Diamond abrasive grains, powder material, and method for manufacturing diamond abrasive grains
By introducing internal stress through heat treatment in an oxidizing atmosphere, diamond abrasive grains with a compressive strain of 0.3 to 0.9 are developed, addressing inefficiencies in processing difficult materials by maintaining sharp edges and improving machining efficiency.
Patent Information
- Application Number
- JP2023050141
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
AI Technical Summary
Existing diamond abrasive grains lack the appropriate microfragility and compressive strain to efficiently process difficult-to-grind materials like SiC, leading to inefficient machining and rapid wear.
Diamond abrasive grains with a compressive strain of 0.3 to 0.9, containing dopants with higher thermal expansion coefficients, are heat-treated in an oxidizing atmosphere at 200°C to 900°C to introduce internal stress, enhancing microfragility and maintaining sharp cutting edges.
The improved diamond abrasive grains exhibit increased microfragility, leading to enhanced processing efficiency and sustainability during grinding and polishing of materials like SiC.
Smart Images

Figure 2024139273000007 
Figure 2024139273000001 
Figure 2024139273000002
Abstract
Description
[Technical field]
[0001] The technology disclosed herein relates to diamond abrasive grains, powder materials, and methods for making diamond abrasive grains. [Background technology]
[0002] In recent years, diamond abrasive grains have been widely used for grinding various materials. For example, diamond abrasive grains are used to manufacture machining tools (vitrified grinding wheels, etc.) for grinding hard-to-grind materials such as SiC (see Patent Document 1). These diamond abrasive grains are required to have appropriate micro-friability depending on the object to be processed. For example, diamond abrasive grains that frequently break down on a microscopic scale during processing (high micro-friability) have excellent machining efficiency because they can maintain a sharp cutting edge.
[0003] It is known that diamond abrasive grains tend to fracture as their internal stress (tensile stress) increases. Here, the internal stress of diamond abrasive grains can be evaluated based on Raman spectroscopy. Specifically, when the Raman spectrum of diamond abrasive grains is obtained, a peak due to the lattice vibration of diamond crystals is observed at 1333 cm -1 The Raman peak position is confirmed near the center of the diamond abrasive grain. The diamond abrasive grain has the Raman peak position shifted to the low wavenumber side by the introduction of internal stress or the incorporation of impurities into the crystal. Non-Patent Document 1 reports that the diamond abrasive grain to which internal stress has been introduced by heat treatment has a Raman peak position shifted to the low wavenumber side, improving micro-fracturability. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2017-80847 A [Non-patent literature]
[0005] [Non-Patent Document 1] Hitoshi Kakutani et al., "Internal Strain Distribution and Microfracture Behavior of Various Single Crystal Diamonds for Cutting Tools," Proceedings of the JSPE Spring Meeting, Academic Lecture Series, 2019, P644-P645 Summary of the Invention [Problem to be solved by the invention]
[0006] However, in recent years, with the increase in demand for semiconductor wafers, there is a demand for highly efficient grinding and polishing of difficult-to-grind materials such as SiC. The technology disclosed here has been made in response to such demand, and aims to provide a diamond abrasive grain that can be broken at an appropriate frequency during processing and maintain a sharp cutting edge. [Means for solving the problem]
[0007] The diamond abrasive grain disclosed herein has a compressive breaking point strain of 0.3 or more and 0.9 or less. As a result of various studies and experiments, the inventor has succeeded in realizing diamond abrasive grains having this very high compressive breaking point strain. As will be described in detail later, the compressive breaking point strain of general diamond is 0.1 or less, and at most less than 0.25. In other words, diamond abrasive grains having a high compressive breaking point strain of 0.3 or more have not yet been reported. And, since the diamond abrasive grains of this configuration have very excellent micro-fracturability, a sharp cutting edge is easily formed during processing. Therefore, the diamond abrasive grains disclosed herein can exhibit excellent processing efficiency.
[0008] In one embodiment of the diamond abrasive grain disclosed herein, a dopant other than carbon element is contained. This makes it easier to introduce internal stress into the diamond abrasive grain in the heat treatment process described below, so that the micro-crushability can be improved more suitably. The content of the dopant relative to the total weight of the diamond abrasive grain is preferably 0.1wt% or more. This makes it easier to introduce strong internal stress into the diamond abrasive grain in the heat treatment process. Furthermore, the thermal expansion coefficient of this dopant is preferably higher than that of the diamond abrasive grain. This makes it easier to introduce internal stress.
[0009] In one embodiment of the diamond abrasive grains disclosed herein, the compressive fracture strength is 1.5 Gpa or more and 4.0 Gpa or less, which allows the diamond abrasive grains to have a high level of both processability and micro-friability.
[0010] In one embodiment of the diamond abrasive grains disclosed herein, the compression fracture test force is 6.5 N or more and 20 N or less. This allows the diamond abrasive grains to have a high level of both processability and micro-friability.
[0011] In one embodiment of the diamond abrasive grains disclosed herein, the compressive fracture stress is 3 GPa or more and 10 GPa or less, which allows the diamond abrasive grains to have a high level of both processability and micro-fracturability.
[0012] In one embodiment of the diamond abrasive grains disclosed herein, the diamond abrasive grains have a Raman spectrum of 1325 cm -1 From 1334cm -1 The average peak position of the Raman peaks that exist in the range of 1329.5 cm -1 This further improves the micro-crushing properties of the diamond abrasive grains.
[0013] In one embodiment of the diamond abrasive grains disclosed herein, the diamond abrasive grains have a Raman spectrum of 1325 cm -1 From 1334cm -1 The average half-width of the Raman peaks is 4.5 cm -1 This makes it possible to improve the durability of the diamond abrasive grains.
[0014] The diamond abrasive grains disclosed herein are used, for example, in SiC machining tools, which can efficiently machine SiC because the cutting edges of the abrasive grains are easily maintained in a sharp state.
[0015] In addition, as another aspect of the technology disclosed herein, a powder material containing a plurality of diamond abrasive grains is provided. In this powder material, the average value of the compression fracture point strain of the diamond abrasive grains is 0.3 or more and 0.8 or less. Since the powder material of this configuration contains diamond abrasive grains with excellent micro-fracturability, it can efficiently process difficult-to-grind materials such as SiC.
[0016] In one embodiment of the powder material disclosed herein, the number of diamond abrasive grains having a compressive fracture strain of 0.2 or more and 0.9 or less is 50% or more by number. Since the diamond abrasive grains having excellent micro-fracturability account for more than half of the abrasive grains in this powder material, it can exhibit even better processability.
[0017] In addition, as another aspect of the technology disclosed herein, a method for manufacturing diamond abrasive grains is provided. The manufacturing method includes a heat treatment step of heating diamond abrasive grains at a temperature of 200°C or more and 900°C or less. According to an experiment conducted by the present inventor, by carrying out heat treatment under the above-mentioned conditions, diamond abrasive grains having a compressive fracture strain of 0.3 or more and 0.9 or less can be manufactured.
[0018] In one embodiment of the manufacturing method disclosed herein, the heating atmosphere in the heat treatment process is an oxidizing atmosphere.The heat treatment of general diamond abrasive grains is carried out in an inert atmosphere to prevent the oxidation of diamond.However, in the experiment carried out by the present inventor, it has been confirmed that when diamond abrasive grains are heated in an oxidizing atmosphere, the compression fracture point strain of the abrasive grains after heating increases rapidly, and the micro-fracturability is significantly improved.
[0019] In one embodiment of the manufacturing method disclosed herein, the heating temperature in the heat treatment step is 400° C. or higher and 600° C. or lower, which makes it easier to manufacture diamond abrasive grains having a high compressive fracture strain.
[0020] In one embodiment of the manufacturing method disclosed herein, the diamond abrasive grains contain a dopant other than carbon element. This makes it easier to introduce internal stress into the diamond abrasive grains, so that the micro-crushing property can be improved more suitably. In addition, the content of the dopant relative to the total weight of the diamond abrasive grains is preferably 0.1wt% or more. This makes it easier to introduce strong internal stress into the diamond abrasive grains in the heat treatment process. Furthermore, the thermal expansion coefficient of the dopant is preferably higher than that of the diamond abrasive grains. This makes it easier to introduce internal stress. [Brief description of the drawings]
[0021] [Figure 1] FIG. 1 is a graph showing the results of a SiC grinding test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] An embodiment of the technology disclosed herein will be described below. Matters other than those specifically mentioned in this specification and necessary for implementing the technology disclosed herein can be understood as design matters of a person skilled in the art based on the conventional technology in the field. The technology disclosed herein can be implemented based on the contents disclosed in this specification and the technical common sense in the field. In this specification, the expression "A to B" indicating a numerical range means "A or more and B or less" unless otherwise specified. The drawings are drawn diagrammatically, and the dimensional relationships (length, width, thickness, etc.) in the drawings do not reflect the actual dimensional relationships.
[0023] <Diamond abrasive grains> The diamond abrasive grains disclosed herein will be described below. The diamond abrasive grains are diamond particles having a predetermined hardness. The diamond abrasive grains may be natural diamond or artificial diamond.
[0024] The diamond abrasive grain disclosed herein has a compressive fracture point strain of 0.3 or more. This compressive fracture point strain is the ratio of fracture point displacement to sample height (fracture point displacement / sample height). These sample height and fracture point displacement can be measured by observing the sample with a camera or a microscope or by a displacement sensor of a compression fracture tester, respectively. As the compressive fracture point strain increases, the micro-fracturability of the diamond abrasive grains tends to improve. Specifically, when a diamond abrasive grain is pressurized in a specific direction, it breaks after a certain amount of displacement (deformation) along the pressure direction. Here, the compressive fracture point strain is a parameter obtained by dividing the fracture point displacement, which indicates the physical property of how much displacement is required to cause fracture, by the size (sample height) of the abrasive grains. Abrasive grains with a large compressive fracture point strain have the property of being easily micro-fractured. Abrasive grains with high micro-fracturability generally tend to have high processing efficiency, and this tendency is particularly noticeable in grinding difficult-to-grind materials. Here, the compressive fracture point strain of a typical diamond is 0.1 or less, and at most less than 0.25. Therefore, it can be said that the diamond abrasive grains disclosed herein have a significantly improved micro-fracturability compared to conventional abrasive grains. The means for realizing diamond abrasive grains with such a large compression failure point strain will be described later. The compression failure point strain of the diamond abrasive grains disclosed herein is preferably 0.33 or more, and particularly preferably 0.35 or more. This can further improve the micro-fracturability of the diamond abrasive grains. On the other hand, if the compression failure point strain becomes too large (too high micro-fracturability), it can be a factor in reducing the durability of the abrasive grains. From this perspective, the upper limit of the compression failure point strain of the diamond abrasive grains disclosed herein is set to 0.9 or less (preferably 0.85 or less, more preferably 0.82 or less).
[0025] In addition, the compressive fracture strength of the diamond abrasive grains disclosed herein is preferably 1.5 Gpa or more, more preferably 1.8 Gpa or more, even more preferably 2.5 Gpa or more, and particularly preferably 2.8 Gpa or more. This compressive fracture strength indicates the pressure at which the abrasive grains break when pressure is applied along a predetermined direction. The fact that the compressive fracture strength is large in the diamond abrasive grains having the above-mentioned compressive fracture point strain means that the abrasive grains are not easily broken completely even when micro-fracture is repeated. That is, in the diamond abrasive grains disclosed herein, when the compressive fracture strength is large, the processing durability during grinding and polishing tends to improve. On the other hand, the compressive fracture strength of the diamond abrasive grains is preferably 4.0 Gpa or less, more preferably 3.5 Gpa or less, and particularly preferably 3.3 Gpa or less. This allows the diamond abrasive grains to be micro-fractured at a certain frequency, so that the processing efficiency can be further improved. In addition, the "compressive fracture strength" in this specification is a value calculated based on the calculation formula of JIS R1639-5.
[0026] In addition, the compression failure point test force of the diamond abrasive grain is preferably 6.5N or more, more preferably 7.0N or more, even more preferably 7.2N or more, and particularly preferably 7.3N or more. This compression failure point test force indicates the load at which the diamond abrasive grain breaks when a load is applied to the diamond abrasive grain. Abrasive grains with a large compression failure point strain and this compression failure point test force also have the property that the abrasive grains are not completely broken even while repeatedly undergoing micro-fracture. That is, in the diamond abrasive grains disclosed herein, when the compression failure point test force is large, the processing durability during grinding and polishing tends to improve. On the other hand, the compression failure point test force of the diamond abrasive grain is preferably 20N or less, more preferably 15N or less, and particularly preferably 12N or less. This allows the diamond abrasive grains to be micro-fractured at a certain frequency, thereby further improving the processing efficiency.
[0027] The compressive breaking stress of the diamond abrasive grain is preferably 3 Gpa or more, more preferably 3.2 Gpa or more, even more preferably 3.5 Gpa or more, and particularly preferably 4 Gpa or more. This compressive breaking stress indicates the stress at which the abrasive grain breaks when stress is applied along the height direction of the cylinder, assuming that the shape of the abrasive grain is cylindrical. It means that the abrasive grain with a large compressive breaking strain and compressive breaking stress is difficult to break completely even if it repeats micro-fracture. That is, in the diamond abrasive grain disclosed here, when the compressive breaking stress is large, the processing durability during grinding and polishing tends to improve. On the other hand, the compressive breaking stress of the diamond abrasive grain is preferably 10 Gpa or less, more preferably 7.5 Gpa or less, and particularly preferably 5 Gpa or less. This allows the diamond abrasive grain to be micro-fractured at a certain frequency, so that the processing efficiency can be further improved.
[0028] The diamond abrasive grains disclosed herein preferably contain a predetermined dopant. This makes it easier for internal stress to be introduced into the abrasive grains in the heat treatment process described below. The dopant here refers to an element other than carbon (C). The dopant may react with diamond (carbon element) to form a chemical bond, or may be diffused into the crystal lattice of diamond. Examples of dopants include metal elements such as Fe, Ni, Co, Mn, Al, Ti, Cr, Zr, and V. The dopant may also be an element other than a metal element. Examples of dopants other than metal elements include N, B, Si, and P. These dopants may be unavoidably mixed in the manufacturing process, or may be intentionally introduced into the abrasive grains. The dopant preferably has a higher thermal expansion coefficient than diamond. In this case, the difference in thermal expansion between diamond and the dopant makes it easier to introduce internal stress into the abrasive grains during the heat treatment process, improving micro-crushing properties. A suitable example of the dopant is a metal (typically a metal particle), and the constituent elements thereof include the above-mentioned metal elements. The content of the dopant relative to the total weight (100wt%) of the diamond abrasive grains is preferably 0.1wt% or more, more preferably 0.2wt% or more, even more preferably 0.3wt% or more, and particularly preferably 0.5wt% or more. This makes it easier to introduce internal stress in the heat treatment process. On the other hand, in consideration of the strength of the diamond abrasive grains, the upper limit of the content of the dopant is preferably 10wt% or less, more preferably 5wt% or less, even more preferably 3wt% or less, and particularly preferably 1wt% or less. The content of the dopant in the diamond abrasive grains can be measured based on X-ray fluorescence analysis (XRF: X-Ray Fluorescence).
[0029] In addition, diamond abrasive grains have a Raman spectrum of 1325 cm -1 From 1334cm -1 The average peak position of the Raman peaks that exist in the range of 1329.5 cm -1 Less than or equal to 1329.4 cm -1The diamond abrasive grains in which the Raman peak position is shifted to the low wavenumber side have a large internal stress introduced therein, and therefore exhibit more suitable micro-fracturability during grinding and polishing. On the other hand, the lower limit of the average value of the Raman peak position is 1328.8 cm -1 More than 1328.9cm is preferable. -1 The above is more preferable. As the Raman peak position becomes higher, the internal stress of the diamond abrasive grain becomes smaller, so that excessive fracture tends to be suppressed.
[0030] In this specification, the "Raman peak position" is measured under the following conditions. First, a commercially available microscopic Raman spectrophotometer can be used as the measuring device. The measurement conditions are, for example, set to a measurement temperature of 24°C, a calibration sample of Si, and an excitation laser wavelength of 532 nm, and other conditions are appropriately adjusted so that clear measurement results are obtained. When Raman spectroscopy of diamond abrasive grains is performed under the above conditions, a peak due to the lattice vibration of diamond crystals appears at the Raman shift of 1333 cm. -1 A Raman spectrum present in the vicinity is detected. Then, using a specified waveform analysis software (such as Labspec6), baseline correction, peak search, and fitting are performed on this Raman spectrum, and the position of the peak top (Raman shift) is regarded as the "Raman peak position." This allows the Raman peak position to be measured. The "average Raman peak position" is the arithmetic mean of the Raman peak positions obtained from at least 500 measurement points (the number of measurement points within the same particle is constant) for 100 or more randomly selected diamond abrasive grains.
[0031] The diamond abrasive grains have an average Raman peak half-width of 4.5 cm -1 Less than 4.4 cm (more preferably -1 Less than 4.3 cm, more preferably -1(below). This allows the diamond abrasive grains to have excellent crystallinity and extremely high hardness. In this specification, the "Raman peak half-width" refers to the wavenumber width of the peak at half the intensity of the peak top of the Raman spectrum obtained by the above-mentioned procedure. In addition, the "average Raman peak half-width" is the arithmetic average of the Raman peak half-widths obtained at at least 500 measurement points (the number of measurement points within the same particle is constant) for 100 or more randomly selected diamond abrasive grains.
[0032] The size of the diamond abrasive grains does not limit the technology disclosed herein, and can be changed appropriately depending on the purpose and mode of use. For example, 50 The particle size may be 0.1 μm or more, 0.5 μm or more, 1 μm or more, 5 μm or more, or 10 μm or more. 50 The particle size may be 1000 μm or less, 500 μm or less, 250 μm or less, or 100 μm or less. 50 "Particle size" is the particle size that corresponds to a cumulative frequency of 50 volume % from the small particle side in the volume-based particle size distribution based on a general laser diffraction / light scattering method (dispersion medium: water).
[0033] The shape of the diamond abrasive grains is not particularly limited, and can be appropriately selected from conventionally known shapes. For example, the diamond abrasive grains may be spherical, plate-like, or irregularly shaped (such as confetti-like). The average aspect ratio of the diamond abrasive grains may be 1 or more and 2 or less, or 1.1 or more and 1.8 or less. The "aspect ratio" in this specification can be obtained by drawing a rectangle circumscribing the abrasive grains in an electron microscope image and calculating the ratio (b / a) of the length (a) of the short side of the rectangle to the length (b) of the long side of the rectangle. The "average aspect ratio" is the arithmetic average value of the aspect ratios of 100 or more particles.
[0034] The diamond abrasive grains disclosed herein are used, for example, in SiC machining tools. Such a SiC machining tool can efficiently machine SiC because the cutting edge of the abrasive grains is easily maintained in a sharp state. An example of a SiC machining tool is a vitrified grinding wheel. This vitrified grinding wheel includes a plurality of diamond abrasive grains and a vitrified bond that bonds the plurality of diamond abrasive grains. The vitrified bond is a bonding agent whose main component is glass. The vitrified grinding wheel is manufactured by firing a clay mixture of the vitrified bond and the diamond abrasive grains. In the vitrified grinding wheel after firing, a bond network is formed in which a plurality of abrasive grains are bonded via the vitrified bond.
[0035] <Powder material> Next, the powder material containing the diamond abrasive grains of the above-mentioned configuration will be described. The diamond abrasive grains of the above-mentioned configuration can be used in the state of a powder material (a group of fine particles) mainly composed of the abrasive grains. Here, "mainly composed of abrasive grains" means that the fine particles contained in the powder material in the largest amount by weight are diamond abrasive grains. More specifically, the powder material disclosed herein preferably contains 50% by weight or more of diamond abrasive grains (preferably 60% by weight or more, more preferably 70% by weight or more, even more preferably 80% by weight or more, and particularly preferably 90% by weight or more). Note that this powder material may contain fine particles other than the abrasive grains of the above-mentioned configuration, as long as the effect of the technology disclosed herein is not significantly impaired. Examples of such subcomponents include silica particles, alumina particles, ceria particles, and organic binder particles.
[0036] The diamond abrasive grains contained in the powder material disclosed herein have an average compression strain of 0.3 or more and 0.8 or less. As described above, diamond abrasive grains having a high compression strain of 0.3 or more have excellent micro-fracturability. The average compression strain in the powder material is preferably 0.32 or more, and particularly preferably 0.35 or more. This allows the diamond abrasive grains in the powder material to have a higher micro-fracturability. On the other hand, the average compression strain is preferably 0.7 or more, more preferably 0.6 or less, and particularly preferably 0.5 or less. This allows the diamond abrasive grains in the powder material to be prevented from being broken at an excessive frequency.
[0037] The "average value of the compression failure point strain" here can be obtained, for example, by randomly selecting 100 or more abrasive grains from a plurality of diamond abrasive grains contained in the powder material, measuring the compression failure point strain of each abrasive grain, and calculating the average value of the measurement results. When measuring the average value of the compression failure point strain, it is preferable to measure abrasive grains with a grain size of 5 μm or more. This is because it is difficult to accurately measure the compression failure point strain of abrasive grains with a grain size of less than 5 μm with the technology at the time of filing this application. However, the grain size of the measurement target is not limited to the technology disclosed herein. For example, when the compression failure point strain of abrasive grains with a grain size of less than 5 μm can be measured, the average value of the compression failure point strain including abrasive grains with a grain size of less than 5 μm may be measured using the technology.
[0038] In addition, the powder material disclosed herein preferably has a number of diamond abrasive grains with a compression failure point strain of 0.2 to 0.9 of 50% or more (preferably 60% or more, more preferably 70% or more, even more preferably 80% or more, and particularly preferably 90% or more). Since such a powder material contains a large amount of diamond abrasive grains with suitable grindability, it can exhibit higher processability. On the other hand, the upper limit of the number percentage of diamond abrasive grains that satisfy the compression failure point strain of 0.2 to 0.9 is not particularly limited, and may be 100% or less, 99% or less, or 98% or less. In addition, the "number percentage" in this specification refers to the percentage calculated by randomly selecting 100 diamond abrasive grains from among the multiple particles contained in the powder material and using the 100 abrasive grains as the denominator.
[0039] In addition, the average value of the compressive fracture strength of the diamond abrasive grains contained in the powder material is preferably 1.8 Gpa or more, and particularly preferably 2.0 Gpa or more. This allows the powder material as a whole to have a suitable processing durability. On the other hand, the average value of the compressive fracture strength of the powder material is preferably 3.5 Gpa or less, more preferably 3.2 Gpa or less, and particularly preferably 3.0 Gpa or less. This increases the frequency of crushing the abrasive grains contained in the powder material, thereby further improving processing efficiency.
[0040] In addition, the powder material disclosed herein preferably has a number percentage of diamond abrasive grains having a compressive fracture strength of 1.5 Gpa or more and 4.0 Gpa or less (preferably 1.8 GPa or more and 3.5 GPa or less) of 50% or more by number. The powder material of this configuration contains a large amount of diamond abrasive grains having both a large compressive fracture strain and a large compressive fracture strength, so that it can obtain a suitable processing durability. The number percentage of diamond abrasive grains having the compressive fracture strength in the above-mentioned range is more preferably 60% or more by number, even more preferably 70% or more by number, particularly preferably 80% or more by number, and most preferably 90% or more by number. On the other hand, the upper limit of the number percentage of diamond abrasive grains satisfying the above-mentioned compressive fracture strength is not particularly limited, and may be 100% or less by number, 99% or less by number, or 98% or less by number.
[0041] In addition, the powder material disclosed herein has a Raman spectrum at multiple measurement points by microscopic Raman spectroscopy targeting diamond abrasive grains in the powder material, and the Raman peak position is 1327 cm -1 Over 1329.8cm -1 It is preferable that 50% or more of the measurement points (preferably 60% or more of the measurement points, more preferably 70% or more of the measurement points, even more preferably 80% or more of the measurement points, and particularly preferably 90% or more of the measurement points) are within the range of less than 100%. Since the powder material of such a configuration contains a large number of diamond abrasive grains to which a suitable internal stress has been introduced, it can exhibit higher workability. On the other hand, the upper limit of the number of measurement points showing the above-mentioned predetermined Raman peak position is not particularly limited, and may be 100% or less of the measurement points, 99% or less of the measurement points, or 98% or less of the measurement points. In addition, the "measurement point %" in this specification is a ratio calculated by randomly selecting 100 or more diamond abrasive grains from among the multiple particles contained in the powder material, acquiring Raman spectra at one or more measurement points for each selected abrasive grain (the same number for each abrasive grain in the evaluation of the same powder material), and using the total number of acquired Raman spectra as the denominator. In addition, from the viewpoint of measuring an accurate Raman spectrum, it is preferable to select and measure abrasive grains having a particle size equal to or greater than the spatial resolution (e.g., 0.3 μm) of the microscopic Raman spectrometer. In addition, since the Raman spectrum has a particle size dependency, from the viewpoint of appropriately evaluating the internal stress, the particle size of the selected abrasive grains is preferably 10 μm or more. However, the particle size of the object for which the Raman spectrum is measured does not limit the technology disclosed herein.
[0042] In addition, the powder material disclosed herein has a Raman peak half-width of 4.2 cm when the Raman spectrum of diamond abrasive grains is obtained at 100 or more measurement points. -1It is preferable that the measurement points where the crystallinity is confirmed are 50% or more (preferably 60% or more, more preferably 70% or more, even more preferably 80% or more, and particularly preferably 90% or more). Since the powder material of this configuration contains a large amount of diamond abrasive grains with suitable crystallinity, it has higher hardness and can exhibit high processing efficiency and durability. On the other hand, the upper limit of the proportion of the measurement points where the above-mentioned crystallinity is confirmed is not particularly limited, and may be 100% or less, 99% or less, or 98% or less.
[0043] <Manufacturing method of diamond abrasive grains> Next, a method for producing the diamond abrasive grains having the above-mentioned structure will be described. The manufacturing method disclosed herein includes at least a heat treatment step.
[0044] In this heat treatment process, the diamond abrasive grains are heated at a predetermined temperature. This introduces internal stress into the diamond abrasive grains. One of the factors that improves the micro-fracturability (increase in compressive fracture strain) in the technology disclosed herein is that the heat treatment introduces an appropriate internal stress. In the manufacturing method disclosed herein, the heating temperature in the heat treatment process is set to a range of 200°C to 900°C. According to an experiment conducted by the inventor, when the heat treatment is performed at a temperature in this range, the compressive fracture strain of the diamond abrasive grains increases to 0.3 or more. Considering that the compressive fracture strain of a typical diamond is about 0.15 (at most less than 0.25), this increase in compressive fracture strain can be said to be significant. In addition, the "heating temperature" here refers to the maximum temperature in the heat treatment.
[0045] In addition, the heating temperature in the heat treatment process is preferably 250°C or more, more preferably 300°C or more, even more preferably 350°C or more, and particularly preferably 400°C or more. This can more reliably increase the compression fracture strain of the diamond abrasive grains after heating. On the other hand, the upper limit of the heating temperature is preferably 800°C or less, more preferably 700°C or less, even more preferably 650°C or less, and particularly preferably 600°C or less. This can suppress the denaturation of the diamond abrasive grains (such as changes in surface properties and oxidation).
[0046] By the way, in the manufacturing process of general diamond abrasive grains, heating is performed in a non-oxidizing atmosphere (such as N2 gas atmosphere or Ar gas atmosphere) to suppress oxidation of diamond. In contrast, in the manufacturing method disclosed herein, it is preferable to set the heating atmosphere in the heat treatment process to an oxidizing atmosphere. Although heating in this oxidizing atmosphere was considered to be inappropriate from the viewpoint of oxidation of diamond, the inventor's experiments have shown that it is a very effective heating condition from the viewpoint of increasing the compression failure point strain (improving micro-fracturability). Specifically, it has been confirmed by experiments that when the heat treatment process is performed in an oxidizing atmosphere, the frequency of diamond abrasive grains with a compression failure point strain of 0.3 or more is extremely increased. Also, as described above, in the manufacturing method disclosed herein, the upper limit of the heating temperature is set to 900°C or less (preferably 600°C or less) from the viewpoint of suppressing the denaturation (oxidation) of diamond abrasive grains. Therefore, the compression failure point strain can be increased while sufficiently suppressing the oxidation of diamond abrasive grains.
[0047] In addition, the oxygen concentration in the heating atmosphere is preferably 1% or more, more preferably 5% or more, even more preferably 10% or more, and particularly preferably 15% or more. This can increase the compression fracture strain of the diamond abrasive grains more efficiently. On the other hand, the upper limit of the oxygen concentration is preferably 90% or less, more preferably 50% or less, even more preferably 30% or less, and particularly preferably 25% or less. This can more effectively suppress the oxidation of the diamond abrasive grains.
[0048] The heating time may be, for example, 0.1 hours or more, preferably 0.5 hours or more, more preferably 1 hour or more, even more preferably 1.5 hours or more, and particularly preferably 2 hours or more. This can more reliably increase the compression fracture strain of the diamond abrasive grains. On the other hand, the upper limit of the heating time is preferably 5.5 hours or less, more preferably 5 hours or less, even more preferably 4.5 hours or less, and particularly preferably 4 hours or less. This can shorten the heat treatment process and improve manufacturing efficiency. The "heating time" here refers to the time during which the above-mentioned heating temperature (maximum temperature) is maintained.
[0049] Furthermore, in the manufacturing method disclosed herein, it is preferable to subject the diamond abrasive grain containing dopant other than carbon element to heat treatment process.As mentioned above, the diamond abrasive grain containing this kind of dopant is easy to introduce the internal stress originating from dopant during heat treatment process.Therefore, it can increase the compression fracture point strain of the diamond abrasive grain after heating more reliably.
[0050] In addition, the diamond abrasive grains are preferably heated in a state where no softened glass or molten glass is present on the surface of the diamond abrasive grains. When the diamond abrasive grains are heated together with such glass (typically vitrified bond), there are cases where the internal stress to the extent that it can impart micro-fracturability is not introduced into the abrasive grains. The mechanism is considered to be that during the heating process of the diamond abrasive grains, a compressive force is applied, and internal stress (typically tensile stress) tends to be difficult to introduce. That is, in the manufacturing method disclosed herein, it is preferable to carry out the heat treatment process without applying an external force in the compressive direction to the diamond abrasive grains. This makes it possible to improve the micro-fracturability of the diamond abrasive grains more efficiently. Here, "no external force in the compressive direction is applied to the diamond abrasive grains" includes not only the above-mentioned glass not present on the diamond abrasive grains surface, but also the state where a material with a smaller thermal expansion coefficient in the heating temperature range than the diamond abrasive grains is present on the diamond abrasive grains surface, and the state where no external force is applied by a pressure device or the like.
[0051] An embodiment of the technology disclosed herein has been described above. However, the above embodiment is not intended to limit the technology disclosed herein. In other words, the technology disclosed herein may include various modifications of the above embodiment.
[0052] For example, in the manufacturing method disclosed herein, an inspection step may be performed to inspect the compression failure point strain of the diamond abrasive grains after the heat treatment step. By performing this inspection step, it is possible to determine whether diamond abrasive grains having the desired compression failure point strain have been manufactured. In addition, after performing the inspection step, a selection step may be performed to select diamond abrasive grains showing the desired compression failure point strain. This allows diamond abrasive grains having excellent micro-fracturability to be manufactured more stably. In addition, the diamond abrasive grains excluded in the selection step may be subjected to the heat treatment step again. This prevents a decrease in yield in the manufacturing process. In addition, in the inspection step, it is preferable to measure the compression failure point strain of the diamond abrasive grains according to the above-mentioned procedure. In addition, it is not necessary to perform this inspection step on all diamond abrasive grains after the heat treatment step. For example, the inspection step may be performed when the lot of diamond abrasive grains supplied to the heat treatment step is changed or when the conditions of the heat treatment step are changed. This allows diamond abrasive grains having the desired compression failure point strain to be manufactured stably without significantly reducing the manufacturing efficiency.
[0053] [Test example] Next, test examples related to the technology disclosed herein will be described. Note that the technology disclosed herein is not limited to the following test examples.
[0054] 1. Sample Preparation (1) Example 1 In Example 1, the diamond abrasive grains were subjected to heat treatment under predetermined conditions. Specifically, first, commercially available diamond abrasive grains (manufactured by Global Diamond Co., Ltd., FRM-DN 40-60) were prepared. Note that, as a result of performing laser diffraction analysis, the D 50The particle diameter was 40 μm. In addition, the result of the component analysis based on XRF showed that the diamond abrasive grains contained 0.176 wt% Ni and 0.389 wt% Mn as impurities. Next, the above-mentioned diamond abrasive grains were heated in an oxidizing atmosphere (air). The temperature rise rate in this heat treatment was set to 100 ° C / h, and the maximum temperature was set to 400 ° C. Then, the heating time (holding time at the maximum temperature) was set to 3 hours. In this way, heat-treated diamond abrasive grains (Example 1) were produced. The weight reduction rate of the diamond abrasive grains before and after the heat treatment was 1% or less.
[0055] (2) Example 2 In Example 2, diamond abrasive grains were produced using the same procedure as in Example 1, except that the maximum temperature during the heat treatment was changed to 500°C.
[0056] (3) Example 3 In Example 3, diamond abrasive grains were produced in the same manner as in Example 1, except that the maximum temperature during the heat treatment was changed to 600°C.
[0057] (4) Comparative Example 1 In Comparative Example 1, diamond abrasive grains that were not subjected to heat treatment were prepared. The diamond abrasive grains prepared in Comparative Example 1 were the same as the commercially available diamond abrasive grains used in Example 1.
[0058] (5) Comparative Example 2 In Comparative Example 2, diamond abrasive grains were produced in the same manner as in Example 2, except that the atmosphere during the heat treatment was changed to a non-oxidizing atmosphere (N2 gas).
[0059] (6) Comparative Example 3 In Comparative Example 3, diamond abrasive grains were produced in the same manner as in Comparative Example 2, except that the maximum temperature during the heat treatment was changed to 1000°C.
[0060] 2.Evaluation Test (1) SiC grinding test First, an alumina substrate with a paste containing glass powder (TMX-501F, manufactured by TOMATEC Corporation) printed on its surface was prepared as a substrate. Then, the diamond abrasive grains of each example were sprinkled on the paste of the substrate, and the paste was dried. After that, a firing process was performed in an air atmosphere (maximum firing temperature: 570°C, firing time: 2h), and then the substrate was cooled to room temperature. As a result, the abrasive grains were fixed to the alumina substrate by the glass. Then, after cutting the substrate, a part of the abrasive grains was removed, and a test grinding jig was created in which one abrasive grain was fixed to the alumina substrate. In this grinding jig, the height from the substrate surface to the top end of the abrasive grain (abrasive grain height) was 18 to 30 μm.
[0061] Next, the grinding process of the SiC wafer was performed using this grinding jig. In this grinding process, the target value of the cutting depth was set to 2 μm, the processing speed was set to 6 mm / s, and the processing distance was set to 5 mm / pass × 20. This processing test was repeated by replacing the SiC wafer until grinding became difficult due to wear of the abrasive grains. Then, the abrasive grain height was measured with a laser microscope every time the grinding process was performed, and the difference between the abrasive grain height before the start of the test and the abrasive grain height at the time of measurement (abrasive grain wear height) was calculated. In addition, the depth of the grinding marks on each SiC wafer after the grinding process was measured, and the total value of the depth of each grinding mark (SiC cumulative processing depth) was calculated. In addition, in the measurement of the "grinding mark depth of the SiC wafer", the depth of both ends of the grinding mark was measured using a laser microscope, and the average value of the depth of both ends was calculated. In this test, four grinding jigs were made for each example, and the "abrasive grain wear height" and "SiC cumulative processing depth" of each were measured to obtain the average value. The results are shown in Figure 1.
[0062] As shown in FIG. 1, in Examples 1 to 3, deep grinding marks were formed relative to the abrasive grain wear height. In particular, in Examples 1 and 2, the third grinding process, and in Example 3, the second grinding process, the cumulative depth of the grinding marks was confirmed to increase rapidly. This is expected to be because, in Examples 1 to 3, the diamond abrasive grains were broken during grinding and sharp cutting edges were formed. From the above, it was found that excellent SiC processability can be imparted to the diamond abrasive grains by performing heat treatment under specified conditions as in Examples 1 to 3. In addition, the abrasive grains of Examples 1 to 3 were able to perform more grinding processes before the wear amount reached 15 μm or more than those of Comparative Examples 1 to 3. From this, it was found that the durability of the abrasive grains of Examples 1 to 3 was also improved.
[0063] In addition, Comparative Example 1 (untreated diamond abrasive grains) of this test was heated (570°C, 2h) when the abrasive grains were fixed to the alumina substrate via glass. However, in this Comparative Example 1, the improvement in SiC processability as in Examples 1 to 3 was not confirmed. The cause of this phenomenon is presumed to be as follows. If heat treatment is performed while a part or all of the abrasive grains are covered with another material (glass), an external force in the compressive direction is applied to the diamond abrasive grains during heat treatment, making it difficult to introduce internal stress (typically tensile stress) into the abrasive grains. In other words, it is presumed that the heat treatment (firing of a mixture of vitrified bond and diamond abrasive grains) used in manufacturing a general vitrified grinding wheel does not easily introduce internal stress that can impart micro-fracturability to the diamond abrasive grains.
[0064] (2) Compression fracture test Next, in this test, in order to investigate the changes in physical properties occurring in the diamond abrasive grains after heat treatment, a compression fracture test was carried out on the abrasive grains of Example 2, Comparative Example 1, and Comparative Example 2. In this test, eight items were measured: "sample height", "sample grain size", "fracture point displacement", "compressive fracture point test force", "compressive fracture point stress", "compressive fracture point strain", "Young's modulus", and "compressive fracture strength". The measurement results are shown in Tables 1 to 3. Detailed measurement conditions are shown below.
[0065] [Compression test conditions] Testing equipment: Micro Autograph MST-I HR Load cell capacity: 500N (50N range) Load speed: 2μm / sec Stroke origin test force: 0.02N Compression tool: Diamond indenter with a flat surface of φ200 μm Lower pressure table: Pressure plate with hardness of 700 Measurement method: Place one sample grain on the lower pressure table and compress it one grain at a time. Number of measurements: 5
[0066] [Sample height] The distance from the stroke position of the compression jig to the lower pressure plate when the indenter contacted the sample (abrasive grain) was measured with a displacement sensor, and the measurement result was recorded as "sample height (μm)."
[0067] [Sample particle size] The sample (abrasive grain) was observed under a stereo microscope, and the long diameter was measured with a micrometer attached to an XY stage and recorded as the "sample grain size (μm)."
[0068] [Compressive breaking point test force / compressive breaking point stress] In this test, the pressure at which the abrasive grain broke was measured as the "compressive breaking point test force P." Then, assuming that the grain shape was cylindrical, the "compressive breaking point stress" was calculated by substituting the compressive breaking point test force P into the following formula (1). Compressive breaking stress = P / (πr 2 ) (1) P = Compressive breaking point test force r = particle radius (1 / 2 of sample particle size d)
[0069] [Displacement at breaking point / Compressive strain at breaking point] In this test, the displacement (deformation) of the abrasive grain when fracture occurred was measured as the "fracture point displacement." The "compressive fracture point strain" was calculated by substituting the fracture point displacement and sample height into the following formula (2). Compressive strain at break = Displacement at break / Sample height (2)
[0070] Young's Modulus Next, the Young's modulus was calculated by substituting the compressive failure stress and compressive failure strain into the following equation (3). Young's modulus = compressive stress at break / compressive strain at break (3)
[0071] [Compressive fracture strength] Next, the "compressive fracture strength" was calculated by substituting the compressive fracture test force and the sample grain size into the following formula (4). Cs = 2.48P / (πd 2 ) (4) Cs: Compressive fracture strength P: Compressive breaking point test force d: Sample particle size
[0072] [Table 1]
[0073] [Table 2]
[0074] [Table 3]
[0075] As shown in Tables 1 to 3, Example 2 had various improved physical properties compared to Comparative Examples 1 and 2. In particular, Example 2 was confirmed to have a significantly improved compressive fracture strain compared to Comparative Examples 1 and 2. This shows that the abrasive grains heat-treated in an oxidizing atmosphere at low temperature have the property of increasing micro-fracturability and maintaining a sharp cutting edge. The results of the compressive fracture test are understood to be consistent with the fact that very deep grinding marks were formed in Examples 1 to 3 in the SiC grinding test shown in FIG. 1.
[0076] In addition, in Example 2, not only the compressive fracture strain but also the compressive fracture strength was improved. This shows that the abrasive grains heat-treated in an oxidizing atmosphere at a low temperature are endowed with excellent strength. This result is understood to be consistent with the small wear amount of Examples 1 to 3 in the SiC grinding test shown in FIG. 1.
[0077] (3) Raman spectroscopic analysis In this study, 500 Raman spectra were acquired for each example. -1 ~1334cm -1 The waveforms of the Raman peaks were separated and the positions and half-widths of the Raman peaks were measured. In this test, the positions and half-widths of the Raman peaks were measured according to the following procedure. First, a microscopic Raman spectrophotometer (LabRAM HR Evolution manufactured by Horiba, Ltd.) was used as the measuring device. The measurement conditions were, for example, set to 24°C measurement temperature, Si calibration sample, 532nm excitation laser wavelength, 1800gr / mm grating, exposure time 8 seconds, and 2 integration times. Then, baseline correction, peak search, and fitting were performed on the obtained Raman spectrum using waveform analysis software (Labspec6). The position of the peak top was regarded as the "position of the Raman peak", and the wavenumber width of the peak at half the intensity of the peak top was regarded as the "half-width of the Raman peak". Then, the peak positions and half-widths at five non-overlapping measurement points were measured for each of 100 randomly selected diamond abrasive grains. In addition, all diamond abrasive grains selected in this evaluation had a circle equivalent diameter in the range of 25 μm to 75 μm. In this test, the average values of "Raman peak position" and "Raman peak half width" at 500 measurement positions were calculated. The calculation results are shown in Table 4.
[0078] In this test, the distribution of Raman peak positions for each example was also created. The results are shown in Table 5. In measuring the "distribution of Raman peak positions," 500 Raman spectra were recorded on a 0.2 cm -1The wavenumber range was divided into multiple wavenumber ranges at intervals of 0.2 cm, and the frequency (%) at which the peak position was confirmed in each wavenumber range was calculated. In this test, the distribution of the Raman peak half-width for each example was also calculated. The results are shown in Table 6. In creating this "Raman peak half-width distribution," the Raman peak half-width was divided into 0.2 cm -1 The spectrum was divided into multiple intervals, and the frequency (%) of the Raman spectra belonging to each interval was calculated.
[0079] [Table 4]
[0080] [Table 5]
[0081] [Table 6]
[0082] First, as shown in Table 4, the average value of the Raman peak position of Examples 1 to 3 was lower than that of Comparative Examples 1 and 2. From this, it was found that the diamond abrasive grains heat-treated in an oxidizing atmosphere under a specified temperature condition have an appropriate internal stress introduced, so that the Raman peak position shifts to the low wave number side. It is expected that this appropriate stress introduction is one of the factors that improves the micro-fracturability. In addition, in Comparative Example 3, in which the heating temperature was raised to 1000°C, excessive internal stress was introduced.
[0083] As shown in Table 5, in Examples 1 to 3, the Raman peak position was 1327 cm -1 Over 1329.8cm -1 The number of measurement points within the range of less than 4.2 cm was 50% or more. From this, it can be said that appropriate internal stress was introduced overall in Examples 1 to 3, even when viewed as powder materials. Furthermore, as shown in Table 6, in Examples 1 to 3, the half-width of the Raman peak was 4.2 cm. -1The number of measurement points where the crystallinity was less than this was 50% or more of the measurement points. From this, it can be said that Examples 1 to 3 have favorable crystallinity overall, even when viewed as powder materials.
[0084] Although the technology disclosed herein has been described in detail above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and changes to the specific examples exemplified above. In other words, the technology disclosed herein includes the embodiments described in items 1 to 7 below.
[0085] <Item 1> A diamond abrasive having a compressive breaking strain of 0.3 or more and 0.9 or less.
[0086] <Item 2> 2. The diamond abrasive grain according to claim 1, containing a dopant other than carbon element.
[0087] <Item 3> 3. The diamond abrasive grain according to claim 2, wherein the content of the dopant relative to the total weight of the diamond abrasive grain is 0.1 wt % or more.
[0088] <Item 4> 4. The diamond abrasive grain according to claim 2 or 3, wherein the thermal expansion coefficient of the dopant is higher than the thermal expansion coefficient of the diamond abrasive grain.
[0089] <Item 5> 5. The diamond abrasive grain according to any one of items 1 to 4, having a compressive fracture strength of 1.5 Gpa or more and 4.0 Gpa or less.
[0090] <Item 6> 6. The diamond abrasive grain according to any one of items 1 to 5, wherein the compression fracture test force is 6.5 N or more and 20 N or less.
[0091] <Item 7> 7. The diamond abrasive grain according to any one of items 1 to 6, having a compressive fracture stress of 3 Gpa or more and 10 Gpa or less.
[0092] <Item 8> Based on Raman spectroscopy, the 1325 cm -1 From 1334cm -1 The average peak position of the Raman peaks that exist in the range of 1329.5 cm -1 8. The diamond abrasive grain according to any one of items 1 to 7, wherein:
[0093] <Item 9> Based on Raman spectroscopy, the 1325 cm -1 From 1334cm -1 The average half-width of the Raman peaks is 4.5 cm -1 9. The diamond abrasive grain according to any one of items 1 to 8, wherein:
[0094] <Item 10> 10. The diamond abrasive grain according to any one of items 1 to 9, which is used for a SiC machining tool.
[0095] <Item 11> A powder material comprising a plurality of diamond abrasive grains, A powder material, wherein the average compressive fracture strain of the diamond abrasive grains is 0.3 or more and 0.8 or less.
[0096] <Item 12> Item 12. The powder material according to item 11, wherein the number of diamond abrasive grains having a compressive fracture strain of 0.2 or more and 0.9 or less is 50% by number or more.
[0097] <Item 13> A method for manufacturing diamond abrasive grains, comprising a heat treatment step of heating diamond abrasive grains at a temperature of 200°C or higher but 900°C or lower.
[0098] <Item 14> Item 14. The method according to item 13, wherein the heating atmosphere in the heat treatment step is an oxidizing atmosphere.
[0099] <Item 15> Item 15. The method according to item 13 or 14, wherein the heating temperature in the heat treatment step is 400° C. or higher and 600° C. or lower.
[0100] <Item 16> 16. The method according to any one of items 13 to 15, wherein the diamond abrasive grains contain a dopant other than carbon element.
[0101] <Item 17> Item 17. The method according to item 16, wherein the content of the dopant relative to the total weight of the diamond abrasive grains is 0.1 wt% or more.
[0102] <Item 18> Item 18. The method according to item 16 or 17, wherein the dopant has a thermal expansion coefficient higher than the thermal expansion coefficient of the diamond abrasive grains.
Claims
1. A diamond abrasive having a compressive breaking strain of 0.3 or more and 0.9 or less.
2. The diamond abrasive grain according to claim 1 , containing a dopant other than elemental carbon.
3. The diamond abrasive grain according to claim 2, wherein the content of the dopant relative to the total weight of the diamond abrasive grain is 0.1 wt % or more.
4. The diamond abrasive grain according to claim 2 , wherein the thermal expansion coefficient of the dopant is higher than the thermal expansion coefficient of the diamond abrasive grain.
5. 3. Diamond abrasive grains according to claim 1 or 2, having a compressive fracture strength of 1.5 GPa or more and 4.0 GPa or less.
6. 3. Diamond abrasive grains according to claim 1 or 2, having a compression failure point test force of 6.5 N or more and 20 N or less.
7. 3. Diamond abrasive grains according to claim 1 or 2, having a compressive breaking stress of 3 GPa or more and 10 GPa or less.
8. Based on Raman spectroscopy, the Raman spectrum at 1325 cm -1 From 1334 cm -1 The average value of the peak positions of the Raman peaks that exist in the range of -1 3. The diamond abrasive grain according to claim 1 or 2, wherein:
9. Based on Raman spectroscopy, the Raman spectrum at 1325 cm -1 From 1334 cm -1 The average half-width of the Raman peaks that exist in the range of 4.5 cm -1 3. The diamond abrasive grain according to claim 1 or 2, wherein:
10. The diamond abrasive grain according to claim 1 or 2, which is used in a SiC machining tool.
11. A powder material comprising a plurality of diamond abrasive grains, A powder material, wherein the average compressive breaking strain of the diamond abrasive grains is 0.3 or more and 0.8 or less.
12. The powder material according to claim 11, wherein the number of diamond abrasive grains having a compressive failure strain of 0.2 or more and 0.9 or less is 50% or more by number.
13. A method for manufacturing diamond abrasive grains, comprising a heat treatment step of heating diamond abrasive grains at a temperature of 200°C or higher and 900°C or lower.
14. The method according to claim 13 , wherein the heating atmosphere in the heat treatment step is an oxidizing atmosphere.
15. The method according to claim 14, wherein the heating temperature in the heat treatment step is 400° C. or more and 600° C. or less.
16. The method of claim 15, wherein the diamond abrasive grains contain a dopant other than elemental carbon.
17. The manufacturing method according to claim 16, wherein the content of the dopant relative to the total weight of the diamond abrasive grains is 0.1 wt% or more.
18. The method of claim 17, wherein the dopant has a thermal expansion coefficient higher than the thermal expansion coefficient of the diamond abrasive grains.
Citation Information
Patent Citations
Vitrified bond super abrasive grain wheel and method of manufacturing wafer using the same
JP2017080847A