CORE-SHELL Si PARTICLE FILLER AND RESIN COMPOSITION
The core-shell Si particle filler with a shell layer of Al, Zn, and O addresses the challenge of low thermal conductivity and resistivity in resin fillers by providing excellent chemical stability and acid resistance, enhancing resin compositions.
Patent Information
- Application Number
- JP2023049210
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
AI Technical Summary
Existing resin fillers, such as oxide and nitride fillers, have low thermal conductivity and metal fillers with high thermal conductivity suffer from low resistivity, making it difficult to achieve both high thermal conductivity and chemical stability, particularly acid resistance, in resin compositions.
A core-shell type Si particle filler with a shell layer containing Al, Zn, and O on the surface of a metal Si core particle, ensuring minimal elution of Al and Fe, and a specific atomic composition ratio, provides excellent chemical stability and acid resistance.
The core-shell Si particle filler achieves enhanced thermal conductivity and chemical stability, particularly acid resistance, when incorporated into resin compositions, improving their overall performance.
Smart Images

Figure 2024138628000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a core-shell type Si particle filler and a resin composition. [Background technology]
[0002] In recent years, the amount of heat generated by communication devices has increased in line with the increase in communication traffic under 5G high-speed communication, and there is a demand for various heat dissipation components with higher performance. Oxide fillers such as alumina filler and nitride fillers such as aluminum nitride and silicon nitride are widely used as resin fillers for heat dissipation components.
[0003] However, oxide and nitride fillers have low thermal conductivity, making it difficult to achieve high thermal conductivity when mixed with resin. Metal fillers with excellent thermal conductivity have also been considered, but there is a problem that the resistivity, which is a characteristic of metals, is extremely low. Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present invention is to provide a core-shell type Si filler having excellent chemical stability, particularly excellent acid resistance, and a resin composition containing the core-shell type Si filler having excellent chemical stability, particularly excellent acid resistance. [Means for solving the problem]
[0005] As a result of intensive research, the inventors have found that the above-mentioned problems can be solved by a core-shell type Si particle filler in which the amount of Al eluted is 3 ppm or less when immersed in a 6 mol / L hydrochloric acid aqueous solution at 25°C for 2 hours and the core has a shell layer containing Al, Zn and O on the surface of a metal Si particle (core), and have thus completed the present invention. That is, the present invention has the following aspects. [1] A core-shell type silicon particle filler having a shell layer containing Al, Zn and O on the surface of a metal silicon core particle, in which the amount of Al eluted is 3 ppm or less when immersed in a 6 mol / L hydrochloric acid aqueous solution at 25°C for 2 hours. [2] The core-shell type Si particle filler according to [1], in which the amount of Fe eluted is less than 2 ppm when immersed in a 6 mol / L aqueous hydrochloric acid solution at 25° C. for 2 hours. [3] The core-shell type Si particle filler according to [1] or [2], wherein the atomic composition ratio (Al+Zn) / Si, as analyzed by X-ray photoelectron spectroscopy, is 0.015 or more and 0.075 or less. [4] The spherical core-shell type Si particle filler according to any one of [1] to [3], wherein the atomic composition ratio (Al+Zn) / Si, as analyzed by X-ray photoelectron spectroscopy, is 0.02 or more and 0.07 or less. [5] The core-shell type Si particle filler according to any one of [1] to [4], having an average circularity of 0.70 or more. [6] Specific surface area is 1.0 m 2 / g or less. [7] A resin composition comprising a resin and the core-shell type Si particle filler according to any one of [1] to [6]. Effect of the Invention
[0006] According to the present invention, it is possible to provide a core-shell type Si filler having excellent chemical stability, particularly excellent acid resistance, and a resin composition containing the core-shell type Si filler and having excellent chemical stability, particularly excellent acid resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] An embodiment of the present invention will be described in detail below. The present invention is not limited to the following embodiment, and can be implemented by making appropriate modifications within the scope that does not impair the effects of the present invention. In addition, when multiple upper and lower limit values are described for a specific parameter, any upper and lower limit values among these upper and lower limit values can be combined to form a suitable numerical range. When a specific description described for one embodiment also applies to other embodiments, the description may be omitted in other embodiments. In this disclosure, the expression "X to Y" for a numerical range means "X or more and Y or less".
[0008] [Core-shell type Si particle filler] The core-shell type Si particle filler according to this embodiment has an Al elution amount of 3 ppm or less when immersed in a 6 mol / L hydrochloric acid aqueous solution at 25° C. for 2 hours, and has a shell layer containing Al, Zn and O on the surface of the metal Si core particle. By having a shell layer containing Al, Zn and O on the surface of the metal Si core particle, the spherical core-shell type Si particle filler according to this embodiment has better chemical stability, particularly acid resistance, and can thereby provide a resin composition having better chemical stability, particularly acid resistance. In this specification, "filler" means a packing material. In this specification, "core-shell type" means a structure in which a shell layer of an oxide film is provided on at least a part (preferably the entirety) of the surface of a metal Si particle. The "core-shell type" structure can be confirmed by observing the core-shell type Si particle filler with a transmission electron microscope (TEM). In addition, the presence and composition of the shell layer can be confirmed by combining a scanning electron microscope photograph (SEM) with an energy dispersive X-ray analyzer (EDS), and further combining it with chemical analysis as necessary. In this specification, the term "core-shell type Si particle filler" refers to both a single core-shell type Si particle and its aggregate, which are used as a filler. In other words, the term "core-shell type Si particle filler" refers to the same thing as a core-shell type Si particle having a structure in which a shell layer is provided on the surface of a metal Si particle (core) as a substance, covering at least a part of the surface of the particle. In this specification, "spherical" means that the particles are observed to have a circular or rounded grain shape when observed at 10,000 times magnification using a scanning electron microscope.
[0009] (Al elution amount) The amount of Al elution can be measured by quantitative analysis of hydrochloric acid solution using an ICP emission spectrometer. When immersed in 6 mol / L hydrochloric acid solution at 25°C for 2 hours, the amount of Al eluted into the hydrochloric acid solution (hereinafter also simply referred to as "Al elution amount") is 3 ppm or less, so that the chemical stability of the filler itself and the resin composition therewith can be further improved. Examples of methods for adjusting the amount of Al elution to 3 ppm or less include a method of heat treating spheroidized metal Si particles containing a certain amount of Al and / or Zn or a method of mixing spheroidized metal Si particles with powder containing Al and / or Zn and heat treating the mixture to form an oxide film having a high composition ratio of Al and Zn to Si. In the core-shell type Si particle filler according to one embodiment, the amount of Al elution is preferably 2.5 ppm or less, more preferably 2 ppm or less, further preferably 1.5 ppm or less, and particularly preferably 1 ppm or less.
[0010] In one embodiment, the core-shell type Si particle filler can be obtained by subjecting the spherical metal Si particles obtained by spheroidizing the raw material metal Si powder to surface oxidation by heat treatment to form a shell layer of an oxide film on the surface of the spherical metal Si particles. The raw material metal Si may contain impurities, but it is preferable that the purity is 98% or more, more preferably that the purity is 99% or more, and even more preferably that the purity is 99.9% or more. The spheroidization method will be described later.
[0011] (Fe elution amount) In the core-shell type Si particle filler according to an embodiment, the amount of Fe eluted into a hydrochloric acid solution by immersing the filler in a 6 mol / L hydrochloric acid solution at 25° C. for 2 hours (hereinafter, simply referred to as the “Fe elution amount”) is preferably less than 2 ppm, more preferably 1.5 ppm or less, and even more preferably 1 ppm or less. The Fe elution amount can be measured by quantitative analysis of the hydrochloric acid solution using an ICP emission spectrometer. When the Fe elution amount into the hydrochloric acid solution is less than 2 ppm, the chemical stability, particularly the acid resistance, of the resin composition can be further improved. Examples of a method for adjusting the Fe elution amount to less than 2 ppm include a method of subjecting spheroidized metal Si particles containing a certain amount of Al and / or Zn or more to heat treatment, or a method of mixing the spheroidized metal Si particles with a powder containing Al and / or Zn and heat treatment to generate an oxide film having a high composition ratio of Al and Zn to Si.
[0012] (Atomic composition ratio (Al+Zn) / Si) analyzed by X-ray photoelectron spectroscopy The core-shell type Si particle filler according to one embodiment has an Al content measured by X-ray photoelectron spectroscopy. 2s Semi-quantitative value calculated from peak intensity, Zn 3p Semi-quantitative values calculated from peak intensities and Si 2s The semi-quantitative (Al+Zn) / Si ratio calculated from the peak intensity is preferably 0.015 or more and 0.075 or less. By having the (Al+Zn) / Si ratio of 0.015 or more and 0.075 or less, the resin composition has excellent chemical stability, particularly excellent acid resistance, and when used as a filler, the resin composition has excellent chemical stability, particularly excellent acid resistance. In this specification, the "atomic composition ratio (Al+Zn) / Si analyzed by X-ray photoelectron spectroscopy" refers to the ratio of Al to Zn measured by the Shirley method. 2s , Zn 3p and Si 2s The semi-quantitative value was calculated from the peak intensity, and the (Al + Zn) / Si ratio ((Al 2s +Zn3p ) / Si 2s This refers to a value obtained by calculating the ratio of In this specification, the "Shirley method" refers to a method for determining the shape of the background to be subtracted, assuming that the inelastically scattered electrons that cause the background are independent of energy and that the number of inelastically scattered electrons is proportional to the peak intensity.
[0013] In one embodiment, the core-shell type Si particle filler has an atomic composition ratio (Al+Zn) / Si, as analyzed by X-ray photoelectron spectroscopy, of preferably 0.016 or more, more preferably 0.017 or more, and even more preferably 0.02 or more. In one embodiment, the core-shell type Si particle filler has an atomic composition ratio (Al+Zn) / Si analyzed by X-ray photoelectron spectroscopy of preferably 0.07 or less, more preferably 0.065 or less, and even more preferably 0.06 or less. In one embodiment, the core-shell type Si particle filler has an atomic composition ratio (Al+Zn) / Si analyzed by X-ray photoelectron spectroscopy of 0.016 to 0.07, 0.016 to 0.065, 0.016 to 0.06, 0.017 to 0.07, 0.017 to 0.065, 0.017 to 0.06, 0.02 to 0.07, 0.02 to 0.065, or 0.02 to 0.06. Methods for making the atomic composition ratio (Al+Zn) / Si, as analyzed by X-ray photoelectron spectroscopy, 0.015 or more include subjecting spheroidized metal Si particles containing a certain amount of Al and / or Zn to heat treatment, or mixing the spheroidized metal Si particles with a powder containing Al and / or Zn and then heat treating them. By performing the heat treatment, an oxide coating can be formed on the particle surface of the metal Si particles, which gives them suitable properties as a filler. The heat treatment is preferably carried out at a temperature of 850° C. to 1150° C. The greater the Al and Zn contents of the spheroidized metal Si particles, or the greater the amount of powder containing Al and / or Zn that is mixed, the higher the atomic composition ratio (Al+Zn) / Si analyzed by X-ray photoelectron spectroscopy tends to be.
[0014] (Atomic composition ratio O / Si analyzed by X-ray photoelectron spectroscopy) In the core-shell type Si particle filler according to one embodiment, the atomic composition ratio O / Si, as analyzed by X-ray photoelectron spectroscopy, is preferably greater than 1.5 and less than or equal to 2.2. In this specification, the "atomic composition ratio O / Si analyzed by X-ray photoelectron spectroscopy" refers to the ratio of O 1s and Si 2s The semi-quantitative value was calculated from the peak intensity, and the O / Si ratio (O 1s / Si 2s This refers to a value obtained by calculating the ratio of The core-shell type Si particle filler according to one embodiment has an atomic composition ratio O / Si of more than 1.5 and not more than 2.2, and therefore has excellent chemical stability, particularly acid resistance, and when used as a filler, can provide a resin composition having excellent chemical stability, particularly acid resistance.
[0015] (Average circularity) The core-shell type Si particle filler according to one embodiment preferably has an average circularity of 0.70 or more. By having an average circularity of 0.70 or more, it is possible to highly fill the resin, and it is possible to provide a resin composition having excellent thermal conductivity. The core-shell type Si particle filler according to one embodiment has an average circularity of more preferably 0.72 or more, even more preferably 0.75 or more, even more preferably 0.80 or more, and particularly preferably 0.90 or more. The average circularity can be adjusted, for example, by adjusting the shape of the spheroidized metal Si particles. For example, when the metal Si powder is spheroidized by the atomization method or thermal plasma method, the aggregation between the particles is suppressed by reducing the powder supply amount or increasing the melting temperature, and the average circularity tends to be high.
[0016] In this specification, the term "average circularity" refers to a value measured by the following method. The core-shell type Si particle filler is fixed to a sample stage with carbon tape, and then osmium coating is performed. After that, the projected area (S) and projected perimeter (L) of the powder are calculated from an image taken with a scanning electron microscope, and the circularity is calculated from the following formula (1). The circularity is calculated for any 200 powder particles, and the average value is taken as the average circularity. Circularity = 4πS / L 2 (1)
[0017] (specific surface area) The core-shell type Si particle filler according to one embodiment has a specific surface area of 1.0 m 2 / g or less. 2 When the specific surface area of the core-shell type Si particle filler according to one embodiment is less than 0.8 m / g, there is little adhesion to the surface of each particle, and the thermal conductivity of the resin composition can be improved. 2 / g or less is more preferable, and 0.6m 2 More preferably, it is 0.5m 2 It is even more preferable that the value is 0.4m / g or less. 2 It is more particularly preferable that the molecular weight is not more than 1 / g.
[0018] In this specification, the "specific surface area" refers to a value measured using a specific surface area measuring device in accordance with the description of JIS Z8830:2013 "Method for measuring the specific surface area of powders (solids) by gas adsorption", and is a value calculated by applying the BET single point method using nitrogen gas.
[0019] (Average particle size) From the viewpoint of filling properties into resin, the average particle diameter (D50, median diameter) of the core-shell type Si particle filler according to this embodiment is preferably 100 μm or less, more preferably 1 to 80 μm, even more preferably 10 to 60 μm, and particularly preferably 20 to 50 μm. The average particle diameter (D50) of the core-shell type Si particle filler refers to the volume-based cumulative diameter (D50) evaluated by a laser diffraction scattering method after a specific dispersion treatment, for example, homogenizer treatment, is carried out. "Volume-based cumulative diameter (D50)" means the particle diameter at which the cumulative value corresponds to 50% in the volume-based cumulative particle size distribution measured by the laser diffraction scattering method. The cumulative particle size distribution is expressed by a distribution curve with the horizontal axis being particle diameter (μm) and the vertical axis being cumulative value (%).
[0020] (Powder resistivity) The core-shell type Si particle filler according to one embodiment has a powder resistivity of 1×10 measured under a load of 63.7 MPa in an atmosphere of 23° C. and 40% relative humidity. 7 It is preferable that the resistance is Ω·cm or more, and 1×10 8 More preferably, it should be 1×10 9 It is more preferable that the powder resistivity measured under a load of 63.7 MPa is 1×10 7 A resistivity of Ω·cm or more can provide a resin composition with higher resistivity.
[0021] (Thermal Conductivity) The core-shell type Si particle filler according to one embodiment has a thermal diffusivity T(m 2 / s), density D(kg / m 3The thermal conductivity H (W / (m K)) calculated from the formula H = T × D × C using the measured values of heat capacity, specific heat capacity C (J / (kg K)) is preferably 5.0 W / m K or more, more preferably 5.1 W / m K or more, and even more preferably 5.2 W / m K or more. When immersed in a 6 mol / L hydrochloric acid solution at 25°C for 2 hours, the amount of Al eluted was 3 ppm or less. The core-shell type Si particle filler, which has a shell layer containing Al, Zn, and O on the surface of the metal Si core particle, can achieve excellent thermal conductivity of 5.0 W / m K or more when mixed with resin.
[0022] [Application] The core-shell type Si particle filler according to this embodiment can provide a resin composition having better chemical stability, particularly better acid resistance, when filled into a resin, and can therefore be suitably used as a filler for resin materials.
[0023] [Method of manufacturing core-shell type Si particle filler] The method for producing the core-shell type Si particle filler according to this embodiment includes (1) spheroidizing metal Si powder, and (2) subjecting the spheroidized metal Si particles to a heat treatment at a temperature of 850° C. to 1150° C. By combining the methods (1) and (2), a sufficient but not excessive oxide film is easily obtained on the metal filler, and a resin composition having high resistivity and excellent thermal conductivity can be obtained when filled into a resin. (1) Spheroidizing the metal Si powder according to this embodiment may further include (3) spheroidizing the metal Si powder by a thermal plasma method, an atomization method, or the like, and may further include (4) removing fine particles having a particle size of less than 1 μm by classification after spheroidization. By combining the methods (3) and (4), it is easier to obtain spherical Si metal with high sphericity and uniformity, and when filled into a resin, a resin composition with superior thermal conductivity can be obtained.
[0024] (Raw material preparation process) Prior to the spheroidizing step, a silicon raw material may be prepared as necessary. Examples of the silicon raw material include commercially available metal silicon powder and metal silicon ingot, and it is preferable to use one or more selected from these.
[0025] In one embodiment, the raw metal Si is preferably metal Si in powder form (metal Si powder). The volume-based average particle size (D50) of the particles after pulverization is preferably 10 to 100 μm, more preferably 20 to 80 μm, and even more preferably 30 to 60 μm. The method for measuring the average particle size (D50) is as described above.
[0026] In one embodiment, the raw material Si may contain Al and / or Zn. By adding Al and / or Zn, it is possible to easily prepare a core-shell type Si particle filler with a small amount of Al elution. The Al and Zn to be added are preferably metal Al, metal Zn, or oxides containing Al and / or Zn, and are particularly preferably in powder form. The amount of Al and / or Zn to be added is preferably 1 to 10,000 ppm, more preferably 100 to 5,000 ppm, and even more preferably 200 to 3,000 ppm, based on the total amount of raw material Si.
[0027] (Spheroidization process) In one embodiment, when a thermal plasma method is used as a method for spheroidizing metal Si powder, it can be performed by applying, for example, any of DC arc plasma, high frequency plasma, microwave plasma, low frequency AC plasma, or a superposition of these plasmas, or plasma generated by an electrical method in which a magnetic field is applied to DC plasma, plasma generated by irradiation with a high output laser, or plasma generated by a high output electron beam or ion beam. In any case where any thermal plasma is used, it is preferable that the thermal plasma has a high temperature part of 10000 to 15000K, and in particular, that the plasma capable of controlling the generation time of fine particles is used. In one embodiment, it is preferable to supply a carrier gas in which the raw material powder is dispersed into a thermal plasma flame, and supply a cooling gas to the end of the thermal plasma flame to generate particles. From the viewpoint of the ease of formation of N-Si bonds on the surfaces of the spheroidized Si particles, which can improve the thermal conductivity of the spheroidized Si particles, it is preferable to use a plasma gas derived from a mixed gas of argon and nitrogen as the thermal plasma flame. When atomization is used as a method for spheroidizing metal Si powder, it can be performed by applying water atomization, gas atomization, centrifugal atomization, etc. For example, when gas atomization is used, a molten metal in which materials prepared to a desired composition are dissolved is sprayed with high-pressure gas, the parameters of which are set to obtain desired cooling conditions and particle size, to cause the molten metal to scatter and solidify, thereby obtaining powder.
[0028] (Classification process) The method for removing fine particles having a particle size of less than 1 μm from the spheroidized Si particles by classification is not limited, and can be performed by a commercially available wet or dry classification device, elutriation classification, etc. It is preferable to remove fine particles having a particle size of less than 1 μm using a wet classification device, and it is more preferable to remove fine particles having a particle size of 2 μm or less.
[0029] (Heat treatment) In one embodiment, the temperature of the heat treatment performed on the spheroidized metal Si particles is preferably 850°C or more and 1150°C or less, more preferably 875°C or more and 1150°C or less, and even more preferably 900°C or more and 1100°C or less. In one embodiment, from the viewpoint of the purity of the spheroidized metal Si particles, the spheroidized metal Si particles may be mixed with a powder containing Al and / or Zn and then heat treated. The heat treatment can be performed using a commercially available electric furnace under atmospheric pressure. The heat treatment is preferably performed for 4 hours or more and 16 hours or less under the above temperature conditions. By performing the heat treatment on the spheroidized metal Si particles, a shell layer of an oxide film is formed on the spheroidized metal Si particles, and a core-shell type Si particle filler is obtained. The obtained spherical core-shell type Si particle filler may be classified to remove fine particles. In this case, it is preferable to remove fine particles having a particle size of 1 μm or less, and more preferably to remove fine particles having a particle size of 2 μm or less.
[0030] [Resin composition] The resin composition according to the present embodiment contains a resin and the above-mentioned core-shell type Si particle filler. Details of the core-shell type Si particle filler are as described above. The content of the core-shell type Si particle filler in the resin composition is not particularly limited and can be appropriately adjusted according to the purpose. For example, when used in a heat dissipation member, the content may be in the range of 1 to 95 mass % relative to the total mass of the resin composition, more preferably in the range of 10 to 80 mass %, even more preferably in the range of 20 to 70 mass %, and particularly preferably in the range of 30 to 60 mass %.
[0031] (resin) The resin used in the resin composition according to the present embodiment is not particularly limited and can be appropriately selected according to the purpose. For example, polyethylene resin; polypropylene resin; epoxy resin; silicone resin; phenol resin; melamine resin; urea resin; unsaturated polyester resin; fluororesin; polyamide resin such as polyimide resin, polyamideimide resin, polyetherimide resin; polyester resin such as polybutylene terephthalate resin, polyethylene terephthalate resin; polyphenylene sulfide resin; wholly aromatic polyester resin; polysulfone resin; liquid crystal polymer resin; polyethersulfone resin; polycarbonate resin; maleimide modified resin; ABS resin; AAS (acrylonitrile-acrylic rubber-styrene) resin; AES (acrylonitrile-ethylene-propylene-diene rubber-styrene) resin; hydrocarbon elastomer resin; polyphenylene ether resin; aromatic polyene resin, etc. can be mentioned. These may be used alone or in combination of two or more. The resin composition according to this embodiment may contain a curing agent, a curing accelerator, a release agent, a coupling agent, a colorant, a flame retardant, an ion scavenger, etc., within the scope of not impairing the effects of the present invention.
[0032] The method for producing the resin composition is not particularly limited, and the resin composition can be produced by stirring, dissolving, mixing, and dispersing a predetermined amount of each material. The apparatus for mixing, stirring, dispersing, etc. of the mixture is not particularly limited, but a mortar and pestle machine equipped with a stirring and heating device, a three-roll mill, a ball mill, a planetary mixer, etc. can be used. These apparatuses may also be used in appropriate combination. EXAMPLES
[0033] The present invention will be described in more detail below with reference to examples, but the interpretation of the present invention is not limited to these examples.
[0034] A core-shell type Si particle filler was prepared by the following procedure. (1) Spheroidal metal Si particles The raw material spheroidized metal Si particles according to Examples 1-4 and Comparative Examples 1-5 shown in Table 1 were prepared as follows. Metal Si powder with a median diameter of 50 μm (high-purity silicon manufactured by Japan NER Co., Ltd.) was prepared, and each raw material metal Si powder was subjected to spheroidization treatment by a thermal plasma method using a plasma treatment device under the following conditions. In addition, when treating the raw material Si particles according to Example 3, an Si-Al-Zn alloy was used, which was prepared by adding 0.2 mass% metal Al and 0.2 mass% metal Zn to metal Si to prepare an ingot and pulverizing it to a median diameter of 50 μm. <Thermal plasma treatment conditions> Carrier gas type: Argon gas Plasma gas type: Mixture of argon (75% by volume) and nitrogen (25% by volume) ·Raw material supply rate: 0.6kg / hr High frequency output: 35kW 50 g of pure water was added to 50 g of metal silicon particles that had been subjected to thermal plasma treatment, and the mixture was treated in an ultrasonic bath (manufactured by Branson) for 2 minutes, then left to stand for 10 minutes and decanted. This process was repeated three times, and fine particles with a particle size of less than 1 μm were removed by elutriation. The resulting particles were dried at 120°C for 24 hours to obtain each type of spheroidized metal silicon particles. The Al and Zn contents of each of the obtained spheroidized metal Si particles were measured by quantitative analysis using an ICP spectrometer (manufactured by Agilent Technologies, product name: 5110VDV).
[0035] (2) Heat treatment Each of the spheroidized metal Si particles according to Examples 1-4 and Comparative Examples 1-5 was placed in an alumina crucible and heat-treated under atmospheric pressure in an air atmosphere furnace (Motoyama Corporation: hearth lift furnace) under the time and temperature conditions shown in Table 1 to obtain each of the core-shell type Si particle fillers according to Examples 1-4 and Comparative Examples 1-5. The following measurements were carried out on each of the obtained core-shell type Si particle fillers. Al and Zn content Atomic composition ratio (Al+Zn) / Si and O / Si Average circularity ·Specific surface area ·Average particle size ·Powder resistivity Fe and Al elution amount
[0036] [measurement] (Al and Zn content) The Al and Zn contents of each of the core-shell type Si particle fillers according to Examples 1-4 and Comparative Examples 1-5 were determined by quantitative analysis using an ICP emission spectrometer (ICP spectrometer: Agilent Technologies: 5110VDV).
[0037] (Atomic composition ratio (Al+Zn) / Si, and O / Si) The core-shell type Si particle fillers according to Examples 1-4 and Comparative Examples 1-5 were measured using an X-ray photoelectron spectrometer (Thermo Corporation: K-Alpha type X-ray photoelectron spectrometer), an Al-X-ray source with a monochromator, and a measurement area of 400×200 μm. The spectrum was then subjected to background removal by the Shirley method, and the Al 2s , Zn 3p , O 1s and Si 2s The semi-quantitative value was calculated from the peak intensity, and (Al 2s +Zn 3p) / Si 2s Ratio and O 1s / Si 2s The ratio was calculated.
[0038] (Average circularity) The core-shell type Si particle filler was fixed to the sample stage with carbon tape, and then osmium coating was performed. Then, an image taken with a scanning electron microscope [JEOL Ltd.: JSM-7001FSHL] at a magnification of 500 to 10,000 times and a resolution of 1280 x 1024 pixels was imported into a personal computer. This image was used with an image analyzer [Nippon Roper Co., Ltd.: Image-Pro Premier Ver. 9.3] to calculate the projected area (S) and projected perimeter (L) of the powder, and then the circularity was calculated using the following formula (1). The circularity was calculated for 200 random powders, and the average value was taken as the average circularity. Circularity = 4πS / L 2 (1)
[0039] (specific surface area) The core-shell type Si particle filler according to Examples 1-4 and Comparative Examples 1-5 was filled in a measurement cell with 3 g each, and the specific surface area was measured using a fully automatic specific surface area diameter measuring device [Macsorb HM model-1201 (BET single point method) manufactured by Mountech Co., Ltd.]. The degassing conditions before the measurement were 200°C and 10 minutes.
[0040] (Average particle size) The average particle diameter (D50, median diameter) of each core-shell type Si particle filler according to Examples 1-4 and Comparative Examples 1-5 was obtained by volume-based particle size distribution measurement by a laser diffraction scattering method using a particle size distribution measurement device [Beckman Coulter: LS 13 320]. In the measurement, 0.1 g of the core-shell type Si particle filler and 60 ml of pure water were mixed in an autosampler, and a dispersion treatment was performed for 60 seconds using an ultrasonic homogenizer [BRANSON: SFX250] as a pretreatment. The dispersion liquid that had been subjected to the dispersion treatment was added drop by drop to a laser diffraction type particle size distribution measurement device, and measurement was performed 30 seconds after the addition of a predetermined amount. The refractive index of pure water was 1.33, the refractive index of the core-shell type Si particle filler was 4.2, and the birefringence was 0.1.
[0041] (Powder resistivity) Using a resistivity meter [Loresta GP (powder resistivity measurement system MCP-PD51 type) manufactured by Mitsubishi Chemical Analytech Co., Ltd.], the powder resistivity of each of the core-shell type Si particle fillers according to Examples 1-4 and Comparative Examples 1-5 was measured by a four-probe method under conditions of 23°C, 40% relative humidity, and a load of 63.7 MPa. 5.0 g of each sample was prepared and used for the measurement.
[0042] (Fe and Al elution amount) Each of the core-shell type Si particle fillers according to Examples 1-4 and Comparative Examples 1-5 was immersed in a 6 mol / L hydrochloric acid aqueous solution at 25° C. for 2 hours. The hydrochloric acid aqueous solution after immersion was quantitatively analyzed using an ICP spectrometer (Agilent Technologies: 5110VDV) to calculate the amount of Fe and Al eluted from each of the core-shell type Si particle fillers.
[0043] In addition, the viscosity and thermal conductivity of the resin composition were measured as follows. (viscosity) 60% by volume of bisphenol A type liquid epoxy resin (epoxy equivalent: 184 to 194; JER828 manufactured by Mitsubishi Chemical Corporation) and 40% by volume of each of the core-shell type Si particle fillers according to Examples 1-4 and Comparative Examples 1-5 were mixed and kneaded with a planetary mixer (Thinky Corporation: Awatori Rentaro (registered trademark) AR-250, rotation speed 2000 rpm) to obtain each resin composition. The viscosity of each of these resin compositions at 25° C. was measured under the following conditions using a rotational rheometer (MCR-302, manufactured by Anton Paar). <Condition> Plate shape: circular flat plate 10mmφ Sample thickness: 1mm ·Temperature: 25±1℃ ·Shear rate: 1.0 / s
[0044] (Thermal Conductivity) Each core-shell type Si particle filler and spherical alumina filler according to Examples 1-4 and Comparative Examples 1-5 (mixture of "DAW-10", "DAW-03" and "ASFP-40" manufactured by Denka Co., Ltd.). (DAW-10):(DAW-03):(ASFP-40)=3 / 25 / 15 (volume ratio)) were mixed in a volume ratio of 57:43 to prepare a mixed powder. The mixed powder was filled into a bisphenol A type liquid epoxy resin (epoxy equivalent: 184-194. Mitsubishi Chemical Co., Ltd.: JER828) so that the ratio of the mixed powder was 75% by volume, and kneaded with a planetary mixer (Thinky Co., Ltd.: Awatori Rentaro (registered trademark) AR-250, rotation speed 2000 rpm). The mixture obtained was poured into a silicone mold (2 cm square x 6 mm thick) that had been preheated to 80°C, and press-heated and cured in a vacuum heating press (Imoto Manufacturing Co., Ltd.: IMC-1674-A model) at 80°C / 1 hour / 3 kN, 150°C / 1 hour / 5 kN, and 200°C / 0.5 hour / 7 kN in that order, to obtain a resin composition. The thermal conductivity H (unit: W / (m K)) of a resin composition is calculated by multiplying its thermal diffusivity T (unit: m 2 / s]), density D (unit [kg / m 3The thermal diffusivity was calculated from the measured values of the thermal conductivity (H) and specific heat capacity C (unit: [J / (kg K)]) according to the formula H=T×D×C. The cured resin composition was processed into a disk sample with a diameter of 10 mm and a thickness of 1 mm, and the thermal diffusivity was measured by the laser flash method. A xenon flash analyzer (NETZSCH: LFA447 NanoFlash) was used as the measuring device. The specific gravity was measured using the Archimedes method. The specific heat was measured using a differential scanning calorimeter (NETZSCH: DSC214). The above results are shown in Table 1.
[0045] [Table 1]
[0046] As shown in Table 1, the core-shell type Si particle filler according to Example 1-4, which has a shell layer containing Al, Zn and O on the surface of the metal Si core particle, has an Al elution amount of 3 ppm or less when immersed in a 6 mol / L hydrochloric acid aqueous solution at 25 ° C. for 2 hours, and therefore has excellent chemical stability, particularly acid resistance, and it was found that a resin composition having excellent chemical stability, particularly acid resistance, can be obtained when blended with a resin. On the other hand, the resin composition using the core-shell type Si particle filler according to Comparative Example 1-5 has an Al elution amount of 4 ppm or more when immersed in a 6 mol / L hydrochloric acid aqueous solution at 25 ° C. for 2 hours, and therefore does not satisfy the configuration of the present invention. It can be said that the resin composition using the core-shell type Si particle filler according to Comparative Example 1-5 is inferior in chemical stability, particularly acid resistance, to the resin composition using the core-shell type Si particle filler according to Example 1-4. From the above results, it has been confirmed that the core-shell type Si particle filler according to this embodiment has excellent chemical stability, particularly acid resistance, and therefore, when blended with a resin, a resin composition having excellent chemical stability, particularly acid resistance, can be obtained.
Claims
1. A core-shell type Si particle filler having a shell layer containing Al, Zn and O on the surface of a metal Si core particle, in which the amount of Al eluted is 3 ppm or less when immersed in a 6 mol / L hydrochloric acid aqueous solution at 25° C. for 2 hours.
2. 2. The core-shell type Si particle filler according to claim 1, which has an amount of Fe eluted of less than 2 ppm when immersed in a 6 mol / L aqueous hydrochloric acid solution at 25° C. for 2 hours.
3. 3. The core-shell type Si particle filler according to claim 1, wherein the atomic composition ratio (Al+Zn) / Si analyzed by X-ray photoelectron spectroscopy is 0.015 or more and 0.075 or less.
4. 3. The core-shell type Si particle filler according to claim 1, wherein the atomic composition ratio (Al+Zn) / Si analyzed by X-ray photoelectron spectroscopy is 0.02 or more and 0.07 or less.
5. 3. The core-shell type Si particle filler according to claim 1, having an average circularity of 0.70 or more.
6. Specific surface area is 1.0 m 2 The core-shell type Si particle filler according to claim 1 or 2, wherein the surface area of the core-shell type Si particle filler is 0.1 μm or less.
7. A resin composition comprising a resin and the core-shell type Si particle filler according to claim 1 or 2.
Citation Information
Patent Citations
Magnetite particle
JP2010222154A
High thermal conductor and manufacturing method therefor
JP2015108066A
Production of Si / C composite particles
JP2019528227A
Labeling inorganic nanoparticle agent
WO2010004777A1
Method for producing silicon-containing particles for anode active material for non-aqueous electrolyte secondary battery, anode member for non-aqueous electrolyte secondary battery, non-aqueous electrolyte secondary battery, and silicon-containing particles for anode active material for non-aqueous electrolyte secondary battery
WO2014073155A1