made of aluminum foil, dried, and then pressed with a roll press machine until the density of the positive electrode active material layer was 2.8 g / cm. 3 Compression molded to a size of 15cm 2 To obtain a positive electrode of Example 7. The density of the positive electrode active material layer was calculated by dividing the mass of the positive electrode active material layer by the volume of the positive electrode active material layer calculated by measuring the thickness of the positive electrode active material layer with a micrometer.

[0128] Assembling the evaluation battery A battery for evaluation was obtained in the same manner as in cycle characteristic evaluation 2, except that the positive electrode obtained above was used.

[0129] [Example 8] The density of the positive electrode active material layer is 3.3 g / cm 3 A positive electrode of Example 8 was obtained in the same manner as in Example 7, except that the positive electrode was compression molded so as to have a thickness of 100 μm. Then, a battery for evaluation was obtained in the same manner as in Example 7, except that the positive electrode was used.

[0130] [Example 9] The density of the positive electrode active material layer is 3.5 g / cm 3 A positive electrode of Example 9 was obtained in the same manner as in Example 7, except that the positive electrode was compression molded so as to have a thickness of 100 μm. Then, a battery for evaluation was obtained in the same manner as in Example 7, except that the positive electrode was used.

[0131] [Example 10] The density of the positive electrode active material layer is 3.7 g / cm 3A positive electrode of Example 10 was obtained in the same manner as in Example 7, except that the positive electrode was compression molded so as to have a thickness of 100 μm. A battery for evaluation was then obtained in the same manner as in Example 7, except that the positive electrode was used.

[0132] [Comparative Example 8] A positive electrode was obtained in the same manner as in Example 7, except that the positive electrode active material obtained by the manufacturing method of Comparative Example 5 was used as the positive electrode active material. Then, a battery for evaluation was obtained in the same manner as in Example 7, except that this was used.

[0133] [Comparative Example 9] The density of the positive electrode active material layer is 3.3 g / cm 3 A positive electrode of Comparative Example 9 was obtained in the same manner as in Comparative Example 8, except that the positive electrode was compression molded so that the positive electrode had a thickness of 100 μm or less. A battery for evaluation was then obtained in the same manner as in Example 7, except that the positive electrode was used.

[0134] [Comparative Example 10] The density of the positive electrode active material layer is 3.5 g / cm 3 A positive electrode of Comparative Example 10 was obtained in the same manner as in Comparative Example 8, except that the positive electrode was compression molded so that the positive electrode had a thickness of 100 μm. A battery for evaluation was then obtained in the same manner as in Example 7, except that the positive electrode was used.

[0135] [Comparative Example 11] The density of the positive electrode active material layer is 3.7 g / cm 3 A positive electrode of Comparative Example 11 was obtained in the same manner as in Comparative Example 8, except that the positive electrode was compression molded so that the positive electrode had a thickness of 100 μm or more. A battery for evaluation was then obtained in the same manner as in Example 7, except that the positive electrode was used.

[0136] [Comparative Example 12] A positive electrode was obtained in the same manner as in Example 7, except that the positive electrode active material obtained by the manufacturing method of Comparative Example 6 was used as the positive electrode active material. Then, a battery for evaluation was obtained in the same manner as in Example 7, except that this was used.

[0137] [Comparative Example 13] The density of the positive electrode active material layer is 3.3 g / cm 3A positive electrode of Comparative Example 13 was obtained in the same manner as in Comparative Example 12, except that the positive electrode was compression molded so that the positive electrode had a thickness of 100 μm. Then, a battery for evaluation was obtained in the same manner as in Example 7, except that the positive electrode was used.

[0138] [Comparative Example 14] The density of the positive electrode active material layer is 3.5 g / cm 3 A positive electrode of Comparative Example 14 was obtained in the same manner as in Comparative Example 12, except that the positive electrode was compression molded so that the positive electrode had a thickness of 100 μm or more. A battery for evaluation was then obtained in the same manner as in Example 7, except that the positive electrode was used.

[0139] [Comparative Example 15] The density of the positive electrode active material layer is 3.7 g / cm 3 A positive electrode of Comparative Example 15 was obtained in the same manner as in Comparative Example 12, except that the positive electrode was compression molded so that the positive electrode had a thickness of 100 μm. Then, a battery for evaluation was obtained in the same manner as in Example 7, except that the positive electrode was used.

[0140] aging The obtained evaluation battery was subjected to one charge / discharge cycle consisting of a constant-voltage / constant-current charge at a charge voltage of 4.2 V (counter electrode C) and a charge current of 0.1 C, and a constant-current discharge at a discharge voltage of 2.75 V (counter electrode C) and a discharge current of 0.2 C. Thereafter, the charge current was changed to 0.2 C and charge / discharge was performed twice to allow the positive electrode and negative electrode to become familiar with the nonaqueous electrolyte.

[0141] AC impedance measurement After aging, the battery was charged to a state of charge (SOC) of 100% by constant-voltage constant-current charging at a charging voltage of 4.2V and a charging current of 0.2C. Resistance measurements were performed in the range of 1MHz to 0.1Hz by an AC impedance method using impedance measuring devices (1470E and 1455A, both manufactured by SOLARTRON), and a Nyquist plot was obtained. After the above resistance measurements, the battery was discharged at a constant current of 2.75V and a discharge current of 0.2C at a constant temperature of 45°C, with one cycle consisting of a constant-voltage constant-current charge at a charging voltage of 4.2V and a charging current of 1C, and a constant-current discharge at a discharge voltage of 2.75V and a discharge current of 1C. After the 200 cycles of charging and discharging, the battery was charged to a state of charge of 100% by constant-voltage constant-current charging at a charging voltage of 4.2V and a charging current of 0.2C, and the resistance measurements were performed in the same manner using the impedance measuring device, and a Nyquist plot was obtained.

[0142] Calculation of resistance increase rate Based on the obtained Nyquist plot, the equivalent circuit model of FIG. 4 was constructed and fitting calculation was performed. The higher peak frequency of the arc component of the impedance obtained by the measurement was taken as the resistance derived from the negative electrode, and the lower peak frequency was taken as the resistance R derived from the positive electrode. The resistance value derived from the positive electrode before the cycle was taken as R(p), and the resistance value derived from the positive electrode after the cycle was taken as R(a), and R(a) / R(p)×100(%) was calculated as the resistance increase rate. Next, as in Comparative Example 8 for Example 7, the resistance increase rate calculated in the Example or Comparative Example washed with a washing solution was divided by the resistance increase rate in the Comparative Example prepared with the same electrode plate density and washed with pure water to calculate the relative resistance increase rate. Table 6 shows the evaluation results for Examples 7 to 10 washed with a sodium sulfate aqueous solution and Comparative Examples 12 to 15 washed with a lithium sulfate aqueous solution.

[0143] [Table 6]

[0144] As shown in Table 6, the relative resistance increase rate was low in the positive electrodes of the examples containing the positive electrode active material obtained through the washing process using an aqueous solution containing sodium ions, regardless of the plate density, and deterioration in output after cycling was suppressed. This result confirmed that the characteristics of the nonaqueous electrolyte secondary battery containing the positive electrode active material obtained through the washing process using an aqueous solution containing sodium ions were improved not only in capacity retention rate but also in resistance.

Claims

1. contacting first particles containing a lithium transition metal composite oxide having a layered structure and having a ratio of the number of moles of nickel to the total number of moles of metals other than lithium in the composition of the first particles with a solution containing sodium ions to obtain second particles containing the lithium transition metal composite oxide and elemental sodium; mixing the second particles with a boron compound to obtain a mixture; heat treating the mixture at a temperature of 100° C. or more and 450° C. or less; A method for producing a positive electrode active material comprising the steps of:

2. The method according to claim 1 , wherein the content of sodium element contained in the second particles is 100 ppm or more and 1400 ppm or less.

3. 3. The method according to claim 1, wherein the mixture contains the boron compound in an amount such that a ratio of the number of moles of boron element to the total number of moles of metals other than lithium in the lithium transition metal composite oxide is 0.1 mol % or more and 2 mol % or less.

4. 4. The method according to claim 1, wherein the lithium transition metal composite oxide contains cobalt, and the ratio of the number of moles of cobalt to the total number of moles of metals other than lithium is 0.3 or less.

5. 5. The method according to claim 1, wherein the lithium transition metal composite oxide contains at least one of manganese and aluminum, and the ratio of the number of moles of manganese and aluminum to the total number of moles of metals other than lithium is 0.3 or less.

6. The method according to claim 1 , wherein the lithium transition metal composite oxide has a composition represented by the following formula (1): Li (1+p) Ni (1-x-y-z-w) Co x Mn y A z M w O 2 (1) (-0.05≦p≦0.2, 0<x+y+z+w≦0.3, 0≦x≦0.3, 0≦y≦0.3, 0≦z≦0.1, 0≦w≦0.03, and M is at least one element selected from the group consisting of Zr, Ti, Mg, Ta, Nb, Mo, and W).

7. The secondary particles are formed by aggregating a plurality of primary particles that include a lithium transition metal composite oxide having a layered structure and having a ratio of the number of moles of nickel to the total number of moles of metals other than lithium in the composition of the lithium transition metal oxide of 0.7 or more and less than 1, a compound containing boron adheres to at least a portion of the surface of the primary particles; a compound containing sodium is present in at least a portion of the grain boundaries of the secondary particles; a value obtained by dividing the standard deviation of the detected amount by the average detected amount of boron element in any three regions in a cross section of the secondary particle is less than 0.18;

8. 8. The positive electrode active material according to claim 7, wherein the content of sodium element is 100 ppm or more and 1400 ppm or less.

9. 9. The positive electrode active material according to claim 7, wherein the ratio of the number of moles of elemental boron to the total number of moles of metals other than lithium is 0.1 mol % or more and 2 mol % or less.

10. 10. The positive electrode active material according to claim 7, wherein the lithium transition metal composite oxide contains cobalt, and a ratio of the number of moles of cobalt to the total number of moles of metals other than lithium is 0.3 or less.

11. 11. The positive electrode active material according to claim 7, wherein the lithium transition metal composite oxide contains at least one of manganese and aluminum, and the ratio of the number of moles of manganese and aluminum to the total number of moles of metals other than lithium is 0.3 or less.

12. The positive electrode active material according to claim 7 , wherein the lithium transition metal composite oxide has a composition represented by the following formula (1): Li (1+p) Ni (1-x-y-z-w) Co x Mn y A z M w O 2 (1) (-0.05≦p≦0.2, 0<x+y+z+w≦0.3, 0≦x≦0.3, 0≦y≦0.3, 0≦z≦0.1, 0≦w≦0.03, and M is at least one selected from the group consisting of Zr, Ti, Mg, Ta, Nb, Mo, and W).

13. A non-aqueous electrolyte secondary battery comprising the positive electrode active material according to claim 7 in a positive electrode.

14. A positive electrode active material layer is disposed on the current collector. The positive electrode active material layer contains the positive electrode active material according to any one of claims 7 to 12, Density is 2.8 g / cm 3 3.7g / cm or more 3 An electrode for a non-aqueous electrolyte secondary battery, comprising:

Citation Information

Patent Citations

  • Non-aqueous secondary battery and its manufacturing method

    JP2009076383A

  • Positive electrode for nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery using it

    JP2011060541A

  • Positive electrode active material for nonaqueous electrolyte secondary battery, method for manufacturing the same, and nonaqueous electrolyte secondary battery

    JP2018049685A

  • Positive electrode active material for lithium secondary battery, manufacturing method thereof, and lithium secondary battery

    JP2011124086A

  • Method for manufacturing positive electrode active material for nonaqueous electrolyte secondary batteries

    JP2015088343A