Join including insulating component particularly with at least partially crystallized glass, use thereof, crystallizable or at least partially crystallized glass, and use thereof
A bonded assembly using crystallizable or partially crystallized glass with a structured surface addresses the issue of unreliable electrical resistance and mechanical instability in high-temperature environments by ensuring high DC resistance and mechanical stability.
Patent Information
- Application Number
- JP2024110162
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-06-21
- Filing Date
- 2024-07-09
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2039-11-07
AI Technical Summary
Existing insulating materials used in high-temperature environments, such as exhaust gas installations in internal combustion engines, suffer from unreliable electrical resistance due to condensation and environmental influences, leading to impaired control behavior and mechanical instability.
A bonded assembly using an electrically insulating member made of crystallizable or partially crystallized glass with a structured surface to extend the creepage distance, ensuring high electrical resistance and mechanical stability, even under varying ambient conditions.
The solution provides a bonded assembly with a DC resistance of over 100 MΩ and high mechanical stability, maintaining electrical insulation and mechanical integrity under extreme temperatures and environmental changes.
Smart Images

Figure 2024138388000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a bonded assembly comprising an insulating member, in particular with at least partially crystallized glass, uses thereof, to a crystallizable glass and an at least partially crystallized glass, and uses thereof.
[0002] There are a variety of applications for bonded joints where temperature resistance, mechanical stability, and resistance to both can be important.
[0003] If such a joint assembly is part of an exhaust gas system of an internal combustion engine, for example for transmitting electrical or electronic signals, for example in a motor vehicle with controlled exhaust gas cleaning, the ambient conditions change frequently and greatly. For example during cold start operation, especially in relatively cold regions or when the air humidity is high, such a joint assembly can become covered with a water film from condensed atmospheric components. This condensation can appear as the formation of droplets or even as a coating of the entire surface of the joint assembly. This can cause the electrical resistance between the joint partners to change undesirably and the corresponding control of the exhaust gas cleaning can be impaired in its control behavior.
[0004] Although very resistant insulating materials can be used, as will be exemplarily explained in more detail below for crystallizable or at least partially crystallized glasses, they are often not reliable enough in such environments to withstand the above losses in order to ensure that the control behavior is not compromised.
[0005] In document DE 102008045816 A1, an elastomeric material is proposed surrounding the conductor in order to increase the creepage distance, which in the context of the present disclosure is the distance over which creepage currents can occur between the mating partners. The disadvantage of this solution is that the elastomeric material often does not have the thermal stability and long-term operational durability required for the high-temperature areas of exhaust gas installations.
[0006] One aspect of the present invention addresses better preserving the electrical or electronic properties, especially the high resistivity properties, of the insulating materials disclosed herein, especially the crystallizable or partially crystallized glasses disclosed herein, from environmental influences.
[0007] This aspect of the problem to be solved by the present invention is solved by a bonded assembly comprising an electrically insulating member and at least two bonded partners, in which at least one of the bonded partners 51, 52 is kept electrically insulated from at least the other of the bonded partners 51, 52 by an electrically insulating member 53, and a surface of the electrically insulating member 53 extending between the bonded partners forms a structure S, in particular a bump or depression, by which in particular a direct path along the surface from at least one bonded partner to at least the other bonded partner is extended compared to a surface not having this structure S, and the structure preferably completely surrounds at least one of the bonded partners, and the insulating member or structure comprises or consists of a crystallizable glass or an at least partially crystallized glass, as well as by the use thereof.
[0008] In the context of the present disclosure, "maintained electrically insulated" refers to a DC resistance of greater than 100 MΩ between bonded partners in a dry atmosphere of a bonded assembly as described herein that is free of deposits that may compromise this resistance, the electrical resistance being measured at a voltage of less than 100 V.
[0009] The structure S mentioned above may be formed integrally with and of the same material as a portion of an insulating member, which portion extends between and is respectively joined to and preferably glass-fused to the joining partners, preferably the material of the insulating member comprising at least partially crystallized glass and the use thereof.
[0010] In the case of the bonded joints of the present disclosure, the transition area between the surface of the bonded partner and the surface of the at least partially crystallized glass is preferably less than 1 cm 3 An at least largely amorphous glass layer can be arranged which contains fewer than 10 pores per 100 μm and / or has a thickness of preferably 5 μm or less, particularly preferably 2 μm or less, very particularly preferably 1 μm or less.
[0011] In the case of the bonded assemblies described herein, the structure S may comprise a crystallizable glass or at least partially crystallized glass, and at the surface of the structure S, at least a predominantly amorphous glass layer is formed, in particular substantially free of open pores, in particular less than 10 pores / cm. 3 It may be formed as a glass layer having a thickness of less than or equal to 5 μm, preferably less than or equal to 2 μm, very particularly preferably less than or equal to 1 μm.
[0012] Also disclosed below are embodiments of joint assemblies in which the structure S is not of the same material as the portions of the insulating members to which it extends, each being joined and preferably glass-fused to the joint partners.
[0013] In such a joint assembly, the structure S comprises a high temperature stable ceramic material, such as forsterite, an aluminum oxide based ceramic, or a zirconium oxide based ceramic, such as a Y-stabilized zirconium oxide, rather than the same material as the portions of the insulating members to which it extends and which are respectively bonded and preferably glass fused to the joint partners.
[0014] In the case of a joint assembly in which the structure S is not of the same material as the portion of the insulating member to which it extends, respectively joined and preferably glass-fused to the joint partners, the structure S may be positioned approximately radially centrally in this portion of the insulating member, preferably at least partially recessed therein.
[0015] In the case of advantageous bonded combinations in which the structure S includes a reinforcement, the reinforcement includes a metal sheet, a metal foil, or a metal-containing scrim, mesh or braid, preferably the metal includes or consists of steel.
[0016] In an embodiment of the present disclosure, the structure S may have an end with a radius of curvature Rv of less than a tenth of a millimeter, preferably less than a twentieth of a millimeter, and greater than 10 μm.
[0017] Using a crystallizable or at least partially crystallized glass corresponding to the embodiments described herein, the structure S described herein makes it possible to enlarge the surface of the insulating material disposed between the joining partners to be separated from one another, thus extending the creepage distance over the surface of the insulating member.
[0018] The crystallizable or at least partially crystallized glasses according to the embodiments described herein allow the formation of high-temperature stable and / or mechanically strong bonded joints. As explained above, the crystallizable or at least partially crystallized glasses according to the embodiments described allow the formation of particularly stable structures in the at least partially crystallized glasses, in particular structures that are mechanically stable even at high temperatures up to 1000° C. or even higher.
[0019] A further aspect therefore relates to crystallizable glasses and glasses that are present at least partially crystallized, in particular for use in the field of solder glasses. Solder glasses (also called glass solders or in English "sealing glasses") are used to create tight bonds between the parts to be joined. These bonds are also called bonded composites or bonded bonds.
[0020] To produce stable joint assemblies which are exposed in operation to very high temperatures, for example temperatures above 900° C., for example even around 1000° C., solder glasses are always required which, on the one hand, can withstand these high temperatures and, on the other hand, are adapted in terms of their expansion behavior to the materials to be joined. The materials to be joined are, for example, high-temperature resistant metals and / or metal alloys or high-temperature resistant non-metallic materials such as yttrium-stabilized ZrO2.
[0021] Furthermore, the joint combination must be gas-tight and, in particular when used in electrical components such as sensor technology and / or fuel cells, must have an electrically insulating effect, i.e. have a very low electrical conductivity.
[0022] However, commercially available glass solders with high thermal expansion generally have low melting temperatures, limiting their thermal stability and therefore they cannot be used at high temperatures. In contrast, glass solders have thermal expansion coefficients in the high temperature range that are much lower than the thermal expansion coefficients of their high temperature resistant joining partners.
[0023] The prior art has suggested various glass solders for producing bonded joints.
[0024] German patent application DE 10016416 A1 describes a glass-ceramic melt seal in which the starting glass used consists of 38-48% by weight SiO2, 15-19% by weight Al2IO3, 4.5-11% by weight TiO2, 0-1.5% by weight Na2O, 0-1.5% by weight K2O, and 23-30% by weight CaO, with up to 1.5% by weight Li2O also being added. These compositions result in a maximum melting point of 8.8°C in the temperature range 100°C to 500°C. * 10 -6 A thermal expansion coefficient of 0.15-0.25 K can be achieved.
[0025] German patent DE 10 2012206266 A1 describes a barium- and strontium-free glassy or glass-ceramic joining material and its use. In order to adequately wet the components to be joined, the joining material contains B2O3.
[0026] The German published patent application DE 10 2014 218 983 A1 describes a feedthrough element for harsh operating conditions. Here too, the joining material contains B2O3.
[0027] The published patent application DE 10 2010035251 A1 describes a high-temperature glass solder and its use. The glass solder contains at least 10% by weight of BaO. However, BaO is disadvantageous since barium reacts with Cr contained in high-temperature, i.e. high-temperature resistant steels.
[0028] The published patent application DE 10 2015 207 285 A1 describes a vitreous or at least partially crystallized melt sealing material, which contains at least 5 mol % B2O3.
[0029] DE 10 2011080352 A1 describes a high-temperature glass solder and its use. The described high-temperature glass solder contains 13% to 50% by weight of Al2O3, SiO2 being only optionally contained in the glass solder.
[0030] The US patent application US2007 / 0238599 describes highly crystalline sintered glass-ceramics containing cyclosilicates. According to one embodiment, the glass-ceramics of US2007 / 0238599 contain as necessary components 30% to 55% by weight of SiO2, 5% to 40% by weight of CaO, and 0.1% to 10% by weight of Al2O3, the sum of the oxides BaO, CaO, and SrO contained in the glass-ceramics being 40% to 65% by weight. In other words, the glass-ceramics of US2007 / 0238599 do not only contain CaO, but always further contain BaO and / or SrO.
[0031] The United States patent application US 2010 / 0129726 describes lead-free glasses having a low B2O3 content, where the content of the oxides SiO2, MgO, CaO, SrO, BaO, ZnO, and Al2O3 in the glass is at least 97 mol%.
[0032] Glass-ceramic compositions for sealing materials are further described in US Patent Application Publication No. 2013 / 0108946. These compositions consist of either SiO2, Al2O3, and CaO, or SiO2, Al2O3, CaO, and SrO, or SiO2, Al2O3, and La2O3, as well as other selected additional components.
[0033] Reddy et al. in RSC Advances, 2012, 2, 10955-10967, describe melilite-based glasses and glass-ceramics for functional applications such as sealing materials, with Bi2O3 acting as a crystallizing agent in particular.
[0034] International patent application WO 2017 / 220700 describes a bond made with at least partially crystallized glass, the at least partially crystallized glass having at least one crystalline phase and pores arranged in a structured and distributed manner in the at least partially crystallized glass, and a method for making such a bond.
[0035] Finally, the international patent application WO 2018 / 066635 describes a glass composition for joining or bonding, which contains 43 mol% to 53 mol% SiO2, 12 mol% to 33 mol% CaO, 12 mol% to 33 mol% MgO, and 1 mol% to 7 mol% La2O3, and 0 mol% to 4.5 mol% ZnO.
[0036] All of the above mentioned materials of the prior art have drawbacks.
[0037] For example, compositions according to DE 102012206266, DE 102014218983 and DE 102015207285 necessarily contain B2O3. Glasses according to the international patent application WO 2017 / 220700 also preferably contain B2O3. However, since B2O3 is already a material that melts at relatively low temperatures, as already mentioned above, it is often used in order to sufficiently wet the components to be joined in the melt. However, this approach does not allow high heat resistance of the joining bond to be achieved.
[0038] When the joining material contains BaO and / or SrO, adverse contact reactions occur with high temperature resistant steels, which generally contain Cr.
[0039] When cyclosilicates form as a crystalline phase, they form a * 10 -6 / K.
[0040] Moreover, a high content of nucleating materials, such as TiO2, is disadvantageous as it may lead to uncontrolled crystallization of the crystallizable glass and may even lead to the formation of low-expansion crystalline phases, which is most unfavorable for the applications considered here.
[0041] For example, as described in US Patent Application Publication No. 2010 / 0129726, if the content of components incorporated in the crystalline phase is very high, the wetting of the materials to be joined and therefore its suitability as a joining material is questionable.
[0042] There is therefore a need for crystallizable glasses that have high heat resistance, preferably of 900° C. or higher, that wet the materials and / or components to be joined when melted, and that preferably have a high coefficient of thermal expansion.
[0043] It is therefore also a further aspect of the object of the present invention to provide a crystallizable glass which overcomes or at least mitigates the aforementioned drawbacks of the prior art.
[0044] This further aspect of the problem of the invention is solved by the subject matter of the independent claims. Further configurations and special embodiments can be found in the dependent claims as well as in the figures and the description.
[0045] The disclosure of this further aspect of the invention relates to a bonded assembly, in particular a bonded assembly that is stable at high temperatures and / or can withstand high mechanical loads, comprising an at least partially crystallized glass and a bonded partner, in which the at least partially crystallized glass comprises a volumetric proportion of residual glass of less than 10%, preferably less than 5%, where the at least partially crystallized glass comprises a crystalline aggregate. The crystalline aggregate is formed from a large number of crystallites. Preferably, the crystallites are formed in the form of needles and / or platelets. Preferably, the crystallites are distributed throughout the at least partially crystallized glass and may be arranged radially, for example in the form of sphaeroliths and / or fans and / or rods and / or platelets.
[0046] Such construction of the bonded joint has many advantages.
[0047] In particular, a high dimensional stability of the bonded joint is achieved with a low percentage of residual glass, less than 10% by volume, preferably even less than 5% by volume.
[0048] Furthermore, advantageously, the high dimensional stability of the bonded bond is ensured by the aggregation of the crystallites contained in the crystallized glass. Here, it is particularly advantageous for the crystallites to be formed in the form of needles and / or platelets. The inventors have found that the needle-shaped and / or platelet-shaped crystallites in the crystallized aggregates result in the formation of an at least partially crystallized glass that is mechanically stable. This is particularly true if the crystallites, which are preferably formed in the form of needles and / or platelets, are distributed throughout the at least partially crystallized glass, for example arranged in the form of spherulites and / or fans and / or rods or platelets. The inventors believe that the crystallites, which are preferably formed in the form of needles and / or platelets, distributed throughout the at least partially crystallized glass, and their arrangement, for example in the form of spherulites or radial or random rods, interlock with each other, thereby advantageously increasing the mechanical stability of the at least partially crystallized glass, for example against shear, compressive or tensile forces. This interlocking can also take place in the form of a kind of "house of cards".
[0049] Crystallites can also be formed in platelets, i.e. distributed as small platelets in the crystallized glass. In cross-sectional view, such formations can also appear as rods, so that it is difficult to distinguish between them. In the context of the present disclosure, platelets are understood to be geometric shapes whose transverse dimension (thickness) in one spatial direction of the Cartesian coordinate system is an order of magnitude smaller than the transverse dimensions (length, width) in the other two directions perpendicular to the first direction.
[0050] The present disclosure further provides a bonded assembly, in particular a bonded assembly that is stable at high temperatures and / or capable of withstanding high mechanical loads, comprising an at least partially crystallized glass and a bonded partner, wherein the glass is La2O3: more than 0.3 mol% to less than 5 mol%, preferably 4.5 mol% or less, particularly preferably 4 mol% or less; Nb2O50mol%~9mol%, Ta2O50mol%~7mol%, where Σ(A2O5) 0.2mol% to 9mol%, where A is an element which in the oxide normally has the oxidation number V+, and which may include, for example, Nb, and / or Ta, or P, and / or mixtures thereof. The present invention relates to a conjugate comprising:
[0051] It has been shown that strong bonded joints, for example bonded joints that are stable at high temperatures and / or can withstand high mechanical loads, can be obtained by adding the oxides La2O3, Ta2O5, and / or Nb2O5, and optionally further oxides of composition A2O5, in sufficient amounts, i.e. in the ranges mentioned above.
[0052] Here, A represents an element that in its oxide usually has the oxidation number V+. Thus, the atoms "A" contained in a crystallizable or at least partially crystallized glass may not all be in the same oxidation state.
[0053] Here, in the context of the present disclosure, the oxides La2O3, Nb2O5, and Ta2O5, as well as the further oxide A2O5 optionally contained in the glass, are also referred to as "glass matrix forming oxides", which in the context of the present disclosure means that such oxides initially remain in the glass matrix after heat treatment of the crystallizable glass, i.e. when the glass is present as an at least partially crystallized glass. The term "glass matrix forming oxides" is therefore different from the more general term "glass forming oxides". In particular, in the context of the present disclosure, the oxides MgO and CaO are not glass matrix forming oxides, even though, for example, CaO is a common constituent of conventional glasses, e.g. soda-lime glass. In glasses according to embodiments of the present disclosure, oxides such as CaO and MgO are incorporated into the crystalline phase, i.e. do not remain in the glass matrix, and therefore are not glass matrix forming oxides either.
[0054] However, it is entirely possible that at least a portion of the glass matrix-forming oxides, for example La2O3, may be at least partially incorporated into the crystalline phase in the further course of ceramization, but usually a small residual content of the glassy phase, formed in particular by the glass matrix-forming oxides, remains.
[0055] The formation of the bonded joint according to the present disclosure with the oxides La2O3, and Nb2O5, and / or Ta2O5 in the above-mentioned ranges, and optionally further oxides A2O5, is advantageous since the at least partially crystallized glass is thus particularly advantageously constituted in such a way that glass welding occurs during the temperature treatment for producing the joint. That is to say, particularly advantageously, strong bonds are thus generated between the individual parts of the bonded joint, in particular allowing a strong bond of the at least partially crystallized glass to the joint partner. However, by limiting the glass matrix-forming oxides to the aforementioned ranges, it is advantageously ensured that a high temperature stability and / or a high mechanical strength of the bonded composite occurs at the same time.
[0056] In the context of this disclosure, the following definitions apply: In the context of the present disclosure, a crystallizable glass is understood to be a glass capable of crystallization, in particular of controlled or at least controllable crystallization. Here, controlled crystallization is understood to mean that a crystallizable glass can be brought to a state in which the glass is at least partially crystallized by targeted temperature treatment, and the crystallographic composition of the at least partially crystallized glass and / or its structure, i.e. the spatial arrangement and / or size of the crystals and / or crystallites contained in the at least partially crystallized glass, can be preferably targeted and adjusted. Preferably, by controlling the crystallization, it is possible to obtain a structure in which the crystallites have a substantially uniform size, for example in the single-digit micrometer range, i.e. for example all crystallites have an equivalent diameter of about 1 μm to 3 μm.
[0057] Of course, other textures having larger or smaller crystallites are possible.
[0058] When an at least partially crystallized glass contains multiple different crystalline phases, the average crystal size or average crystallite size within the crystalline phases will be relatively similar, although there may be significant differences between the individual crystalline phases with respect to crystallite size.
[0059] In contrast to the preferred controlled or controllable crystallization, spontaneous crystallization of glasses is observed, which can result in unexpected and often undesirable crystalline phases, especially complete devitrification.
[0060] In the context of the present disclosure, a crystal aggregate or crystal association is understood to be an intergrowth of at least two crystals or crystallites, where the crystals or crystallites may in particular be intergrown randomly, meaning that the individual crystallites or crystals of the aggregate may not be intergrown along a preferred direction or specific crystallographic plane.
[0061] By "crystals or crystallites formed in needle-like shapes" it is understood that the crystals or crystallites have a dimension in one direction that is at least an order of magnitude larger than the dimensions in the other two spatial directions. In other words, crystals or crystallites formed in needle-like shapes can be formed in needle-like or rod-like shapes, or in prismatic shapes, with the transverse dimension of the prismatic basic shape being at least an order of magnitude smaller than the length of the crystal or crystallite. Such crystals or crystallites are also referred to as "prismatically formed".
[0062] Crystallites can also be formed in platelets, i.e. distributed as small platelets in the crystallized glass. In cross-sectional view, such formations can also appear as rods, so that it is difficult to distinguish between them. In the context of the present disclosure, platelets are understood to be geometric shapes whose transverse dimension (thickness) in one spatial direction of the Cartesian coordinate system is an order of magnitude smaller than the transverse dimensions (length, width) in the other two directions perpendicular to the first direction.
[0063] In the context of the present disclosure, "arrangement of crystals or crystallites radially" is understood to mean that needle- or platelet-shaped crystals, e.g., needle- or prismatic crystals or crystallites, are arranged around a center with one end pointing toward this point and the other ends pointing radially outward in different spatial directions. For example, the ends pointing toward the center may be in contact with the center point. However, this is not necessary. Such formed crystal aggregates radially outward from the center are present, for example, in the form of spherulitically formed crystal aggregates. Such spherulitically formed ones are crystal aggregates of approximately spherical or elliptical configuration, which in a two-dimensional representation may show an approximately circular shape. However, in practice, based on the intergrowth of crystals and crystal aggregates in the tissue, they often differ from the ideally spherical or circularly formed spherulites. In particular, the crystals or crystallites forming the spherulites may have different lengths and / or thicknesses.
[0064] A further configuration of the radial arrangement is the formation of a fan shape in a two-dimensional cross section. For example, it may not be possible to form crystals or crystallites in a particular spatial direction in the tissue. Here again, the crystallites or crystals extend from the center outwards, but only within a particular solid angle.
[0065] By "distributed arrangement in the form of rods or platelets" it is understood that the individual crystals or crystallites do not extend outwards in different spatial directions from a common center, but are arranged randomly, e.g. without a particular preferred direction. In particular, the crystallites or crystals may be arranged in relation to one another. Such a structure may also be likened, for example, to that of a "house of cards" in which the individual platelets (such as the cards in a house of cards) are arranged on top of one another to form a stable structure.
[0066] In the context of the present disclosure, a crystallization nucleus is understood to be the starting point of crystallization. A crystallization nucleus promotes the accumulation of atoms to build a crystal lattice, for example, thermodynamically or kinetically. In particular, a crystallization nucleus may be a lattice defect and / or an aggregate of atoms. In many cases, an interface may be the starting point of crystallization, or an interface may include such a starting point of crystallization.
[0067] According to one embodiment of the bonded bond, the crystallites comprise crystallization nuclei at least partially at the grain boundaries and / or the deposits comprising lanthanum, in particular comprising lanthanum compounds, are at least partially located at the grain boundaries of the crystallites.
[0068] Such a configuration of the joint bond is advantageous in that it makes it possible to form a particularly strong bond between the at least partially crystallized glass and the joint partner, which, if the crystallites contain crystallization nuclei at least partially at the grain boundaries, promotes the formation of a structure of the at least partially crystallized glass with crystal aggregates arranged, for example, radially or rod-like or platelet-like in distribution, for example, like a house of cards.
[0069] This is true even when the deposits containing lanthanum, particularly those containing lanthanum compounds, are at least partially located at the grain boundaries of crystallites, and the inventors believe that deposits of lanthanum, e.g., lanthanum compounds, may act as effective crystallization nuclei.
[0070] According to a further embodiment of the bonded assembly, the difference between the thermal expansion coefficients of the bonded partners and the at least partially crystallized glass has a value of 5. * 10 -6 / K or less, preferably 3 * 10 -6 / K or less, particularly preferably 1×10 -6 / K or less. Such a configuration of the bonded joint, in particular the matching of the thermal expansion coefficients of the glass and the bonded partner, has the advantageous effect that the heat resistance and / or the mechanical durability of the bonded joint thus obtained can be further improved.
[0071] The bonded assembly can be subjected to high operating temperatures, in particular operating temperatures of 1000° C. and above. It is believed that the presence of the crystalline aggregates and the described structure mechanically stabilize the material, for example by the crystalline aggregates interlocking with one another, so to speak. If a residual glass phase is included, the crystalline aggregates and / or their structure can also stabilize the residual glass phase, even if the residual glass phase would, so to speak, soften under the influence of temperature.
[0072] Equally advantageously, the bonded joint is mechanically stable, especially against vibration loads, as also measured as a function of temperature in shake and vibration tests according to ISO 16750-3 (ed. 2007-08-01). It is believed that the crystalline aggregates inhibit the propagation of initial cracks in the material, so that even in the event of localized damage, failure of the component with the bonded joint is avoided.
[0073] According to one embodiment of the present disclosure, the bonded combination withstands an operating temperature of at least 1000° C., and preferably the bonded combination is vibration and vibration resistant as measured in accordance with ISO 16750-3.
[0074] In other words, the crystal aggregates appear to mutually inhibit the displacement of the at least partially crystallized glass volume elements in the operating state. This can be assumed considering any two adjacent volume elements that contain a crystal aggregate. In the operating state under mechanical load, forces, such as shear forces, that tend to displace the volume elements relative to each other can act on the volume elements. If the crystal aggregates have a suitable structure, in particular the mentioned structures, they can interlock with each other and thus already purely mechanically inhibit the volume elements from displacing each other.
[0075] That is to say, according to yet another embodiment of the bonded assembly, the crystalline aggregates inhibit the volume elements of the at least partially crystallized glass from being displaced relative to one another in the operating state.
[0076] The measures mentioned here can also be combined, particularly advantageously.
[0077] Advantageously, the bonded assembly is configured such that there is no meniscus or there is a neutral meniscus on the surface of the at least partially crystallized glass.
[0078] Here, "forming a meniscus-free surface" is understood to mean that the surface is not curved. A curved surface of the at least partially crystallized glass can occur, for example, when the glass is heated for the production of the bonded joint and at least partially melts (so-called glass welding) and the bonded partner wets it particularly well, so that the glass rises due to capillary forces at the interface to the bonded partner. In this case, the meniscus is formed concavely. Conversely, if there is only little wetting, for example when a very viscous glass is present, a convex meniscus can be formed. However, optimally, the bonded joint is designed in such a way that the surface of the at least partially crystallized glass is formed without a meniscus, i.e. without any upward or downward curvature. In this case, it is also called a neutral meniscus.
[0079] According to a further embodiment of the bonded joint, in the transition area between the surface of the bonded partner and the surface of the at least partially crystallized glass, preferably 1 cm 3 An at least largely amorphous glass layer is arranged which contains fewer than 10 pores per 100 μm and / or has a thickness of preferably 5 μm or less, particularly preferably 2 μm or less, very particularly preferably 1 μm or less.
[0080] Such a bonded joint is advantageous since a particularly strong bond can be achieved in this way. In particular, the low porosity at the interface between the at least partially crystallized glass and the bonded partner advantageously further increases the mechanical durability and / or heat resistance of the joint. That is, pores at or near the interface can be the initiation point for mechanical failure, especially if the bonded joint is exposed to high temperatures.
[0081] Furthermore, the small thickness of the amorphous glass layer at the interface advantageously aids in the formation of a bonded bond that can withstand high loads, for example thermally and / or mechanically. "Forming a glass layer" means that there is a chemical bond between the bonded partner and the glass. However, according to the present disclosure, it is particularly advantageous if the at least partially crystallized glass has a proportion of residual glass of less than 10% by volume, preferably less than 5% by volume. In other words, the at least partially crystallized glass should only have a small proportion of residual glass. This is because the thermal and / or mechanical stability of the bonded bond is caused in particular by the formation of a crystalline phase or crystalline phases. Thus, advantageously, in particular, a high thermal resistance and / or mechanical durability is ensured if the amorphous glass layer has a small thickness of at most 5 μm or less, preferably 2 μm or less, particularly preferably 1 μm or less.
[0082] According to one embodiment of the joining combination, the joining partners are metals, in particular steels, such as plain steels, stainless steels, stainless steels, and high-temperature stable ferritic steels, also known as Thermax, for example under the trade names Thermax 4016, Thermax 4742 or Thermax 4762, or under the trade names Crofer22 APU or Crofer22 H, or NiFe-based materials, for example NiFe45, NiFe47 or nickel-plated pins, or Inconel, for example under the trade names Inconel 718 or X-750, or NiFe-based materials, for example CF25, Alloy 600, Alloy 601, Alloy 625, Alloy 630, Alloy 640, Alloy 650, Alloy 660, Alloy 670, Alloy 680, Alloy 690, Alloy 700, Alloy 710, Alloy 720, Alloy 730, Alloy 740, Alloy 750, Alloy 760, Alloy 770, Alloy 780, Alloy 790, Alloy 800, Alloy 810, Alloy 820, Alloy 830, Alloy 840, Alloy 850, Alloy 860, Alloy 870, Alloy 880, Alloy 890, Alloy 900, Alloy 910, Alloy 920, Alloy 930, Alloy 940, Alloy 950, Alloy 960, Alloy 970, Alloy 980, Alloy 990, Alloy 1000, Alloy 1010, Alloy 690, SUS310S, SUS430, SUH446 or SUS316, or austenitic steels such as 1.4762, 1.4828 or 1.4841, metals from the Kanthal heating wire group, or high-temperature stable ceramic compounds such as forsterite, aluminium oxide based ceramics or zirconium oxide based ceramics, for example Y-stabilised zirconium oxide based ceramics.
[0083] According to one embodiment, the conjugate is 10 -8 mbar * It exhibits a helium leak rate of less than l / s and / or according to one embodiment comprises at least partially crystallized glass with an elastic modulus of 80 GPa to 200 GPa, preferably with an elastic modulus of 100 GPa to 125 GPa. Such a configuration is advantageous since in this way a sufficient mechanical stiffness is achieved, but such a bond is nevertheless more elastic, for example compared to conventional ceramics. This is advantageous in the case of loads of temperature changes, thus advantageously resulting in a bonded bond that is particularly temperature stable.
[0084] The present disclosure further comprises: La2O3: more than 0.3 mol% to less than 5 mol%, preferably 4.5 mol% or less, particularly preferably 4 mol% or less; Nb2O50mol%~9mol%, Ta2O50mol%~7mol%, where Σ(A2O5) 0.2mol% to 9mol%, where A is an element which in the oxide normally has the oxidation number V+, and may include, for example, Nb, and / or Ta, or P, and / or mixtures thereof. The present invention relates to a crystallizable or at least partially crystallized glass comprising:
[0085] It has been shown that a strong bond between the glass and the joining partner can be obtained by adding the oxides La2O3, Ta2O5 and / or Nb2O5, and optionally further oxides of composition A2O5, in sufficient amounts, i.e. in the ranges mentioned above.
[0086] Here, A represents an element that in its oxide usually has the oxidation number V+. Thus, the atoms "A" contained in a crystallizable or at least partially crystallized glass may not all be in the same oxidation state.
[0087] Here, in the context of the present disclosure, the oxides La2O3, Nb2O5, and Ta2O5, as well as the further oxide A2O5 optionally contained in the glass, are also referred to as "glass matrix forming oxides", which in the context of the present disclosure means that such oxides initially remain in the glass matrix after heat treatment of the crystallizable glass, i.e. when the glass is present as an at least partially crystallized glass. The term "glass matrix forming oxides" is therefore different from the more general term "glass forming oxides". In particular, in the context of the present disclosure, the oxides MgO and CaO are not glass matrix forming oxides, even though, for example, CaO is a common constituent of conventional glasses, e.g. soda-lime glass. In glasses according to embodiments of the present disclosure, oxides such as CaO and MgO are incorporated into the crystalline phase, i.e. do not remain in the glass matrix, and therefore are not glass matrix forming oxides either.
[0088] However, it is entirely possible that one or more glass matrix forming oxides, such as La2O3, are at least partially incorporated into the crystalline phase in the subsequent steps of ceramization, but essentially a residual glass fraction remains, which is formed by the so-called glass matrix forming oxides.
[0089] The addition of the components La2O3, Ta2O5 and / or Nb2O5, and possibly the further oxide A2O5, primarily contributes to the high glass stability of the starting material. As explained above, these oxides are the oxides which remain, at least initially, in the crystallites and / or in the glass matrix surrounding the crystals after a heat treatment, i.e. after a heat treatment capable of turning the crystallizable glass into an at least partially crystallized glass.
[0090] The inventors assume that these elements are transformed into and / or incorporated into the crystalline structure components, if at all, only during subsequent heat treatments. In particular, at least the element La2O3 may be at least partially incorporated into the crystalline phase.
[0091] It has now surprisingly been shown that it is precisely this vitreous structure component, which may in particular comprise the abovementioned oxides such as La2O3, Ta2O5 and / or Nb2O5, and optionally the further oxide A2O5, that ensures a strong bond with the joining partners, i.e. the materials and / or components to be joined, without nevertheless inhibiting the high dimensional stability of the resulting joint at high temperatures, such as temperatures of 900°C or even temperatures of 950°C or even 1000°C or higher.
[0092] In the context of the present disclosure, a material and / or component is referred to as being high-temperature resistant or high-temperature stable if it can be used at temperatures of 900° C. or more, preferably 950° C. or more, particularly preferably 1000° C. or more, in particular if it can be used at temperatures of 900° C. or more, preferably 950° C. or more, particularly preferably 1000° C. or more, for 100 hours or more, preferably 500 hours or more, particularly preferably 1000 hours. In particular, the material and / or component can be formed such that it is stable against deformation at these temperatures for the periods mentioned.
[0093] This high dimensional stability is also due to the relatively early onset of crystallization. However, due to the glass matrix, this does not inhibit a strong bond of the joining partners. This is particularly surprising, since up until now it was assumed that crystallization only occurred after sintering was completed, allowing a strong and dense bond to be obtained (see, for example, Tulyaganov et al., Journal of Power Sources 242 (2013), 486-502).
[0094] Further components that may be included in the glass and that remain at least partially in the glass matrix after heat treatment are Bi2O3 and / or P2O5. However, these components are disadvantageous in terms of the high temperature stability of the glass considered here and the bonded joints made with it. Therefore, according to one embodiment, the glass advantageously does not contain oxides of Bi and / or P, except in unavoidable trace amounts.
[0095] In the context of this disclosure, a content of 500 ppm or less of this component is referred to as an unavoidable trace component, where the unit "ppm" is based on weight.
[0096] According to yet another embodiment, the glass does not contain oxides of alkali metals and / or boron, except for unavoidable traces. In particular, this means that according to a particularly preferred embodiment of the invention, the glass contains a maximum of 500 ppm of B2O3. The absence of glasses according to these embodiments from alkali metal oxides and / or B2O3 is advantageous, since said components reduce the temperature resistance of crystallizable or at least partially crystallized glasses. Furthermore, these components, for example certain alkali metals, can form low-expansion crystalline phases that are undesirable for the applications discussed here. Furthermore, the alkali metal content is disadvantageous, since it reduces the electrical resistance.
[0097] According to one embodiment, the glass comprises the oxide RO, and Σ(RO)≦55mol% where R is an element which in its oxide normally has the oxidation number II+, and in particular includes Ca, Mg, or Zn, and / or mixtures thereof. holds true.
[0098] In other words, RO contains alkaline earth metal oxides and ZnO. According to a preferred embodiment of the present disclosure, the glass does not contain alkaline earth metal oxides BaO and / or SrO, except for unavoidable trace amounts, in order to avoid undesirable contact reactions between the glass and chromium-containing joining materials, such as chromium-containing steels.
[0099] According to a further embodiment, the glass comprises: SiO2 30mol%~40mol%, Al2O3 3mol% to 12mol%, CaO 32mol%~46mol%, MgO 5mol% to 15mol%, ZnO 0mol% to 10mol%, and optionally, ZrO 20 mol % to 4 mol %, preferably up to 3 mol %, and / or TiO 20 mol % to 4 mol %, preferably up to 3 mol %, and / or MnO20mol%~5mol% Includes.
[0100] According to one embodiment, TiO2, ZrO2 and / or MnO2 may be optionally included in the glass. However, the content of these components in the glass is limited. In particular, in crystallizable glasses, TiO2 and ZrO2, which are known nucleating agents, are not required as nucleating agents. Moreover, their presence may be disturbing, since in the most unfavorable cases for the application, undesirable crystalline phases with low expansion may occur.
[0101] According to a further embodiment, the CaO content of the glass is at least 35 mol % and up to 46 mol %, preferably at least 35 mol % and less than 43.5 mol %, and / or the MgO content of the glass is 5 mol % and less than 13 mol %.
[0102] The CaO and / or MgO content of the glass, which is limited according to one embodiment, results in an even greater stability of the crystallizable glass against spontaneous crystallization. CaO and MgO are each components that are incorporated into the crystalline phases that are generated by heat treating the crystallizable glass. As explained above, it is particularly important for the application in question here that crystalline phases with a high thermal expansion coefficient are obtained. Therefore, preferably, the CaO and MgO content of the glass is further limited as explained above, so that the desired crystalline phases with a high thermal expansion coefficient are mainly obtained. This limitation serves in particular to prevent the formation of wollastonite, enstatite, diopside or mixed crystals of these crystalline phases, at least as far as possible, or even completely.
[0103] According to a further embodiment, the glass is present as a crystallizable glass and has a transformation temperature above 720°C.
[0104] The transformation temperature of a glass is an important characteristic parameter that reflects both the processing properties of this glass and its heat resistance. In particular, a high transformation temperature of a glass is also accompanied by a high dimensional stability of the glass.
[0105] Thus, preferably, according to one embodiment, the crystallizable glass has a particularly high dimensional stability, which is due to the high transformation or glass transition temperature T ≥ 720 ° C. g This is reflected in
[0106] According to a further embodiment, the crystallizable glass has a linear thermal expansion coefficient of 8×10 in the temperature range from 20° C. to 300° C. -6 / K, and preferably 9×10 -6 / K. In this way, it is advantageously possible, by means of a crystallizable glass, to better match the vitreous material to the linear thermal expansion coefficient of the materials to be joined, for example highly refractory materials such as Y-stabilized ZrO2 and / or alloys, preferably already before the end of the heat treatment for producing the gas-tight bond.
[0107] Transformation temperature T g is determined by the intersection of the tangents at the two branches of the expansion curve when measured at a heating rate of 5 K / min. This corresponds to measurements according to ISO 7884-8 or DIN 52324.
[0108] The softening temperature of glass, also abbreviated as "Ew", is the temperature range in which the viscosity of the glass is 10 7.6 dPa * Represents the temperature at the value of s.
[0109] In the context of the present disclosure, the coefficient of linear thermal expansion is referred to as the coefficient of linear thermal expansion. If the coefficient of linear thermal expansion of a crystallizable glass is described, this is the nominal average coefficient of linear thermal expansion according to ISO 7991, determined by static measurement (using a push rod dilatometer). The coefficient of linear thermal expansion of an at least partially crystallized glass is determined by dilatometry.
[0110] In the context of this disclosure, the linear thermal expansion coefficient is also referred to as α. For example, α(20-700) or α 20-700 represents the linear thermal expansion coefficient in the temperature range of 20°C to 700°C.
[0111] According to yet another embodiment of the present disclosure, the glass exists as an at least partially crystallized glass and has a crystallization temperature of 90° C. to 700° C. * 10 -6 / K, preferably 10×10 -6 / K, and particularly preferably the linear thermal expansion coefficient of the at least partially crystallized glass is 9. * 10 -6 / K above 9.5, preferably * 10 -6 / K or more.
[0112] According to embodiments of the present disclosure, the glass is not only formed such that a preferably gas-tight and / or electrically insulating bond can be made, but in particular according to embodiments, a preferably gas-tight and / or electrically insulating bond can also be made that continues to ensure sufficient electrical insulation even at high temperatures.
[0113] Such a combination, for example a metal-glass combination, is said to be fluid-tight if the combination is sealed, i.e. in this case sealed against the escape or passage of a fluid medium, and preferably substantially completely (hermetically) sealed. Here, the sealing can usually be determined by a leak test using a helium leak tester. At room temperature, the * 10 -8 mbar * A helium leak rate of less than 1 / s indicates that a substantially perfectly gas-tight seal has occurred. This measurement may preferably be carried out at an applied pressure of 1 bar.
[0114] According to these embodiments, the glass is present as a crystallizable glass, and the temperature of the crystallizable glass is 10 8 Ω * The specific electrical resistivity in cm is preferably measured according to DIN 52326 and is k The number is 100.
[0115] According to one embodiment, the crystallizable or at least partially crystallized glass comprises, in particular, SiO2, and CaO, and MgO, and Al2O3, and optionally ZnO.
[0116] In the SiO2-Al2O3-CaO-MgO system, crystalline phases with high thermal expansion coefficients can be realized. These include, for example, mixed crystals from the CaO-rich calcium-magnesium silicate family, such as akermanite and / or merwinite, which also form, for example, gehlenite and / or augite as mixed crystals with Al2O3. If the glass also contains ZnO, hardystonite can additionally be formed as a mixed crystal.
[0117] According to one embodiment, the glass is present as an at least partially crystallized glass, preferably comprising crystallites of CaO-rich calcium-magnesium silicates, in particular CaO-rich calcium-magnesium island silicates and / or sorosilicates. Here, island silicates are silicates in which the SiO 4 tetrahedra contained in the silicate are present individually, i.e. not bonded to each other. In sorosilicates, silicates are present in which two SiO 4 tetrahedra are bonded to each other via a common bridging oxygen, so that a SiO 2 O 7 aggregate exists as a silicate structural unit. Preferably, the at least partially crystallized glass may comprise marwinite Ca 3 Mg(SiO 4 ) 2 and / or mixed crystals with a marwinite structure as the island silicate. Furthermore, the at least partially crystallized glass may alternatively or additionally comprise a crystalline phase with a melilite structure, such as akermanite Ca 2 MgSiO 7 or gehlenite Ca 2 Al[AlSiO 7 ] or mixed crystals thereof, as sorosilicates. Additionally, the at least partially crystallized glass may also include a crystalline phase having an augite structure, according to one embodiment.
[0118] When mixed crystals are mentioned in the context of the present disclosure, these are crystals that do not correspond to a stoichiometric compound. For example, when "akermanite mixed crystals" are mentioned, these are understood to be crystals that do not have the stoichiometric composition Ca2MgSi2O7. For example, it is possible that the mixed crystal contains more Ca than the stoichiometric composition, or that instead of Ca, Zn is also incorporated. However, the mixed crystals crystallize in a crystal structure that corresponds approximately to that of akermanite, i.e., except for small deviations, for example with respect to the lattice parameters.
[0119] According to one embodiment, the glass is present as an at least partially crystallized glass, preferably comprising crystallites of CaO-rich calcium-magnesium silicates, in particular CaO-rich calcium-magnesium island silicates and / or sorosilicates, e.g. merwinite and / or mixed crystals with a merwinite structure, and alternatively or additionally crystalline phases with a melilite structure such as akermanite Ca2MgSiO7 and / or gehlenite Ca2Al[AlSiO7] and / or mixed crystals thereof, and / or crystalline phases with an augite structure.
[0120] The present disclosure also relates to a bonded bond comprising an at least partially crystallized glass, where the glass is an at least partially crystallized glass according to an embodiment of the present disclosure, or is made or producible from a crystallizable glass according to an embodiment of the present disclosure.
[0121] In the context of this disclosure, a joining partner is understood to be a material or part that is or is to be assembled or joined together with other materials or parts, preferably into a hermetically assembled part. If there are several joining partners to be joined, these may be of the same or different composition.
[0122] In the context of this disclosure, the conjugate is also referred to as a conjugate complex or conjugate.
[0123] The present disclosure also relates to articles of manufacture, in particular retaining and / or insulating elements and / or additional structures, comprising at least partially crystallized glass according to embodiments of the present disclosure.
[0124] Preferably, the product can be produced from a sintered body comprising a crystallizable glass according to an embodiment of the present disclosure. Preferably, the sintered body here comprises a crystallizable glass as a glass powder. Very particularly preferably, the glass powder comprises powder particles having a particle surface.
[0125] Further, the present disclosure relates to the use of the bonded combination according to the embodiments of the present disclosure. In particular, the combination may be used in conjunction with an exhaust gas sensor, such as in an exhaust gas system of an automobile, a pressure sensor, a particle sensor, such as a soot particle sensor, and / or a temperature sensor, and / or a NO x They can be used in sensors, such as oxygen sensors, and / or in feedthroughs for compressors and / or electric compressors, and / or as current feedthroughs in exhaust gas elements and / or fuel cells, and / or in feedthroughs for chemical reactors.
[0126] Working Example The crystallizable or at least partially crystallized glasses disclosed herein, as well as their uses, are explained in more detail below on the basis of examples.
[0127] The following table shows by way of example compositions of crystallizable or at least partially crystallized glasses. These compositions are in each case listed in mol %. The characteristic temperatures are those temperatures usually used to describe the melting behavior of ashes, such as the softening temperature (abbreviation: softening), the sintering temperature (abbreviation: sintering), the sphere temperature (abbreviation: sphere), the hemisphere temperature (abbreviation: hemisphere) and the flow temperature, which are determined using a hot spot microscope (abbreviation: HSM). These temperatures are determined in accordance with or on the basis of DIN 51730. The thermal expansion coefficient α is in each case 10 -6 It is shown in units of / K.
[0128] [Table 1-1]
[0129] [Table 1-2]
[0130] [Table 2-1]
[0131] [Table 2-2]
[0132] [Table 3-1]
[0133] [Table 3-2]
[0134] Table 2 below lists comparative examples of crystallizable or at least partially crystallized glasses.
[0135] [Table 4-1]
[0136] [Table 4-2]
[0137] In Comparative Examples 1, 5, and 6, the glass began to flow specifically at flow temperatures of 1128° C. (Comparative Example 1), 1166° C. (Comparative Example 5), and 1147° C. (Comparative Example 6).
[0138] In Comparative Examples 2, 3, and 4, glasses could no longer be obtained: rather, these compositions, after melting, crystallized in an uncontrolled manner on cooling.
[0139] The glasses according to the embodiments of the present disclosure are obtained in a vitreous state from a melting process. A fast cooling rate is not required during casting. In particular, a cooling rate of at least 30 cm 3This is all the more surprising since the specialist literature states that vitreous solidification is only possible on a small scale in the case of ribbons.
[0140] The crystallized or at least partially crystallized glass according to the present disclosure has a particularly advantageous dimensional stability. This is shown, for example, by the fact that the shape deviation between a sintered body comprising a crystallizable glass according to an embodiment of the present disclosure and a shaped body comprising an at least partially crystallized glass obtained by crystallizing the sintered body by temperature treatment is only very small, i.e., the length deviation is only in the single digit percent range, as shown, for example, in the measurement data in the table below. To determine these data, compacts were made with an average transverse dimension (here average diameter) of about 10-12 mm. After sintering, the sintered shaped body thus obtained was heated to 1200 ° C. in a muffle furnace with a heating rate of 4 K / min. The temperature of 1200 ° C. was kept constant for 10 minutes. Cooling was then performed. After cooling, the average transverse dimension (here average diameter) was determined again. The relative deviation of the average transverse dimension before and after the heat treatment at 1200 ° C. was then determined.
[0141] [Table 5]
[0142] Due to the described high dimensional stability of the shaped bodies, such as pressed bodies or sintered bodies, which initially contain a crystallizable glass and are then converted during temperature treatment into shaped bodies at least partially containing at least partially crystallized glass, it is now possible to carry out particularly advantageously, for example, a reliable extension of the creepage distance in feedthroughs. In particular, the shaped bodies do not round during temperature treatment. The very good resistance to urea and substances resulting therefrom, in particular in concentrations such as those used in certain AdBlue for SCR catalysts, allows the use of the bonded assemblies described herein in exhaust gas installations with exhaust gas cleaning systems for long-term operation. [Brief description of the drawings]
[0143] Hereinafter, the embodiments of the present disclosure will be further described with reference to the drawings. [Figure 1] FIG. 1b is a cross-sectional view of a first embodiment of a bonded assembly disclosed herein, the cross-section being taken along plane AA from FIG. 1a and passing approximately through the center of the bonded assembly. [Figure 1a] FIG. 2 is a plan view of the first embodiment illustrated in cross section in FIG. [Diagram 2] FIG. 1 is a cross-sectional view of a second embodiment of a bonded assembly disclosed herein, the cross-section being taken approximately through the center of the bonded assembly as illustrated in FIGS. 1 and 1a. [Figure 2a] FIG. 2 is a plan view of a creepage distance extension of the first disclosed embodiment, on which graphite pen or pencil marks are visible. [Figure 2b] FIG. 2 is a plan view of the creepage distance extension of the first disclosed embodiment, on which a graphite pen or pencil mark is visible after it has been at least partially removed with a cellulose cloth using a lateral wiping motion. [Figure 2c] FIG. 2 is a plan view of the creepage distance extension of the first disclosed embodiment, on which a graphite pen or pencil mark is visible after it has been at least partially removed with a cellulose cloth using a lateral wiping motion. [Diagram 3] FIG. 1 is a cross-sectional view of a third embodiment of a bonded assembly disclosed herein, the cross-section being taken approximately through the center of the bonded assembly as illustrated in FIGS. 1 and 1a. [Figure 4] FIG. 1 is a cross-sectional view of a fourth embodiment of a bonded assembly disclosed herein, the cross-section being taken approximately through the center of the bonded assembly as illustrated in FIGS. 1 and 1a. [Diagram 5] FIG. 13 is a cross-sectional view of a fifth embodiment of a bonded assembly disclosed herein, the cross-section being taken approximately through the center of the bonded assembly as illustrated in FIGS. 1 and 1a. [Figure 6] 13 is a cross-sectional view of a sixth embodiment of a bonded joint as disclosed herein, the cross-section being taken approximately through the center of the bonded joint. [Figure 7] 1 is a scanning micrograph of an at least partially crystallized glass according to an embodiment of the present disclosure. [Figure 8] 1 is a scanning micrograph of an at least partially crystallized glass according to an embodiment of the present disclosure. [Figure 9] 1 is a scanning micrograph of an at least partially crystallized glass according to an embodiment of the present disclosure. [Figure 10] 1 is a scanning micrograph of an at least partially crystallized glass according to an embodiment of the present disclosure. [Figure 11] 1 is a scanning micrograph of a conjugate according to one embodiment of the present disclosure.
[0144] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS In the following detailed description of the embodiments disclosed herein, the components are not drawn to scale for ease of understanding, and like reference symbols represent the same or functionally corresponding components in each embodiment.
[0145] FIG. 1 is a cross-sectional view of a first embodiment of a bonded joint 5 disclosed herein, the cross-section being taken along plane AA from FIG. 1 a through approximately the center of the bonded joint 5 and including centerline M.
[0146] The joint combination 5 includes an electrically insulating member 53 and at least two joint partners 51, 52. In the embodiment disclosed herein, the joint partner 51 is formed, without limiting generality, in a hollow cylindrical shape and includes a metal or ceramic material as described in more detail below. The joint partner 52 may likewise be made of a metal as described in more detail below and may be, for example, part of an electrical or electronic feedthrough and thus part of an electrical or electronic combination in its intended use.
[0147] At least one of the joining partners 51 , 52 is kept electrically insulated from at least the other of the joining partners 51 , 52 by an electrically insulating member 53 .
[0148] This member 53 may include or consist of a crystallizable or partially crystallized glass as disclosed herein.
[0149] The insulating member 53 has a portion 54 extending between and connected to the joining partners 51, 52, respectively, and preferably glass-fused thereto. Here, in the context of the present disclosure, "glass-fused" means that the crystallizable glasses or partially crystallized glasses disclosed herein form, during their heat treatment, an amorphous or vitreous layer on their surface that can, so to speak, melt-adhere to the material of the respective joining partner, and in this melt-adhere state, they are referred to as "glass-fused".
[0150] 1, the upper surface O of the insulating element is shown separated from the portion 54 by a dotted line L, which merely illustrates diagrammatically the profile of the upper surface O without the structures S and thus without the creepage extensions, as compared to a joint combination with the structures S and thus with the creepage extensions. Without the structures S, the upper surface would form a planar surface on which a meniscus may possibly be formed with respect to the respective joint partner.
[0151] However, in the embodiment disclosed herein, a protuberance formed by the structure S, in this case the portion 55, is disposed on this surface of the portion 54 of the electrically insulating member 53 that extends between the joining partners.
[0152] This portion 55 forming the structure S allows the distance on the surface of the insulating member 53 from the inner mating partner 52 to the outer mating partner 51 to be extended, and thus the presence of the structure S allows the creepage distance extension to be up to seven times longer or more.
[0153] Thereby, the low resistance deposits on each surface can contribute to a much lesser extent to the reduction of the electrical resistance between the joining partners 51 and 52 .
[0154] In the case of deposits forming droplets and / or surface films, it can be very advantageous if the structure S has an edge with a radius of curvature Rv of less than one tenth of a millimeter, preferably less than one twentieth of a millimeter and more than 10 μm, such that in most cases, even under the influence of gravity, the surface film or coating by the droplets will not extend over this edge with the radius of curvature Rv, so that a closed surface coating cannot occur.
[0155] Instead of the ridges shown in this embodiment, the structures S may also form recessed depressions in the insulating member 53. In any case, however, in particular the direct path from at least one joining partner to at least the other joining partner along the surface is extended compared to a surface that does not have this structure S. A direct path is here understood to be the shortest path from one joining partner to the other joining partner along a surface that does not have the structure S on the one hand and has the structure S according to the invention on the other hand.
[0156] Preferably, the structure S completely surrounds at least one of the joining partners, here the joining partner 52 as an annular structure, as can be seen in Fig. 1a by way of example. In the context of the present disclosure, the expression "completely surrounded" does not mean here that a complete three-dimensional surrounding is required, although this can basically be the case. In the context of the present disclosure, a complete surrounding is already achieved, in particular if a complete annular surrounding is achieved, such that this surrounding can already result in a complete seal.
[0157] The structure S may be formed integrally with and of the same material as a portion 54 of an insulating member 53 extending between and connected to the joining partners 51, 52, respectively, and preferably glass-fused thereto, respectively.
[0158] Preferably herein, the material of the insulating member 53 comprises an at least partially crystallized glass as described in further and greater detail elsewhere in the context of this disclosure.
[0159] In this case, the insulating parts 53 can be formed together with the structure S in a single heat treatment step and, in particular, their crystallinity can be adjusted.
[0160] Advantageously, the crystallizable glass disclosed herein allows the formation of a lattice of a glass during the heat treatment, in particular during glass fusing in the transition area between the surface of the joining partner and the surface of the at least partially crystallized glass, preferably of 1 cm 2 or less, arranged for a later long-term operational durability at this point. 3 An at least largely amorphous glass layer is formed which contains less than 10 pores per 100 μm and / or has a thickness of preferably 5 μm or less, particularly preferably 2 μm or less, very particularly preferably 1 μm or less, whereby a gas-tight bond is produced between the joining partners 51, 52 and the insulating element 53.
[0161] In a preferred embodiment, the structure comprises a crystallizable glass or at least partially crystallized glass, and at the surface of the structure, at least a mostly amorphous boundary layer, in particular, substantially free of open pores, in particular less than 10 pores / cm. 3 A glass layer is formed having a thickness of less than or equal to 5 μm, preferably less than or equal to 2 μm, very particularly preferably less than or equal to 1 μm.
[0162] Depending on the embodiment, in this at least largely amorphous boundary layer having a thickness of 5 μm or less, preferably 2 μm or less, very particularly preferably 1 μm or less, the proportion of the amorphous phase or the glassy phase, each measured in weight percent, is higher than the proportion of all the respective crystalline phases as a whole, also measured in weight percent.
[0163] However, it is entirely possible that at least a part of the glass matrix-forming oxides, for example La2O3, can be at least partially incorporated into the crystalline phase in the further course of ceramization, but there usually remains a small residual content of the glassy phase, which is formed in particular by the glass matrix-forming oxides and forms the amorphous boundary layer mentioned above.
[0164] To determine whether the embodiments disclosed herein are compatible, the inventors developed a test.
[0165] When a pen, for example a graphite pen of hardness HB, is used to press the pen perpendicularly to the surface of the structure S or surface O with a force of about 100 mN to draw, for example, a line St, as illustrated in Figures 2a to 2c, this line St is obtained as illustrated in Figure 2a.
[0166] Since the graphite of the graphite pen or pencil cannot be retained in the pores of an otherwise smooth surface, wiping parallel to the surface or surface O of the structure S, for example with a Zewa brand cellulose cloth, also with a contact pressure of about 100 mN, results in a very high removal rate for the components disclosed herein that include crystallizable or partially crystallized glass. Typically, the contrast between the line St and the surface or surface O of the structure S is now significantly reduced, for example to values below 50% or below 0.5 depending on the notation of contrast.
[0167] However, the graphite of the graphite pen or pencil can be retained in the pores of the ceramic surface, so that wiping parallel to the surface or surface O of the structure S, for example with a cellulose cloth under the brand name Zewa, also with a contact pressure of about 100 mN, results in only a small amount of removal, for example in the case of a component made of zirconium oxide. Here, the contrast between the line St and the surface or surface O of the structure S generally only decreases slightly, for example to values of more than 50% or, depending on the expression of the contrast, to values of more than 0.5.
[0168] In a further embodiment, as shown in Figures 3 and 4, merely by way of example, the structure is not of the same material as the portion 54 of the insulating member 53, which extends between and is respectively joined to and preferably glass-fused to the joining partners 51, 52. Here, this structure S may comprise or consist of a high-temperature stable ceramic material, such as forsterite, an aluminium oxide based ceramic or a zirconium oxide based ceramic, such as a ceramic containing Y-stabilised zirconium oxide. If the structure S is not made of a material according to the invention, the pencil test cannot be carried out positively either.
[0169] FIG. 2 shows a cross-sectional view of a second embodiment of the bonded assembly disclosed herein, the cross-section being taken through approximately the center of the bonded assembly as illustrated in FIGS. 1 and 1a.
[0170] In this embodiment, the structure S includes a reinforcement 56 that includes or consists of a metal foil, metal sheet, or a scrim, mesh, or knit that includes a metal, the metal preferably consisting of or including steel. This substantially annular reinforcement 56 is preferably held within further insulating members 57, 58, 59 that are formed as sintered bodies and can contain the reinforcement 56, and that can be glass fused thereto after heat treatment. Here, the material of the substantially annular members 57, 58, and 59 can consist of a crystallizable glass of the present disclosure.
[0171] FIG. 3 shows a cross-sectional view of a third embodiment of a bonded assembly disclosed herein, the cross-section being taken through approximately the center of the bonded assembly as illustrated in FIGS. 1 and 1a.
[0172] In this embodiment, the structure S is not of the same material as the portion 54 of the insulating member 53 which extends between and is bonded to, and preferably glass-fused to, the joining mates 51, 52, respectively. The structure S comprises or consists of a high temperature stable ceramic material, such as a ceramic including forsterite, an aluminum oxide based ceramic, or a zirconium oxide based ceramic, such as Y-stabilized zirconium oxide.
[0173] As can be seen best in Figure 3, the structure S is recessed into the insulating member 53 and is surrounded by the insulating member 53 such that glass fusing occurs during heat treatment, preferably in the recessed region of the structure S. Here, the structure S is approximately centrally disposed radially in, and preferably at least partially recessed within, a portion 54 of the insulating member 53. This radial direction is illustrated by the arrow R in Figure 3.
[0174] FIG. 4 shows a cross-sectional view of a fourth embodiment of a bonded assembly disclosed herein, the cross-section being taken through approximately the center of the bonded assembly as illustrated in FIGS. 1 and 1a.
[0175] This further schematic, not to scale, view of the joint combination 5 differs from the joint combination 5 shown in FIGS. 1 to 8 in that a structure S is configured forming the creepage extension 55. This includes not only the material of the portion 54 but also a second material. This second material is likewise an insulating material, but different from the material of the portion 54. In this embodiment, the material of the portion 54 is formed as a crystallizable or at least partially crystallized glass, as will be described in further detail later, and the second material has a different chemical and / or crystallographic composition. That is to say, the second material differs from the material of the portion 54 in that it has a different chemical composition and / or in that it has a different crystalline content. In particular, the second material may be formed from or may include ZrO2. It has been shown that a particularly dimensionally and temperature-stable structure S is possible as a creepage extension when 5% by weight to 25% by weight of the second material, preferably ZrO2, is added as the second material. A content of 10 to 15% by weight is particularly preferred.
[0176] Fig. 5 shows very diagrammatically the configuration of a joint assembly 5 according to a fifth embodiment. Here, the outer side wall 552 of the part 55 has a slightly curved or bent shape and is therefore not formed perfectly planar. In contrast thereto, the inner side wall 553 of the part 55 is here formed planar. As can be seen from Fig. 5, the flatness of the side wall 552 differs from the flatness of the side wall 553. Here, the side wall 552 is shown somewhat distorted, since in reality it does not deviate so greatly from a planarly formed side wall.
[0177] Figure 6 shows the case of a joint assembly 5 according to a sixth further embodiment, where both the inner sidewall 552 and the outer sidewall 553 are not perfectly flat or planar, respectively. However, here the flatness is made approximately the same for both sidewalls 552 and 553. Again, strong distortions have been introduced so that the effect of the sidewalls not being perfectly flat can be shown. Essentially the deviation from flat sidewalls becomes much smaller.
[0178] 7 shows a first scanning micrograph of an at least partially crystallized glass according to one embodiment of the present disclosure. The at least partially crystallized glass comprises a crystal aggregate 1 formed from a number of crystallites, which are preferably formed in a needle shape. Here, in FIG. 1, the crystal aggregate 1 is shown as such for illustrative purposes. Furthermore, crystallites 21 are visible at the grain boundaries, which are shown for illustrative purposes, as are crystallites 22, which are formed in a needle shape.
[0179] 8 shows a second scanning micrograph of an at least partially crystallized glass according to a further embodiment of the present disclosure. Here again, the at least partially crystallized glass comprises a crystalline aggregate formed from a number of crystallites, which are preferably formed in a needle shape. In addition, pores are partially arranged between the individual crystallites, and the at least partially crystallized glass further still comprises a residual glass phase arranged between the crystallites. Here, exemplarily, crystallites 2 are shown forming a crystalline aggregate formed in a star shape. The residual glass phase 3, which is gray in the scanning microscopic view, and exemplarily shown pores 4 (black) can also be recognized.
[0180] 9 is a third scanning micrograph of an at least partially crystallized glass according to yet another embodiment of the present disclosure. Here again, crystalline aggregates can be recognized. Here, the crystallites are so finely formed that they are hardly perceptible as such at the selected resolution. In this way, a very dense and fine structure is obtained. Here, by way of example, one can refer to the very fine crystals 22 shown.
[0181] Figure 10 is a scanning micrograph of yet another at least partially crystallized glass according to an embodiment of the present disclosure. In contrast to the crystallites of the at least partially crystallized glass shown in Figure 9, the crystallites 23 contained in the crystalline aggregate of the at least partially crystallized glass are not as finely formed, but rather, their rod-like or perhaps platelet-like morphology is discernible. Here, the crystallites 23 are arranged interlocking with one another, similar to a "house of cards" structure.
[0182] 11 shows a scanning micrograph of a bonded assembly according to one embodiment of the present disclosure, with 10 pores / cm at the interface between the bond partner and the at least partially crystallized glass, located on the left side of the picture. 3 A very thin boundary layer, including less than 5 μm, is formed, which is an at least largely amorphous glass layer having a thickness of less than 5 μm, preferably less than 2 μm, very particularly preferably less than 1 μm.
[0183] The following statements apply to all embodiments disclosed above.
[0184] The above embodiments have been described with respect to only two mating partners, however, it is within the scope of the present disclosure that three or more mating partners can be held together in a mating combination by insulating members in the same manner as disclosed herein.
[0185] The bonded combinations of the present disclosure allow for many-fold extensions in creepage distance, with over 7-fold extensions being achieved here.
[0186] The combination of water resistance in environments susceptible to galvanic corrosion and high dimensional stability of the bonded joints disclosed herein is also advantageous.
[0187] A sufficiently high electrical resistance allows the use of the crystallizable glass as a creepage extension (e.g. as a feedthrough in an electric compressor) even under (typically) water condensation or even under coolant condensation.
[0188] The advantage compared to ceramics is that the pores of the structure S, i.e. the protruding material, are closed.
[0189] Here, long-term operational durability applications include electrical or power supply feedthroughs for heating elements (mainly for use in heatable catalytic elements, for example), for sensors in exhaust gas systems, and also generally feedthroughs for electric compressors, mainly for automotive applications.
[0190] In the embodiments disclosed above, the crystallites may contain crystallization nuclei at least partially at their grain boundaries and / or the deposits comprising lanthanum, and in particular comprising lanthanum compounds, are at least partially located at the grain boundaries of the crystallites.
[0191] Under operating conditions, the crystalline aggregates of the crystallizable or partially crystallized glasses disclosed herein inhibit volume elements of the at least partially crystallized glasses from displacing one another.
[0192] In the bonded joints of the present disclosure, the surface of the at least partially crystallized glass is free of a meniscus.
[0193] In the case of the joint assembly of the present disclosure, the joint partners are metals, in particular steels, such as plain steels, stainless steels, stainless steels, and high temperature stable ferritic steels also known as Thermax, for example under the trade names Thermax 4016, Thermax 4742 or Thermax 4762, or under the trade names Crofer22 APU or Crofer22 H, or NiFe based materials, for example NiFe45, NiFe47 or nickel plated pins, or Inconel, for example under the trade names Inconel 718 or X-750, or NiFe based materials, for example CF25, Alloy 600, Alloy 601, Alloy 625, Alloy 630, Alloy 640, Alloy 650, Alloy 660, Alloy 670, Alloy 680, Alloy 690, Alloy 700, Alloy 710, Alloy 720, Alloy 730, Alloy 740, Alloy 750, Alloy 760, Alloy 770, Alloy 780, Alloy 790, Alloy 800, Alloy 810, Alloy 820, Alloy 830, Alloy 840, Alloy 850, Alloy 860, Alloy 870, Alloy 880, Alloy 890, Alloy 900, Alloy 910, Alloy 920, Alloy 930, Alloy 940, Alloy 950, Alloy 960, Alloy 970, Alloy 980, Alloy 990, Alloy 1000, Alloy 1010, Alloy 1 The steels may include those known under the designations 690, SUS310S, SUS430, SUH446 or SUS316, or austenitic steels such as 1.4762, 1.4828 or 1.4841, metals from the Kanthal heating wire group, or high temperature stable ceramic compounds such as forsterite, aluminium oxide based ceramics or zirconium oxide based ceramics, for example Y-stabilised zirconium oxide based ceramics.
[0194] The conjugates of the present disclosure are -8 mbar * It comprises an at least partially crystallized glass having a helium leak rate of less than 1 / s and / or having an elastic modulus of 80 GPa to 200 GPa, preferably 100 GPa to 125 GPa.
[0195] For the crystallizable or at least partially crystallized glasses of the present disclosure, the CaO content of the crystallizable or at least partially crystallized glass may be at least 35 mol% and up to 46 mol%, preferably at least 35 mol% and less than 43.5 mol%, and / or the MgO content of the crystallizable or at least partially crystallized glass may be 5 mol% and less than 13 mol%.
[0196] In the case of the crystallizable or at least partially crystallized glasses of the present disclosure, the glasses can exist as at least partially crystallized glasses and can be used at temperatures ranging from 20° C. to 700° C. for up to 90 minutes. * 10 -6 / K, preferably 10 * 10 -6 / K, and particularly preferably, the linear thermal expansion coefficient of the at least partially crystallized glass is greater than 9 / K in the temperature range of 20 ° C. to 1000 ° C. * 10 -6 / K above 9.5, preferably * 10 -6 / Super.
[0197] In the case of the crystallizable or at least partially crystallized glasses of the present disclosure, the glass exists as a crystallizable glass and has a transformation temperature T above 720° C. g may have:
[0198] For the crystallizable or at least partially crystallized glasses of the present disclosure, the temperature of the crystallizable glass is 10 8 Ω * The specific electrical resistivity in cm is preferably measured according to DIN 52326 and is k The number is 100.
[0199] In the case of the crystallizable or at least partially crystallized glasses of the present disclosure, the at least partially crystallized glass comprises crystallites of calcium-magnesium silicate, preferably a CaO-rich calcium-magnesium silicate, in particular a CaO-rich calcium-magnesium island silicate and / or sorosilicate, e.g. merwinite and / or mixed crystals having a merwinite structure, and alternatively or additionally, crystalline phases having a melilite structure such as akermanite CaMgSiO and / or gehlenite CaAl[AlSiO] and / or mixed crystals thereof, and / or crystalline phases having an augite structure. [Explanation of symbols]
[0200] 1. Crystalline aggregates 2. Crystallites 21 Crystallites at grain boundaries 22 Needle-shaped crystallites 23 Crystallites formed into rods or platelets 3. Residual glass 4. Pore 5 conjugate 51 First joint partner 511 Upper end of first joining partner 52 Second Joint Partner 521 Upper end of second joint partner 53 Insulating materials 54 A part of an insulating part placed between mating parts 55 A part of the insulating member protruding from the joining partner 51, i.e., a creepage distance extension part 56 Reinforcement 57 Substantially annular members 58 Substantially annular members 59 Substantially annular members M center line S Structure forming creepage distance extension O. Upper surface of insulating member 53 Rv Radius of curvature at the end St: A line drawn with a pen on the surface of structure S or on surface O R Radial direction
Claims
1. A joint assembly (5) comprising an electrically insulating member (53) and at least two joint partners (51, 52), At least one of the joining partners (51, 52) is kept electrically insulated from at least the other of the joining partners (51, 52) by the electrical insulating member (53), the surface of the electrically insulating member (53) extending between the joining partners forms structures (S), in particular bumps or depressions, said structures (S) in particular extend the direct path along the surface from at least one joining partner to at least the other joining partner compared to a surface not having said structures (S); The structure (S) preferably completely surrounds at least one joining partner, The insulating member (53) or the structure (S) comprises or consists of a crystallizable glass or an at least partially crystallized glass; Conjugate (5).
2. 2. The bonded assembly according to claim 1, wherein the structure (S) is integral with and of the same material as a portion (54) of the insulating member (53) extending between and connected to the bond partners (51, 52), preferably glass-fused thereto, and preferably the material of the insulating member (53) comprises at least partially crystallized glass.
3. In the transition area between the surface of the joining partner and the surface of the at least partially crystallized glass, preferably 3 3. The bonded assembly according to claim 1 or 2, wherein an at least largely amorphous glass layer is arranged, which contains less than 10 pores per 100 μm and / or has a thickness of preferably 5 μm or less, particularly preferably 2 μm or less, very particularly preferably 1 μm or less.
4. The structure (S) comprises a crystallizable glass or at least partially crystallized glass, and at the surface of the structure (S) there is at least a mostly amorphous boundary layer, in particular substantially free of open pores, in particular less than 10 pores / cm 3 4. The joint assembly according to claim 1 , which is in the form of a glass layer having a thickness of 5 μm or less, preferably 2 μm or less, very particularly preferably 1 μm or less.
5. 2. The joint assembly according to claim 1, wherein the structure (S) is not made of the same material as a portion (54) of the insulating member (53) extending between and connected to the joint partners (51, 52), preferably glass-fused thereto.
6. 6. The joint assembly of claim 5, wherein the structure (S) is not made of the same material as the portion (54) of the insulating member (53) extending between and bonded to the joint partners (51, 52), preferably glass-fused thereto, but is made of a high-temperature stable ceramic material, such as forsterite, an aluminum oxide-based ceramic, or a zirconium oxide-based ceramic, such as a ceramic containing Y-stabilized zirconium oxide.
7. the structure (S) is not made of the same material as the portion (54) of the insulating member (53) extending between and connected to the joining partners (51, 52), preferably glass-fused thereto, the structure (S) is disposed approximately centrally in the radial direction in the portion (54) of the insulating member (53), and preferably at least partially recessed therein; The conjugate of claim 5 or 6.
8. 8. The bonded assembly of claim 1, wherein the structure (S) comprises a reinforcement (56), the reinforcement (56) comprising a metal foil, a metal sheet, or a scrim, mesh or braid comprising a metal, the metal preferably consisting of a ferritic steel or comprising steel.
9. 9. A joint assembly according to any one of the preceding claims, wherein the structure (S) has an end with a radius of curvature Rv of less than one tenth of a millimeter, preferably less than one twentieth of a millimeter, and more than 10 μm.
10. A joint assembly, in particular according to any one of claims 1 to 9, comprising an at least partially crystallized glass and a joint partner, in particular a high-temperature stable and / or mechanically strong joint assembly. the at least partially crystallized glass comprises, by volume, a fraction of residual glass of less than 10%, preferably less than 5%, the at least partially crystallized glass comprises crystalline aggregates; The crystal aggregate is formed from a large number of crystallites, The crystallites are preferably formed in the form of needles and / or platelets, The crystallites are particularly preferably distributed throughout the at least partially crystallized glass and arranged radially, for example in the form of spherulites and / or fans and / or rods and / or platelets, in particular comprising one or the insulating element (53); conjugate.
11. A joint assembly, in particular according to any one of claims 1 to 10, comprising an at least partially crystallized glass and a joint partner, in particular a joint assembly which is stable at high temperatures and / or can withstand high mechanical loads. In particular, a joint combination according to any one of claims 1 to 10, The glass, La 2 O 3 More than 0.3 mol% to less than 5 mol%, preferably 4.5 mol% or less, particularly preferably 4 mol% or less; Nb 2 O 5 0 mol% to 9 mol%, T 2 O 5 0 mol% to 7 mol%, where Σ(A 2 O 5 ) more than 0.2 mol% to 9 mol%, where A is an element that in its oxide normally has the oxidation number V+, and may include Nb, and / or Ta, or P, and / or mixtures thereof. A conjugate comprising:
12. the crystallites contain crystallization nuclei at least partially at grain boundaries, and / or At least partially located at the grain boundaries of the crystallites are deposits containing lanthanum, in particular containing lanthanum compounds; The conjugate of claim 10 or 11.
13. The difference in the thermal expansion coefficients of the joining partners and the at least partially crystallized glass is 5 * 10 -6 / K or less, preferably 3 * 10 -6 / K or less, particularly preferably 1×10 -6 13. The conjugate according to claim 1, in particular according to claim 10, wherein the molecular weight of the conjugate is less than or equal to 1. / K.
14. A joint assembly according to any one of claims 1 to 13, in particular according to any one of claims 10 to 13, which withstands an operating temperature of at least 1000° C. and is in particular vibration- and vibration-resistant, measured in accordance with ISO 16750-3.
15. A bonded assembly according to any one of claims 1 to 14, in particular according to any one of claims 10 to 14, in which in the operating state, the crystalline aggregates prevent the volume elements of the at least partially crystallized glass from being displaced relative to one another.
16. 16. A bonded assembly according to claim 1, in particular according to claim 10, in which the surface of the at least partially crystallized glass is free of a meniscus.
17. In the transition area between the surface of the joining partner and the surface of the at least partially crystallized glass, preferably 3 17. The bonded assembly according to claim 1 , in particular according to claim 10 , in which an at least largely amorphous glass layer is arranged, which comprises less than 10 pores per 100 μm and / or has a thickness of preferably 5 μm or less, particularly preferably 2 μm or less, very particularly preferably 1 μm or less.
18. The joining partners are preferably metals, in particular steels, such as plain steels, stainless steels, stainless steels and high temperature stable ferritic steels, also known as Thermax, for example under the trade names Thermax 4016, Thermax 4742 or Thermax 4762, or under the trade names Crofer 22 APU or Crofer 22 H, or NiFe based materials, for example NiFe 45, NiFe 47 or nickel plated pins, or Inconel, for example under the trade names Inconel 718 or X-750, or for example CF25, Alloy 600, Alloy 625, Alloy 630, Alloy 640, Alloy 650, Alloy 660, Alloy 670, Alloy 680, Alloy 690, Alloy 700, Alloy 710, Alloy 720, Alloy 730, Alloy 740, Alloy 750, Alloy 760, Alloy 770, Alloy 780, Alloy 790, Alloy 800, Alloy 810, Alloy 820, Alloy 830, Alloy 840, Alloy 850, Alloy 860, Alloy 870, Alloy 880, Alloy 890, Alloy 900, Alloy 910, Alloy 920, Alloy 930, Alloy 940, Alloy 950, Alloy 960, Alloy 970, Alloy 980, Alloy 990, Alloy 1000, Alloy 1010, Alloy 1020, Alloy 1030, Alloy 104 18. A joint assembly according to any one of claims 1 to 17, in particular according to any one of claims 10 to 17, comprising a metal from the group of austenitic steels such as 1.4828 or 1.4841, such as steels known under the names SUS 690, SUS 310S, SUS 430, SUH 446 or SUS 316, or a high-temperature stable ceramic compound, such as an aluminium oxide based ceramic or a zirconium oxide based ceramic, such as a ceramic containing Y-stabilised zirconium oxide.
19. 10 -8 mbar * and / or has a helium leak rate of less than 1 / s; at least partially crystallized glass having an elastic modulus of 80 GPa to 200 GPa, preferably 100 GPa to 125 GPa; A joint combination according to any one of claims 1 to 18, in particular according to any one of claims 10 to 18.
20. La 2 O 3 More than 0.3 mol% to less than 5 mol%, preferably 4.5 mol% or less, particularly preferably 4 mol% or less; Nb 2 O 5 0 mol% to 9 mol%, T 2 O 5 0 mol% to 7 mol%, where Σ(A 2 O 5 ) more than 0.2 mol% to 9 mol%, where A is an element which in its oxide normally has the oxidation number V+, and includes in particular Nb, Ta, or P, and / or mixtures thereof. A crystallizable or at least partially crystallized glass comprising:
21. Contains an oxide RO, and Σ(RO) ≦55mol% where R is an element which in its oxide normally has the oxidation number II+, and in particular includes Ca, Mg, or Zn, and / or mixtures thereof.
21. The crystallizable or at least partially crystallized glass of claim 20, wherein:
22. SiO 2 30 mol% to 40 mol%, A 2 O 3 3 mol% to 12 mol%, CaO 32 mol% to 46 mol%, MgO 5 mol% to 15 mol%, ZnO 0 mol% to 10 mol%, and optionally, ZrO 2 0 mol % to 4 mol %, preferably up to 3 mol %, and / or TiO 20 mol % to 4 mol %, preferably up to 3 mol %, and / or MnO 2 0mol%~5mol% 22. The crystallizable or at least partially crystallized glass of claim 20 or 21, comprising:
23. the CaO content of said crystallizable or at least partially crystallized glass is at least 35 mol % and up to 46 mol %, preferably at least 35 mol % and up to less than 43.5 mol %, and / or the MgO content of said crystallizable or at least partially crystallized glass is between 5 mol% and less than 13 mol%, 23. The crystallizable or at least partially crystallized glass according to any one of claims 20 to 22.
24. The glass is present as a crystallizable glass and has a transformation temperature T g 24. The crystallizable or at least partially crystallized glass according to claim 20, having
25. The crystallizable glass has a linear thermal expansion coefficient of 8 or less in the temperature range of 20° C. to 300° C. * 10 -6 / K, and preferably in the temperature range of 20°C to 700°C. * 10 -6 25. The crystallizable or at least partially crystallized glass according to claim 20, wherein the crystallization temperature is greater than 100° C. / K.
26. the glass is present as an at least partially crystallized glass, In the temperature range of 20°C to 700°C, 9 * 10 -6 / K, preferably 10 * 10 -6 / K, Particularly preferably, the at least partially crystallized glass has a linear thermal expansion coefficient of 9 or less in the temperature range of 20° C. to 1000° C. * 10 -6 / K, preferably 9.5 * 10 -6 / K is more than 26. The crystallizable or at least partially crystallized glass according to any one of claims 20 to 25.
27. The temperature of the crystallizable glass is 10 8 Ω * The specific electrical resistivity in cm is preferably measured according to DIN 52326 and is k 27. The crystallizable or at least partially crystallized glass according to any one of claims 20 to 26, wherein the crystallizable glass has a refractive index of 100.
28. The at least partially crystallized glass is preferably composed of crystallites of calcium-magnesium silicates, preferably CaO-rich calcium-magnesium silicates, in particular CaO-rich calcium-magnesium island silicates and / or sorosilicates, e.g. merwinite and / or mixed crystals having a merwinite structure, and alternatively or additionally akermanite Ca 2 MgSi 2 O 7 and / or Ca Gehlenite 2 Al[AlSiO 7 28. The crystallizable or at least partially crystallized glass according to claim 20, comprising a crystalline phase having a melilite structure such as, for example, ] and / or mixed crystals thereof, and / or a crystalline phase having an augite structure.
29. comprising an at least partially crystallized glass and a joining partner; The glass is an at least partially crystallized glass according to any one of claims 20 to 28 or is made or can be made from an at least partially crystallizable glass according to any one of claims 20 to 28. conjugate.
30. 29. An article of manufacture, in particular a holding element and / or an insulating element and / or an additional structure, comprising an at least partially crystallized glass according to any one of claims 20 to 28.
31. 31. The product according to claim 30, which can be produced from a sintered body comprising at least partially a crystallizable glass according to any one of claims 20 to 28, wherein the sintered body comprises a crystallizable glass, preferably as a glass powder, particularly preferably the glass powder comprises powder particles having a particle surface.
32. Exhaust gas sensors, pressure sensors, particle sensors, such as soot particle sensors, and / or temperature sensors, and / or NO x Use of a joint combination according to any one of claims 1 to 19 or a product according to claim 30 or 31 in sensors, such as oxygen sensors, and / or in feedthroughs for compressors and / or electric compressors, and / or as a current feedthrough in exhaust gas components and / or fuel cells, and / or in feedthroughs for chemical reactors.
Citation Information
Patent Citations
Crystallized calcium phosphate glass having high strength
JP1985096544A
High-strength crystallized glass containing apatite crystal and anorthite crystal and its manufacture
JP1986136939A
Glalss ceramic containg zirconium oxide
JP1996040744A
Glass ceramic substrate for information recording medium
JP2001184624A
Glass-ceramic seals for use in solid oxide fuel cells
JP2009533310A