Granular thin film

By optimizing the Co/Fe atomic ratio and using BaF as the dielectric matrix, the granular thin film enhances current detection sensitivity and noise reduction, addressing the low sensitivity issue in existing magnetic field sensor elements.

JP2024139308APending Publication Date: 2024-10-09CITIZEN FINEDEVICE CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023050187
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

The granular thin film used as a magnetic field sensor element for current detection has a low figure of merit FOM, leading to low current detection sensitivity.

Method used

A granular thin film with magnetic nanoparticles composed of Co and Fe, where the (Co/Fe) atomic ratio is adjusted to 1.2 to 17.0, and a dielectric matrix of BaF is used, achieving a figure of merit FOM of 1.00×10 -4 [°/Oe·dB] or more.

Benefits of technology

The granular thin film achieves high sensitivity in current detection with reduced noise levels, enabling a magnetic field sensor element with a high signal-to-noise ratio.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139308000001_ABST
    Figure 2024139308000001_ABST
Patent Text Reader

Abstract

To provide a granular thin film having a high performance index FOM (° / Oe dB) and high current detection sensitivity.SOLUTION: A granular thin film 1 with magnetic nanoparticles dispersed in a dielectric matrix, the granular thin film 1 is characterized in that the magnetic nanoparticles 3 are composed of Co and Fe, a (Co / Fe) atomic ratio obtained by dividing an atomic weight of Co contained in the magnetic nanoparticles 3 by an atomic weight of Fe contained in the magnetic nanoparticles 3 is 1.2 or more and 17.0 or less, and a performance index FOM is 1.00×10-4 (° / Oe dB) or more.SELECTED DRAWING: Figure 5
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a granular thin film. [Background technology]

[0002] A light-transmitting magnetic thin film is known that exhibits a magneto-optical effect, also called the Faraday effect, in which the plane of polarization rotates when linear light is transmitted through a magnetic field (see, for example, Patent Document 1). The magnetic thin film described in Patent Document 1 has a composition in which L is one or more elements selected from Fe, Co, and Ni, M is at least one element selected from Li, Be, Mg, Al, Si, Ca, Sr, Ba, and Bi, rare earth elements, and F. In the magnetic thin film described in Patent Document 1, the atomic ratio of M is 10% or more and 40% or less, the atomic ratio of F is 20% or more and 70% or less, and the total atomic ratio of M and F is 60% or more. The magnetic thin film described in Patent Document 1 has such a composition, and thus has high magnetization properties and good light transmittance, and also exhibits excellent magneto-optical properties in the near-infrared region, making it applicable to various optical communication devices.

[0003] Also, Patent Document 2 describes a magnetic field sensor that uses a granular thin film containing magnetic particles such as FeNi alloy, FeCo alloy, FeNiCo alloy, and NiCo alloy, and a dielectric material that is a fluoride that is stably separated from the magnetic particles, as a magnetic field sensor element. The magnetic field sensor element described in Patent Document 2 can be made smaller by using a granular thin film as a magnetic field sensor element for detecting current. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2017-98423 A [Patent Document 2] JP 2020-126006 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, the granular thin film used as the magnetic field sensor element for current detection in Patent Document 2 has an insufficient figure of merit FOM [° / Oe·dB], which is defined as the Faraday rotation angle per unit magnetic field and unit light transmission loss, and therefore has an issue of low current detection sensitivity.

[0006] The present invention is devised to solve such problems, and provides a granular thin film that has a high figure of merit (FOM) and is capable of detecting current with high sensitivity. [Means for solving the problem]

[0007] The granular thin film of the present invention is a granular thin film in which magnetic nanoparticles are dispersed in a dielectric matrix, the magnetic nanoparticles are composed of Co and Fe, the (Co / Fe) atomic ratio obtained by dividing the atomic weight of Co contained in the magnetic nanoparticles by the atomic weight of Fe contained in the magnetic nanoparticles is 1.2 or more and 17.0 or less, and the figure of merit FOM is 1.00×10-4 [° / Oe·dB] or more.

[0008] In the granular thin film according to the present invention, the (Co / Fe) atomic ratio is preferably 3.5 or more and 10.0 or less, and the figure of merit FOM is preferably 1.25×10 −4 [° / Oe·dB] or more.

[0009] In the granular thin film according to the present invention, the dielectric matrix contains BaF, The content of BaF in the granular thin film is preferably 75 at % or more and 90 at % or less. Effect of the Invention

[0010] The granular thin film according to the present invention has a high figure of merit (FOM) and is capable of detecting electric current with high sensitivity. [Brief description of the drawings]

[0011] [Figure 1]FIG. 2 is a diagram showing a TEM image of a granular thin film according to an embodiment. [Diagram 2] 2A is a perspective view of a magnetic field sensor device in which the granular thin film shown in FIG. 1 is used as a magnetic field sensor element, and FIG. 2B is an enlarged cross-sectional view of a portion surrounded by dashed line A shown in FIG. [Diagram 3] FIG. 3 is an internal block diagram of the current calculation device shown in FIG. [Figure 4] 13 shows the results of measuring a pulse current by a magnetic field sensor device using Example 5 as a magnetic field sensor element for current detection. [Diagram 5] The horizontal axis shows the relationship between the (Co / Fe) atomic ratio and the figure of merit FOM for the granular thin films of Examples 1 to 9 and Comparative Examples 1 to 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, preferred embodiments of the present invention will be described with reference to the drawings. Note that the present invention is not limited to the following embodiments, and can be modified as appropriate without departing from the spirit of the present invention. In addition, in each drawing, parts having the same or corresponding functions are given the same reference numerals, and their description may be omitted or simplified.

[0013] (Overview of Granular Thin Film According to an Embodiment) The inventors of the present invention have found that, in magnetic nanoparticles composed of Co and Fe, by setting the (Co / Fe) atomic ratio within a predetermined range, the figure of merit FOM can be increased when the granular thin film is used as a magnetic field sensor element for detecting current. The (Co / Fe) atomic ratio is a value obtained by dividing the atomic weight of Co contained in the magnetic nanoparticles by the atomic weight of Fe contained in the magnetic nanoparticles. The (Co / Fe) atomic ratio is preferably 1.2 to 17.0, and more preferably 3.5 to 10.0. By setting the (Co / Fe) atomic ratio to 1.2 to 17.0, the figure of merit FOM of the granular thin film can be increased to 1.00×10 -4The noise level during current detection is reduced to 10 A or less, realizing a magnetic field sensor element for current detection with a high S / N ratio. In addition, by setting the (Co / Fe) atomic ratio to 3.5 or more and 10.0 or less, the figure of merit FOM is 1.25×10 -4 [° / Oe·dB] or more, and the noise level when detecting current is further reduced to 5 [A] or less, making it possible to realize a magnetic field sensor element for current detection with an even higher S / N ratio.

[0014] (Configuration of Granular Thin Film According to the Embodiment) FIG. 1 is a diagram showing a transmission electron microscope (TEM) image of a granular thin film according to an embodiment.

[0015] The granular thin film 1 is a granular film having a dielectric matrix 2 and magnetic nanoparticles 3 dispersed in the dielectric matrix 2 in a state of being stably phase-separated from the dielectric matrix 2.

[0016] The material of the dielectric matrix 2 is preferably a fluoride (metal fluoride) such as barium fluoride (BaF), magnesium fluoride (MgF2), aluminum fluoride (AlF3), yttrium fluoride (YF3), etc., and particularly preferably barium fluoride (BaF2). The material of the dielectric matrix 2 may be an oxide such as tantalum oxide (Ta2O5), silicon dioxide (SiO2), titanium dioxide (TiO2), diniobium pentoxide (Nb2O5), zirconium dioxide (ZrO2), hafnium dioxide (HfO2), and dialuminum trioxide (Al2O3). For good phase separation between the dielectric matrix 2 and the magnetic nanoparticles 3, the material of the dielectric matrix 2 is preferably a fluoride rather than an oxide.

[0017] The material of the magnetic nanoparticles 3 is preferably composed of ferromagnetic metals, iron (Fe) and cobalt (Co). Note that the material of the magnetic nanoparticles 3 may be any material that produces the Faraday effect, and may be nickel (Ni), such as an FeNi alloy, an FeCo alloy, an FeNiCo alloy, or an NiCo alloy, or an alloy of iron (Fe), cobalt (Co) and nickel (Ni).

[0018] The (Co / Fe) atomic ratio, calculated by dividing the atomic weight of Co contained in the magnetic nanoparticles by the atomic weight of Fe contained in the magnetic nanoparticles, is preferably 1.2 or more and 17.0 or less, and more preferably 3.5 or more and 10.0 or less.

[0019] (Method of manufacturing granular thin film 1) The granular thin film 1 was formed by depositing 5.0×10 raw materials of the dielectric matrix 2 and the magnetic nanoparticles 3 in a deposition apparatus and an RF sputtering apparatus. -4 The film is formed on a substrate heated to 500°C in a vacuum of 0.1 Pa or less. The content ratio of Co and Fe atoms in the magnetic nanoparticles 3 is controlled by adjusting the content of the target containing Co and Fe that constitutes the magnetic nanoparticles 3. The obtained granular thin film 1 is subjected to a vacuum heat treatment at 500°C or more.

[0020] (Magnetic field sensor device using granular thin film 1 as a magnetic field sensor element) FIG. 2(a) is a perspective view of a magnetic field sensor device in which the granular thin film 1 is used as a magnetic field sensor element, and FIG. 2(b) is an enlarged cross-sectional view of a portion surrounded by a dashed line A shown in FIG. 2(a).

[0021] The magnetic field sensor device 10 includes a granular thin film 1, a mirror element 11, an optical fiber 12, and a current calculation device 13, and detects the current value of a direct current flowing through a conductor 14 with a diameter of 0.5 mm. The granular thin film 1 is disposed at the tip of the optical fiber 12, and the light incident through the optical fiber 12 is modulated in response to a magnetic field generated around the conductor 14 when a current flows through the conductor 14.

[0022] The mirror element 11 is formed on the granular thin film 1, and reflects the light transmitted through the granular thin film 1 back towards the granular thin film 1 to generate return light. The mirror element 11 emits, to the granular thin film 1, circularly polarized light having an opposite rotation direction to the circularly polarized light transmitted through the granular thin film 1. As the mirror element 11, for example, a silver (Ag) film, a gold (Au) film, an aluminum (Al) film, a dielectric multilayer film mirror, or the like can be used.

[0023] The optical fiber 12 has a first optical fiber 15 and a second optical fiber 16, and optically connects between the granular thin film 1 and the current calculation device 13. The first optical fiber 15 and the second optical fiber 16 are PANDA (Polarization-maintaining AND Absorption-reducing) fibers, and propagate the incident light and the return light while maintaining the polarization planes of the incident light and the return light. The first optical fiber 15 has a beat length L b The first optical fiber 15 has a length a quarter of that of the first optical fiber 15, and is connected to the second optical fiber 16 at a connection portion 17 so that its slow axis and fast axis are inclined at 45 degrees with respect to the slow axis and fast axis of the second optical fiber 16. The first optical fiber 15 converts the linearly polarized light introduced from the second fiber into circularly polarized light, and also functions as a quarter-wave plate that converts the circularly polarized light introduced from the granular thin film 1 into linearly polarized light. The second optical fiber 16 optically connects the first optical fiber 15 and the current calculation device 13.

[0024] FIG. 3 is an internal block diagram of the current calculation device 13. As shown in FIG.

[0025] The current calculation device 13 has a light emitting unit 20, a circulator 30, a first optical element 40, an optical path unit 50, and a detection signal generating unit 60. The optical paths between the light emitting unit 20, the circulator 30, the first optical element 40, the optical path unit 50, and the detection signal generating unit 60 are formed by a PANDA fiber 80. The optical paths between the first optical element 30, the optical path unit 40, the pressure sensor 50, and the detection signal generating unit 60 may be formed by a polarization maintaining optical fiber such as a bow-tie fiber and an elliptical jacket fiber.

[0026] The light emitting section 20 includes a light emitting element 21, an isolator 22, and a polarizer 23. The light emitting element 21 is, for example, a semiconductor laser or a light emitting diode. Specifically, a Fabry-Perot laser, a superluminescence diode, or the like can be preferably used as the light emitting element 21.

[0027] The isolator 22 transmits the light incident from the light emitting element 21 to the circulator 30 side, and does not transmit the light incident from the circulator 30 to the light emitting element 21 side, thereby protecting the light emitting element 21. The isolator 22 is, for example, a polarization-dependent optical isolator, and may also be a polarization-independent optical isolator.

[0028] The polarizer 23 is an optical element for converting the light emitted by the light emitting element 21 into linearly polarized light, and the type of the polarizer 23 is not particularly limited. The first linearly polarized light obtained by the polarizer 23 is incident on the first optical element 40 via the circulator 30.

[0029] The circulator 30 is an optical branching unit that transmits the first linearly polarized light emitted from the light emitting unit 20 to the first optical element 40 and branches the second linearly polarized light emitted from the first optical element 40 to the detection signal generating unit 60. The circulator 30 is formed by, for example, a Faraday rotator, a half-wave plate, a polarizing beam splitter, and a reflecting mirror.

[0030] The first optical element 40 is, for example, a half-wave plate arranged so that the azimuth angle is 22.5 degrees with respect to the polarization plane of the first linearly polarized light incident from the circulator 30. The first optical element 40 rotates the polarization plane of the first linearly polarized light incident from the circulator 30 by 45 degrees, and emits the first linearly polarized light to the optical path section 50. The first linearly polarized light whose polarization plane has been rotated 45 degrees by the first optical element 40 has a first linearly polarized light CW1 that is P-polarized light, and a second linearly polarized light CCW1 that is S-polarized light orthogonal to the first linearly polarized light CW1.

[0031] Moreover, the first optical element 40 rotates the plane of polarization of the second linearly polarized light, which is the linearly polarized light incident from the optical path section 50, by 45 degrees, and outputs the second linearly polarized light to the circulator 30.

[0032] The optical path section 50 includes a first beam splitter 51, a second beam splitter 52, a first optical path 53, a second optical path 54, and a second optical element 55.

[0033] The first beam splitter 51 outputs the first linearly polarized light CW1 to the first optical path 43, and outputs the second linearly polarized light CCW1 to the second optical path 54. Furthermore, the first beam splitter 51 receives the third linearly polarized light CW2 from the second optical path 54, and the fourth linearly polarized light CCW2 from the first optical path 53. The third linearly polarized light CW2 and the fourth linearly polarized light CW2 are polarization components of the second linearly polarized light output to the first optical element 40 that are orthogonal to each other.

[0034] The second beam splitter 52 receives the first linearly polarized light CW1 from the first optical path 43 and the second linearly polarized light CCW1 from the second optical path 44, and outputs the input first linearly polarized light CW1 and second linearly polarized light CCW1 to the second optical fiber 16. In addition, the second beam splitter 52 outputs the third linearly polarized light CW2 input from the second optical fiber 16 to the second optical path 54, and outputs the fourth linearly polarized light CCW2 input from the second optical fiber 16 to the first optical path 53.

[0035] The first beam splitter 51 and the second beam splitter 52 separate the incident light into a P-polarized component and an S-polarized component, and then combine and emit the P-polarized component and the S-polarized component. The first beam splitter 51 and the second beam splitter 52 are, for example, prism-type beam splitters, but may also be flat-type beam splitters or wedge-type beam splitters.

[0036] The first optical path 53 guides the first linearly polarized light CW1 introduced from the first beam splitter 51 to the second beam splitter 52, and also guides the fourth linearly polarized light CCW2 introduced from the second beam splitter 52 to the first beam splitter 51. The second optical path 54 guides the second linearly polarized light CCW2 introduced from the first beam splitter 51 to the second beam splitter 52, and also guides the third linearly polarized light CW2 introduced from the second beam splitter 52 to the first beam splitter 51.

[0037] The first optical path 53 is a PANDA fiber having one end optically connected to the first beam splitter 51 and the other end optically connected to the second beam splitter 52. The second optical path 54 is a PANDA fiber having one end optically connected to the first beam splitter 51 and the other end optically connected to the second beam splitter 52. Note that the first optical path 53 and the second optical path 54 may be polarization maintaining fibers such as a bowtie fiber and an elliptical jacket fiber. A second optical element 55 is disposed in the second optical path 54.

[0038] The second optical element 55 has a first (¼) wave plate 56 , a second (¼) wave plate 57 , and a 45° Faraday rotator 58 .

[0039] The first (1 / 4) wave plate 56 is a 1 / 4 wave plate whose optical axis is inclined at 45 degrees with respect to the slow axis and fast axis of the PANDA fiber forming the second optical path 54. The first (1 / 4) wave plate 56 converts linearly polarized light into circularly polarized light and also converts circularly polarized light into linearly polarized light.

[0040] The second (1 / 4) wave plate 57 is a 1 / 4 wave plate arranged with its optical axis tilted at -45 degrees with respect to the slow axis and fast axis of the PANDA fiber forming the second optical path 54. The second (1 / 4) wave plate 57 converts the circularly polarized light from the 45 degree Faraday rotator 58 into linearly polarized light, and also converts the linearly polarized light into circularly polarized light.

[0041] The 45-degree Faraday rotator 58 is a Faraday rotator that changes the phase of the circularly polarized light incident from each of the first (¼) wave plate 56 and the second (¼) wave plate 57.

[0042] The 45-degree Faraday rotator 58 changes the phase of the circularly polarized light incident from the first (¼) wave plate 46 such that the phase of the second linearly polarized light CCW1 output from the second (¼) wave plate 57 is shifted by 45 degrees from the phase of the second linearly polarized light CCW1 that is the linearly polarized light input to the first (¼) wave plate 56. In addition, the 45-degree Faraday rotator 58 changes the phase of the circularly polarized light such that the phase of the third linearly polarized light CW2 output from the first (¼) wave plate 56 is shifted by −45 degrees from the phase of the third linearly polarized light CW2 input to the second (¼) wave plate 57.

[0043] The detection signal generating unit 60 has a third beam splitter 61, a first light receiving element 62, a second light receiving element 63, and a signal processing circuit 70, and receives the second linearly polarized light branched by the circulator 30. The detection signal generating unit 60 splits the second linearly polarized light into an S-polarized component and a P-polarized component, receives the S-polarized component and the P-polarized component, converts them into electrical signals, and differentially amplifies them to output a detection signal Ed corresponding to the magnetic field applied to the granular thin film 1. The third beam splitter 61 is a polarizing beam splitter (PBS) such as a prism type, a flat type, a wedge substrate type, or an optical waveguide type, and splits the second linearly polarized light branched by the circulator 30 into an S-polarized component 64 and a P-polarized component 65.

[0044] Each of the first light receiving element 62 and the second light receiving element 63 is, for example, a PIN photodiode. The first light receiving element 62 receives an S-polarized component 64, and the second light receiving element 63 receives a P-polarized component 65. Each of the first light receiving element 62 and the second light receiving element 63 photoelectrically converts the received light and outputs an electrical signal corresponding to the amount of light received. The signal processing circuit 70 differentially amplifies the electrical signal indicating the S-polarized component and the electrical signal indicating the P-polarized component, thereby outputting a detection signal Ed corresponding to the magnetic field applied to the granular thin film 1.

[0045] (Granular thin film 1 evaluation method) The granular thin film 1 is evaluated by a figure of merit (FOM), which is the ratio of the magnitude of the Faraday rotation angle to the loss of light passing through the granular thin film 1. As the thickness of the granular thin film 1 increases, the Faraday rotation angle according to the applied magnetic field increases, but the loss of light passing through the granular thin film 1 also increases. By defining the figure of merit FOM as the ratio of the magnitude of the Faraday rotation angle to the loss of light passing through the granular thin film 1, the performance of the granular thin film 1 can be evaluated according to the content ratio of Co and Fe in the magnetic nanoparticles, regardless of the film thickness.

[0046] (Calculation method of figure of merit FOM for granular thin film 1) The figure of merit FOM [° / Oe dB] of the granular thin film 1 is expressed by the following formula (1). Here, M is the magnetic field [Oe] applied to the granular thin film 1, and θ F is the Faraday rotation angle [°] in the granular thin film 1 when a magnetic field M is applied, and P loss is the loss of light passing through the granular thin film 1 [dB].

[0047]

number

[0048] Loss of light passing through granular thin film 1, P loss is expressed by the following formula (2): where T is the transmittance of light passing through the granular thin film 1.

[0049]

number

[0050] (Faraday rotation angle θ of granular thin film 1 F (Method of measurement) Faraday rotation angle θ of granular thin film 1 Fis measured by using the magnetic field sensor device and applying a magnetic field of 1 kOe to the granular thin film 1. At this time, the wavelength of light used is 1550 nm.

[0051] (Method of measuring transmittance T of granular thin film 1) The transmittance T of the granular thin film 1 is measured by a spectrophotometer. The spectrophotometer used to measure the transmittance T of the granular thin film 1 is a Hitachi U4100 spectrophotometer, and the wavelength of light incident on the granular thin film 1 when the transmittance T of the granular thin film 1 is measured is 1550 [nm].

[0052] (Method of measuring the (Co / Fe) atomic ratio in granular thin film 1) The (Co / Fe) atomic ratio in granular thin film 1 was calculated from the amount of each element quantified using EDX (X-ray fluorescence analysis). Similar measurements can also be made using other common surface analysis techniques such as EPMA (electron probe microanalyzer), AES (Auger electron spectroscopy), and XPS (X-ray photoelectron spectroscopy).

[0053] (Method of measuring MgF2 content in granular thin film 1) The content of MgF2 in the granular thin film 1 was also calculated in the same manner as described above.

[0054] (Evaluation of Granular Thin Film 1) Several granular thin films were manufactured in which the main components of the magnetic nanoparticles 3 were Co and Fe, and the main component of the dielectric matrix 2 was BaF, and the FOM was evaluated when the (Co / Fe) atomic ratio of the magnetic nanoparticles and the BaF content were changed.

[0055] In the granular thin films produced, the contents of Co and Fe were adjusted so that the (Co / Fe) atomic ratios of the magnetic nanoparticles were 0.7, 1.2, 3.5, 5.0, 5.5, 6.0, 8.5, 10.0, 15.0, 17.0, 18.0 and 21.0. In addition, the contents of Co and BaF were adjusted so that the content of BaF was 75 at% or more and 90 at% or less. The Faraday rotation angle θ of the granular thin film 1 produced was measured as described above. F The Faraday rotation angle θ based on the measurement by the "Method of measuring the transmittance T of granular thin film 1" and the "Method of measuring the transmittance T of granular thin film 1" F and transmittance T were measured. The measured Faraday rotation angle θ F and transmittance T were used to calculate the figure of merit FOM of each granular thin film based on the above-mentioned equation (1).

[0056] Table 1 shows the composition of the granular thin film, the composition (Co / Fe) atomic ratio of the magnetic nanoparticles, the BaF content [at%], and the figure of merit FOM [° / Oe·dB] for the 12 types of granular thin films produced.

[0057] In addition, the figure of merit FOM [° / Oe·dB] was evaluated for the 12 types of granular thin films produced in Table 1. As mentioned above, the figure of merit FOM was 1.00×10 -4 If the noise level is greater than 1.25×10[° / Oe·dB], the noise level is expected to drop to 10[A] or less, so we marked it as "〇". -4 If the noise level is 5A or less, the symbol "◎" is used because it is considered that the noise level will drop to 5A or less when the figure of merit (FOM) is 1.00×10 -4 If it is less than [° / Oe·dB], the noise level will be high and there is a risk that a magnetic field sensor element for current detection with a high S / N ratio will not be realized, so "X" is entered.

[0058] In Table 1, the granular thin films marked with "◯" and "◎" in the "FOM" column are Examples 1 to 9, and the granular thin films marked with "×" in the "FOM" column are Comparative Examples 1 to 3.

[0059] Here, the reason why the figure of merit FOM is improved in the composition range of the present invention will be explained. Generally, the magnitude of the Faraday rotation angle is proportional to the magnitude of the saturation magnetization of the magnetic film. Therefore, when the Co / Fe ratio is around 1, the saturation magnetization is maximized and the Faraday rotation angle is maximized. However, as the Fe content increases, the light transmission loss also increases, and as a result, the figure of merit FOM decreases. Conversely, when the Fe content is extremely low and Co is the main component, the saturation magnetization is small and the Faraday rotation angle is small, so the figure of merit FOM decreases. On the other hand, FeCo alloys have the property of magnetostriction (the phenomenon in which a magnetic body changes shape when an external magnetic field is applied to magnetize it), and it is known that when the Co / Fe ratio is 4 or more, the magnetostriction decreases significantly and when the Co / Fe ratio is around 15, the magnetostriction becomes zero. In particular, when processed at high temperature, the magnetostriction becomes small when the Co / Fe ratio is in the range of 4 to 15. Since the range of Co / Fe ratios in which magnetostriction is reduced roughly coincides with the range of Co / Fe ratios in which the figure of merit (FOM) of the present invention increases, it is believed that suppressing magnetostriction contributes to improving the figure of merit (FOM).

[0060] [Table 1]

[0061] 4 is a diagram showing the change over time of the current I measured by the magnetic field sensor device 10 using Example 5 as a magnetic field sensor element for current detection. In FIG. 4, the horizontal axis indicates time, the vertical axis indicates the current value, and the waveform W101 is the measurement result of the current flowing through the conductor 14.

[0062] The magnetic field sensor device 10 detects the current value when the current flowing through the conductor 14 transitions from 0 [A] to 100 [A]. The noise superimposed on the current flowing through the conductor 14 via the granular thin film 1 was calculated as a 3σ value of the current value detected during the period from -2 [μs] to 0 [μs] when the current flowing through the conductor 14 was 0 [A].

[0063] In the current I measured by the magnetic field sensor device 10 using Example 5 as a magnetic field sensor element for current detection, the noise was 3.68 A, confirming that a magnetic field sensor element for current detection with a high S / N ratio was realized.

[0064] Fig. 5 is a diagram showing the relationship between the (Co / Fe) atomic ratio and the figure of merit FOM of the granular thin films shown in Examples 1 to 9 and Comparative Examples 1 to 3. In Fig. 5, the horizontal axis shows the (Co / Fe) atomic ratio of Examples 1 to 9 and Comparative Examples 1 to 3, and the vertical axis shows the figure of merit FOM [° / Oe·dB] of the granular thin films. In Fig. 5, Examples 1 to 9 are shown with the symbol P W 1~P W 9, and Comparative Examples 1 to 3 are indicated by the symbol P C 1~P C As shown in 3.

[0065] As shown in Table 1 and FIG. 5, each of Examples 1 to 9 has a figure of merit FOM of 1.00×10 -4 It is possible to realize a magnetic field sensor element for detecting a current having a high S / N ratio with a noise level of 10 [A] or less and a figure of merit FOM of 1.25×10 -4 [° / Oe·dB] or more and a noise level of 5 [A] or less, it is possible to realize a magnetic field sensor element for detecting a current with a higher SN ratio. -4 [° / Oe·dB], and the noise level is 10 [A] or more, making it impossible to realize a magnetic field sensor element for current detection with a high S / N ratio. [Explanation of symbols]

[0066] 1 Granular thin film 2. Dielectric matrix 3. Magnetic Nanoparticles 10. Magnetic field sensor device

Claims

1. A granular thin film having magnetic nanoparticles dispersed in a dielectric matrix, The magnetic nanoparticles are composed of Co and Fe, A granular thin film characterized in that the (Co / Fe) atomic ratio, obtained by dividing the atomic weight of Co contained in the magnetic nanoparticles by the atomic weight of Fe contained in the magnetic nanoparticles, is 1.2 or more and 17.0 or less, and the figure of merit FOM is 1.00 x 10-4 [° / Oe dB] or more.

2. 2. The granular thin film according to claim 1, wherein the (Co / Fe) atomic ratio is 3.5 or more and 10.0 or less, and the figure of merit (FOM) is 1.25×10 −4 [° / Oe·dB] or more.

3. the dielectric matrix comprises BaF; 3. The granular thin film according to claim 1, wherein the content of said BaF in said granular thin film is 75 at % or more and 90 at % or less.

Citation Information

Patent Citations

  • Translucent magnetic material

    JP2017098423A

  • Magnetic field sensor device

    JP2020126006A