Laser welding method and laser welding device
The laser welding method addresses cracks in aluminum alloy welds by gradually reducing power density and adjusting beam parameters, stabilizing the molten pool to enhance weld quality.
Patent Information
- Application Number
- JP2023050485
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
AI Technical Summary
Laser welding of aluminum alloy materials or aluminum die-cast products often results in cracks at the end of the bead due to rapid temperature changes and tensile forces during the welding process.
A laser welding method that includes multiple steps to gradually reduce power density and adjust the laser beam's power and spot size, such as by defocusing, intermittent irradiation, and spiral scanning, to stabilize the molten pool and suppress temperature changes.
The method significantly reduces the occurrence of cracks at the end of the bead by maintaining the molten pool in a stable state, thereby improving the quality of the weld.
Smart Images

Figure 2024139513000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a laser welding method and a laser welding apparatus. [Background technology]
[0002] Laser welding by irradiating laser light is known as one of the techniques for welding workpieces made of metallic materials (see, for example, Patent Document 1). Laser welding is a technique in which a surface of a workpiece is irradiated with laser light, multiple members are partially melted by the energy of the laser light, and then solidified to form a weld, thereby joining multiple members via the weld. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2022-069169 A Summary of the Invention [Problem to be solved by the invention]
[0004] The inventors' research has revealed that in laser welding of processing objects in which at least one of multiple components is made of an aluminum alloy material or an aluminum die-cast product, if the processing object is scanned while being irradiated with laser light, cracks are likely to occur at the end of the bead formed by the scanning.
[0005] Therefore, one object of the present invention is to provide a new and improved laser welding method and laser welding apparatus that is less likely to cause cracks at the end of the bead. [Means for solving the problem]
[0006] The laser welding method of the present invention is, for example, a laser welding method for laser welding a plurality of members including an aluminum alloy material or an aluminum die-cast product as a processing target by irradiating a laser beam, and includes a first step of scanning the surface of the processing target while irradiating the laser beam on the surface, and a second step of scanning the surface after the first step while irradiating the surface with the laser beam at a power density lower than that of the first step before stopping the irradiation of the laser beam.
[0007] The laser welding method may include a third step of irradiating the laser light onto a fixed point on the surface after the second step and before stopping the irradiation of the laser light.
[0008] The laser welding method may include a fourth step of irradiating the surface with the laser light while rotating the laser light around a fixed point on the surface, after the second step and before stopping the irradiation of the laser light.
[0009] In the laser welding method, the second step may include the step of reducing a power density by reducing a power of the laser light from a conventional power.
[0010] In the laser welding method, the second step may include a step of reducing power density by expanding a spot size of the laser light on the surface by defocusing.
[0011] In the laser welding method, the second step may include a step of lowering the power density by changing the power of the laser light and widening the spot size of the laser light on the surface by defocusing.
[0012] In the laser welding method, the second step may include a plurality of steps of gradually decreasing the power density of the laser light.
[0013] In the laser welding method, the second step may include a step of decreasing a power density of the laser light over time.
[0014] In the laser welding method, in the third step, the laser beam may be irradiated at a power density lower than that in the second step.
[0015] In the laser welding method, in the fourth step, the laser beam may be scanned in a spiral manner while a turning radius of the laser beam is reduced over time.
[0016] The laser welding method may include a step of intermittently irradiating the laser light onto the surface at a predetermined frequency.
[0017] In the laser welding method, the laser light may include a plurality of beams, and the beams may form a power region on a surface of the object to be processed.
[0018] The laser welding apparatus of the present invention is, for example, a laser welding apparatus that irradiates laser light to laser-weld a plurality of members including an aluminum alloy material or an aluminum die-cast product as a processing object, and is equipped with a laser device that outputs the laser light, an optical head that irradiates the laser light output from the laser device onto a surface of the processing object, a scanning mechanism that relatively scans the surface with the laser light irradiated onto the surface, and a power density changing mechanism that changes the power density of the laser light on the surface, and performs a first step of scanning the surface of the processing object while irradiating it with the laser light, and a second step of scanning the surface while irradiating it with a power density lower than that of the first step after the first step and before stopping the irradiation of the laser light.
[0019] In the laser welding apparatus, the power density changing mechanism may change the power density by changing the power of the laser light.
[0020] In the laser welding method, the power density changing mechanism may change the power density by changing a spot size of the laser light on the surface by defocusing. Effect of the Invention
[0021] According to the present invention, for example, it is possible to obtain a novel and improved laser welding method and laser welding apparatus that is less likely to cause cracks at the end of the bead. [Brief description of the drawings]
[0022] [Figure 1] FIG. 1 is an exemplary schematic configuration diagram of a laser welding device according to a first embodiment. [Diagram 2] FIG. 2 is a diagram showing an example of changes over time in the position and power density of a laser beam spot in the laser welding method of the reference example. [Diagram 3] FIG. 3 is an exemplary photographic image showing a bead formed on a surface of a workpiece by the laser welding method of the reference example. [Figure 4] FIG. 4 is a diagram showing an example of changes over time in the position and power density of the laser beam spot in the laser welding method according to the first embodiment. [Diagram 5] FIG. 5 is a diagram showing another example of the change over time in the position and power density of the laser beam spot in the laser welding method according to the first embodiment, different from that in FIG. [Figure 6] FIG. 6 is a diagram showing another example of the change over time in the position and power density of the laser beam spot in the laser welding method according to the first embodiment, different from those shown in FIGS. [Figure 7] FIG. 7 is a diagram showing another example of the change over time in the position and power density of the laser beam spot in the laser welding method according to the first embodiment, different from those shown in FIGS. [Figure 8] FIG. 8 is a diagram showing another example of the change over time in the position and power density of the laser beam spot in the laser welding method according to the first embodiment, different from those shown in FIGS. [Figure 9] FIG. 9 is a schematic plan view showing an example of a scanning trajectory near the end of scanning of a laser beam in the laser welding method according to the first embodiment. [Figure 10] FIG. 10 is an exemplary schematic configuration diagram of the laser welding device according to the second embodiment. [Figure 11]FIG. 11 is an explanatory diagram showing the concept of the principle of the diffractive optical element included in the laser welding apparatus of the second embodiment. [Figure 12] FIG. 12 is an illustrative schematic plan view of a laser light spot formed on the surface of an object to be processed by the laser welding device of the second embodiment. [Figure 13] FIG. 13 is an exemplary schematic configuration diagram of the laser welding device according to the second embodiment. [Figure 14] FIG. 14 is an illustrative schematic plan view of a laser light spot formed on the surface of an object to be processed by the laser welding device of the third embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] Exemplary embodiments of the present invention are disclosed below. The configurations of the embodiments shown below, and the actions and results (effects) brought about by the configurations are merely examples. The present invention can be realized by configurations other than those disclosed in the following embodiments. Furthermore, according to the present invention, it is possible to obtain at least one of the various effects (including derivative effects) obtained by the configurations.
[0024] The embodiments described below have similar configurations. Therefore, according to the configurations of the respective embodiments, similar actions and effects based on the similar configurations can be obtained. In addition, in the following, the similar configurations are given the same reference numerals, and duplicated descriptions may be omitted.
[0025] In each drawing, the X direction is represented by an arrow X, the Y direction is represented by an arrow Y, and the Z direction is represented by an arrow Z. The X direction, the Y direction, and the Z direction intersect with each other and are perpendicular to each other. The Z direction is, for example, the normal direction of the surface Wa (machining surface) of the processing object W.
[0026] In this specification, ordinal numbers are given for the sake of convenience to distinguish between processes and the like, and do not indicate priority or order, nor do they limit the number.
[0027] [First embodiment] 1 is a schematic configuration diagram of a laser welding apparatus 100A (100) according to the first embodiment. As shown in FIG. 1, the laser welding apparatus 100 includes a laser device 111, an optical fiber 130, an optical head 120A (120), and a position adjustment mechanism 140.
[0028] The laser device 111 has a laser oscillator as a light source, and is configured to be able to output laser light with a power of several kW, for example. The laser device 111 may also be configured to have a plurality of semiconductor laser elements therein, and to be able to output multimode laser light with a power of several kW as the total output of the plurality of semiconductor laser elements. The laser device 111 may also be equipped with various laser light sources, such as a fiber laser, a YAG laser, and a disk laser.
[0029] The laser device 111 outputs laser light having a wavelength of, for example, 800 [nm] or more and 1200 [nm] or less. The laser device 111 may also be referred to as a first laser device, and the laser oscillator of the laser device 111 may also be referred to as a first laser oscillator. The laser light output by the laser device 111 may also be referred to as a first laser light.
[0030] The optical fiber 130 guides the laser light output from the laser device 111 to the optical head 120 .
[0031] The optical head 120 is an optical device for irradiating the laser light input from the laser device 111 via the optical fiber 130 toward the workpiece W. The optical head 120 includes a collimator lens 121, a condenser lens 122, a mirror 123, a galvanometer scanner 126, and a focusing mechanism 127. The collimator lens 121, the condenser lens 122, the mirror 123, the galvanometer scanner 126, and the focusing mechanism 127 may also be referred to as optical components.
[0032] The collimating lens 121 collimates the laser light input via the optical fiber 130. The collimated laser light becomes parallel light.
[0033] Mirror 123 reflects the laser light that has been collimated by collimator lens 121. The laser light reflected by mirror 123 travels toward focus mechanism 127. Depending on the layout of optical components within optical head 120, mirror 123 may not be necessary.
[0034] The focus mechanism 127 includes a lens 127a and a driving mechanism 127b. The driving mechanism 127b changes the position of the lens 127a in the optical axis direction to change the beam diameter of the laser light.
[0035] The galvano scanner 126 has two mirrors 126a and 126b, and is a device that can control the angles of the two mirrors 126a and 126b to move the irradiation position of the laser light L on the surface Wa of the processing object W and scan the surface Wa with the laser light L. The angles of the mirrors 126a and 126b can be changed by actuators (not shown) including, for example, motors.
[0036] The condenser lens 122 condenses the laser light that has passed through the focus mechanism 127 and the galvano scanner 126, and irradiates the laser light to be processed W as laser light L (output light).
[0037] The position adjustment mechanism 140 is configured to be able to change the position of the optical head 120 relative to the workpiece W.
[0038] The laser welding apparatus 100 can scan a spot of the laser light L on the surface Wa of the workpiece W by operating at least one of the galvano scanner 126 and the position adjustment mechanism 140. The galvano scanner 126 and the position adjustment mechanism 140 are an example of a scanning mechanism.
[0039] The workpiece W has a plurality of members each made of a metal material. At least one of the plurality of members constituting the workpiece W of the laser welding apparatus 100 of this embodiment, particularly the member having the surface Wa to be irradiated with the laser light L, is made of an aluminum alloy material or an aluminum die-cast product.
[0040] [Reference example] Fig. 2 is a diagram showing an example of the change over time in the position (scanning distance) along the scanning direction of the spot of the laser light and the power density in the laser welding method of the reference example. As shown in Fig. 2, in the laser welding of the reference example, the irradiation of the laser light L is started at time ts, the irradiation of the laser light is stopped at time te, and the spot of the laser light L is scanned on the surface Wa at a constant speed and a constant power density from time ts to time te.
[0041] FIG. 3 is an exemplary photographic image showing the vicinity of the end Bde of the bead Bd formed on the surface Wa of the workpiece W by the laser welding method of the reference example shown in FIG. 2, that is, a plan view of the vicinity of the end Bde when viewed in the opposite direction to the Z direction. Through intensive research by the inventors, it has been found that cracks Ck are more likely to occur at the end Bde of the bead Bd than at the middle part of the bead Bd. In the middle part of the bead Bd, a molten pool having unsolidified fluidity exists adjacent to a part where the molten pool is cooled and solidified (hereinafter simply referred to as a solidified part), so that a large tensile force is unlikely to occur at the solidified part. In contrast, at the end Bde of the bead Bd, there is no unsolidified molten pool adjacent to the solidified part, and the solidified part is surrounded by the base material, so it is presumed that cracks Ck occur due to the tensile force between the solidified part and the base material when the solidified part solidifies. Furthermore, through intensive research by the inventors, it was found that when at least one of the multiple components constituting the workpiece W, as in this embodiment, particularly the component having the surface Wa to be irradiated with the laser light L, is made of an aluminum alloy material or an aluminum die-cast product, cracks Ck are more likely to occur than when it is made of other metal materials.
[0042] As a result of extensive research, the inventors have found that the cracks Ck can be reduced by changing the power density and irradiation position over time as described below.
[0043] [Time-dependent change pattern (1)] Fig. 4 illustrates a time-dependent change pattern (1) of the power density at the position (scanning distance) along the scanning direction on the surface Wa of the spot of the laser light and at the center position of the spot in the welding method of the first embodiment. In the example of Fig. 4, the laser welding method has a first step S1 from time ts to time t1 and a second step S2 from time t1 to time te.
[0044] In the first step S1, the laser welding apparatus 100 scans the surface Wa of the workpiece W while irradiating it with the laser light L. In the first step S1, the power density is constant.
[0045] In the second step S2, after the first step S1 and before the irradiation of the laser light L is stopped, the laser light L is irradiated and scanned on the surface Wa of the object W to be processed at a power density lower than that in the first step S1.
[0046] It was found that the number of cracks Ck generated can be significantly reduced by providing the second step S2 as described above, compared to the reference example (FIG. 2). This is presumably because the rapid temperature change at the terminal end Bde can be suppressed.
[0047] 4, the power density on the surface Wa is changed by changing the power of the laser light output from the laser device 111. As an example, if the laser device 111 has an optical amplifier, the power of the laser light output from the laser device 111 can be changed relatively easily by adjusting the power supplied to the optical amplifier. The laser device 111 is an example of a power density changing mechanism.
[0048] As described above, according to the example of FIG. 4, the laser welding method includes a first step S1 and, after the first step S1, a second step S2 in which, before stopping the irradiation of the laser light L, the laser light L is irradiated and scanned over the surface Wa of the workpiece W at a power density lower than that of the first step S1, thereby making it possible to reduce the number of cracks Ck that occur at the terminal end Bde.
[0049] In the example of Fig. 4, the second step S2 includes a step of gradually decreasing the power density of the laser beam L over time from time t1 to time t2, and a step of maintaining the power density of the laser beam L constant at a lower power density than that of the first step S1 from time t2 to time te. If the temperature of the molten pool changes suddenly, the molten pool may become unstable and spatters may easily occur. In this regard, in the example of Fig. 4, the step of gradually decreasing the power density of the laser beam L over time has the advantage of suppressing sudden changes in the temperature of the molten pool, thereby suppressing the occurrence of spatters.
[0050] [Changes over time (2)] Fig. 5 illustrates a time-dependent change pattern (2) of the power density at the position (scanning distance) along the scanning direction on the surface Wa of the spot of the laser light and at the center position of the spot in the welding method of the first embodiment. In the example of Fig. 5, the laser welding method has a first step S1 from time ts to time t1, a second step S2 from time t1 to time t3, and a third step S3 from time t3 to time te.
[0051] The first step S1 and the second step S2 are the same as those in the example of Fig. 4. Therefore, in this case as well, the same effects as those in the example of Fig. 4 can be obtained.
[0052] In the third step S3, the laser light L is irradiated to a fixed point on the surface Wa for a predetermined time before stopping the irradiation of the laser light L. In the example of Fig. 5, the power density in the third step S3 is lower than the power density in the first step S1 and is the same as the power density in the second step S2.
[0053] It was found that by performing such a third step S3, the number of cracks Ck that occurred could be reduced compared to the example in Fig. 4. This is presumably because the third step S3 maintains the molten pool in a molten state for a predetermined period of time, thereby further suppressing a sudden temperature change at the termination portion Bde.
[0054] 5, the power density is decreased from time t1 to time t2 in the second step S2 by shifting the focal position of the laser light L in the Z direction or in the opposite direction to the Z direction to increase the spot diameter, in other words, by defocusing. The focal position is changed by operating the focus mechanism 127. The spot diameter includes the peak of the spot and is 1 / e of the peak intensity. 2 The diameter of the region having the intensity equal to or greater than the power density can be defined as the diameter of the region having the intensity equal to or greater than the power density. The focus mechanism 127 is an example of a power density changing mechanism.
[0055] In this case, the laser light L heats not only the molten pool that is the terminal portion Bde, but also the peripheral portion of the molten pool in the base material. This reduces the Young's modulus of the peripheral portion, making it easier to stretch, and therefore prevents the tensile force of the solidified portion from increasing when the solidified portion cools, compared to when the peripheral portion is not heated, and thus reduces the number of cracks Ck.
[0056] The change in power density can be performed by at least one of changing the power of the laser light output from the laser device 111 and changing the focal position by operating the focus mechanism 127. The change in power density may also be performed by a combination of changing the power of the laser light output from the laser device 111 and changing the focal position by operating the focus mechanism 127. In this case, for example, by appropriately increasing the power while enlarging the spot diameter, a more preferable decrease in power density over time can be obtained, and thus the occurrence of cracks Ck can be further suppressed.
[0057] In addition, the power density may be gradually decreased in the second step S2 and the third step S3. In this case, too, a more preferable decrease in the power density over time may be obtained, and the occurrence of cracks Ck may be further suppressed.
[0058] [Changes over time (3)] Fig. 6 illustrates a time-dependent change pattern (3) of the power density at the position (scanning distance) along the scanning direction on the surface Wa of the spot of the laser light and at the center position of the spot in the welding method of the first embodiment. In the example of Fig. 6, the laser welding method has a first step S1 from time ts to time t1, a second step S2 from time t1 to time t3, and a third step S3 from time t3 to time te, similar to the case of Fig. 5.
[0059] However, as is clear from a comparison of Fig. 6 with Fig. 5, in the example of Fig. 6, the power density in the third step S3 is set lower than in the case of Fig. 5. That is, in the example of Fig. 6, the power density in the third step S3 is lower than the power density in the first step S1 and is also lower than the power density in the second step S2.
[0060] According to the example of FIG. 6, the number of cracks at the terminal end Bde can be reduced more than in the examples of FIG. 4 and FIG.
[0061] [Changes over time (4)] Fig. 7 illustrates a time-dependent change pattern (4) of the power density at the position (scanning distance) along the scanning direction on the surface Wa of the spot of the laser light and at the center position of the spot in the welding method of the first embodiment. In the example of Fig. 7, the laser welding method has a first step S1 from time ts to time t1, a second step S2 from time t1 to time t3, and a third step S3 from time t3 to time te, similar to the case of Fig. 6.
[0062] 7, the laser light L is intermittently irradiated onto the surface Wa at a predetermined frequency in the first step S1, the second step S2, and the third step S3. In this case, the power density can be adjusted by setting the intermittent frequency and the duty ratio indicating the ratio of the irradiation time to one cycle, which has the advantage of making it easier to set more suitable conditions depending on, for example, the material of the workpiece W and the surrounding environment. According to the inventors' intensive research, it has been found that the intermittent frequency is preferably 5 [kHz] or more and 10 [kHz] or less, and the duty ratio indicating the ratio of the irradiation time to one cycle is preferably 60 [%] or more and 95 [%] or less.
[0063] In the example of FIG. 7, the power density is gradually reduced in stages or over time in the third step S3, but this is not limiting, and the power density may be the same as that in the second step S2.
[0064] According to the example of FIG. 7, the number of cracks at the terminal end Bde was able to be reduced more than in the examples of FIG. 4, FIG. 5, and FIG.
[0065] [Changes over time (5)] Fig. 8 illustrates a time-dependent change pattern (5) of the power density at the position (scanning distance) along the scanning direction on the surface Wa of the spot of the laser light and at the center position of the spot in the welding method of the first embodiment. In the example of Fig. 8, the laser welding method has a first step S1 from time ts to time t1 and a second step S2 from time t1 to time t3, as in the case of Fig. 6. However, in the example of Fig. 8, after the second step S2, a fourth step S4 is included in which the laser light L is irradiated while rotating around a fixed point on the surface Wa before the irradiation of the laser light L is stopped.
[0066] Fig. 9 is a plan view showing an example of a scanning trajectory Pt near the end of the scan in the fourth step S4 of Fig. 8. As shown in Fig. 9, in this example, the spot of the laser light L is scanned in a spiral shape while the turning radius is reduced over time toward the end Pte of the scanning trajectory Pt. A terminal end Bde of the bead Bd is formed on the spiral scanning trajectory Pt. In the vicinity of the end Pte, the laser light L scans the molten pool (solidified portion).
[0067] It was found that the number of cracks Ck generated can be further reduced by performing the fourth step S4. This is presumably because the fourth step S4 keeps the molten pool near the end portion Bde in a molten state for a predetermined period of time, thereby further suppressing abrupt temperature changes at the end portion Bde.
[0068] Furthermore, as shown in Figure 9, by scanning in a spiral manner while gradually decreasing the rotation radius over time, the temperature of the molten pool (solidified portion) forming the terminal portion Bde can be gradually reduced from the peripheral portion to the central portion, and it is estimated that the occurrence of cracks Ck at the terminal portion Bde can be further suppressed.
[0069] In addition, the spiral scan in Fig. 9 may be performed by gradually increasing the turning radius from the center to the periphery over time, so as to proceed in the opposite direction to the scanning trajectory Pt in Fig. 9. In this case, too, the temperature of the molten pool (solidified portion) forming the terminal end Bde can be gradually decreased from the center to the periphery, so that it is estimated that the occurrence of cracks Ck in the terminal end Bde can be further suppressed.
[0070] 8 and 9, the number of cracks in the terminal end portion Bde was able to be reduced more than in the examples of FIGS. 4, 5, 6, and 7.
[0071] As described above, according to this embodiment, the laser welding method includes a first step S1 and, after the first step S1, a second step S2 in which, before stopping the irradiation of the laser light L, the laser light L is irradiated and scanned over the surface Wa of the workpiece W at a power density lower than that of the first step S1, thereby making it possible to reduce the number of cracks Ck that occur at the terminal end Bde.
[0072] [Second embodiment] 10 is a schematic diagram of a laser welding apparatus 100B (100) of the second embodiment. In this embodiment, an optical head 120B (120) has a diffractive optical element 125 (hereinafter referred to as DOE 125) between a collimator lens 121 and a mirror 123. Except for this point, the laser welding apparatus 100B has a similar configuration to the laser welding apparatus 100A of the first embodiment.
[0073] The DOE 125 shapes the shape of a laser beam (hereinafter referred to as the beam shape). Fig. 11 is an explanatory diagram showing the concept of the principle of the DOE 125. As shown in Fig. 11, the DOE 125 has a configuration in which, for example, a plurality of diffraction gratings 125a with different periods are superimposed. The DOE 125 can shape the beam shape by bending parallel light in a direction influenced by each diffraction grating 125a or by superimposing the diffraction gratings 125a. The DOE 125 can also be called a beam shaper.
[0074] FIG. 12 is an exemplary schematic plan view of a spot S of the laser light L formed on the surface Wa of the workpiece W. As shown in FIG. 12, the laser light L can form an irradiation area of a plurality of beams Bm on the surface Wa by the action of the DOE 125. In the example of FIG. 12, the plurality of beams Bm form a power area formed by four beams Bm gathered in the center on the surface Wa, and a substantially annular power area formed by twelve beams Bm surrounding the power area. By appropriately designing the DOE 125, various power areas having different specifications such as the number of beams, the arrangement of the beams, the shape, the size, and the power density can be formed on the surface Wa, not limited to the example shown in FIG. 12. In addition, in a configuration having the DOE 125, a wider spot S can be easily formed on the surface Wa, and a wider range of the peripheral portion of the molten pool can be easily heated, compared to a configuration not having the DOE 125. Therefore, according to this embodiment, the occurrence of a crack Ck at the terminal end Bde can be further suppressed.
[0075] [Third embodiment] 13 is a schematic diagram of a laser welding apparatus 100C (100) according to the third embodiment. As shown in FIG. 13, the laser welding apparatus 100C includes the same components as the laser welding apparatus 100A according to the first embodiment, and also includes a laser device 112, an optical fiber 130, a collimating lens 121-2, and a filter 124.
[0076] The laser device 112 has a laser oscillator as a light source, and outputs a laser light having a wavelength different from that of the laser device 111. As an example, the laser device 112 outputs a laser light having a wavelength of 550 [nm] or less, preferably a laser light having a wavelength of 400 [nm] or more and 500 [nm] or less. The laser device 112 may also be called a second laser device, and the laser oscillator of the laser device 112 may also be called a second laser oscillator. The laser light output by the laser device 112 may also be called a second laser light. The laser device 112 may also operate as a power density changing mechanism.
[0077] The filter 124 is a high-pass filter that transmits the laser light output from the laser device 111 and reflects the laser light output from the laser device 112 without transmitting it.
[0078] The laser light that has passed through the filter 124 passes through a focus mechanism 127, a galvanometer scanner 126, and a condenser lens 122, and is then irradiated onto a surface Wa of the workpiece W. The laser light output from the optical head 120C and irradiated onto the surface Wa contains two laser lights with different wavelengths, i.e., the laser light output by the laser device 111 and the laser light output by the laser device 112.
[0079] The absorptance of blue or green laser light, i.e., laser light with a wavelength of 400 [nm] or more and 550 [nm] or less, in metallic materials is higher than the absorptance of infrared laser light, i.e., laser light with a wavelength of 800 [nm] or more and 1200 [nm] or less, in metallic materials. Therefore, according to this embodiment, by efficiently heating the workpiece W with blue or green laser light and forming a relatively deep keyhole in the workpiece W with infrared laser light, it is possible to efficiently form a molten pool in the workpiece W while suppressing abrupt temperature changes depending on the location of the surface Wa. By suppressing abrupt temperature changes depending on the location of the surface Wa, the molten pool is stabilized and the occurrence of spatters can be suppressed. Therefore, according to this embodiment, highly efficient and high-quality welding can be realized.
[0080] 14 is a plan view of a spot S of laser light L formed on a surface Wa. The laser light L includes a beam Bm1 of laser light output from a laser device 111 and a beam Bm2 of laser light output from a laser device 112, and an irradiation area (power area) corresponding to the beams Bm1 and Bm2 is formed on the surface Wa. The irradiation area by the beam Bm2 is wider than the irradiation area by the beam Bm1, and at least partially includes the irradiation area by the beam Bm1.
[0081] Research by the inventors has revealed that this embodiment can further suppress the occurrence of cracks Ck at the terminal end Bde. This is presumably because the beam Bm2, which has a higher absorption rate, can heat the peripheral part of the molten pool formed mainly by the beam Bm1, so that the temperature of the molten pool (solidified part) forming the terminal end Bde can be gradually lowered from the peripheral part to the center part.
[0082] Although the embodiment of the present invention has been illustrated above, the above embodiment is merely an example and is not intended to limit the scope of the invention. The above embodiment can be implemented in various other forms, and various omissions, substitutions, combinations, and modifications can be made without departing from the gist of the invention. In addition, the specifications of each configuration, shape, and the like (structure, type, direction, model, size, length, width, thickness, height, number, arrangement, position, material, etc.) can be appropriately changed and implemented. [Explanation of symbols]
[0083] 100, 100A~100C...Laser welding equipment 111, 112...Laser device (power density changing mechanism) 120, 120A~120C...Optical head 121, 121-1, 121-2...Collimating lenses 122...Condenser lens 123…Mirror 124…Filter 125...DOE (diffractive optical element) 125a...Diffraction grating 126...Galvano scanner (scanning mechanism) 126a, 126b…Mirror 127…Focus mechanism 127a...Lens 127b...Drive mechanism 130...Optical fiber 140...Position adjustment mechanism (scanning mechanism) Bd…Bead Bde…Terminal part Bm, Bm1, Bm2...Beam (irradiation area, power area) Ck...Crack L: Laser light Pt…Scanning trajectory Pte…Terminal S…Spot S1…first process S2…Second process S3…Third process S4…Fourth process t1,t2,t3,ts,te…time W…Processing target Wa…Surface X…direction Y...Direction Z…direction
Claims
1. A laser welding method for laser welding a plurality of members including an aluminum alloy material or an aluminum die-cast product as a processing target by irradiating a laser beam, comprising: a first step of scanning the laser light on a surface of the object to be processed while irradiating the surface with the laser light; a second step of scanning the surface with the laser light while irradiating the surface with the laser light at a power density lower than that of the first step, before stopping the irradiation of the laser light after the first step; A laser welding method comprising:
2. 2. The laser welding method according to claim 1, further comprising a third step of irradiating the fixed point on the surface with the laser light after the second step and before stopping the irradiation of the laser light.
3. 2. The laser welding method according to claim 1, further comprising a fourth step of irradiating the surface with the laser light while rotating the laser light around a fixed point on the surface after the second step and before stopping the irradiation of the laser light.
4. The laser welding method according to claim 1 , wherein the second step includes the step of reducing a power density of the laser beam by reducing a power of the laser beam from a power density of the laser beam.
5. 2. The laser welding method according to claim 1, wherein the second step includes the step of reducing a power density by defocusing the laser beam to increase a spot size of the laser beam on the surface from a conventional spot size.
6. 2. The laser welding method according to claim 1, wherein the second step includes a step of lowering a power density by changing a power of the laser beam and defocusing the laser beam to increase a spot size of the laser beam on the surface from a previous spot size.
7. 7. The laser welding method according to claim 1, wherein the second step includes a plurality of steps of gradually decreasing the power density of the laser beam.
8. 7. The laser welding method according to claim 1, wherein the second step includes a step of decreasing a power density of the laser beam over time.
9. The laser welding method according to claim 2 , wherein in the third step, the laser beam is irradiated at a power density lower than that in the second step.
10. The laser welding method according to claim 3 , wherein in the fourth step, the laser beam is scanned in a spiral manner while a turning radius of the laser beam is reduced over time.
11. 4. The laser welding method according to claim 1, further comprising the step of intermittently irradiating the surface with the laser light at a predetermined frequency.
12. the laser light includes a plurality of beams; 4. The laser welding method according to claim 1, wherein the beam forms a power field on the surface of the workpiece.
13. A laser welding device that irradiates a laser beam to laser-weld a plurality of members including an aluminum alloy material or an aluminum die-cast product as a processing target, A laser device that outputs the laser light; an optical head that irradiates a surface of the object to be processed with a laser beam output from the laser device; a scanning mechanism for relatively scanning the laser light irradiated onto the surface on the surface; a power density changing mechanism for changing a power density of the laser light on the surface; Equipped with a first step of scanning the laser light on a surface of the object to be processed while irradiating the surface with the laser light; a second step of scanning the surface with the laser light while irradiating the surface with the laser light at a power density lower than that of the first step, before stopping the irradiation of the laser light after the first step; Laser welding equipment.
14. The laser welding apparatus according to claim 13, wherein the power density changing mechanism changes the power density by changing the power of the laser light.
15. 15. The laser welding apparatus according to claim 13, wherein the power density changing mechanism changes the power density by changing a spot size of the laser light on the surface by defocusing.
Citation Information
Patent Citations
Welding method and structure
JP2022069169A
Spiral laser welding methods for joining metal
WO2022253568A1