Hydroxyapatite porous structure and production method of the same

A simple acid-hydrolysis method for α-TCP molded bodies creates a hydroxyapatite porous structure with a flaky surface layer and network interior, addressing the complexity of existing methods and achieving high biocompatibility and mechanical strength for bone applications.

JP2024138891APending Publication Date: 2024-10-09NATIONAL INSTITUTE OF ADVANCED INDUSTRIAL SCIENCE & TECHNOLOGY
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023049607
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

Existing methods for producing hydroxyapatite porous structures are complex and do not efficiently create large, biocompatible crystal grains with high porosity and mechanical strength.

Method used

A method involving the acid-hydrolysis of α-TCP molded bodies to form a flaky texture surface layer and network structure in hydroxyapatite, using a simple process without hydrothermal treatment, resulting in a porous structure with a 'card house' structure and graded material properties.

Benefits of technology

The method produces a hydroxyapatite porous structure with excellent biocompatibility, high porosity, and mechanical strength, suitable for bone integration and load-bearing applications, while maintaining the shape of the original mold.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138891000001_ABST
    Figure 2024138891000001_ABST
Patent Text Reader

Abstract

To provide: a porous structure consisting of hydroxyapatite, which is obtained by a simple method and is excellent in biocompatibility; and a production method thereof.SOLUTION: There is disclosed a porous structure consisting of hydroxyapatite and having, in a surface layer portion, a flake aggregate structure in which flake-like particle pieces oriented in a c-plane are bonded to each other with their side portions and face portions abutted on each other. The production method includes a step to immerse a molded body containing a powder composed of α-TCP in a hydrochloric acid aqueous solution to perform acid hydrolysis.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a porous structure made of hydroxyapatite and a method for producing the same. [Background technology]

[0002] Hydroxyapatite (HA) tends to grow in the c-axis direction, forming hexagonal columnar or plate-shaped crystal grains. However, in general, the crystal grains do not grow to large sizes, and are hydrothermally treated to form relatively large needle-shaped crystal grains.

[0003] For example, Patent Document 1 discloses a method for producing needle-shaped polycrystalline HA consisting of an aggregate of primary crystals selectively grown on the c-plane, in which a calcium phosphate slurry or solution containing an additive selected from hydroxycarboxylic acids or aminocarboxylic acids that form complexes with calcium and with a Ca (calcium) / P (phosphorus) ratio adjusted to 3.0 or more is subjected to hydrothermal treatment at a temperature above the boiling point, for example 165°C, under saturated water vapor pressure.

[0004] Patent Document 2 discloses a method for producing a plate-shaped HA single crystal with a c-plane orientation. 2+ Ion, PO4 3- When an acidic aqueous solution containing ions, urea, and urease is prepared and placed in a container and kept in gas-liquid contact with the outside air, HA crystal nuclei are generated as the pH of the solution rises due to hydrolysis of urea by urease, and crystals grow in the a-axis and b-axis directions.The precipitate floating in the solution is then separated and collected from the solution, and subjected to hydrothermal treatment at about 120℃, resulting in plate-shaped HA single crystals. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 10-236806 [Patent Document 2] JP 2010-208896 A Summary of the Invention [Problem to be solved by the invention]

[0006] Meanwhile, HA, which has excellent biocompatibility and porosity, is used in various biomaterials. Therefore, it is considered to form a porous structure by assembling the crystal-grown HA as described above. Here, a method for obtaining a porous structure made of HA more easily is required.

[0007] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a porous structure made of hydroxyapatite that can be obtained by a simple method and has excellent biocompatibility, and a method for producing the same. [Means for solving the problem]

[0008] The porous structure made of hydroxyapatite according to the present invention is characterized in that it has a flake texture in its surface layer, which is formed by bonding together c-plane oriented flake-like particle pieces by butting their sides and faces together.

[0009] According to such characteristics, the surface layer has a highly porous flake aggregate structure having spaces separated by flake-like particle fragments, a so-called house of cards structure, which provides excellent strength against porosity and excellent biocompatibility.

[0010] In the above-mentioned invention, a mesh-like structure in which spaces are formed in a mesh shape may be provided in the lower part of the surface layer. According to this feature, the mesh-like structure in which spaces are formed in a mesh shape before developing into a flake shape has a strength and porosity different from those of the surface layer, and a gradient material is provided.

[0011] The method for producing a porous structure made of hydroxyapatite according to the present invention is characterized in that a molded body containing a powder of α-TCP is immersed in an aqueous hydrochloric acid solution for acid hydrolysis to produce a porous structure having a flake texture in the surface layer portion, in which flake-like particle pieces made of c-plane oriented hydroxyapatite are butted together at their sides and faces to be fixed together.

[0012] According to this feature, a porous structure having a so-called house of cards structure on the surface and excellent biocompatibility can be easily obtained without using a heating process such as hydrothermal treatment.

[0013] In the above-mentioned invention, the molded body may be a dried gel. Furthermore, the molded body may be obtained by mixing the powder made of α-TCP with an aqueous sodium alginate solution, exposing it to an aqueous calcium chloride solution to gel it, molding it, and then drying it. According to this feature, a porous structure having excellent biocompatibility can be easily obtained regardless of the shape.

[0014] In the above-mentioned invention, the pH of the hydrochloric acid aqueous solution may be 2 to 4. According to this feature, a porous structure having excellent biocompatibility can be obtained stably and easily. [Brief description of the drawings]

[0015] [Figure 1] FIG. 2 is a diagram of a porous structure according to the present invention. [Diagram 2] 2 is a SEM photograph of a porous structure according to the present invention. [Diagram 3] FIG. 1 illustrates a house of cards structure. [Figure 4] This is a diffraction profile of a particle fragment by powder X-ray diffraction. [Diagram 5] 1 is a SEM photograph of the vicinity of the center of a porous structure. [Figure 6] 1 is a table showing the results of a compression test. [Figure 7] 1 is a SEM photograph of HA obtained from α-TCP powder, which is a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, a porous structure made of hydroxyapatite (HA) and a method for producing the same, which is one embodiment of the present invention, will be described with reference to FIGS. 1 to 5. FIG.

[0017] As shown in Fig. 1, the porous structure 1 is typically a granular material having a structural difference, such as a surface layer 1a having a flake texture and a central portion 1b having a mesh-like texture therebelow, and is, for example, approximately spherical. As will be described later, it is also possible for the central portion 1b to have a flake texture similar to the surface layer 1a.

[0018] As shown in FIG. 2, the surface layer 1a has a flake texture formed by c-plane oriented flaky (plate-like) particle pieces 2. That is, the particle pieces 2 have a c-plane wider than the a-plane, and are plate-like bodies with the c-plane as the main surface. Such flake texture forms a porous structure with high porosity, so-called a house of cards structure, in which the side (peripheral) part of a particle piece 2 is connected and fixed to the face (flat) part of another particle piece 2 by butting it against each other, and the spaces are divided by the flaky particle pieces. That is, the particle pieces 2 are fixed without overlapping their main surfaces. The particle pieces 2 are plate-like bodies based on a hexagonal crystal structure of single crystal HA.

[0019] Also, as shown in FIG. 3, the particle piece 2 partially has a gusset-like structure. For example, the particle piece 2-1 abuts its side portion 2-1r against the surface portion 2-2f of the particle piece 2-2. The particle piece 2-3 connects the opposing positions of its side portion 2-3f to the surface portion 2-1f of the particle piece 2-1 and the surface portion 2-2f of the particle piece 2-2. In other words, the connection angle between the particle piece 2-1 and the particle piece 2-2 is fixed by the particle piece 3-3 interposed therebetween. The porous structure 1 has high mechanical strength as described later, and it is believed that this structure is the cause of this.

[0020] Furthermore, as shown in Fig. 4, the X-ray diffraction profile of particle piece 2 obtained by powder X-ray diffraction shows that the strongest peak is located near 2θ = 25 to 27° originating from the c-plane (0,0,2), and there is also a clear peak located near 31 to 32.5° originating from the a-plane (3,0,0). In other words, particle piece 2 is considered to be a crystal in which the c-plane is wider than the a-plane, and it can be said that the c-plane is oriented as described above.

[0021] On the other hand, as shown in Fig. 5, the central portion 1b, which is the lower part of the surface layer portion 1a, has a mesh-like structure in which the polycrystalline hydroxyapatite has spaces in a mesh-like pattern. The central portion 1b also contains a plate-like structure similar to that of the surface layer portion 1a, but it is a continuous mesh-like structure, unlike the connected structure of the particle pieces 2. This structure is thought to be a structure in a preliminary stage in which the hydroxyapatite grows into c-plane-oriented flaky (plate-like) particle pieces 2, like the house-of-cards structure of the surface layer portion 1a.

[0022] For example, when HA is used as an artificial bone, since HA itself does not have bone formation function, it is important to incorporate the bone formation environment (osteoblasts, bone formation factors, etc.), which is mainly a liquid component, near its surface in order to allow it to heal with bone. The porous structure 1 has a card house structure in the surface layer 1a, and therefore has a certain level of mechanical strength despite its high porosity, can effectively incorporate the bone formation environment, and has excellent adhesion to bone. In other words, it has excellent biocompatibility.

[0023] Moreover, the porous structure 1 can be made into a granular body as described above, and by using it to fill a defect in a bone, etc., it can be arranged with good adhesion according to the shape of the defect, etc. In addition, since the porous structure 1 has excellent mechanical strength as described later, it is also suitable for application to sites where a load is applied.

[0024] Next, a method for producing the porous structure 1 will be described. The porous structure 1 can be produced by hydrolyzing α-TCP (monoclinic tricalcium phosphate) formed into a desired shape through gelation in an acidic aqueous solution, thereby simultaneously causing dissolution and precipitation. Specifically, the method is as follows.

[0025] First, α-TCP powder is mixed with a 1% sodium alginate aqueous solution to obtain a slurry. The mass ratio of α-TCP in the slurry is 50% or less. Next, the slurry is dripped and exposed to a 1% calcium chloride aqueous solution to gel, for example, to obtain gel beads formed into a spherical shape. Note that other methods may be used to obtain gelled beads. The obtained gel beads are kept at 60°C for 24 hours and dried. This results in a molded product of α-TCP gel formed into a spherical shape.

[0026] The α-TCP molded body is immersed in an acidic aqueous solution adjusted to pH 2.5 and kept in the range of room temperature to 40°C, for example, and left to stand or shaken. The immersion time was set to 24 hours here. If the immersion time is shortened, the thickness of the surface layer 1a having a house-of-cards structure can be made thinner and the central part can remain α-TCP. On the other hand, if the immersion time exceeds a certain time, the thickness of the surface layer 1a and the thickness of the central part 1b will be a given value, but if the immersion time is longer, the entire body can become a house-of-cards structure.

[0027] The pH of the acidic aqueous solution is preferably adjusted by adding hydrochloric acid to ultrapure water. Although acids other than hydrochloric acid can be used, the acid should not contain elements that inhibit the precipitation of HA (e.g., magnesium, zinc, etc.). The pH of the acidic aqueous solution is within the range of pH2 to pH4, preferably pH2 to pH3, allowing for fluctuations due to the ingress of carbon dioxide from the atmosphere, desorption into the atmosphere, and errors in measuring instruments. In addition, the mixture ratio is preferably such that the pH is 6 or higher when the α-TCP molded body is immersed and dissolved, and for example, the mass ratio of the α-TCP molded body to the acidic aqueous solution is 20:1 (500g:25g).

[0028] During this immersion, α-TCP is dissolved by acid hydrolysis and precipitates to become HA. When α-TCP is dissolved, the concentrations of phosphate and calcium in the acidic aqueous solution are increased, changing the pH to about 6. The dissolved α-TCP then precipitates to become HA. The resulting precipitate is suction filtered and washed to obtain porous structure 1 made of HA. Note that dissolution and precipitation are thought to proceed simultaneously, and porous structure 1 is formed while maintaining most of the shape of the α-TCP compact.

[0029] During acid hydrolysis of α-TCP, the following three reactions are thought to occur: a)Ca3(PO4)2+4H2O→2CaHPO4·2H2O+Ca(OH)2 b)3Ca3(PO4)2+7H2O→CaHPO4·5H2O+Ca(OH)2 c) (10-z) Ca3(PO4)2+3(2+nz)H2O →3Ca 10-z (HPO4) z (PO4) 6-z (OH) 2-z nH2O +2(1-z)H3PO4

[0030] Since the pH value increases when the α-TCP is dissolved, it is presumed that among these reaction formulas, a) and b) are predominantly progressing on the surface of the molded α-TCP body. In this example, in addition to hydrolysis, dissolution of α-TCP by the acid and dissolution of calcium hydrogen phosphate dihydrate (DCPD) produced by hydrolysis may also occur, and some of them are thought to be ionized. In addition, the concentrations of phosphorus and calcium are thought to increase due to the acid. All of these promote the precipitation of HA, and it is thought that even if the dissolution of α-TCP progresses due to these factors, the shape of the molded body can be maintained due to the precipitation of HA that occurs at the same time.

[0031] On the other hand, HA precipitation consumes Ca(OH)2, and HA precipitation can also occur according to reaction c), which means that HA precipitation lowers the pH value.

[0032] In this way, a reaction cycle can occur: 1) pH is raised by promoting the dissolution of α-TCP, 2) raising the pH promotes the precipitation of HA, 3) pH is lowered by precipitating HA, and 4) pH is lowered to promote the dissolution of α-TCP. As cycles 1) to 4) are repeated locally, the dissolution of α-TCP and the precipitation of HA proceed simultaneously overall, and it is believed that the reaction can proceed while maintaining the shape of the molded body.

[0033] In the case of α-TCP molded by drying the gel, it is believed that the drying process makes the density of the α-TCP powder higher inside the molded body than on the surface. When the powder density is high, many HA precipitation nuclei are formed at the same time, and due to the pinning effect, the crystals cannot grow large. On the other hand, on the surface where the powder density is low, these effects are small, so it is believed that the crystals can grow large.

[0034] In addition, the above-mentioned hydrolysis and other reactions should start from the surface of the molded body. It is thought that the crystals that quickly become HA near the surface can grow larger by consuming phosphorus and calcium supplied by the dissolution of α-TCP. On the other hand, in the interior, which is far from the acidic aqueous solution, the above-mentioned cycle of dissolution and precipitation is relatively slow, and as a result, it is thought that HA only grows to relatively small crystals.

[0035] It is believed that the above-mentioned mechanism enables the porous structure 1 to form the surface layer portion 1a made of a flake texture and the central portion 1b made of a mesh-like texture underneath.

[0036] In this way, the porous structure 1 can be manufactured. That is, the porous structure 1 can be obtained by a simple manufacturing method in which a powder made of α-TCP is molded into various shapes and then immersed in an acid aqueous solution and subjected to acid hydrolysis. As described above, the porous structure 1 can be obtained while maintaining the shape of the molded body of α-TCP, so that the porous structure 1 can be obtained in a relatively free shape. For example, a molded body can be obtained by filling a mold with a large number of granulated gels to obtain a desired shape, or a sol containing α-TCP powder can be poured into such a mold and dried to obtain a molded body. Note that, as the molded body, a molded body other than a dried gel body, such as ceramics obtained by firing α-TCP powder, can also be used.

[0037] Next, the porous structure 1 was manufactured by the above-mentioned manufacturing method, and its characteristics were investigated. Here, 3 μL of a slurry with a mass ratio of α-TCP of 30% was dropped to form gel beads, which were then dried to obtain α-TCP spheres. The spheres were then immersed in an acid solution (hydrochloric acid solution at 40°C and pH 2.5) in a sealed container and shaken (5 × 10 rpm) for 24 hours to obtain the porous structure 1.

[0038] The resulting porous structure 1 had a card house structure as described above, and its porosity was measured to be 41.9%.

[0039] The solubility of the porous structure 1 was also evaluated. In detail, when one piece of the porous structure 1 (3 μL of slurry) was immersed in 0.1 mL of 1% agarose gel, it was confirmed that the pH was less than 7 and on the acidic side even after 25 days. When HA dissolves, it increases the pH and makes the solution alkaline. For example, when commercially available sintered powder of HA (HAP-100 / manufactured by Taihei Chemical Industry Co., Ltd.) was similarly immersed in agarose gel, the pH exceeded 7. In other words, it can be said that the solubility of the porous structure 1 is relatively low.

[0040] 6, a compression fracture test was carried out on the porous structure 1, its sintered body, and the dried body of α-TCP. The porous structure 1 was shown in Examples 1 to 5. The dried body of α-TCP was a spherical body of α-TCP, which is a dried body of the gel beads described above, and was shown in Comparative Examples 1 to 5. In the sintered body of the porous structure 1, HA was converted to α-TCP by heating, and it was shown as a sintered body of α-TCP in Comparative Examples 6 to 10.

[0041] Compression tests were performed on the particles of each of Examples 1 to 5 and Comparative Examples 1 to 10, and the maximum load until destruction was recorded. As a result, it was found that the porous structures of Examples 1 to 5 have mechanical strengths about six times that of the dried α-TCP bodies of Comparative Examples 1 to 5, and equivalent to the sintered α-TCP bodies of Comparative Examples 6 to 10. The sintered α-TCP bodies of Comparative Examples 6 to 10 had a porosity of 15%, and were close to a solid structure. In addition, the mechanical strength of the porous structure 1, which has a card house structure, is higher than that of the structures of Comparative Examples 6 to 10, and considering the porosity, it can be said that a higher specific strength can be obtained. It is believed that the reason why the mechanical strength can be increased in this way is mainly due to the mesh-like structure, especially in the central portion 1b.

[0042] For comparison, as shown in Figure 7, α-TCP in powder form without being molded was immersed in an acidic aqueous solution in the same manner as above to produce HA. It can be seen from the figure that even if HA was produced from powdered α-TCP in the same way, it did not result in a porous structure. Here, although plate-like HA was observed, the C-face was narrow and the overall product was in the form of fine particles. Compared to the molded product, the contact area with the acidic aqueous solution was larger and the reaction was faster, so it is thought that the particles grew less and became HA crystals while remaining finely divided.

[0043] Although the representative embodiments of the present invention have been described above, the present invention is not necessarily limited thereto, and a person skilled in the art will be able to find various alternative embodiments and modifications without departing from the spirit of the present invention or the scope of the appended claims. [Explanation of symbols]

[0044] 1 Porous structure 1a Surface layer 1b Central part (lower part of the surface layer) 2 particle pieces

Claims

1. A porous structure made of hydroxyapatite, A porous structure characterized in that a flake texture is formed in a surface layer portion thereof, the flake-like particle pieces being c-plane oriented and bonded together by butting their sides and faces against each other.

2. 2. The porous structure according to claim 1, further comprising a mesh-like structure in which spaces are formed in a mesh pattern in the lower part of said surface layer.

3. A molded body containing powder made of α-TCP is immersed in an aqueous hydrochloric acid solution to perform acid hydrolysis. A method for producing a porous structure, characterized in that a porous structure having a flake texture in a surface layer portion is obtained by butting together and fixing together flaky particle pieces made of c-plane oriented hydroxyapatite at their sides and faces.

4. 4. The method for producing a porous structure according to claim 3, wherein the molded body is a gel body.

5. The method for producing a porous structure according to claim 4, characterized in that the molded body is obtained by mixing the powder made of α-TCP with an aqueous sodium alginate solution, gelling the mixture by exposing the mixture to an aqueous calcium chloride solution, and then drying the mixture.

6. 6. The method for producing a porous structure according to claim 3, wherein the pH of the aqueous hydrochloric acid solution is 2 to 4.

Citation Information

Patent Citations

  • High-mechanical-property tetracalcium phosphate nano-powder for 3D printing and preparation method thereof

    CN112607719A

  • Calcium phosphate nanoparticle and producing method therefor

    JP2006008429A

  • Porous body of calcium phosphate-based shaped body and its production method

    JP2009084147A

  • Method of manufacturing plate-like hydroxyapatite single crystal

    JP2010208896A

  • Hydroxyapatite composite for use in removal of contaminants from effluents and methods of making

    US20200385270A1