Manufacturing method of electrode

The electrode manufacturing method addresses dimensional instability and peeling issues by heating the base material and applying a coating layer to prevent oligomer migration, resulting in enhanced stability and durability.

JP2024140020APending Publication Date: 2024-10-10NITTO DENKO CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023051005
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing electrode manufacturing methods lack sufficient dimensional stability during heating and durability, particularly due to peeling issues between layers.

Method used

A manufacturing method involving heating the base material layer to 110°C or higher, forming a coating layer to prevent oligomer migration, and sequentially adding a metal base and conductive carbon layers to enhance adhesion and durability.

Benefits of technology

The method produces electrodes with improved dimensional stability and durability by preventing oligomer migration and reducing peeling, ensuring long-term performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024140020000001_ABST
    Figure 2024140020000001_ABST
Patent Text Reader

Abstract

To provide a manufacturing method of an electrode, excellent in dimensional stability when heating a substrate layer as well as excellent in durability.SOLUTION: A manufacturing method is of an electrode 1 including a substrate layer 2, a coat layer 3, a metal underlayer 4 and a conductive carbon layer 5 sequentially toward one side in a thickness direction. The manufacturing method includes: a step (1) of heating the substrate layer 2 with the coat layer 3 arranged on one side in the thickness direction to 110°C or higher; a step (2) of forming the metal underlayer 4 on one side of the coat layer 3 in the thickness direction; and a step (3) of forming the conductive carbon layer 5 on one side of the metal underlayer 4 in the thickness direction.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing an electrode. [Background technology]

[0002] 2. Description of the Related Art There is known a method for manufacturing an electrode having a film substrate, a coating layer, a metal underlayer, and a conductive carbon layer in this order toward one side in the thickness direction (see, for example, Patent Document 1 below).

[0003] In the manufacturing method described in Patent Document 1, a coating layer, a metal underlayer, and a conductive carbon layer are formed in this order on one side of a film substrate in the thickness direction. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] WO2016 / 013478 issue Summary of the Invention [Problem to be solved by the invention]

[0005] Depending on the application and purpose of the electrode, the film substrate is required to have dimensional stability when heated.

[0006] Furthermore, the electrode is required to have excellent durability, which includes the resistance of the metal underlayer to peeling off from the substrate layer when the electrode is used repeatedly.

[0007] The present invention provides a method for producing an electrode having excellent dimensional stability when a substrate layer is heated and also excellent durability. [Means for solving the problem]

[0008] The present invention [1] includes a method for manufacturing an electrode, comprising the steps of: (1) heating a base layer having the coating layer disposed on one surface in the thickness direction to 110°C or higher; (2) forming the metal base layer on one surface in the thickness direction of the coating layer; and (3) forming the conductive carbon layer on one surface in the thickness direction of the metal base layer. Effect of the Invention

[0009] The method for producing an electrode of the present invention can produce an electrode that has excellent dimensional stability when the substrate layer is heated and also has excellent durability. [Brief description of the drawings]

[0010] [Figure 1] 1A is an explanatory diagram of one embodiment of a method for producing an electrode of the present invention, FIG. 1B is a first step, FIG. 1C is a second step, and FIG. 1C is a third step. [Diagram 2] FIG. 2 is an image processing diagram of the optical microscope observation in Example 1. [Diagram 3] FIG. 1 is an image processed view of optical microscope observation of Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] 1. One embodiment of a method for manufacturing an electrode An embodiment of a method for producing an electrode of the present invention will be described with reference to FIGS. 1A to 1C.

[0012] 1.1 Layer structure of electrode 1 1C, the electrode 1 manufactured by this manufacturing method includes, in order toward one side in the thickness direction, a base layer 2, a coating layer 3, a metal base layer 4, and a conductive carbon layer 5. In this embodiment, the electrode 1 preferably includes only the base layer 2, the coating layer 3, the metal base layer 4, and the conductive carbon layer 5.

[0013] 1.2 Base material layer 2 The base layer 2 is disposed at the other end of the electrode 1 in the thickness direction. The base layer 2 forms the other surface of the electrode 1 in the thickness direction. The base layer 2 extends in a planar direction. The planar direction is perpendicular to the thickness direction. The base layer 2 has a film shape. Examples of the material of the base layer 2 include organic materials. Examples of the organic materials include polymeric materials. Examples of the polymeric materials include polyester, polyolefin, acrylic, and polycarbonate. Examples of the polyester include polyethylene terephthalate (PET) and polyethylene naphthalate. Examples of the material of the base layer 2 include preferably polyester, and more preferably PET. The base layer 2 has flexibility. The thickness of the base layer 2 is, for example, 2 μm or more, preferably 20 μm or more, and, for example, 1000 μm or less, preferably 500 μm or less.

[0014] 1.3 Coating layer 3 The coating layer 3 is disposed on one surface of the base layer 2 in the thickness direction. Specifically, the coating layer 3 is in contact with one surface of the base layer 2 in the thickness direction. The coating layer 3 extends in the planar direction. The coating layer 3 is a barrier layer. The barrier layer prevents oligomers, which are generated on one surface of the base layer 2 in the thickness direction, from migrating to one side, as described below. The coating layer 3 can also function as an easy-adhesion layer and / or an anti-scratch layer.

[0015] The material of the coating layer 3 is the solid content (coating film component) of a coating composition described below.

[0016] The coating layer 3 has a thickness of, for example, 0.5 μm or more, preferably 1 μm or more, and for example, 20 μm or less, preferably 10 μm or less.

[0017] 1.4 Metal base layer 4 The metal underlayer 4 is disposed on one surface of the coating layer 3 in the thickness direction. Specifically, the metal underlayer 4 is in contact with one surface of the coating layer 3 in the thickness direction. The metal underlayer 4 extends in the planar direction. The metal underlayer 4 is a conductive layer. The material of the metal underlayer 4 is a metal material.

[0018] Examples of the metal material include titanium, chromium, tungsten, aluminum, silicon, niobium, molybdenum, tantalum, and copper. The metal material may be, for example, an alloy of the above. That is, the metal material includes at least one metal selected from the group consisting of titanium, chromium, tungsten, aluminum, silicon, niobium, molybdenum, tantalum, and copper. In terms of adhesion, titanium is preferably used as the metal material.

[0019] The thickness of the metal underlayer 4 is, for example, 1 nm or more, preferably 5 nm or more, more preferably 10 nm or more, and even more preferably 12 nm or more, and for example, 50 nm or less, preferably 30 nm or less, and more preferably 20 nm or less.

[0020] 1.5 Conductive carbon layer 5 The conductive carbon layer 5 is disposed at one end of the electrode 1 in the thickness direction. The conductive carbon layer 5 forms one surface of the electrode 1 in the thickness direction. The conductive carbon layer 5 is disposed on one surface of the metal base layer 4 in the thickness direction. The conductive carbon layer 5 is in contact with one surface of the metal base layer 4 in the thickness direction. The conductive carbon layer 5 extends in the planar direction.

[0021] The conductive carbon layer 5 has a thickness of, for example, 2 nm or more, preferably 10 nm or more, more preferably 20 nm or more, and for example, 100 nm or less, preferably 50 nm or less, more preferably 40 nm or less.

[0022] 1.6 Manufacturing method of electrode 1 The method for producing the electrode 1 includes steps (1), (2), and (3). In this embodiment, steps (1), (2), and (3) are carried out in this order.

[0023] 1.6.2 Process (1) In this embodiment, in step (1), the base material layer 2 having the coating layer 3 disposed on one surface in the thickness direction is heated.

[0024] For example, first, the coating layer 3 is formed on one surface of the substrate layer 2 in the thickness direction. To form the coating layer 3 on one surface of the substrate layer 2 in the thickness direction, for example, a coating composition is applied to one surface of the substrate layer 2 in the thickness direction. The coating composition includes, for example, a coating component and a solvent. Examples of the coating component include an acrylate resin. Examples of the solvent include MEK and water. Thereafter, the coating composition is dried to remove the solvent. In this way, a substrate 20 with a coating layer including the substrate layer 2 and the coating layer 3 is prepared. The substrate 20 with a coating layer corresponds to the substrate layer 2 having the coating layer 3 disposed on one surface in the thickness direction.

[0025] Alternatively, a commercially available substrate 20 with a coating layer can be prepared as is.

[0026] In step (1), the substrate layer 2 having the coating layer 3 disposed on one surface in the thickness direction is then heated. Specifically, the coating layer 3 is heated together with the substrate layer 2. In other words, the substrate 20 with the coating layer is heated. The heating in step (1) improves the dimensional stability of the substrate 20 with the coating layer, including the substrate layer 2, during heating.

[0027] In the heating of the substrate layer 2 in step (1), for example, the substrate layer 2 having the coating layer 3 disposed on one surface in the thickness direction (substrate 20 with a coating layer) is placed in a heating furnace.

[0028] The heating temperature is preferably 110° C. or higher, more preferably 120° C. or higher, even more preferably 130° C. or higher, and particularly preferably 140° C. or higher. The upper limit of the heating temperature is, for example, 200° C. When the heating temperature is equal to or higher than the above-mentioned lower limit, the dimensional stability of the substrate layer 2 (substrate 20 with a coating layer) during heating can be improved.

[0029] The heating time is preferably 10 minutes or more, more preferably 30 minutes or more, and is, for example, 3 hours or less, preferably 1.5 hours or less. If the heating time is equal to or more than the above-mentioned lower limit, the dimensional stability of the substrate layer 2 (substrate 20 with coating layer) during heating can be improved. If the heating time is equal to or less than the above-mentioned upper limit, the manufacturing efficiency can be improved and the tact time can be shortened.

[0030] The heating can be carried out, for example, in an air atmosphere or in an inert atmosphere. An example of the inert atmosphere is a nitrogen atmosphere. The heating can be carried out, for example, under atmospheric pressure or under reduced pressure. From the viewpoint of carrying out the process easily, the heating is carried out in an air atmosphere and under atmospheric pressure.

[0031] The heating in step (1) causes oligomers contained in the base layer 2 to precipitate (distribute unevenly) on one surface of the base layer 2 in the thickness direction. However, in the present embodiment, the oligomers are prevented from penetrating the coating layer 3 in the thickness direction and precipitating on one surface of the coating layer 3 in the thickness direction.

[0032] After step (1), the ratio of oligomers on one surface of the coating layer 3 (substrate 20 with a coating layer) in the thickness direction is, for example, 1.5 × 10 -2 Less than or equal to 1.0×10 -2 Less than or equal to 5×10 -3 The following is particularly preferably 4×10 -3 For example, 1×10 -4 More than 5×10 -4The ratio of oligomers is the ratio of the intensity at m / z=577 to the intensity at m / z=104 when one surface of the coating layer 3 in the thickness direction is measured by TOF-SIMS. When the material of the base layer 3 is PET, m / z=104 is C7H4O derived from terephthalic acid, which is a monomer raw material of PET. + When the material of the base layer 3 is PET, m / z=577 is a C fragment peak derived from an oligomer of terephthalic acid (specifically, a cyclic trimer). 30 H 25 O 12 + The low ratio of the oligomers means that the amount of oligomers on one side of the coating layer 3 is small.

[0033] If the oligomer ratio on one side of the coating layer 3 is equal to or less than the above upper limit, peeling of the metal underlayer 4 from the coating layer 3 (substrate 20 with a coating layer) can be suppressed when the electrode 1 is used for a long period of time.

[0034] The conditions for the TOF-SIMS measurement will be described in the Examples section below.

[0035] 1.6.3 Process (2) In step (2), a metal underlayer 4 is formed on one surface in the thickness direction of the coating layer 3. In this embodiment, the metal underlayer 4 is formed by, for example, sputtering.

[0036] 1.6.4 Process (3) In step (3), the conductive carbon layer 5 is formed on one surface in the thickness direction of the metal base layer 4. In this embodiment, the conductive carbon layer 5 is formed by, for example, sputtering.

[0037] In this way, the electrode 1 is manufactured.

[0038] 1.7 Use of Electrode 1 The electrode 1 can be used, for example, as an electrode for electrochemical measurements and as an electrode for batteries, and preferably as an electrode for electrochemical measurements.

[0039] 2. Effects of one embodiment In the method for producing an electrode of the present invention, since the base layer 2 is heated to 110° C. or higher in step (1), the base layer 2 has excellent dimensional stability during heating.

[0040] On the other hand, if the base layer 2 is heated to 110°C or higher, oligomers originating from the material of the base layer 2 precipitate on one surface of the base layer 2 in the thickness direction and then tend to migrate to one side of the base layer 2 in the thickness direction, i.e., to the other surface of the metal base layer 4 in the thickness direction. If the oligomers migrate to the other surface of the metal base layer 4, the metal base layer 4 is likely to peel off from the base layer 2 side.

[0041] However, in this embodiment, since the coating layer 3 is disposed on one surface of the base layer 2 in the thickness direction, the coating layer 3 can suppress the migration of oligomers of the base layer 2 to the other surface of the metal underlayer 4.

[0042] Therefore, even if the electrode 1 is used for a long period of time, the metal base layer 4 is prevented from peeling off, and thus the durability of the electrode 1 can be improved. EXAMPLES

[0043] The present invention will be described in more detail below with reference to examples and comparative examples. The present invention is not limited to the examples and comparative examples. The specific numerical values ​​of the blending ratio (content ratio), physical property values, parameters, etc. used in the following description can be replaced with the upper limit (a numerical value defined as "less than or equal to" or "less than") or lower limit (a numerical value defined as "more than or equal to" or "exceeding") of the corresponding blending ratio (content ratio), physical property values, parameters, etc. described in the above "Form for carrying out the invention".

[0044] Example 1 Step (1): A commercially available substrate 20 with a coated layer (model number A4160, manufactured by Toyobo Co., Ltd.) was prepared. The substrate 20 with a coated layer includes a substrate layer 2 and a coating layer 3 in this order toward one side in the thickness direction. The substrate 20 with a coated layer had a thickness of 188 μm. The material of the substrate layer 2 was PET. The substrate layer 2 had a thickness of 187 μm. The coating layer 3 had a thickness of 1 μm.

[0045] Next, the substrate 20 with the coated layer was heated for 1 hour at 150° C. The substrate 20 with the coated layer was heated in an air atmosphere and under atmospheric pressure.

[0046] Step (2): A metal underlayer 4 was formed by sputtering on one surface of the coating layer 3 in the thickness direction. The sputtering conditions were as follows:

[0047] Target: Titanium Output: 3.3W / cm 2 Sputtering gas: Argon Pressure in sputtering chamber: 0.2 Pa

[0048] The material of the metal underlayer 4 was titanium, and the thickness of the metal underlayer 4 was 15 nm.

[0049] Step (3): A conductive carbon layer 5 was formed by sputtering on one surface of the metal underlayer 4 in the thickness direction. The sputtering conditions were as follows:

[0050] Target: Sintered carbon Power: 3.3 W / cm 2 Sputtering gas: Argon Pressure in sputtering chamber: 0.4 Pa

[0051] The conductive carbon layer had a thickness of 30 nm.

[0052] In this way, an electrode 1 was manufactured which was provided with the base layer 2, the coating layer 3, the metal underlayer 4, and the conductive carbon layer 5 in this order towards one side in the thickness direction.

[0053] Comparative Example 1 An electrode 1 was produced in the same manner as in Example 1. However, this electrode 1 did not include a coating layer 3. Specifically, the substrate 20 with a coating layer was not heated, and the substrate layer 2 was heated.

[0054] Comparative Example 2 An electrode 1 was produced in the same manner as in Example 1. However, the heating conditions in step (1) were changed to 80° C. and 1 minute.

[0055] evaluation The following items were evaluated, and the results are shown in Table 1.

[0056] <Oligomer ratio> One surface of the substrate 20 with the coating layer (coating layer 3) in the thickness direction during production, after step (1) and before step (2), was measured by TOF-SIMS. Then, the ratio of the intensity at m / z=577 to the intensity at m / z=104 was calculated. The conditions for the TOF-SIMS measurement are described below.

[0057] TOF-SIMS IONTOF Japan Primary ion Bi3 2+ Primary ion acceleration voltage: 25 kV Measurement area: 300μm square

[0058] In addition, for Comparative Example 1, one surface of the base layer 2 immediately before step (2) was measured by TOF-SIMS.

[0059] <Durability (degree of deterioration)> An insulating tape having a circular hole with a diameter of 1 mm was attached to one surface of the conductive carbon layer 5 in the thickness direction to prepare a sample electrode. This sample electrode was used as a working electrode.

[0060] After that, the sample electrode was immersed in a nitric acid solution, lead nitrate was added to the aqueous solution as an electrode active material, and electrochemical measurements were performed. In the electrochemical measurements, a voltage of -1.4 V was applied for 240 seconds by amperometry, and then square wave voltammetry (SWV) was performed. The SWV conditions were as follows:

[0061] Solution: 0.1M KCl+1mM HNO 3 +Pb 10ppb aqueous solution Cell: BAS radial flow cell Counter electrode: platinum electrode Reference electrode:Ag / AgCl electrode

[0062] The above electrochemical measurements were carried out 60 times.

[0063] Thereafter, the conductive carbon layer 5 in the round hole was observed under an optical microscope, and the area ratio of the deteriorated part was calculated based on a binarization method. The deteriorated part is a discolored part due to peeling of the metal base layer 4. As shown in Figure 3, the deteriorated part is a streaky part.

[0064] Degree of deterioration = area of ​​deteriorated part / area of ​​conductive carbon layer 5 in round hole

[0065] The durability of the electrode 1 was evaluated based on the following criteria.

[0066] A: The degree of deterioration was 0.2 or less. ×: The degree of deterioration exceeded 0.2.

[0067] An image processed from the optical microscope observation of Example 1 is shown in Fig. 2. An image processed from the optical microscope observation of Comparative Example 1 is shown in Fig. 3.

[0068] <Dimensional stability when heated> The substrate 20 with the coating layer immediately before step (2) was cut into a 30 mm square to prepare a sample. The sample was then heated for 1 hour in a heating oven at 150° C. The dimensions of the sample before and after heating were measured with an image dimension measuring device (Keyence, IM-6020), and the thermal shrinkage rate was calculated by the following formula.

[0069] Heat shrinkage rate [%] = (length of one side of sample after heating - length of one side of sample before heating) / length of one side of sample before heating × 100 The dimensional stability of the substrate 20 with the coating layer during heating was evaluated based on the following criteria.

[0070] A: The thermal shrinkage rate was 0.3% or less. ×: The thermal shrinkage rate exceeded 0.3%.

[0071] In Comparative Example 1, the base layer 2 immediately before the step (2) was used for evaluation of dimensional stability during heating.

[0072] [Table 1] [Explanation of symbols]

[0073] 1 electrode 2 Base material layer 3 Coating Layer 4 Metal base layer 5 Conductive carbon layer

Claims

[Claim 1] A method for manufacturing an electrode including a base layer, a coating layer, a metal underlayer, and a conductive carbon layer in this order toward one side in a thickness direction, A step (1) of heating a substrate layer having the coating layer disposed on one surface in a thickness direction to 110° C. or higher; (2) forming the metal underlayer on one surface of the coating layer in the thickness direction; and (3) forming the conductive carbon layer on one surface of the metal base layer in a thickness direction.