Manufacturing method of diamond abrasive grains

The method of heat treatment and ultrasonic application for diamond abrasive grains introduces stable microcracks, enhancing microfragility and maintaining sharp edges, addressing shape changes and crushing issues in existing methods.

JP2024139656APending Publication Date: 2024-10-09NORITAKE MACHINE TECHNO CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
JP2023139721
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-27
Filing Date
2023-08-30
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

Existing methods for introducing microcracks into diamond abrasive grains to enhance microfragility are unstable and can cause shape changes or crushing, making it difficult to maintain cutting edges in a sharp state.

Method used

A manufacturing method involving heat treatment to introduce internal stress followed by ultrasonic wave application to release stress and introduce cracks, without applying large external forces, thereby stabilizing the introduction of microcracks.

Benefits of technology

Stable production of diamond abrasive grains with high microfragility and maintained sharp cutting edges, reducing shape changes and crushing, while improving crystallinity and hardness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139656000001
    Figure 2024139656000001
  • Figure 2024139656000002
    Figure 2024139656000002
Patent Text Reader

Abstract

To stably introduce a crack in diamond abrasive grains while suppressing a shape change or pulverization of the diamond abrasive grains.SOLUTION: A manufacturing method disclosed herein includes: a heat treatment process of heating diamond abrasive grains; and an ultrasonic wave application process of applying an ultrasonic wave to the diamond abrasive grains after having been heated. In a manufacturing method of such a constitution, strong internal stress is introduced into the diamond abrasive grains in the heat treatment process, and the internal stress is released in the ultrasonic wave application process. Thus, a crack can be stably introduced into the diamond abrasive grains. Further, because large external force is not added to the diamond abrasive grains in the manufacturing method, a shape change or pulverization of the diamond abrasive grains can be suppressed.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The technology disclosed herein relates to a method for producing diamond abrasive grains. [Background technology]

[0002] In recent years, diamond abrasive grains have been widely used for grinding and polishing various materials. These diamond abrasive grains are required to have appropriate micro-friability according to the object being processed. For example, diamond abrasive grains that frequently break into tiny scales during processing (high micro-friability) have excellent processing efficiency because they can maintain a sharp cutting edge.

[0003] It is known that diamond abrasive grains tend to fracture as their internal stress (tensile stress) increases. Here, the internal stress of diamond abrasive grains can be evaluated based on Raman spectroscopy. Specifically, when the Raman spectrum of diamond abrasive grains is obtained, a peak due to the lattice vibration of diamond crystals is observed at 1333 cm -1 The Raman peak position is confirmed near the center of the diamond abrasive grain. The diamond abrasive grain has the Raman peak position shifted to the low wavenumber side due to the introduction of internal stress or the inclusion of impurities in the crystal. Non-Patent Document 1 reports that the diamond abrasive grain to which internal stress is introduced by heat treatment has a Raman peak position shifted to the low wavenumber side, improving micro-fracturability. [Prior art documents] [Non-patent literature]

[0004] [Non-Patent Document 1] Hitoshi Kakutani et al., "Internal Strain Distribution and Microfracture Behavior of Various Single Crystal Diamonds for Cutting Tools," Proceedings of the JSPE Spring Meeting, Academic Lecture Series, 2019, P644-P645 Summary of the Invention [Problem to be solved by the invention]

[0005] By the way, in order to improve the micro-fracturability of diamond abrasive grains, it is effective to introduce micro-cracks into the abrasive grains. This allows appropriate fracture starting from the cracks, so that the cutting edge of the diamond abrasive grains can be kept sharp. As an example of this type of crack introduction method, a method of applying a large external force to the diamond abrasive grains using a pressurizing device is considered. However, this pressurizing method may cause the abrasive grains to change shape or be crushed, so it is difficult to stably introduce only cracks. [Means for solving the problem]

[0006] The inventor of the present invention has conducted various experiments and studies, and has surprisingly found that when ultrasonic waves are applied to diamond abrasive grains, the internal stress of the diamond abrasive grains changes.For example, when ultrasonic waves are applied to diamond abrasive grains in which strong internal stress is introduced, the internal stress is released and the Raman peak position shifts to the high wave number side.On the other hand, when ultrasonic waves are applied to diamond abrasive grains in which internal stress is weak, internal stress is introduced and the peak position shifts to the low wave number side.The inventor of the present invention has further studied and found that when ultrasonic waves are applied to diamond abrasive grains after heat treatment, the very strong internal stress introduced by heat treatment is released, and cracks are introduced.

[0007] The manufacturing method disclosed herein is based on the above findings. This manufacturing method of diamond abrasive grains includes a heat treatment process of heating diamond abrasive grains and an ultrasonic application process of applying ultrasonic waves to the diamond abrasive grains after heating. As described above, according to the manufacturing method configured as above, diamond abrasive grains with cracks can be stably manufactured. In addition, since the manufacturing method disclosed herein does not apply a large external force to the diamond abrasive grains, it is possible to suppress the shape change or crushing of the abrasive grains during manufacturing.

[0008] In one embodiment of the manufacturing method disclosed herein, the heat treatment step introduces internal stress into the diamond abrasive grain. This allows the diamond abrasive grain to be appropriately cracked in the ultrasonic application step. The internal stress introduced into the abrasive grain is preferably tensile stress.

[0009] In one embodiment of the manufacturing method disclosed herein, the ultrasonic wave application step relieves the internal stress induced in the diamond abrasive grains, thereby allowing cracks to be appropriately induced in the diamond abrasive grains.

[0010] In one embodiment of the manufacturing method disclosed herein, the diamond abrasive grains after the heat treatment step have a Raman spectrum of 1325 cm -1 From 1334cm -1 The average peak position of the Raman peaks that exist in the range of 1329 cm -1 This makes it possible to easily introduce cracks into the diamond abrasive grains in the ultrasonic application step.

[0011] In one embodiment of the manufacturing method disclosed herein, the content of impurities relative to the total weight of the diamond abrasive grains is 0.1wt% or more. This allows strong internal stress to be easily introduced into the diamond abrasive grains in the heat treatment process. The thermal expansion coefficient of the impurities is preferably higher than that of the diamond abrasive grains. This allows internal stress to be introduced more easily. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] An embodiment of the technology disclosed herein will be described below. Matters other than those specifically mentioned in this specification and necessary for implementing the technology disclosed herein can be understood as design matters of a person skilled in the art based on the conventional technology in the field. The technology disclosed herein can be implemented based on the contents disclosed in this specification and the technical common sense in the field. In this specification, the expression "A to B" indicating a numerical range means "A or more and B or less" unless otherwise specified. The drawings are drawn diagrammatically, and the dimensional relationships (length, width, thickness, etc.) in the drawings do not reflect the actual dimensional relationships.

[0013] The manufacturing method disclosed herein includes a heat treatment step and an ultrasonic application step. Hereinafter, the diamond abrasive grains used in the manufacturing method disclosed herein will be described, and then each step will be described in detail.

[0014] (1) Diamond abrasive grains The diamond abrasive grains are diamond particles having a predetermined hardness. The diamond abrasive grains may be natural diamond or artificial diamond. In the technology disclosed herein, it is preferable to use diamond abrasive grains containing impurities. This makes it easier to introduce internal stress into the abrasive grains in the heat treatment process described below. The impurities here refer to elements other than carbon (C). Examples of the impurities include metal elements such as Fe, Ni, Co, Mn, Al, Ti, Cr, Zr, and V. The diamond abrasive grains may also contain impurities other than metal elements. Examples of the impurities other than metal elements include N, B, Si, and P. These impurities may be unavoidably mixed in during the manufacturing process, or may be intentionally introduced into the abrasive grains. In addition, it is preferable that the impurities have a higher thermal expansion coefficient than diamond. This makes it easier to introduce internal stress in the heat treatment process. A suitable example of the impurity is a metal (typically a metal particle), and examples of its constituent elements include the above-mentioned metal elements. In addition, the content of the metal element relative to the total weight (100wt%) of the diamond abrasive grains is preferably 0.1wt% or more, more preferably 0.2wt% or more, even more preferably 0.3wt% or more, and particularly preferably 0.5wt% or more. This makes it easier to introduce internal stress in the heat treatment process. On the other hand, the upper limit of the content of the metal element is not particularly limited, and may be 3wt% or less, 2wt% or less, or 1wt% or less. The content of the metal element in the diamond abrasive grains can be measured based on X-ray fluorescence analysis (XRF: X-Ray Fluorescence).

[0015] In addition, the diamond abrasive grains before heat treatment had a Raman spectrum of 1325 cm -1 From 1334cm -1 The average peak position of the Raman peaks that exist in the range of 1331 cm -1 Less than 1330.5 cm -1 More preferably, 1330 cm -1In the manufacturing method disclosed herein, it is preferable to prepare diamond abrasive grains in advance, the Raman peak position of which is shifted to a certain degree toward the low wavenumber side due to the inclusion of impurities or the introduction of stress during manufacturing, and then subject the diamond abrasive grains to a heat treatment process. This makes it easier to introduce internal stress in the heat treatment process.

[0016] In this specification, the "Raman peak position" is measured under the following conditions. First, a commercially available microscopic Raman spectrophotometer can be used as the measuring device. The measurement conditions are, for example, set to a measurement temperature of 24°C, a calibration sample of Si, and an excitation laser wavelength of 532 nm, and other conditions are appropriately adjusted so that clear measurement results are obtained. When Raman spectroscopy of diamond abrasive grains is performed under the above conditions, a peak due to the lattice vibration of diamond crystals appears at the Raman shift of 1333 cm. -1 A Raman spectrum present in the vicinity is detected. Then, using a predetermined waveform analysis software (such as Labspec6), baseline correction, peak search and fitting are performed on this Raman spectrum, and the position of the peak top (Raman shift) is regarded as the "Raman peak position". In this specification, the "average value of the Raman peak positions" is adopted when evaluating the internal stress of diamond abrasive grains. This "average value of the Raman peak positions" is the arithmetic average of the Raman peak positions obtained at at least 500 measurement points (the number of measurement points within the same grain is constant) for 100 or more randomly selected diamond abrasive grains.

[0017] The size of the diamond abrasive grains does not limit the technology disclosed herein, and can be changed as appropriate depending on the purpose and mode of use. For example, 50 The particle size may be 0.1 μm or more, 0.5 μm or more, 1 μm or more, 5 μm or more, or 10 μm or more. 50 The particle size may be 1000 μm or less, 500 μm or less, 250 μm or less, or 100 μm or less. 50"Particle size" is the particle size that corresponds to a cumulative frequency of 50 volume % from the small particle side in the volume-based particle size distribution based on a general laser diffraction / light scattering method (dispersion medium: water).

[0018] The shape of the diamond abrasive grains is not particularly limited, and can be appropriately selected from conventionally known shapes. For example, the diamond abrasive grains may be spherical, plate-like, or irregular (such as confetti-like). The average aspect ratio of the diamond abrasive grains may be 1 or more and 2 or less, or 1.1 or more and 1.8 or less. The "aspect ratio" in this specification can be obtained by drawing a rectangle circumscribing the abrasive grains in an electron microscope image and calculating the ratio (b / a) of the length (a) of the short side of the rectangle to the length (b) of the long side of the rectangle. The "average aspect ratio" is the arithmetic average value of the aspect ratios of 100 or more particles.

[0019] (2) Heat treatment process In this process, the diamond abrasive grains are heated. This allows the diamond abrasive grains to be introduced with internal stress. The stress introduced in this process is preferably tensile stress. The abrasive grains to which tensile stress is introduced have the effect that they are likely to shrink and crack during the stress release process because the abrasive grains are subjected to a force in the direction in which they expand. For example, if the abrasive grains contain impurities with a higher thermal expansion coefficient than diamond, it is easier to introduce such tensile stress into the abrasive grains.

[0020] The detailed heating conditions in the heat treatment step (heating temperature, heating time, etc.) may vary as appropriate depending on the particle size distribution of the diamond abrasive grains, the amount of processing, the components (type and amount of impurities), etc. For this reason, the detailed heating conditions in the heat treatment step are not limited to the technology disclosed herein, and are preferably adjusted as appropriate from the viewpoint of introducing appropriate cracks into the diamond abrasive grains in the next step (ultrasonic application step). For example, the heat treatment step is preferably performed such that the average peak position of the diamond abrasive grains after heating is 1329 cm -1 Less than or equal to 1328.9 cm -1 Less than 1328.8 cm, more preferably -1The following is particularly preferably 1328.7 cm -1 It is preferable to adjust various conditions so that the diamond abrasive grains have a maximum internal stress of 1326.0 cm or less. By introducing a large internal stress into the diamond abrasive grains in this way, cracks are likely to be introduced due to the release of the internal stress in the ultrasonic application process described below. The lower limit of the average peak position of the diamond abrasive grains after heating is not particularly limited, and is 1326.0 cm -1 More than 1327.0cm is fine. -1 More than 1328.0cm is fine. -1 More than 1328.4cm is fine. -1 More than that is fine.

[0021] In addition, the heating temperature in this step is, for example, preferably 300°C or higher, more preferably 500°C or higher, even more preferably 700°C or higher, and particularly preferably 900°C or higher. As the heating temperature increases, the internal stress of the diamond abrasive grains after heating tends to increase. On the other hand, the upper limit of the heating temperature is preferably 1600°C or lower, more preferably 1400°C or lower, and particularly preferably 1200°C or lower. As the heating temperature decreases, it becomes easier to suppress diamond wear and unintended changes in diamond physical properties (for example, surface properties). Note that the "heating temperature" here refers to the maximum temperature in the heat treatment. In addition, when the heating temperature is set to 500°C or higher, it is preferable to set the heating atmosphere to a non-oxidizing atmosphere (such as an N2 gas atmosphere or an Ar gas atmosphere). This can prevent the oxidation of the diamond abrasive grains.

[0022] The heating time may be, for example, 0.1 hours or more, preferably 0.5 hours or more, more preferably 1 hour or more, even more preferably 1.5 hours or more, and particularly preferably 2 hours or more. This allows sufficient internal stress to be introduced into the diamond abrasive grains. On the other hand, the upper limit of the heating time is preferably 24 hours or less, more preferably 12 hours or less, even more preferably 6 hours or less, and particularly preferably 4 hours or less. This allows the heat treatment process to be shortened and manufacturing efficiency to be improved. Note that the "heating time" here refers to the time during which the above-mentioned heating temperature (maximum temperature) is maintained.

[0023] In addition, the diamond abrasive grains are preferably heated in a state where no softened glass or molten glass is present on the surface of the diamond abrasive grains. When the diamond abrasive grains are heated together with such glass (typically vitrified bond), there are cases where the internal stress to the extent that it can impart micro-fracturability is not introduced into the abrasive grains. The mechanism is considered to be that during the heating process of the diamond abrasive grains, a compressive force is applied, and internal stress (typically tensile stress) tends to be difficult to introduce. That is, in the manufacturing method disclosed herein, it is preferable to carry out the heat treatment process without applying an external force in the compressive direction to the diamond abrasive grains. This makes it possible to improve the micro-fracturability of the diamond abrasive grains more efficiently. Here, "no external force in the compressive direction is applied to the diamond abrasive grains" includes not only the above-mentioned glass not present on the diamond abrasive grains surface, but also the state where a material with a smaller thermal expansion coefficient in the heating temperature range than the diamond abrasive grains is present on the diamond abrasive grains surface, and the state where no external force is applied by a pressure device or the like.

[0024] (3) Ultrasonic impression process In this process, ultrasonic waves are applied to the diamond abrasive grains after heating. This allows cracks to be introduced into the diamond abrasive grains. This introduction of cracks using ultrasonic waves does not require the application of a large external force to the diamond abrasive grains, so that changes in shape and crushing of the abrasive grains can be suppressed. That is, according to the manufacturing method disclosed herein, cracks can be stably introduced into the abrasive grains while suppressing changes in shape and crushing of the abrasive grains, so that diamond abrasive grains with high micro-fracturability can be efficiently manufactured. Although it is not intended to limit the technology disclosed herein, the reason for obtaining such an effect is presumed to be as follows. First, a very strong internal stress is introduced into the diamond abrasive grains to which heat treatment has been applied. Then, when ultrasonic waves are applied to the diamond abrasive grains, the pressure fluctuation applied by the ultrasonic application acts as a force to release the internal stress. At this time, it is understood that cracks are introduced into the diamond abrasive grains by suddenly releasing the very strong internal stress. And, it has been confirmed by experiments that such diamond abrasive grains have high micro-fracturability.

[0025] In addition, an example of the ultrasonic wave application device used in this process is an ultrasonic wave application device for liquids such as an ultrasonic dispersion device or an ultrasonic cleaning device. When using this ultrasonic wave application device for liquids, it is preferable to prepare an abrasive grain dispersion liquid in which diamond abrasive grains are dispersed in a predetermined dispersion medium. This allows ultrasonic waves to be applied uniformly to the diamond abrasive grains in the abrasive grain dispersion liquid. In addition, the dispersion medium at this time is preferably a low-viscosity liquid medium. This makes it easier to apply ultrasonic waves to the diamond abrasive grains in the abrasive grain dispersion liquid. Specifically, the viscosity of the dispersion medium at room temperature (20°C) may be 100 mPa·s or less, preferably 10 mPa·s or less, more preferably 7 mPa·s or less, even more preferably 5 mPa·s or less, and particularly preferably 3 mPa·s or less. On the other hand, the lower limit of the viscosity of the dispersion medium is not particularly limited, and may be 0.05 mPa·s or more, 0.1 mPa·s or more, or 0.3 mPa·s or more. Examples of dispersion media having such a viscosity include water, ethanol, 2-propanol, 1-propanol, and ethylene glycol. The ultrasonic wave application device used in this step is not limited to the above-mentioned device for liquids, and any conventional ultrasonic wave generating device can be used without particular limitation. For example, in this step, a device that directly applies ultrasonic waves to a powder material (such as an ultrasonic sieve) can also be used.

[0026] The ultrasonic wave application step is not limited to the mode of releasing all of the internal stress introduced in the heat treatment step, but may be sufficient to release a part of the internal stress introduced in the heat treatment step. Even in this case, appropriate cracks can be introduced into the diamond abrasive grains. The ultrasonic wave application time at this time is preferably set appropriately according to the amount of the processing target (diamond abrasive grains) from the viewpoint of introducing appropriate cracks into the abrasive grains. As an example, the application time is preferably 1 minute or more, more preferably 2 minutes or more. This allows the internal stress to be released to the extent that cracks can be introduced into the diamond abrasive grains. On the other hand, the upper limit of the application time is preferably 60 minutes or less, more preferably 30 minutes or less, and particularly preferably 10 minutes or less. This allows the reduction in manufacturing efficiency and excessive temperature rise to be suppressed. The ultrasonic wave may be applied continuously, or may be applied intermittently at a predetermined interval. For example, an ultrasonic wave application process with an application time of 1 minute may be performed multiple times (for example, 2 to 10 times). This allows the temperature rise caused by the continuous application of ultrasonic waves to be suppressed. The ultrasonic wave application process may be performed continuously while cooling appropriately.

[0027] In addition, the output of the ultrasonic generator is preferably set appropriately according to the amount of diamond abrasive grains to be processed in order to introduce appropriate cracks. As the output is increased, the time required for releasing internal stress tends to be shortened. As an example, the output of the ultrasonic generator is preferably 100W or more, more preferably 200W or more, even more preferably 300W or more, and particularly preferably 400W or more. On the other hand, when using the maximum output of the ultrasonic generator, the output is preferably 1200W or less, more preferably 1000W or less, and particularly preferably 800W or less. This allows efficient processing in a short time while suppressing overheating of the dispersion medium and abrasive grains.

[0028] In addition, the frequency of the ultrasonic waves is preferably 15kHz or more, more preferably 20kHz or more, even more preferably 22kHz or more, and particularly preferably 25kHz or more. This allows for efficient processing of abrasive grains of various particle sizes in a short time while suppressing overheating of the dispersion medium and the abrasive grains. On the other hand, the frequency of the ultrasonic waves may be 1000kHz or less, preferably 500kHz or less, more preferably 120kHz or less, even more preferably 80kHz or less, and particularly preferably 40kHz or less. This allows for efficient ultrasonic processing in a short time.

[0029] In addition, in an experiment conducted by the present inventor, it was confirmed that the crystallinity of the diamond abrasive grains, which was reduced by the heat treatment process, was increased by carrying out the ultrasonic application process. Specifically, after the heat treatment process, the crystallinity of the diamond abrasive grains at 1325 cm -1 From 1334cm -1 The average half-width of the Raman peaks whose peak positions are in the range increases (crystallinity decreases). When the ultrasonic wave application process is carried out, the average half-width of the Raman peaks decreases (crystallinity increases). This makes it possible to realize diamond abrasive grains that have excellent crystallinity and extremely high hardness despite having been subjected to heat treatment. Note that the ultrasonic wave application process reduces the average half-width of the Raman peaks by 0.05 cm. -1 or more (preferably 0.10 cm -1 More preferably, 0.15 cm -1 More preferably, 0.20 cm -1 More preferably, 0.30 cm or more -1 For example, 040cm -1 It is preferable to adjust the ultrasonic application conditions so that the half-width of the Raman peak of the diamond abrasive grains after ultrasonic application is 4.8 cm or more. This can suitably improve the crystallinity of the diamond abrasive grains. More preferably, -1 Less than 4.75 cm (preferably -1 Less than 4.7 cm, more preferably -1 Less than 4.65 cm, particularly preferably -1It is preferable to adjust various conditions (ultrasonic output, application time, etc.) so that the crystallinity is 100 or more times higher than that of the abrasive grains (see below). This allows the production of abrasive grains with particularly excellent crystallinity. In this specification, the "Raman peak half-width" refers to the wavenumber width of the peak at half the intensity of the peak top of the Raman spectrum obtained by the above-mentioned procedure. In addition, the "average Raman peak half-width" is the arithmetic average of the Raman peak half-widths obtained at at least 500 measurement points (the number of measurement points within the same grain is constant) for 100 or more randomly selected diamond abrasive grains.

[0030] An embodiment of the technology disclosed herein has been described above. However, the above embodiment is not intended to limit the technology disclosed herein. In other words, the technology disclosed herein may include various modifications of the above embodiment.

[0031] For example, in the manufacturing method disclosed herein, an inspection step may be performed after the heat treatment step and before the ultrasonic application step to inspect the internal stress of the diamond abrasive grains. If the internal stress after the heat treatment step is recognized in this inspection step, it is possible to determine whether or not appropriate cracks can be introduced into the diamond abrasive grains in the ultrasonic application step. In addition, after the inspection step, a selection step may be performed to select diamond abrasive grains that exhibit a desired internal stress (Raman peak position), and the selected diamond abrasive grains may be subjected to the ultrasonic application step. This allows diamond abrasive grains with excellent micro-fracture properties to be manufactured more stably. In addition, the diamond abrasive grains excluded in the selection step may be subjected to the heat treatment step again. This prevents a decrease in yield in the manufacturing process. In addition, in the inspection step, it is preferable to measure the Raman peak position of the Raman spectrum based on Raman spectroscopy according to the above-mentioned procedure. This allows the internal stress of the diamond abrasive grains to be accurately inspected. In addition, this inspection step does not need to be performed on all diamond abrasive grains after the heat treatment step. For example, the inspection process may be carried out when the lot of diamond abrasive grains supplied to the heat treatment process is changed, or when the conditions of the heat treatment process are changed, etc. This allows diamond abrasive grains with appropriate internal stress to be supplied to the ultrasonic application process without significantly reducing the manufacturing efficiency.

[0032] [Test example] Next, test examples related to the technology disclosed herein will be described. Note that the technology disclosed herein is not limited to the following test examples.

[0033] 1. Sample Preparation (1) Comparative Example 1 Comparative Example 1 in this test is a commercially available diamond abrasive grain (manufactured by Global Diamond Co., Ltd., FRM-DN 40-60). Note that, as a result of laser diffraction analysis, the D 50 The particle size was 40 μm. Furthermore, the results of the component analysis based on XRF showed that the diamond abrasive grains contained 0.176 wt% Ni and 0.389 wt% Mn as impurities.

[0034] (2) Comparative Example 2 In Comparative Example 2, the diamond abrasive grains were subjected to heat treatment. Specifically, the same diamond abrasive grains as those in Comparative Example 1 were heated in a reducing atmosphere (N2 gas containing 3% H2). The temperature rise rate in this heat treatment was set to 100°C / h, and the maximum temperature was set to 1000°C. The heating time (holding time at the maximum temperature) was set to 3 hours. This resulted in the production of diamond abrasive grains (Comparative Example 2) in which a large internal stress was introduced.

[0035] (3) Example 1 In Example 1, ultrasonic application treatment was performed on the diamond abrasive grains after heat treatment. Specifically, 3 g of diamond abrasive grains heated under the same conditions as Comparative Example 2 were weighed and mixed with 100 ml of pure water to prepare an abrasive grain dispersion. Next, ultrasonic waves were applied to the diamond abrasive grains in the dispersion using an ultrasonic disperser (manufactured by SMT Corporation, model: UH-600S). Note that this ultrasonic disperser has an output of 600 W, an oscillation frequency of 20 kHz, and a diameter of the vibrator irradiation part of 36 mm. Then, the OUTPUT of the ultrasonic disperser was set to 10 (maximum), and a treatment cycle including a 1-minute ultrasonic treatment and a 1-minute interval was repeated 5 times. Thereafter, the diamond abrasive grains were separated from the dispersion by filtration, washed with ethanol, and then dried at room temperature. As a result, the diamond abrasive grains of Example 1 were obtained.

[0036] (4) Comparative Example 3 In Comparative Example 3, an ultrasonic wave application treatment was performed on diamond abrasive grains that had not been subjected to heat treatment. Specifically, the same diamond abrasive grains as those in Comparative Example 1 were subjected to an ultrasonic wave application treatment according to the same procedure as in Example 1.

[0037] 2.Evaluation Test (1) Crystallinity evaluation In this study, 500 Raman spectra were acquired for each example. -1 ~1334cm -1 The positions and half-widths of the Raman peaks having peak positions at and are shown in Table 1.

[0038] In this test, the position and half-width of the Raman peak were measured according to the following procedure. First, a microscopic Raman spectrophotometer (LabRAM HR Evolution manufactured by Horiba, Ltd.) was used as the measuring device. The measurement conditions were, for example, a measurement temperature of 24°C, a calibration sample of Si, an excitation laser wavelength of 532 nm, a grating of 1800 gr / mm, an exposure time of 8 seconds, and an accumulation count of 2 times. Then, baseline correction, peak search, and fitting were performed on the obtained Raman spectrum using waveform analysis software (Labspec6). Then, the position of the peak top was regarded as the "position of the Raman peak", and the wavenumber width of the peak at half the intensity of the peak top was regarded as the "half-width of the Raman peak". Then, for each of 100 randomly selected diamond abrasive grains, the peak position and half-width were measured at five non-overlapping measurement points, and the average values ​​(average value of the Raman peak position and the average value of the Raman peak half-width) were obtained. That is, the "Raman peak position" and "Raman peak half-width" in Table 1 are the average values ​​of the measurement results at 500 measurement positions. All of the diamond abrasive grains selected in this evaluation had a circle equivalent diameter in the range of 25 μm to 75 μm.

[0039] [Table 1]

[0040] First, the Raman peak position of Comparative Example 1 is 1329.64 cm -1 This shows that the diamond abrasive grains used in this test have a high degree of uniformity due to the presence of impurities or the introduction of stress during manufacturing. -1 ) to the lower wavenumber side.

[0041] Next, the Raman peak position of Comparative Example 2 is 1328.66 cm -1 This shows that the heat-treated diamond abrasive grains have a large internal stress, which causes the Raman peak position to shift to the lower wavenumber side.

[0042] In Example 1, the Raman peak position was 1329.10 cm by applying ultrasonic waves. -1 From this, it was found that when ultrasonic waves are applied to diamond abrasive grains in which strong internal stress has been introduced by heat treatment, the internal stress is released. This release of internal stress indicates that at least a part of the internal stress has been converted into cracks. On the other hand, in Comparative Example 3, ultrasonic waves were applied without heat treatment, and as a result, the Raman peak position shifted to the low wave number side after ultrasonic application. From this, it is understood that tensile stress was introduced into the diamond abrasive grains by applying ultrasonic waves in Comparative Example 3.

[0043] In addition, as a result of comparing Comparative Example 2 with Example 1, it was confirmed that the Raman peak half-width increases by heat treatment, while it decreases by ultrasonic application treatment. From this, it was found that ultrasonic application treatment has the effect of increasing the crystallinity of diamond abrasive grains that is reduced by heat treatment. Generally, diamond abrasive grains have higher crystallinity, so it is understood that by increasing crystallinity by ultrasonic treatment, higher quality abrasive grains can be manufactured.

[0044] (2) Micro-fracture evaluation In this test, a compression fracture test was carried out to examine the micro-fracturability of each diamond abrasive grain. Specifically, a compression fracture test was carried out under the following conditions for the abrasive grains of Comparative Examples 1-2 and Example 1, a test force-displacement diagram was obtained, and the displacement rate at the compression fracture point was calculated.

[0045] [Compression fracture test conditions] Testing equipment: Micro Autograph MST-I HR Load cell capacity: 500N (50N range) Load speed: 2μm / sec Stroke origin test force: 0.02N Compression tool: Diamond indenter with a flat surface of φ200 μm Lower pressure table: Pressure plate with hardness of 700 Measurement method: Place one sample grain on the lower pressure table and compress it one grain at a time. Number of measurements: 5

[0046] [Procedure for measuring displacement rate at compressive failure point] First, the sample (abrasive grain) was placed between the indenter and the lower pressure table of the test device. The distance from the stroke position of the compression jig to the lower pressure table when the indenter contacted the abrasive grain was measured by a displacement sensor and defined as the "initial height of the sample". The compression jig was then lowered, and the displacement (deformation) of the abrasive grain when destruction occurred was measured as the "displacement at the breaking point". Note that "destruction" here refers to a state in which the sample is fragmented and the compressive load from the test is no longer applied to the sample. The "displacement rate at the breaking point of compression" was calculated by substituting the displacement at the breaking point and the initial height of the sample into the following formula (1). The results are shown in Table 2. Note that the displacement rate at the breaking point of compression in Table 2 is the average value of five samples (n=5). Compressive failure point displacement rate = failure point displacement amount / initial height of specimen (1)

[0047] [Table 2]

[0048] First, since ordinary diamond has a high Young's modulus of about 1000 GPa, it breaks with almost no distortion when pressurized. However, in the case of diamond abrasive grains with improved micro-fracturability due to the introduction of cracks, fine fractures and cracks occur during the compression process, so that the diamond abrasive grains are displaced (deformed) while continuously receiving a compressive load. As a result, the apparent compression fracture point displacement rate is large in diamond abrasive grains with excellent micro-fracturability. Here, as shown in Table 2 above, it was confirmed that Example 1 has a larger compression fracture point displacement rate than Comparative Examples 1 and 2. From this, it was found that by performing heat treatment and ultrasonic treatment as in Example 1, diamond abrasive grains that are prone to fine fractures when pressurized (i.e., high micro-fracturability) can be manufactured. This is thought to be because at least a part of the internal stress introduced into the abrasive grains by heat treatment was converted into cracks by ultrasonic treatment.

[0049] Although the technology disclosed herein has been described in detail above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and changes to the specific examples exemplified above. In other words, the technology disclosed herein includes the embodiments described in items 1 to 7 below.

[0050] <Item 1> a heat treatment step of heating the diamond abrasive grains; an ultrasonic wave application step of applying ultrasonic waves to the diamond abrasive grains after heating; A method for producing diamond abrasive grains, comprising:

[0051] <Item 2> 2. The method of claim 1, wherein the heat treatment step introduces internal stress into the diamond abrasive grains.

[0052] <Item 3> 3. The method according to item 2, wherein the internal stress is a tensile stress.

[0053] <Item 4> 4. The manufacturing method according to item 2 or 3, wherein the ultrasonic application step releases internal stress introduced into the diamond abrasive grains.

[0054] <Item 5> The diamond abrasive grains after the heat treatment step have a Raman spectrum of 1325 cm -1 From 1334cm -1 The average peak position of the Raman peaks that exist in the range of 1329 cm -1 The method for producing the present invention according to any one of items 1 to 4, wherein the method is as follows:

[0055] <Item 6> The manufacturing method according to any one of items 1 to 5, wherein the content of impurities relative to the total weight of the diamond abrasive grains is 0.1 wt% or more.

[0056] <Item 7> 7. The manufacturing method according to item 6, wherein the thermal expansion coefficient of the impurities is higher than the thermal expansion coefficient of the diamond abrasive grains.

Claims

1. a heat treatment step of heating the diamond abrasive grains; an ultrasonic wave application step of applying ultrasonic waves to the diamond abrasive grains after heating; A method for producing diamond abrasive grains, comprising:

2. The method of claim 1 , wherein the heat treatment step introduces internal stress into the diamond abrasive grains.

3. The method according to claim 2 , wherein the internal stress is a tensile stress.

4. The manufacturing method according to claim 2 , wherein the ultrasonic application step relieves internal stress induced in the diamond abrasive grains.

5. The diamond abrasive grains after the heat treatment step have a Raman spectrum of 1325 cm -1 From 1334 cm -1 The average peak position of the Raman peaks that exist in the range of 1329 cm -1 The method of claim 1, wherein:

6. The manufacturing method according to claim 1 or 2, wherein the content of impurities relative to the total weight of the diamond abrasive grains is 0.1 wt % or more.

7. The manufacturing method according to claim 6 , wherein the thermal expansion coefficient of the impurities is higher than the thermal expansion coefficient of the diamond abrasive grains.

Citation Information

Cited By

  • Preparation method of long-circulation artificial graphite negative electrode material and graphite negative electrode material

    CN121097074A