Metal resin composite powder and method for producing non-sintered curable metal molding
The metal-resin composite powder addresses the energy and environmental challenges of conventional metal powder metallurgy by using low-pressure, low-temperature curing to produce strong and smooth metal products without sintering, enhancing bonding and surface quality.
Patent Information
- Application Number
- JP2023065243
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
AI Technical Summary
Conventional metal powder metallurgy and metal injection molding processes require high energy consumption, complex equipment, and involve sintering processes that can lead to environmental issues and low strength of the final products, especially when handling fine irregularities and smooth surfaces.
A metal-resin composite powder is created by surface-treating metal powder with a compound having multiple reactive groups and combining it with a thermosetting resin, allowing for low-pressure, low-temperature curing without sintering, using a thermosetting resin as a binder to enhance bonding and improve surface smoothness.
This method reduces energy costs and environmental impact by eliminating the need for high-pressure and high-temperature sintering, while producing metal products with improved surface smoothness and strength through low-temperature curing.
Smart Images

Figure 2024139645000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a metal-resin composite powder used for a cured molded body of metal powder that does not require a sintering step, a thermosetting metal molded body obtained through a hot low-pressure compression molding and a thermosetting step, and a method for producing the same. [Background technology]
[0002] Conventionally, metal products shaped to meet required characteristics are formed by punching, bending, cutting, and other processes from flat or rod-shaped metal ingots using processing equipment appropriate for the process.
[0003] On the other hand, products that require mass production are manufactured using powder metallurgy, in which metal powder is compressed at high pressure using a mold that corresponds to the shape, and then sintered in a furnace where the temperature and atmosphere are controlled. [Prior art documents]
[0004] [Patent Document 1] JP 2008-150648 A [Patent Document 2] JP 2011-140535 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, the pressure in the compression molding process used in the powder metallurgical manufacturing process as shown in Patent Document 1 is usually 5 to 9 tons / cm 2 However, high pressure is required, and since the metal powders are not chemically bonded to each other, a sintering process is necessary as the next step to increase the bonding strength between the metal powders. In this process, a sintering process is required in a furnace at 500°C to 1200°C, where the temperature profile is controlled to increase the temperature, keep the temperature constant, and cool for about 4 to 6 hours. This poses challenges in terms of energy consumption and decarbonization. In addition, the strength of the molded product is low and it may be damaged when transferred to the sintering furnace in the next process, so care must be taken when handling it.
[0006] Furthermore, as shown in Patent Document 2, metal powder injection molding (MIM) is being carried out in which multiple organic binders and metal powder are made into composite pellets, which are then injection molded and then sintered in the same way as in Patent Document 1. However, this method requires a degreasing process in which the binders added to achieve the fluidity and shape formation necessary during injection molding are decomposed and removed before the sintering process. In this process, the temperature must be raised in stages from room temperature to around 600°C in accordance with the decomposition temperatures of the multiple binders contained in an inert atmosphere, and then the temperature must be raised to over 1000°C in the sintering furnace. Therefore, there are more issues than those in Reference 1, including the equipment and process management aspects in the debinding and sintering processes.
[0007] The object of this invention is to provide a metal-resin composite powder for compression molding and a thermosetting metal molded product, and a manufacturing method for the same, in which coarse powders larger than a specified particle size have been removed in order to produce an optimal thermosetting molded product as a metal product with fine irregularities and a smooth surface condition, by using metal powder equivalent to that used in conventional powder metallurgy, through low-pressure molding and low-temperature hardening processes, which do not require special equipment or high energy, and which can be completed at a significantly lower temperature and in a shorter number of labor hours than powder metallurgy and MIM, thereby making a significant contribution to energy costs and environmental issues. [Means for solving the problem]
[0008] In order to achieve the above-mentioned objective, the material composition of the present invention is formed by combining a metal powder that has been surface-treated with a compound having multiple reactive groups in its molecules that chemically bond to inorganic and organic materials, and a thermosetting resin that has a B-stage (semi-cured state) that exhibits a certain plastic state during the middle stage of the curing reaction.
[0009] The metal powder may contain one or more metals selected from iron, aluminum, tungsten, stainless steel, titanium, zinc, tin, copper, lead, magnesium, chromium, cobalt, nickel, zirconium, molybdenum, silver, neodymium, platinum, gold, and samarium. The above metal powders are granulated by a reduction method, an electrolytic method, an atomization method or the like depending on the intended use, and coarse powder and fine powder of a certain particle size are removed so as to obtain a specified particle size distribution, and the maximum particle size is generally controlled to be 105 to 212 μm.
[0010] In order to improve the bonding strength of the thermosetting metal compact, the metal powder of the present invention is classified to remove coarse powder with a particle size of 100 μm or more, preferably 90 μm or more, and is surface-treated with a surface treatment agent having multiple different reactive groups in its molecule to improve the bonding strength with the thermosetting resin that is mixed to form the thermosetting metal compact.
[0011] The surface-treated metal powder is given high fluidity during molding, and in order to increase shape reproducibility and solidification after molding, resulting in a high-density structure, a resin component consisting of epoxy resin or polyester resin as the main component, amine-based or isocyanate-based hardeners, and additives is added and mixed at a ratio of 20 wt% or less, and the kneaded composite material in a paste state plasticized at a certain heating temperature is crushed and classified to produce a metal-resin composite powder.
[0012] Alternatively, surface-treated metal powder is mixed with epoxy resin or polyester resin as the main component, and an amine or isocyanate curing agent and additives are added to a solvent such as methyl ethyl ketone, which vaporizes at a low temperature of around 100°C, to obtain a slurry. The slurry is then flattened using a doctor blade or the like, and the solvent is vaporized to obtain a plate-shaped solidified material, which is then crushed and classified to produce a metal-resin composite powder.
[0013] After the plasticized paste kneaded composite material or solvent mixed composite material is crushed, the metal resin composite powder from which the coarse powder has been removed is put into the space of a mold consisting of upper and lower punches and a die processed according to the product shape, and is molded under low pressure at or above the B stage temperature, and then cooled.
[0014] The equipment used for pressure molding is equipped with a mechanism for controlling the heating and cooling of the mold. A mold containing metal-resin composite powder is installed, and the mechanism controls the temperature range above and below the heat distortion temperature at which the thermosetting resin enters a plastic state (B-stage region), applying pressure at the upper limit and cooling to the lower limit, allowing the solidified molded body to be released from the mold.
[0015] The upper limit temperature for pressure molding is desirably 10°C above the heat distortion temperature and below the curing start temperature of 30°C, and the lower limit temperature for demolding is desirably 20°C below the heat distortion temperature, and these are determined based on the shape and dimensions of the molded product to be formed in the mold and productivity.
[0016] In general powder metallurgy compression molding, in order to increase the final sintering strength, the usual sintering rate is 5 to 9 ton / cm for iron-based materials. 2 In contrast, the process of the present invention requires a high pressure of 2 to 3 tons / cm 2 There is no need to use a large press or take care to avoid damaging the mold.
[0017] During hot compression molding, the thermosetting resin first flows and fills the spaces between the metal particles in the mold in a fluid state, and then becomes a binder between the metal particles as it is cooled from the pressurized temperature range.The resin is then released from the compression molding mold as a solidified molded product that maintains its molded shape.
[0018] In general powder metallurgy molded products, including MIM, sintering is carried out with a temperature profile ranging from 500°C to 1200°C for about 4 to 6 hours in order to chemically bond the parts after molding depending on the metal composition. However, in the present invention, the solidified molded product is removed from the mold in a solidified state where the resin component has functioned as an adhesive, and is placed in a constant temperature bath heated to a hardening temperature of around 200°C for about 10 to 30 minutes until the resin component has completely hardened, after which it is removed from the bath and cooled to obtain the desired hardened molded product.
[0019] The thermostatic bath can be used to load all the molded bodies into a batch-type general-purpose drying device, etc., which allows for significant reductions in equipment cost, installation area, and energy input compared to conventional powder metallurgy molding. It also eliminates the need for temperature profile setting and atmosphere control in the sintering furnace.
[0020] The surface of the molded product obtained after the curing reaction has improved smoothness due to the curable resin used as a binder between the metal powder particles, forming a smoother surface than the surfaces of molded products obtained by ordinary powder metallurgy molding.
[0021] In the present invention, the curable resin is in the plasticized B-stage state in the temperature range of about 60 to 130°C, and is compressed into the compression molding die at a rate of 2 to 3 tons / cm2 per square centimeter. 2 The mold is pressed at 400°C, and the fluidity of the hardening resin allows it to take on a shaped form. The mold is then cooled and solidified to maintain the shape, after which it is released from the mold. Finally, a hardening process is carried out at 160-220°C for 10-30 minutes to obtain a metal molded product with a smooth surface and sufficient strength. Effect of the Invention
[0022] In the present invention, a metal resin composite material is obtained by mixing and kneading a metal powder that has been surface-treated with a coupling agent having two or more different reactive groups in its molecule and a thermosetting resin in a plasticized state by heating them to a certain temperature or higher, or a sheet-shaped metal resin composite material is obtained by dispersing and mixing a mixture of a metal powder and a thermosetting resin in a slurry state using a solvent, and then the solvent is evaporated and removed from the sheet-shaped metal resin composite material. The metal resin composite powder is then crushed and classified, and the resulting material is placed in a mold and compression molding equipment equipped with a heating compression molding and cooling control mechanism is used to perform pressure molding in the B stage (plasticized state) region and demolding in the cooling region. After that, a short curing process is performed in a thermostatic bath at around 200°C, whereby a heat-cured metal molded body with a smooth surface can be produced with simple equipment and process management, making it possible to achieve significant energy cost reductions and decarbonized production. [Brief description of the drawings]
[0023] [Figure 1] 1 is a flowchart of a method for producing a metal-resin composite powder according to an embodiment of the present invention. [Diagram 2] 1 is a flowchart of a method for producing a thermosetting metal molded product obtained by using a metal-resin composite powder according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] Hereinafter, the present embodiment will be described with reference to the drawings, in which: Fig. 1 is a flow chart showing a manufacturing method for obtaining a thermosetting metal molded body according to the present embodiment. This flow chart shows the process for producing a metal resin composite powder, in which metal powder used in powder metallurgy is classified into a predetermined particle size distribution as a pre-process, the metal powder is surface-treated with a coupling agent, a compound having multiple reactive groups in its molecule, and the metal powder is composited with a thermosetting resin and crushed to obtain a metal powder composition for molding, with coarse powder removed. FIG. 2 is a flow chart showing a manufacturing method in which the metal-resin composite powder is used in a post-process, which involves heat compression molding in a B-stage (plasticized state) region and demolding in a cooling region to produce a final hardened metal molded body.
[0025] First, the particle size distribution of metal powder used in ordinary powder metallurgy is adjusted to remove coarse powders above a certain particle size using a vibrating sieve or an air classifier in order to improve the strength and surface smoothness of the hardened molded body. The classification point of the coarse powder is selected based on the mechanical strength and surface smoothness required for the hardened molded product, but a point of approximately 90 μm is desirable.
[0026] In order to enhance the bond with the B-stage (semi-cured) thermosetting resin used as an adhesive, the metal powder is surface-treated with a coupling agent, which is a compound that has multiple reactive groups in its molecules that chemically bond to both inorganic and organic materials.
[0027] In the surface treatment process using a coupling agent, a liquid of the coupling agent diluted with alcohol or water is poured into a mixing and stirring device and an appropriate amount is dropped onto the metal powder in a stirred state. The alcohol and water are evaporated by the shear heat generated during mixing and stirring, and after drying is completed, the surface-treated metal powder is discharged and recovered from the mixing and stirring device.
[0028] Another surface treatment using graphene oxide, a nanocarbon material dispersed in an aqueous medium, is carried out by adding an appropriate amount of graphene oxide solution to metal powder that has been placed in water and stirred and mixed, stirring and mixing for a certain period of time, decanting and washing using filter paper, etc. to remove excess graphene oxide, and then drying at around 110°C to recover the surface-treated metal powder.
[0029] In order to improve fluidity within the mold during hot compression molding, to bond the powder together after hardening, and to create a high-density molded structure, the surface-treated metal powder is composited with a thermosetting resin at a composition ratio of 20 wt% or less.
[0030] The process of compounding thermosetting resin and metal powder can be carried out by heating in the B-stage temperature range to plasticize the thermosetting resin into a paste state, and then uniformly mixing and kneading the thermosetting resin using equipment such as a two-roll mill or kneader. Alternatively, a method is also possible in which the thermosetting resin liquefied using a solvent is uniformly stirred and mixed with the metal powder to create a slurry state, and then flattened with a doctor blade or the like, after which the solvent components are evaporated and removed to produce a plate-like solidified product.
[0031] The mixed material of metal powder and thermosetting resin is compounded by a dry method using heated paste kneading or a wet method using a solvent, in which the thermosetting resin is interposed between the metal powder surface and bonds the metal powder together. In order to make the powder for compression molding in a state in which the surface of the metal powder is covered, in the next process, the powder is crushed and then coarse powder of approximately 90 μm or larger is removed using a vibrating sieve or the like.
[0032] Compression molding uses a die and upper and lower punches, as in conventional powder metallurgy manufacturing, but it is carried out in a press machine equipped with equipment to control the heating and cooling of the mold, and is carried out between the temperature above the plastic state (B stage) of the thermosetting resin and the temperature below the temperature at which the hardening reaction begins.It is characterized by the inclusion of a mechanism that allows pressurization and cooling in the B stage region, and the heated and hardened metal molding to be released from the mold in the region below the B stage temperature.
[0033] Pressurization is carried out between the heat distortion temperature at which the thermosetting resin becomes plastic and the temperature at which the curing reaction begins to proceed, but a temperature 10°C above the heat distortion temperature and 30°C below the curing temperature is desirable, and the temperature is set according to the dimensions and shape of the cured molded product and productivity.
[0034] The molding pressure is required to make the thermosetting resin plastic, giving it the fluidity to permeate between the metal powder as a binder, and it can be done at a significantly lower pressure, about one-quarter to one-third that required for conventional powder metallurgy.
[0035] After pressure molding, the cooling mechanism is operated to lower the temperature of the die and the upper and lower punches to below the thermal deformation temperature of the thermosetting resin, preferably below 20° C., and the mold is then opened to release and recover the molded body.
[0036] After compression molding, the molded body is removed from the mold and left to stand for 10 to 30 minutes in a typical thermostatic chamber set at a heat curing temperature of around 200°C to obtain the final heat-cured metal molded body. The surface of the obtained hardened metal compact is formed of a so-called skin layer, which is made of the thermosetting resin during pressure molding in a plasticized state, and is far superior in smoothness to the surface of ordinary powder metallurgy compacts.
[0037] (Major Effects Obtained by the Present Embodiment) In this embodiment, in order to form metal products by low-pressure compression powder molding, metal powder is surface-treated with a coupling agent having two or more different reactive groups in its molecule, and a thermosetting resin that depopulates in a specific temperature range (B stage) and increases the fluidity of the metal powder is used as a binder to produce a metal-resin composite powder in which coarse particles larger than a specified particle size are removed.The powder is then poured into a mold and subjected to low-pressure heat molding followed by a low-temperature curing process to produce a hardened metal molded product with a smooth surface, which is possible without the use of special equipment or high energy. Compared to products made by conventional powder metallurgy processing and metal injection molding (NIM), low-temperature hardening is possible without the sintering process, which contributes greatly to significant energy cost reductions and the resolution of the decarbonization problem. We can also provide a material composition and manufacturing method that can produce hardened metal compacts with fine irregularities and a smooth surface condition.
[0038] Surface treatment of metal powder using a coupling agent having two or more different reactive groups in its molecule can be carried out by a simple process of dropping an appropriate amount of coupling agent diluted with alcohol or an alcohol aqueous solution onto the mixed metal powder in a mixing and stirring device, and removing the solvent by the shear heat generated during stirring and mixing, or by adding an appropriate amount of graphene oxide solution to the mixed metal powder in water and collecting it by filtration, which easily results in strong bonds between the metal powder and the thermosetting resin.
[0039] The surface-treated metal powder is compounded in advance by methods such as paste mixing in a plasticized state of B-stage thermosetting resin or wet mixing sheet formation using a solvent. After crushing, the powder is fed into the compression molding process after removing the coarse particles. The high fluidity during molding transfers the fine unevenness inside the mold, and the resulting product has ample strength when released from the mold. After the final heat curing, a heat-hardened metal molded product with sufficient strength and a smooth surface is obtained.
[0040] The compounding ratio of the thermosetting resin is 20 wt% or less of the metal powder, and the thermosetting resin reacts at the curing temperature and cools to solidify, resulting in a heat-cured metal molding with high strength and a smooth surface.
[0041] The pressure required for compression molding of the composite thermosetting resin with metal powder in the plasticized temperature range is 2 to 3 tons / cm. 2 In conventional powder metallurgy manufacturing, a large amount of lubricant is added and the pressure is 5 to 7 tons / cm. 2 However, there are limitations to the application of greater pressure due to the strength of the mold and the equipment, and there are also limitations to the smoothness.
[0042] In this embodiment, the heating temperature during compression molding can be set according to the plasticization temperature of the thermosetting resin and can be in the range of 60 to 130° C., and the final hardening temperature after molding and cooling is 160 to 220° C. Furthermore, the final hardening process can be carried out by leaving the material to stand for about 10 to 30 minutes, and in this embodiment, small-scale equipment such as a normal dryer can be used, making it possible to significantly reduce energy costs compared to powder metallurgy processes in which large-scale sintering furnaces are essential. Furthermore, the sintering shrinkage is smaller than that in powder metallurgy, and dimensional accuracy can be improved.
[0043] (Other forms) The manufacturing method of the resin molding die of the present embodiment described above is one example of a preferred form of the present invention, but it is not limited to this and various modifications are possible within the scope that does not change the gist of the present invention.
[0044] The metal powder is not limited to iron powder, but may be a single metal such as aluminum, tungsten, stainless steel, titanium, zinc, tin, copper, lead, magnesium, chromium, cobalt, nickel, zirconium, molybdenum, silver, neodymium, platinum, or gold, or may contain one or more metals or ceramics selected from alloys and ceramics containing iron, aluminum, tungsten, stainless steel, titanium, zinc, tin, copper, lead, magnesium, chromium, cobalt, nickel, zirconium, molybdenum, silver, neodymium, platinum, or gold. For example, the iron-based alloys include alloy steel, tool steel, stainless steel, nickel steel, nickel-chromium steel, chromium steel, maraging steel, etc. Copper alloys, aluminum alloys, titanium alloys, and cemented carbide alloys can also be used.
[0045] In order to improve the bonding strength with the thermosetting resin to form a thermosetting molded body, it is possible to use a titanate-based, silane-based, graphene oxide, or other surface treatment agent for the metal powder.
[0046] The thermosetting resin having a B stage to be added to the metal powder desirably has a plasticization temperature of about 90°C and a hardening temperature of about 200°C.
[0047] In this embodiment, the metal powder and the thermosetting resin are kneaded in the heat distortion temperature range to form a dry composite, or are mixed in a wet composite using a solvent to form a slurry state. The resulting metal-resin composite powder is crushed and classified, and then placed in a mold and compressed at a pressure of 2 to 3 tons / cm. 2 However, depending on the combination of metal powder and added thermosetting particles, the compression pressure can reach 2 tons / cm. 2 It may be less than 3 ton / cm 2 It is okay to exceed that.
[0048] In this embodiment, the plasticization temperature is about 90° C., and the curing temperature is sintering at about 200° C. However, depending on the combination of the metal powder and the added thermosetting resin, the temperature during compression molding in the B stage is preferably in the range of 10° C. or more higher than the heat distortion temperature, and 30° C. lower than the curing temperature, if possible, and the curing time during which the mixture is left to stand in a thermostatic chamber set at the curing temperature is 10 to 30 minutes. EXAMPLES
[0049] The metal powder used was a typical ferrous metal powder (Höganäs Somaloy: ASC100.29) produced by the atomization method, and had the following particle size distribution: TIFF2024139645000002.tif24157
[0050] In order to improve the bond with thermosetting resin, the surface of the metal powder is treated by adding iron powder from which coarse particles over 90μm have been removed to a stirring mixer, and while the powder is mixed, a coupling agent diluted with alcohol is dropped onto it. The alcohol is evaporated by the shear heat generated during mixing, completing the surface treatment. The coupling treatment was carried out under the conditions of putting 6,500 g of iron powder into a Henschel mixer, and dropping a treatment solution prepared by dissolving 12.5 g of Ajinomoto Co.'s Plenact 46B, a titanate-based material, in 62.5 g of ethanol into the mixer at a low speed. In order to evaporate the alcohol with the help of shear heat and heating from the mixing equipment, the mixture was mixed by rotation at 130°C for 45 minutes, then cooled to 40°C using the equipment's cooling device before being discharged and collected.
[0051] The thermosetting resin is E-150BK14S, a Towa Gosei product made of epoxy- and amine-based hardeners, heated above its softening point on a hot plate to form a paste. The titanate-surface-treated iron powder is added in portions until the desired ratio is reached, and the mixture is mixed and kneaded before cooling. The kneading temperature was 130°C, 40°C higher than the softening point of the thermosetting resin E-150BK14S, which is 90°C, and the ratio of thermosetting resin added was 4, 6, and 8 parts by weight per 100 parts of iron powder.
[0052] Iron powder and thermosetting resin are mixed and kneaded in a paste state to form a composite, and after cooling, they are crushed using a grinding device at room temperature and the coarse powder is removed using a 90μm sieve to obtain a particle size equivalent to that of the original iron powder. The obtained lump-like coarse powder is crushed again and as much of it as possible is collected using a 90μm sieve.
[0053] A ring-shaped product (outer diameter 19 mm, inner diameter 10 mm, thickness 5.5 mm) was molded at a mold temperature of 140°C and a pressure of 2 tonnes / cm 2 The uncured molded body was cooled and released from the mold and placed in a thermostatic chamber at 200°C for 15 minutes to complete the curing. The radial crushing strength and surface roughness (Ra, Rz) of the obtained cured molded body were also measured, and the results are shown in the following table. TIFF2024139645000003.tif40110 EXAMPLES
[0054] Using the same process, a ring-shaped product (outer diameter 19 mm, inner diameter 10 mm, thickness 5.5 mm) was molded at a mold temperature of 140°C and a pressure of 3 tons / cm. 2 The uncured molded bodies were molded in the above manner, cooled, and released from the mold. The uncured molded bodies were then placed in a thermostatic chamber at 200°C for 15 minutes to complete the curing. The radial crushing strength and surface roughness (Ra, Rz) of the cured molded bodies were also measured, and the results are shown in the following table. TIFF2024139645000004.tif38111 EXAMPLES
[0055] The radial crushing strength of the uncured molded bodies obtained by molding in the steps of Examples 1 and 2 was measured, and the results are shown in the following table. TIFF2024139645000005.tif33109 comparison example
[0056] As a comparative example, iron-based powder from which coarse powder had been removed using a 90 μm sieve was pressed into a mold by a conventional powder metallurgy molding process, and a similar ring-shaped molded product was produced by sintering at 550°C. The radial crushing strength before and after sintering and the surface roughness (Ra, Rz) after sintering were measured. The results obtained are shown in the following table. TIFF2024139645000006.tif46112 Comparing the examples and comparative examples, there is a difference of nearly 10 times in the compression strength before sintering and there is also a large difference in surface roughness, but these differences are thought to be a major advantage of the present invention in terms of the reproducibility of fine uneven shapes during the molding process.
Claims
1. A method for producing a metal resin composite powder, comprising: a surface treatment step of coating the surface of a metal powder having a predetermined particle size with a coupling agent; a kneading step of mixing the surface-treated metal powder with a plasticized thermosetting resin to obtain a solidified composite; a crushing step of crushing the solidified composite to obtain a powder; and a classification step of removing coarse powder having a particle size equal to or larger than a predetermined particle size from the powder to obtain a powder for compression molding.
2. The method for producing a metal-resin composite powder for compression molding according to claim 1 , wherein the coupling agent is a silane coupling agent, a titanate coupling agent, or graphene oxide.
3. 2. The method for producing a metal-resin composite powder according to claim 1, wherein the compounding process includes bringing the thermosetting resin into a B-stage plastic state at a temperature lower than the curing temperature of the thermosetting resin, kneading the thermosetting resin and the surface-treated metal powder so as to uniformly disperse the thermosetting resin, and then cooling and solidifying the mixture.
4. 2. The method for producing a metal-resin composite powder according to claim 1, wherein the compounding process comprises dissolving the thermosetting resin in a solvent to liquefy it, compounding the surface-treated metal powder in a slurry state so as to uniformly disperse the metal powder, and then removing the solvent by evaporation to solidify the mixture.
5. 2. The method for producing a metal resin composite powder according to claim 1, wherein the powder for compression molding is a mixture of the thermosetting resin with the metal powder at 20 wt % or less, and the particle size of the powder obtained by pulverizing the thermosetting resin and the metal powder after compounding them is 100 μm or less by the classification process.
6. 2. The method for producing a metal resin composite powder compact according to claim 1, wherein the metal resin composite powder is charged into a metal mold, and compressed and molded by heating the metal resin composite powder to a B-stage temperature at which the thermosetting resin is in a plastic state in the metal mold, and then cooled and solidified in the metal mold. After being released from the mold, the thermosetting resin is cured in an atmosphere having a curing temperature to obtain a compact.
Citation Information
Patent Citations
Iron powder for powder metallurgy
JP2008150648A
Method for producing organic binder and organic binder
JP2011140535A