Film structure, piezoelectric film, and super conducting film

The film structure with a tetragonal zirconia buffer layer and platinum group element facilitates the growth of single-crystal piezoelectric and superconducting films, addressing uniform polarization and lattice constant issues, thereby improving film performance.

JP2024138514AActive Publication Date: 2024-10-08I PEX PIEZO SOLUTIONS INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024113785
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-07-31
Filing Date
2024-07-17
Publication Date
2024-10-08
Estimated Expiration
2039-12-27

AI Technical Summary

Technical Problem

Existing piezoelectric materials face challenges in achieving uniform polarization and single-crystallinity due to differences in crystal systems and lattice constants, making it difficult to form thin films with sufficient piezoelectricity, especially when using single-crystal Si substrates.

Method used

A film structure is developed comprising a substrate with a tetragonal zirconia buffer film, an epitaxially grown metal film containing a platinum group element, and a Sr(Ti) film, which facilitates the formation of single-crystal piezoelectric and superconducting films.

Benefits of technology

The proposed film structure enables the growth of single-crystal piezoelectric and superconducting films with improved performance by aligning the crystal structure with the substrate orientation, enhancing uniform polarization and piezoelectric properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138514000001_ABST
    Figure 2024138514000001_ABST
Patent Text Reader

Abstract

To form a film having a single crystal structure on a film structure for various piezoelectric and superconducting materials.SOLUTION: For various piezoelectric materials, a piezoelectric film having a single crystal structure can be formed on a film structure. The film structure 101 includes a substrate 11, a buffer film 12 having a tetragonal crystal structure containing zirconia, formed on the substrate, a conductive film 13 containing an epitaxially grown platinum group element, formed on the buffer film, and a film 16 containing epitaxially grown Sr(Ti1-x,Rux)O3 (0≤x≤1) formed on the conductive film.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a film structure provided with a buffer film that enables a single crystal piezoelectric film or superconductor film to be formed on a substrate by epitaxial growth, and to the piezoelectric film and the superconductor film. [Background technology]

[0002] In the IoT era, where everything is connected to the Internet, sensors play an important role, with the market size reaching $20 billion worldwide and growing at a rate of 7-8%, with 90 billion sensors being produced annually worldwide. Among these, MEMS sensor technology using piezoelectric materials such as PZT is particularly active, and is being widely used in a wide range of applications, including gyro sensors for autonomous driving, piezoelectric microphones, high-frequency filters for 5G communications, and vibration power generation elements.

[0003] With the development of IoT technology, MEMS sensor technology using such piezoelectric materials is required to be smaller, thinner, and more sensitive every year. On the other hand, to achieve high sensitivity, uniform polarization is required to ensure sufficient piezoelectricity, but the polarization is not uniform in piezoelectric materials, which are generally polycrystalline ceramic sintered bodies. In addition, there is a limit to how thin a ceramic sintered body can be made. Therefore, in recent years, attempts have been made to obtain piezoelectric materials as thin single crystals by epitaxial growth (for example, see Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 5-072428 Summary of the Invention [Problem to be solved by the invention]

[0005] In the effort to produce single crystals of such thin films, since most piezoelectric materials are oxides, it is difficult to produce single crystals of piezoelectric materials by epitaxial growth, for example, when using a single crystal Si substrate. Therefore, oxide crystals such as YSZ (Yttria-stabilized zirconia) are sometimes used as buffer layers, but since such oxide crystals have a different crystal system from that of the piezoelectric material, they are dragged by the crystal system of the buffer layer during crystal formation of the piezoelectric material, making it difficult to obtain in-plane single crystallinity as a thin film. In addition, since the lattice constant differs for each piezoelectric material, the configuration of the buffer layer must be considered for each piezoelectric material, and the selection of the buffer layer is also difficult. [Means for solving the problem]

[0006] In order to solve the above problems, the film structure according to the present invention includes a substrate, a buffer film having a tetragonal crystal structure containing zirconia formed on the substrate, an epitaxially grown metal film containing a platinum group element formed on the buffer film, and an epitaxially grown Sr(Ti 1-x ,Ru x )O3 and (0≦x≦1). Effect of the Invention

[0007] According to the present invention, for various piezoelectric materials and superconducting materials, films having a single crystal structure can be formed on the film structure according to the present invention. [Brief description of the drawings]

[0008] [Figure 1] 1 is a cross-sectional view of a substrate on which a buffer film according to the present invention is formed. [Diagram 2] 1 is a cross-sectional view of a substrate having a lower electrode formed on a buffer film according to the present invention. [Diagram 3] 1 is a cross-sectional view of a film structure including a buffer film according to the present invention. [Figure 4]1(a) is a STEM image of a cross section of a substrate 11 after a ZrO2 film was formed on the substrate 11 as a buffer film 12, and the lower image in (b) is an electron diffraction image of the substrate 11, and the upper image is an electron diffraction image of the buffer film 12. [Diagram 5] Regarding the buffer film 12, (a) is a STEM image of a cross section observed when it was formed to a thickness of 1 nm, (b) is a 12 nm, (c) is a 15 nm, and (d) is a 25 nm. [Figure 6] The results of measuring the θ-2θ spectrum of the film structure 101 by XRD are shown. [Figure 7] Regarding the conductive film 13, (a) is a STEM image of a cross section observed when the film was formed to a thickness of 10 nm, (b) is a 20 nm, and (c) is a 150 nm. [Figure 8] 1 shows the results of measuring the θ-2θ spectrum by the XRD method for the film structure 101 according to Example 1. [Figure 9] 1 shows a lattice image by STEM obtained by observing a cross section of PZT (30 / 70) as the piezoelectric film 14 according to Example 1. [Figure 10] Regarding the film structure 101 of Example 1, (a) is a pole figure of the Si(220) surface, (b) is a pole figure of the ZrO2(220) surface, (c) is a pole figure of the Pt(220), and (d) is a pole figure of the PZT(202). [Figure 11] 4 is a diagram showing the voltage dependence of polarization of the piezoelectric film 14 according to Example 1. FIG. [Figure 12] The results of measuring the θ-2θ spectrum by the XRD method for the film structure 101 according to Example 2 are shown. [Figure 13] 1A is a diagram showing an X-ray diffraction pattern by φ scanning of the substrate 11 and FIG. 1B is a diagram showing an X-ray diffraction pattern by φ scanning of the piezoelectric film 14 in the film structure 101 according to Example 2. [Figure 14] 13 shows a lattice image by STEM observing a cross section of BTO as the piezoelectric film 14 according to Example 2. [Figure 15] FIG. 11 is a diagram showing the voltage dependence of polarization of the piezoelectric film 14 according to Example 2. [Figure 16]11 is a diagram showing the piezoelectricity of BTO as the piezoelectric film 14 according to Example 2. FIG. [Figure 17] The results of measuring the θ-2θ spectrum by the XRD method for the film structure 101 according to Example 3 are shown. [Figure 18] 1A is a diagram showing an X-ray diffraction pattern by φ scanning of the substrate 11 and FIG. 1B is a diagram showing an X-ray diffraction pattern by φ scanning of the piezoelectric film 14 in the film structure 101 according to Example 3. FIG. [Figure 19] 13 shows a lattice image by STEM obtained by observing a cross section of BFO as the piezoelectric film 14 according to Example 3. [Figure 20] FIG. 11 is a diagram showing the voltage dependence of polarization of the piezoelectric film 14 according to Example 3. [Figure 21] FIG. 11 is a diagram showing the piezoelectricity of BFO as the piezoelectric film 14 in accordance with Example 3. [Figure 22] 1 shows the results of measuring the out-of-plane θ-2θ spectrum by the XRD method for the film structure 101 according to Example 4. [Diagram 23] 1A is a diagram showing an X-ray diffraction pattern by φ scanning of the substrate 11 and FIG. 1B is a diagram showing an X-ray diffraction pattern by φ scanning of the piezoelectric film 14 in the film structure 101 according to Example 4. FIG. [Figure 24] 13 shows a lattice image by STEM observing a cross section of BLT as the piezoelectric film 14 according to Example 4. [Diagram 25] FIG. 11 is a diagram showing the voltage dependence of polarization of the piezoelectric film 14 according to Example 4. [Figure 26] FIG. 11 is a diagram showing the piezoelectricity of BLT as the piezoelectric film 14 according to Example 4. [Figure 27] The results of measuring the θ-2θ spectrum by the XRD method for the film structure 101 according to Example 5 are shown. [Figure 28] FIG. 13 is a diagram showing an X-ray diffraction pattern by φ scanning for the film structure 101 according to Example 5. [Figure 29] The results of measuring the θ-2θ spectrum by the XRD method for the film structure 101 according to Example 6 are shown. [Diagram 30]FIG. 13 is a diagram showing an X-ray diffraction pattern by φ scanning for the film structure 101 according to Example 6. [Diagram 31] 1 shows the results of STEM observation of cross sections of the buffer film 12 and conductive film 13 for a sample formed with PZT (30 / 70) according to Example 1. [Diagram 32] 1 shows the results of STEM observation of cross sections of the buffer film 12 and the conductive film 13 of a sample formed with BFO according to Example 3. [Diagram 33] 1 shows the results of STEM observation of the cross section of the buffer film 12 and the conductive film 13 for a sample formed with the BLT according to Example 4. [Diagram 34] 1A is a lattice image showing a cross section of the interface between the conductive film 13 and the film 16 when the BFO film of Example 3 is formed, and FIG. 1B is a lattice image showing a cross section of the interface between the conductive film 13 and the film 16 when the BLT film of Example 4 is formed. [Diagram 35] The film structure 101 according to Example 7 was subjected to φ scanning of AlN by the XRD method to measure an X-ray diffraction pattern, and the results are shown. [Diagram 36] 13 shows the results of measuring the X-ray diffraction pattern of the film structure 101 according to Example 8 by φ scanning LiNbO3 by the XRD method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, an embodiment of the present invention will be described with reference to the drawings.

[0010] The disclosure is merely an example, and those who are skilled in the art can easily come up with appropriate modifications that maintain the gist of the invention, and naturally, these modifications are included in the scope of the present invention. In addition, in order to make the explanation clearer, the drawings may show the width, thickness, shape, etc. of each part in a schematic manner compared to the embodiment, but these are merely examples and do not limit the interpretation of the present invention.

[0011] In addition, in this specification and each figure, elements similar to those described above with respect to the previous figures are given the same reference numerals, and detailed descriptions may be omitted as appropriate.

[0012] Furthermore, in the drawings used in the embodiments, hatching (shading) used to distinguish structures may be omitted depending on the drawing.

[0013] (Embodiment) 1 is a cross-sectional view of a substrate on which a buffer film according to the present invention is formed. As shown in FIG 1, a buffer film 12 is formed on a substrate 11.

[0014] The substrate 11 is, for example, a silicon (Si) substrate. In addition to Si, for example, SOI (Silicon on Insulator) substrates, substrates made of various semiconductor crystals other than Si, substrates made of various oxide single crystals such as sapphire, garnet (AlFeSiO 12 ) substrate, or a glass substrate having a polysilicon film formed on the surface thereof. These substrates may be not only 4-inch but also 6-inch or 8-inch substrates.

[0015] The substrate 11 may have any orientation. In the case of a Si substrate, for example, Si(100), Si(110), Si(111), etc. may be used.

[0016] The buffer film 12 includes zirconia (ZrO2) epitaxially grown on the substrate 11, and is composed of a film portion 12a and a protruding portion 12b. It is known that the crystal system of ZrO2 undergoes a phase transition from monoclinic to tetragonal to cubic when energy is applied, but in the present invention, the buffer film 12 has a tetragonal crystal structure. The buffer film 12 is preferably epitaxially grown according to the orientation of the substrate 11.

[0017] It has been reported that the performance of piezoelectric materials improves when they have a tetragonal crystal system, or when they contain tetragonal crystals even if they are not tetragonal. It is believed that providing tetragonal zirconium oxide as a buffer film is advantageous for the formation of single crystals of piezoelectric materials.

[0018] Single crystal ZrO2 contains up to 8% crystal defects, and it is believed that when there are crystal defects, the vacancies of the defects and the adjacent atoms have elasticity in the direction to reduce the lattice distortion. The degree of this elasticity is believed to be proportional to the vacancy concentration. The buffer film 12 according to the present invention can utilize this elasticity to function as a variable crystal structure.

[0019] 1, the buffer film 12 has a protruding portion 12b. The formation of the protruding portion 12b is believed to be due to the fact that, when the raw material concentration is supersaturated during the film formation process of the buffer film 12, the crystal grows anisotropically along a certain axis or edge of the crystal, forming a pyramidal structure.

[0020] The components of the buffer film 12 may include not only ZrO2 but also rare earth elements and alkaline earth elements. In these, ZrO2 may include oxygen defects. In addition, to improve characteristics, the buffer film 12 may include transition metal elements such as Al, Sc, Mn, Fe, Co, and Ni.

[0021] Preferably, the film portion 12a is 10 nm or more, and the protruding portion 12b is 3 to 8 nm.

[0022] Fig. 2 shows a cross-sectional view of a substrate in which a lower electrode is formed on the buffer film 12 shown in Fig. 1. The lower electrode includes a conductive film 13 and a film 16 epitaxially grown on the buffer film 12. The conductive film 13 can be formed using various metals, such as platinum group elements Ru, Rh, Pd, Os, Ir, and Pt. These materials are known to have similar physical and chemical properties.

[0023] The film 16 contains a composite oxide represented by the following general formula (Chemical Formula 1), such as strontium titanate (STO), strontium ruthenate titanate (STRO), or strontium ruthenate (SRO), where 0≦x≦1 is satisfied. Sr(Ti 1-x ,Ru x )O3… (Chem.1)

[0024] The lower electrode preferably has a flat surface, the conductive film 13 may be at least 20 nm thick, and the film 16 may be thinner than the conductive film 13 .

[0025] FIG. 3 shows a cross-sectional view of a film structure 101 according to the present invention, in which a piezoelectric film 14 and a conductive film 15 as an upper electrode are further formed on the substrate shown in FIG.

[0026] The material of the piezoelectric film 14 is, for example, a perovskite oxide such as lead zirconate titanate (PZT) or barium titanate (BaTiO3). Alternatively, for example, trigonal bismuth ferrite (BiFeO3) can be used. Similarly, trigonal lithium niobate (LiNbO3) or lithium tantalate (LiTaO3) can be used. In addition, for example, hexagonal aluminum nitride (AlN) can be used.

[0027] For example, a tungsten bronze type ferroelectric film or a bismuth layer structure ferroelectric film can be used as the piezoelectric film 14. Examples of materials having the crystal structure of a tungsten bronze type ferroelectric film include Ba2NaNb5O 15 It is.

[0028] The crystal structure of the bismuth layer-structured ferroelectric film is represented by the general formula (Bi2O2) 2+ (A m-1 B m O 3m+1 ) 2- (m=1~5), or Bi2A m -1 B m O 3m+3 (m=1-5), (Bi2O2) 2+It has a plurality of suspected perovskite structures between the layers. The bismuth layered structure ferroelectric, for example, is bismuth titanate (Bi4Ti3O 12 ). Or, for example, bismuth lanthanum titanate (Bi 4-x La x )Ti3O 12 (0 < x < 1) can be used.

[0029] Not limited to the above piezoelectric film 14, a superconducting film 14 may be formed using a yttrium-based superconductor such as YBa2Cu3O7 (YBCO) having a perovskite structure or a bismuth-based superconductor such as Bi2SrCa2Cu3O 10 (BSCCO) as a material.

[0030] When using a material for forming the piezoelectric film or superconducting film as described above, a single crystal piezoelectric film 14 or superconducting film 14 can be formed on the buffer film 12.

[0031] A conductive film 15 is formed on the piezoelectric film 14. The conductive film 15 can use the same material as the conductive film 13. Note that the film 16 can be expected to have effects such as enhancing the adhesion between the conductive film 13 and the piezoelectric film 14.

Example

[0032] Hereinafter, this embodiment will be described in more detail based on examples. Note that the present invention is not limited by the following examples.

[0033] In Examples 1 - 4, a film structure 101 shown in FIG. 3 was created using a (100)-oriented Si substrate as the substrate 11. The piezoelectric film 14 was formed using PZT(30 / 70)(Pb(Zr 0.3 ,Ti 0.7 )O3) in Example 1, BTO (BaTiO3) in Example 2, BFO (BiFeO3) in Example 3, and BLT ((Bi 3.25 ,La 0.75 )Ti3O 12 ) as a sputtering material in Example 4.

[0034] First, a ZrO2 film was formed as a buffer film 12 on a substrate 11 by electron beam deposition under the following conditions. Equipment: Electron beam deposition equipment Pressure: 7.0×10 -3 Pa Vapor deposition source: Zr+O2 O2 flow rate: 10sccm Acceleration voltage / emission current: 7.5kV / 1.8mA Thickness: 25nm Substrate temperature: 600℃

[0035] 4(a) is a STEM image of a cross section of a substrate 11 after a ZrO2 film was formed as a buffer film 12 on the substrate 11. The lower image in FIG. 4(b) is an electron diffraction image of the substrate 11, and the upper image in FIG. 4(b) is an electron diffraction image of the buffer film 12.

[0036] As shown in Fig. 4(a), the buffer film 12 has a pyramidal protrusion 12b on its surface, and is composed of a film portion 12a and the protrusion 12b. As can be seen from the upper diagram of Fig. 4(b), the buffer film 12 is an aggregate of fine ZrO2 single crystals, and is epitaxially grown on the upper surface of the substrate 11.

[0037] Fig. 5 shows cross-sectional views of the buffer film 12 taken by STEM at each deposition time. Fig. 5(a) shows the buffer film 12 formed to a thickness of 1 nm, Fig. 5(b) shows the buffer film 12 formed to a thickness of 12 nm, Fig. 5(c) shows the buffer film 12 formed to a thickness of 15 nm, and Fig. 5(d) shows the buffer film 12 formed to a thickness of 25 nm. In Figs. 5(b) to (d), the shape of the protrusion 12b is highlighted by a white dotted line so that it can be seen.

[0038] As shown in FIG. 5(a), it was found that the protrusion 12b was not formed immediately after the buffer film 12 was formed. The film formation time at this time was 3 seconds. Next, a sample was prepared by forming the buffer film 12 for 1 minute, and its cross section was observed (FIG. 5(b)). As shown in FIG. 5(b), it was found that the height of the protrusion 12b was non-uniform. Next, a sample was prepared by forming the buffer film 12 for 5 minutes, and its cross section was observed (FIG. 5(c)). As shown in FIG. 5(c), the protrusion 12b had a more uniform height than the protrusion 12b shown in FIG. 5(b). Next, a sample was prepared by forming the buffer film 12 for 8 minutes, and its cross section was observed (FIG. 5(d)). As shown in FIG. 5(d), the protrusion 12b had a more uniform height than the protrusion 12b shown in FIG. 5(b) or (c).

[0039] The height of the protrusions 12b shown in Figures 5(b)-(d) was calculated based on the images and was 2.2 nm in Figure 5(b), 3.33 nm in Figure 5(c), and 4.67 nm in Figure 5(d). The shape of the protrusions 12b was a quadrangular pyramid, and the length of the diagonal of the base was 3.3 nm in Figure 5(b), 5.0 nm in Figure 5(c), and 7.0 nm in Figure 5(d).

[0040] From the above results, the size of the pyramids increased as the buffer film 12 was formed, and the height of the protrusions 12b increased with the film formation time. In addition, if the buffer film 12 was formed for 0.05 minutes (3 seconds) (FIG. 5(a)) and the surface area was taken as 1.0, the surface areas of the buffer films 12 in FIGS. 5(b)-(d) were 1.30 to 1.60 times the planar surface area.

[0041] The film formation rate was calculated to be 3.33 [nm / sec] for Fig. 5(a), 2.0 [nm / sec] for Fig. 5(b), 0.50 [nm / sec] for Fig. 5(c), 0.50 [nm / sec] for Fig. 5(c), and 0.52 [nm / sec] for Fig. 5(d). Thus, according to the film formation rate for each thickness of the buffer film 12, it was found that the film formation rate becomes constant when the film becomes thicker than 15 nm.

[0042] Figure 6 shows the results of measuring the θ-2θ spectrum by XRD after forming the conductive film 13 and the film 16 by the method described later. As shown in Figure 6, according to the peak positions, it was found that the ZrO2 buffer film 12 has a tetragonal crystal structure oriented in the (200) plane.

[0043] Next, a platinum (Pt) film was formed as the conductive film 13 by sputtering on the buffer film 12 under the following conditions. Equipment: DC sputtering equipment Pressure: 1.2×10 -1 Pa Vapor deposition source: Pt Power: 100W Thickness: 150nm Substrate temperature: 450~600℃

[0044] 7A and 7B are STEM images of the cross section of a Pt conductive film 13 formed on a buffer film 12. Fig. 7A shows the conductive film 13 formed to a thickness of 10 nm, Fig. 7B shows the conductive film 13 formed to a thickness of 20 nm, and Fig. 7C shows the conductive film 13 formed to a thickness of 150 nm.

[0045] As shown in Fig. 7(a), it was found that the surface of the conductive film 13 was almost flat even with a film thickness of 10 nm. Then, as shown in Fig. 7(b), the surface of the conductive film 13 was made even flatter by increasing the film thickness to 20 nm, and even when the conductive film 13 was formed to a thickness of 150 nm, the flatness was maintained as shown in Fig. 7(c).

[0046] Next, a SrRuO3 (SRO) film was formed as the film 16 on the conductive film 13 by sputtering under the following conditions. Equipment: RF magnetron sputtering equipment Power: 300W Gas: Ar Pressure: 1.8Pa Thickness: 20nm Substrate temperature: 600℃

[0047] Next, the piezoelectric film 14 was formed on the film 16. The formation conditions were the same in Examples 1 to 4, and only the sputtering materials were different. Equipment: RF magnetron sputtering equipment Material: [Example 1: PZT (30 / 70)] Pb(Zr 0.3 ,Ti 0.7 )O3, [Example 2: BTO] BaTiO3, [Example 3: BFO] BiFeO3, [Example 4: BLT] (Bi 3.25 ,La 0.75 )TiO 12 Power: 1500W Gas: Ar / O2 Pressure: 1.0Pa Substrate temperature: 450℃

[0048] Example 1 In Example 1, the film structure 101 was formed as Si / ZrO2 / Pt / SRO / PZ / Pt. The substrate 11 was Si(100). After forming PZT(30 / 70) as the piezoelectric film 14, the film thickness was measured by XRF using a Rigaku X-ray fluorescence analyzer (AZX400) and found to be 1.0 μm.

[0049] Fig. 8 shows the results of measuring the θ-2θ spectrum by the XRD method for the film structure 101 according to Example 1. As shown in Fig. 8, it was found that PZT (30 / 70) was preferentially oriented along the c axis. The lattice constants a and c were obtained based on this X-ray diffraction pattern, and the c / a axial ratio was calculated to be 1.046.

[0050] Fig. 9 is a cross-section of the film structure 101, and shows a lattice image by STEM observing PZT (30 / 70) as the piezoelectric film 14. As shown in Fig. 9, it was confirmed that the piezoelectric film 14 was a single crystal without any crystal lattice disturbance such as dislocation.

[0051] Fig. 10 shows the results of measuring pole figures by XRD for each layer in the film structure 101 according to Example 1 to examine the in-plane orientation relationship of the film of each layer. Fig. 10(a) is a pole figure of the Si(220) plane, Fig. 10(b) is a pole figure of the ZrO2(220) plane, Fig. 10(c) is a pole figure of Pt(220), and Fig. 10(d) is a pole figure of PZT(202).

[0052] As shown in Figure 10(a)-(d), peaks with four-fold symmetry were observed, indicating that epitaxial growth had occurred with the in-plane orientation aligned with the substrate.

[0053] 11 is a graph showing the voltage dependence of the polarization of the piezoelectric film 14 according to Example 1. As shown in FIG. 11, the piezoelectric film 14 according to Example 1 exhibits good characteristics, and the remanent polarization Pr is 50 μC / cm 2 and the coercive electric field Ec was 180 kV / cm.

[0054] Example 2 In Example 2, the films were formed as follows: Si / ZrO2 / Pt / SRO / BTO. Si(100) was used as the substrate 11. After forming the BTO as the piezoelectric film 14, the film thickness was measured by XRF and found to be 1.0 μm.

[0055] Fig. 12 shows the results of measuring the θ-2θ spectrum by the XRD method for the film structure 101 according to Example 2. In Fig. 12, the upper curve shows the results of the out-of-plane measurement, and the lower curve shows the results of the in-plane measurement.

[0056] 12, the piezoelectric film 14 was preferentially oriented in the (001) plane. From the measurement results, the a-axis length and c-axis length of the piezoelectric film 14 were calculated to be 0.4012 nm and 0.4262 nm, respectively. Therefore, the c / a ratio was 1.044, which indicates that the c-axis length is longer than the bulk value of 1.01.

[0057] Fig. 13 is a diagram showing an X-ray diffraction pattern by φ scanning for the film structure 101 according to Example 2. (a) is the substrate 11, and (b) is the pattern of the piezoelectric film 14. As can be seen from Fig. 13, the piezoelectric film 14 has a four-fold axis of symmetry at the same angle as the substrate 11, and it was found that up to the piezoelectric film 14, the structure is formed in a cube-on-cube configuration.

[0058] Fig. 14 is a cross-section of the film structure 101 according to Example 2, and shows a lattice image by STEM observing BTO as the piezoelectric film 14. As shown in Fig. 14, it was confirmed that the piezoelectric film 14 was a single crystal without any crystal lattice disturbance such as dislocation.

[0059] Fig. 15 is a graph showing the voltage dependence of the polarization of the piezoelectric film 14. As shown in Fig. 15, the piezoelectric film 14 according to Example 2 exhibited ferroelectric properties.

[0060] FIG. 16 shows the piezoelectricity of the piezoelectric film 14 confirmed by a d33 meter. The d33 meter is a d33 constant measuring device (model: LTFA-01) manufactured by Lead Techno Co., Ltd., and is capable of measuring d33 even without the conductive film 15 as the upper electrode. Specifically, a force is applied to the film structure 101 and the change in the amount of charge is detected by an integrating circuit. If the film structure has piezoelectricity, a pulse-shaped waveform can be observed by applying or not applying force at regular time intervals, as shown in FIG. 16. The d33 value at this time was 24.88 (pC / N).

[0061] Example 3 In Example 3, the films were formed as follows: Si / ZrO2 / Pt / SRO / BFO. Si(100) was used as the substrate 11. After forming BFO as the piezoelectric film 14, the film thickness was measured by XRF and found to be 2.1 μm.

[0062] Fig. 17 shows the results of measuring the θ-2θ spectrum by the XRD method for the film structure 101 according to Example 3. In Fig. 17, the upper curve shows the results of the out-of-plane measurement, and the lower curve shows the results of the in-plane measurement. As shown in Fig. 17, the piezoelectric film 14 was preferentially oriented in the (001) plane.

[0063] Fig. 18 shows an X-ray diffraction pattern by φ scanning, where (a) is the substrate 11 and (b) is the pattern of the piezoelectric film 14. As can be seen from Fig. 18, after the formation of the piezoelectric film 14, it has a four-fold axis of symmetry at the same angle as the substrate 11, and it was found that up to the piezoelectric film 14, it is formed in a cube-on-cube manner.

[0064] Fig. 19 is a cross-section of the film structure 101, and shows a lattice image by STEM of BFO as the piezoelectric film 14. As shown in Fig. 19, it was confirmed that the piezoelectric film 14 was single crystal, without any crystal lattice disturbance such as dislocation.

[0065] 20 is a graph showing the voltage dependence of the polarization of the piezoelectric film 14. As shown in FIG. 20, the piezoelectric film 14 according to Example 3 exhibits good characteristics, and the remanent polarization Pr is 60 μC / cm 2 and the coercive electric field Ec was 100 kV / cm.

[0066] Fig. 21 is a diagram showing the measurement results of the piezoelectric film 14 by a d33 meter. As shown in Fig. 21, it was found that the piezoelectric film 14 has piezoelectricity. The d33 value at this time was 16.69 (pC / N).

[0067] Example 4 In Example 4, the films were formed as follows: Si / ZrO2 / Pt / SRO / BLT. Si(100) was used as the substrate 11. After forming BLT as the piezoelectric film 14, the film thickness was measured by XRF and found to be 1.0 μm.

[0068] Fig. 22 shows the results of measuring the θ-2θ spectrum by the XRD method for the film structure 101 according to Example 4. Fig. 22 shows the results of the out-of-plane measurement. As shown in Fig. 22, the piezoelectric film 14 was preferentially oriented in the (001) plane.

[0069] Fig. 23 shows an X-ray diffraction pattern by φ scanning. (a) is the substrate 11, and (b) is the pattern formed up to the piezoelectric film 14. As can be seen from Fig. 24, after the formation of the piezoelectric film 14, it has a four-fold axis of symmetry at the same angle as the substrate 11, and is formed in a cube-on-cube structure.

[0070] Fig. 24 is a cross-section of the film structure 101, and shows a lattice image by STEM observing BLT as the piezoelectric film 14. As shown in Fig. 24, it was confirmed that the piezoelectric film 14 was single crystal without any crystal lattice disturbance such as dislocation. In Fig. 25, W1 is a perovskite layer, and W2 is a bismuth oxide layer.

[0071] 25 is a graph showing the voltage dependence of the polarization of the piezoelectric film 14. As shown in FIG. 25, the piezoelectric film 14 according to Example 4 exhibits ferroelectricity, and the remanent polarization Pr is 4 μC / cm 2 and the coercive electric field Ec was 4.5 kV / cm.

[0072] Fig. 26 is a diagram showing the measurement results, using a d33 meter, of the piezoelectric film 14. As shown in Fig. 26, it was found that the piezoelectric film 14 had piezoelectricity. The d33 value at this time was 164.7 (pC / N).

[0073] Example 5 In Example 5, the films were formed as follows: Si / ZrO2 / Pt / SRO / PZT. The substrate 11 was Si(111). After forming PZT as the piezoelectric film 14, its film thickness was measured by XRF and found to be 1.0 μm. A target of Pb / Zr / Ti(130 / 52 / 48) was used as the material for PZT.

[0074] Fig. 27 shows the results of measuring the θ-2θ spectrum by the XRD method for the sample produced in Example 5. As shown in Fig. 27, the substrate 11, the buffer film 12, the conductive film 13, and the piezoelectric film 14 were all oriented in the (111) plane.

[0075] Fig. 28 shows the results of a φ scan by the XRD method, in which the (111) plane was measured as the diffraction plane for the sample produced in Example 5. As shown in Fig. 28, the substrate 11, the conductive film 13, and the piezoelectric film 14 exhibited three-fold symmetry. Although the peak of the conductive film 13 is shifted by 60°, it is an epitaxially grown single crystal film, and the piezoelectric film 14 is also an epitaxially grown single crystal film.

[0076] Example 6 In Example 6, the films were formed as follows: Si / ZrO2 / Pt / SRO / PZT. The substrate 11 was Si (110). After forming PZT as the piezoelectric film 14, its film thickness was measured by XRF and found to be 1.0 μm. A target of Pb / Zr / Ti (130 / 52 / 48) was used as the material for PZT.

[0077] Fig. 29 shows the results of measuring the θ-2θ spectrum by the XRD method for the sample produced in Example 2. As shown in Fig. 29, the substrate 11 and the conductive film 13 were preferentially oriented in the (110) plane.

[0078] Fig. 30 shows the results of a φ scan by the XRD method, in which the (111) plane was measured as the diffraction plane for the sample prepared in Example 6. As shown in Fig. 30, the substrate 11, the conductive film 13, and the piezoelectric film 14 exhibited two-fold symmetry. This indicates that the piezoelectric film 14 is an epitaxially grown single crystal film.

[0079] As can be seen from the results of Examples 1-6, the buffer film 12 grows epitaxially in accordance with the orientation of the substrate 11, and the various piezoelectric films 14 formed thereon also grow epitaxially. This is believed to be because, as will be described below, after the buffer film 12 is formed, the crystal structure of the buffer film 12 changes depending on the piezoelectric material formed thereon.

[0080] Fig. 31 shows the results of STEM observation of the cross section of the buffer film 12 and conductive film 13 for the sample formed with PZT (30 / 70) according to Example 1. As shown in Fig. 31(a), the length between the protrusions 12b was 4.2 nm. Fig. 31(b) is an enlarged view of the protrusions 12b.

[0081] Fig. 32 shows the results of STEM observation of the cross section of the buffer film 12 and the conductive film 13 for the sample formed with BFO according to Example 3. As shown in Fig. 32(a), the length between the protruding parts 12b was 3.9 nm. Fig. 32(b) is an enlarged view of the protruding parts 12b.

[0082] Fig. 33 shows the results of STEM observation of the cross section of the buffer film 12 and the conductive film 13 for the sample formed with the BLT according to Example 4. As shown in Fig. 33(a), the length between the protrusions 12b was 5.5 nm. Fig. 33(b) is an enlarged view of the protrusions 12b.

[0083] As shown in Figures 31-33, the height of the protrusion 12b changes depending on the lattice constant of the piezoelectric film 14. For example, the lattice constant of the a-axis of BFO shown in Figure 32 is 0.3971 nm, which is the shortest compared to PZT in Figure 31 and BLT in Figure 33. In this case, the height of the protrusion 12b is 6.3 nm as shown in Figure 32(b), and it is considered that the protrusion 12b is stretched upward to match the BFO with a shorter lattice constant during the deposition process of BFO, which is the piezoelectric film 14.

[0084] On the other hand, the a-axis lattice constant of BLT shown in Fig. 33 is 0.5411 nm, which is the longest compared to PZT in Fig. 31 and BFO in Fig. 32. In this case, the height of protrusion 12b is 2.8 nm as shown in Fig. 33(b), and it is considered that protrusion 12b is crushed downward to match BLT with a long lattice spacing during the deposition process of BLT, which is the piezoelectric film 14.

[0085] In this way, the buffer film 12, particularly the protruding portion 12b, is deformed according to the type of piezoelectric film 14, and further the lattice spacing of the conductive film 13 and film 16 on the buffer film 12 also varies. Figure 34(a) is a lattice image showing a cross section of the interface between the conductive film 13 and film 16 when BFO is formed, and Figure 34(b) is a lattice image showing a cross section of the interface between the conductive film 13 and film 16 when BLT is formed.

[0086] As shown in FIG. 34(b), the molecular spacing between the conductive film 13 and the film 16 when BLT is formed is longer than the molecular spacing between the conductive film 13 and the film 16 when BFO is formed, as shown in FIG. 34(a).

[0087] Example 7 In Example 7, the films were formed as follows: Si / ZrO2 / Pt / SRO / AlN. The substrate 11 was Si(100). The manufacturing conditions up to the SRO film were the same as those in Examples 1-6. The AlN film was formed under the following conditions. Equipment: RF magnetron sputtering equipment Power: 200W Gas: Ar Pressure: 0.5Pa Film formation time: 60 minutes Substrate temperature: 200℃

[0088] Fig. 35 shows the results of measuring the X-ray diffraction pattern of AlN by φ scanning using the XRD method for the film structure 101 according to Example 7. As shown in Fig. 35, it was found that the AlN film exhibited six-fold symmetry, was uniaxially oriented in (0001), and was single crystallized. Note that the circled numbers 1 and 2 in Fig. 35 indicate a 90° rotation in the plane.

[0089] Example 8 In Example 8, the films were formed as follows: Si / ZrO2 / Pt / SRO / LiNbO3 (LN). The substrate 11 was Si (100). The manufacturing conditions up to the SRO film were the same as in Examples 1-6. The LN film was formed under the following conditions. Equipment: RF magnetron sputtering equipment Power: 160W Gas: Ar / O2 ratio 2% Pressure: 0.8Pa Coating time: 9 hours Substrate temperature: 400℃

[0090] Fig. 36 shows the results of measuring the X-ray diffraction pattern of the film structure 101 according to Example 8, in which LN was φ-scanned by the XRD method. As shown in Fig. 35, it was found that the LN film exhibited four-fold symmetry, was uniaxially oriented in (001), and was single crystallized.

[0091] As can be seen from the results of Examples 1 to 8 above, it was found that when a Pt film and an SRO film were epitaxially grown on a buffer film containing zirconium, and a piezoelectric film was then formed thereon, a single-crystallized piezoelectric film could be formed. [Explanation of symbols]

[0092] 11 Substrate 12 Buffer film 12a Membrane part 12b Projection 13, 15 Conductive film 14 Piezoelectric film / Superconductor film 16 membrane 101 Membrane structure

Claims

1. A substrate; a buffer film having a tetragonal crystal structure containing zirconia formed on the substrate; a metal film containing a platinum group element epitaxially grown on the buffer film; An epitaxially grown Sr(Ti) 1-x , Ru x ) O 3 and a film including (0≦x≦1) The membrane structure comprises:

2. The thickness of the metal film is 20 to 150 nm. The membrane structure according to claim 1 .

3. The film structure according to claim 1 or 2, wherein the buffer film further contains a rare earth element or an alkaline earth element.

4. The surface area of ​​the buffer film is 1.30 to 1.60 compared to a plane; The membrane structure according to any one of claims 1 to 3.

5. The substrate is oriented in a (100), (110) or (111) plane. The membrane structure according to any one of claims 1 to 4.

6. The buffer film is epitaxially grown according to the orientation of the substrate. The membrane structure according to any one of claims 1 to 5.

7. A single crystal piezoelectric film formed on the film according to claim 1 .

8. The piezoelectric film according to claim 7 , which has a trigonal crystal structure.

9. The material is BiFeO 3 , LiNbO 3 , or LiTaO 3 The piezoelectric film according to claim 8 ,

10. The piezoelectric film according to claim 7 , which has a hexagonal crystal structure.

11. The piezoelectric film of claim 10 , wherein the material is AlN.

12. The piezoelectric film according to claim 7 , which has a tungsten bronze type crystal structure.

13. The piezoelectric film according to claim 7 , which has a bismuth layer-type crystal structure.

14. The material is Bi 4 Ti 3 O 12 Or (Bi 4-x La x ) Ti 3 O 12 The piezoelectric film according to claim 13 , wherein (0≦x<1).

15. A.B.O. 3 8. The piezoelectric film according to claim 7, which is a perovskite oxide represented by the formula:

16. The piezoelectric film of claim 7 , wherein the material is lead zirconate titanate.

17. The lead zirconate titanate is Pb(Zr 0.3 , Ti 0.7 ) O 3 The piezoelectric film according to claim 16 ,

18. A single crystal superconductor film formed on the film according to any one of claims 1 to 6.

19. 20. The superconductor film of claim 18 which is a bismuth-based superconductor.

20. The material is Bi 2 SrCa 2 Cu 3 O 10 20. The superconductor film of claim 19,

21. 20. The superconductor film of claim 18 which is a yttrium-based superconductor.

22. The yttrium-based superconductor material is YBa 2 Cu 3 O 7 22. The superconductor film of claim 21 ,

Citation Information

Patent Citations

  • Laminated thin film, method of producing the same and electronic device

    JP2002029894A

  • Film structure and manufacturing method thereof

    JP2018081974A

  • Film structure body and method for manufacturing the same

    JP2019016793A

  • Optical waveguide

    JP1993072428A