Inspection method and inspection system for aluminium member

The FT-IR based inspection method and system allow for non-destructive estimation of bonding characteristics in composite members by correlating wave number and intensity of reflected infrared light with aluminum hydroxide modification, addressing the need for destructive testing in existing methods.

JP2024140156APending Publication Date: 2024-10-10SINTOKOGIO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023051172
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing methods for manufacturing composite members with enhanced bonding strength, such as those described in Patent Document 1, require destructive testing to assess joint strength, making it difficult to quantify and ensure the quality of the composite members before they are produced.

Method used

An inspection method and system that utilizes Fourier Transform Infrared Spectroscopy (FT-IR) to detect the wave number and intensity of reflected infrared light on an aluminum member modified with aluminum hydroxide, allowing estimation of bonding characteristics without destructive testing, by correlating these parameters with the pre-obtained relationship between wave number and intensity of reflected infrared light and bonding characteristics.

Benefits of technology

Enables non-destructive estimation of bonding characteristics, specifically bonding strength, of composite members by analyzing the state of aluminum hydroxide modification on the aluminum surface, ensuring quality control before the composite member is manufactured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024140156000001_ABST
    Figure 2024140156000001_ABST
Patent Text Reader

Abstract

To provide an inspection method for an aluminum member and an inspection system for the aluminum member capable of estimating joining characteristics of a composite member without performing destructive inspection relative to the composite member.SOLUTION: A composite member is obtained by joining a resin member to an uneven surface of an aluminum member modified into an aluminum hydroxide. A method for inspecting the aluminum member before being joined to a resin member includes the steps of: detecting a wave number and intensity of reflected light of infrared light with which the aluminum member is irradiated; and estimating bonding characteristics of the composite member based on the wave number and intensity of the reflected light of the detected infrared light, and a previously acquired relation between the wave number and intensity of the reflected light of the infrared light and the bonding characteristics.SELECTED DRAWING: Figure 12
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to an inspection method and an inspection system for aluminum components. [Background technology]

[0002] Patent Document 1 discloses a method for manufacturing a composite member. With this method, a composite member is manufactured by bonding a base material and a resin member. Micro- or nano-order irregularities are formed on the surface of the base material. The resin member penetrates into the micro- or nano-order irregularities and solidifies, resulting in a stronger anchor effect than in the case of millimeter-order irregularities. As a result, the composite member manufactured by this method has excellent bonding strength. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2017 / 141381 Summary of the Invention [Problem to be solved by the invention]

[0004] When obtaining the bonding strength of a composite member as described in Patent Document 1, it is necessary to perform a destructive test after manufacturing the composite member. For this reason, it is difficult to provide the composite member as a product after obtaining the bonding strength of the composite member. In addition, there are cases where unevenness is formed on the surface of an aluminum member by modifying the surface of the aluminum member to aluminum hydroxide. The state of formation of the unevenness is difficult to confirm visually, and there is a risk that quantitative evaluation cannot be performed. The present disclosure provides a technique that can estimate the bonding strength of a composite member without performing a destructive test on the composite member. [Means for solving the problem]

[0005] According to one aspect of the present invention, there is provided a method for inspecting an aluminum member. The method for inspecting an aluminum member is a method for inspecting an aluminum member before it is joined to a resin member, which is a composite member obtained by joining a resin member to an uneven surface of an aluminum member modified to aluminum hydroxide. The method for inspecting an aluminum member includes a detecting step and an estimating step. In the detecting step, the wave number and intensity of reflected light of infrared light irradiated onto the aluminum member are detected. In the estimating step, the joining characteristics of the composite member are estimated based on the detected wave number and intensity of the reflected light of infrared light and a previously acquired correlation between the wave number and intensity of the reflected light of infrared light and the joining characteristics. Effect of the Invention

[0006] According to one aspect and embodiment of the present disclosure, there is provided an aluminum component inspection method and an aluminum component inspection system that can estimate the joining characteristics of a composite component without performing destructive testing on the composite component. [Brief description of the drawings]

[0007] [Figure 1] FIG. [Diagram 2] FIG. 2 is a conceptual diagram of a blast processing device used in the manufacturing method of a composite member. [Diagram 3] FIG. 2 is a diagram illustrating the configuration of a blast processing device used in the manufacturing method of a composite member. [Figure 4] FIG. 2 is a top view of a mold used for injection molding. [Diagram 5] 5 is a cross-sectional view of the mold taken along line VV in FIG. 4. [Figure 6] 1 is a flowchart showing an example of a method for manufacturing a composite member. [Figure 7] FIG. 1 is a conceptual diagram of blast processing. [Figure 8] FIG. 13 is a diagram illustrating scanning in blast processing. [Figure 9] 9 is a cross-sectional view taken along line IX-IX in FIG. 1 for explaining a manufacturing process of the composite material. [Figure 10]FIG. 10 is a conceptual diagram of the aluminum member shown in FIG. [Figure 11] 1 is a conceptual diagram of an inspection system for an aluminum member according to an embodiment. [Figure 12] 4 is a flowchart of an inspection method for an aluminum member according to an embodiment. [Figure 13] 1 is a graph showing the results of measuring an infrared spectrum of a surface of an aluminum member according to an example. [Figure 14] 1 is a table showing the relationship between the strength corresponding to the wave number of the aluminum hydroxide peak on the surface of the aluminum member according to the example and the bonding strength. [Figure 15] 1 is a graph showing the relationship between the strength corresponding to the wave number of the aluminum hydroxide peak on the surface of the aluminum member according to the example and the bonding strength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] [Overview of the embodiment of the present disclosure] First, an overview of the embodiment of the present disclosure will be described.

[0009] (Clause 1) An aluminum inspection method according to one aspect of the present disclosure is a method for inspecting an aluminum component prior to joining with a resin component, which is a composite component obtained by joining a resin component to an uneven surface of an aluminum component modified to aluminum hydroxide. The aluminum component inspection method includes a detecting step and an estimating step. In the detecting step, the wave number and intensity of reflected light of infrared light irradiated onto the aluminum component are detected. In the estimating step, the joining characteristics of the composite component are estimated based on the detected wave number and intensity of the reflected light of infrared light and a previously acquired correlation between the wave number and intensity of the reflected light of infrared light and the joining characteristics.

[0010] This aluminum member inspection method is applied to the aluminum member before the aluminum member and the resin member are joined to obtain a composite member. In this inspection method, the wave number and intensity of the reflected light of infrared light irradiated to the aluminum member are detected. Here, the trend of the wave number and intensity of the reflected light of infrared light reflects the formation state of the compound on the surface of the aluminum member. The formation state of the compound includes, for example, the modified state of the aluminum hydroxide on the surface of the aluminum member. In addition, the modified state of the aluminum hydroxide is related to the bonding characteristics between the aluminum member and the resin member. Therefore, in the estimation step, the bonding characteristics of the composite member are estimated based on the detected wave number and intensity of the reflected light and the previously acquired correlation between the wave number and intensity of the reflected light of infrared light and the bonding characteristics. Therefore, according to this aluminum member inspection method, the bonding characteristics of the composite member can be estimated without performing a destructive inspection on the composite member.

[0011] (Clause 2) In the aluminum component inspection method according to the clause 1, the bonding characteristics may include at least bonding strength. In this case, the aluminum component inspection method makes it possible to estimate at least the bonding strength, among the bonding characteristics of the composite component, without performing a destructive inspection on the composite component.

[0012] (Clause 3) In the method for inspecting an aluminum component according to clause 1 or 2, the wavenumber and intensity of the reflected infrared light in the correlation may include a wavenumber and intensity corresponding to an aluminum hydroxide peak. Here, the intensity of the reflected infrared light corresponding to the aluminum hydroxide peak is correlated with a modified state of the aluminum hydroxide on the surface of the aluminum component. Furthermore, the modified state of the aluminum hydroxide in the aluminum component is correlated with the bonding characteristics between the aluminum component and the resin component. Therefore, in the estimation step, the bonding characteristics of the composite component are estimated based on the wavenumber and intensity of the detected reflected light and the previously acquired correlation between the wavenumber and intensity of the reflected infrared light and the bonding characteristics.

[0013] (Clause 4) The method for inspecting an aluminum component according to any one of clauses 1 to 3 may include a step of determining whether an intensity of the detected reflected infrared light with respect to a wave number corresponding to a wave number of an aluminum hydroxide peak is less than a predetermined threshold, and a step of notifying an abnormality if the intensity is determined to be less than the predetermined threshold in the determining step. In this case, an abnormality is notified if the intensity of the detected reflected infrared light with respect to a wave number corresponding to a wave number of an aluminum hydroxide peak is less than the threshold, so that an aluminum component having inappropriate joining characteristics for a composite component can be detected before the production of the composite component.

[0014] (Clause 5) An inspection system for an aluminum member according to another aspect of the present disclosure is an inspection system for an aluminum member before it is joined to a resin member, of a composite member obtained by joining a resin member to an uneven surface of an aluminum member modified to aluminum hydroxide. The inspection system for an aluminum member includes an irradiation unit, a detection unit, and an estimation unit. The irradiation unit irradiates the aluminum member with infrared light. The detection unit detects the wave number and intensity of the reflected light of the infrared light irradiated by the irradiation unit. The estimation unit estimates the joining characteristics of the composite member based on the wave number and intensity of the reflected light detected by the detection unit and a previously acquired correlation between the wave number and intensity of the reflected light of the infrared light and the joining characteristics.

[0015] This aluminum component inspection system is applied to an aluminum component before the aluminum component and the resin component are joined to obtain a composite component. In this inspection system, the wave number and intensity of the reflected light of infrared light irradiated to the aluminum component by the irradiation unit are detected. Here, the tendency of the wave number and intensity of the reflected light of infrared light reflects the formation state of a compound on the surface of the aluminum component. The formation state of the compound includes, for example, the modified state of aluminum hydroxide on the surface of the aluminum component. In addition, the modified state of the aluminum hydroxide is related to the bonding characteristics between the aluminum component and the resin component. Therefore, the estimation unit estimates the bonding characteristics of the composite component based on the detected wave number and intensity of the reflected light and the previously acquired correlation between the wave number and intensity of the reflected light of infrared light and the bonding characteristics. Therefore, according to this aluminum component inspection system, the bonding characteristics of the composite component can be estimated without performing destructive testing on the composite component.

[0016] (Clause 6) In the aluminum component inspection system according to Clause 5, the bonding characteristics may include at least bonding strength. In this case, the aluminum component inspection system can estimate at least the bonding strength, among the bonding characteristics of the composite component, without performing destructive testing on the composite component.

[0017] (Clause 7) In the inspection system for aluminum components described in Clause 5 or 6, the wavenumber and intensity of the reflected infrared light in the correlation may include a wavenumber and intensity corresponding to an aluminum hydroxide peak. Here, the intensity of the reflected infrared light corresponding to the aluminum hydroxide peak is correlated with a modified state of the aluminum hydroxide on the surface of the aluminum component. Furthermore, the modified state of the aluminum hydroxide in the aluminum component is correlated with the bonding characteristics between the aluminum component and the resin component. Therefore, the estimation unit estimates the bonding characteristics of the composite component based on the wavenumber and intensity of the detected reflected light and a previously acquired correlation between the wavenumber and intensity of the reflected infrared light and the bonding characteristics.

[0018] (Clause 8) The aluminum component inspection system according to any one of clauses 5 to 7 includes a treatment section that modifies the surface of the aluminum component into aluminum hydroxide, and a transport section that transports the aluminum component from the treatment section, and the irradiation section may be provided on the transport section and irradiate infrared light onto the aluminum component transported by the transport section. In this case, a plurality of aluminum components can be efficiently inspected on a production line for aluminum components, which contributes to efficient production of composite components.

[0019] [Examples of the embodiments of the present disclosure] Hereinafter, an embodiment of the present disclosure will be described with reference to the drawings. In the following description, the same or equivalent elements are given the same reference numerals, and overlapping descriptions will not be repeated. The dimensional ratios of the drawings do not necessarily match those in the description. The abrasive material in this embodiment is a member that is sprayed during blast processing, and is, for example, abrasive grains of ceramics (alumina, silicon carbide, etc.). Unless otherwise specified, the particle diameter of the abrasive material in this embodiment is expressed as the average particle diameter (D50).

[0020] [Composite material] FIG. 1 is a perspective view showing a composite member 1 according to an embodiment. As shown in FIG. 1, the composite member 1 is a member in which a plurality of members are integrated by bonding. The composite member 1 is obtained by bonding a resin member 4 to an aluminum member 2. The aluminum member 2 is, for example, a plate-shaped member. The resin member 4 is in direct contact with a part or the whole of the surface of the aluminum member 2. In FIG. 1, the resin member 4 is bonded to a part of the surface of the aluminum member 2, and has a lap joint structure. The material of the aluminum member 2 is not limited, and is, for example, A5052, ADC12, etc. The material of the resin member 4 is a resin such as polybutylene terephthalate, polyphenylene sulfide, polyamide, liquid crystal polymer, polypropylene, or acrylonitrile butadiene styrene.

[0021] [Manufacturing method for composite materials] An outline of an apparatus used in the manufacturing method of the composite material 1 will be described. First, an apparatus for blasting the surface 2a of the aluminum member 2 will be described. The blasting apparatus may be any type, such as a gravity type (suction type) air blasting apparatus, a direct pressure type (pressurized type) air blasting apparatus, or a centrifugal type blasting apparatus. The manufacturing method according to this embodiment uses, as an example, a so-called direct pressure type (pressurized type) air blasting apparatus. FIG. 2 is a conceptual diagram of a blasting apparatus 10 used in the manufacturing method of the composite material 1. The blasting apparatus 10 includes a treatment chamber 11, a spray nozzle 12, a storage tank 13, a pressurized chamber 14, a compressed gas supplier 15, and a dust collector (not shown).

[0022] A spray nozzle 12 is housed inside the treatment chamber 11, and blast processing is performed on a workpiece (here, an aluminum member 2) in the treatment chamber 11. The abrasives sprayed by the spray nozzle 12 fall to the bottom of the treatment chamber 11 together with dust. The fallen abrasives are supplied to a storage tank 13, and the dust is supplied to a dust collector. The abrasives stored in the storage tank 13 are supplied to a pressurizing chamber 14, and the pressurizing chamber 14 is pressurized by a compressed gas supply machine 15. The abrasives stored in the pressurizing chamber 14 are supplied to the spray nozzle 12 together with the compressed gas. In this manner, the workpiece is blast processed while the abrasives are circulated.

[0023] Fig. 3 is a diagram illustrating the configuration of a blast processing device 10 used in the manufacturing method of a composite member 1 according to the embodiment. The blast processing device 10 shown in Fig. 3 is the direct pressure type blasting device shown in Fig. 2. In Fig. 3, the wall surface of a processing chamber 11 is partially omitted.

[0024] As shown in Figure 3, the blast processing device 10 includes a storage tank 13 for abrasives and a pressurized chamber 14 formed into an airtight structure to which a compressed gas supplier 15 is connected, a constant-volume supply section 16 connected to the storage tank 13 within the pressurized chamber 14, a spray nozzle 12 connected to the constant-volume supply section 16 via a connecting pipe 17, a processing table 18 that moves while holding a workpiece below the spray nozzle 12, and a blast control section 19.

[0025] The blast control unit 19 controls the components of the blast processing device 10. The blast control unit 19 includes a display unit and a blast processing unit as an example. The blast processing unit is a general computer having a CPU, a storage unit, and the like. The blast control unit 19 controls the supply amount of the compressed gas supply device 15 that supplies compressed gas to the storage tank 13 and the pressurizing chamber 14 based on the set injection pressure and injection speed. The blast control unit 19 also controls the injection position of the injection nozzle 12 based on the set distance between the workpiece and the nozzle, and the scanning conditions of the workpiece (speed, feed pitch, number of scans, etc.). As a specific example, the blast control unit 19 controls the position of the injection nozzle 12 using the scanning speed (X direction) and feed pitch (Y direction) set before the blast processing. The blast control unit 19 controls the position of the injection nozzle 12 by moving the processing table 18 that holds the workpiece.

[0026] In the blast processing device 10 configured in this manner, compressed gas is supplied from the compressed gas supply machine 15 to the storage tank 13 and the pressurized chamber 14 at an amount controlled by the blast control unit 19. Then, by a constant pressure flow force, the abrasives in the storage tank 13 are metered in the constant quantity supply unit 16 in the pressurized chamber 14 and supplied to the injection nozzle 12 via the connecting pipe 17, and are injected from the injection nozzle 12 onto the processing surface of the workpiece. In this way, a constant amount of abrasives is always injected onto the processing surface of the workpiece. Then, the injection position of the injection nozzle 12 on the processing surface of the workpiece is controlled by the blast control unit 19, and the workpiece is blast processed.

[0027] The sprayed abrasives and cutting powder generated during the blasting process are sucked up by a dust collector (not shown). A classifier (not shown) is arranged on the path from the processing chamber 11 to the dust collector, and separates the abrasives into reusable abrasives and other fine powder (abrasives that have become too large to be reused and cutting powder generated during the blasting process). The reusable abrasives are stored in a storage tank 13 and are supplied to the spray nozzle 12 again. The fine powder is collected by the dust collector.

[0028] Next, a method for joining the aluminum member 2 and the resin member 4 will be described. As an example of the joining method, injection molding will be described. In this embodiment, insert molding is used as the injection molding. In insert molding, an insert part is attached to a predetermined mold, and resin is injected and held for a predetermined time to solidify. After that, residual stress in the resin is removed by heat treatment. FIG. 4 is a top view of a mold used for injection molding. FIG. 5 is a cross-sectional view of the mold taken along line VV in FIG. 4. As shown in FIGS. 4 and 5, the mold 20 includes a mold body 21 (upper mold 21a and lower mold 21b). Between the upper mold 21a and the lower mold 21b, there are provided a space 22 for mounting an insert part (here, the aluminum member 2) and a space 23 into which the resin is injected. A resin injection port is provided on the upper surface of the upper mold 21a. The resin injection port communicates with the space 23 via a sprue 24, a runner 25, and a gate 26. A pressure sensor 27 and a temperature sensor 28 are provided in the space 23 to detect the pressure and temperature in the space 23. Based on the detection results of the pressure sensor 27 and the temperature sensor 28, parameters of a molding machine (not shown) are adjusted to manufacture a molded product. The parameters include the mold temperature, resin temperature during filling, filling pressure, injection rate, holding time, pressure during holding, heat treatment temperature, heat treatment time, etc. The molded product molded in the mold 20 has a lap joint structure that is joined over a specified area.

[0029] Next, a series of steps in the manufacturing method of the composite member 1 will be described. FIG. 6 is a flow chart of the manufacturing method MT of the composite member 1. As shown in FIG. 6, first, in a preparation step (S10), a predetermined abrasive is filled into a blast processing device 10. The particle diameter of the abrasive is, for example, 30 μm to 710 μm. The smaller the particle diameter of the abrasive, the smaller the mass, and therefore the lower the inertial force. For this reason, when the particle diameter of the abrasive is smaller than 30 μm, it is difficult to form the irregularities 2b of a desired shape. Furthermore, the aluminum member 2 used industrially is generally stored in the atmosphere, and its surface is covered with a non-uniform natural aluminum oxide film having a thickness of 60 nm to 300 nm. For this reason, surface etching with a chemical or surface laser processing may result in non-uniform surface treatment due to the presence of the natural aluminum oxide film. In order to uniformly modify the surface 2a of the aluminum member 2 in the surface hydroxylation step described later, it is necessary to make the natural aluminum oxide film a film having a thickness of about 30 nm or less. However, if the particle diameter of the abrasive exceeds 710 μm, it becomes difficult to remove the natural oxide film of aluminum to a thickness of about 30 nm or less. Therefore, the natural oxide film formed on the surface 2a of the aluminum member 2 before the blasting process step (S20) described below is not sufficiently removed. The particle diameter of the abrasive that can achieve both the formation of the irregularities 2b and the removal of the natural oxide film of aluminum is 30 μm to 710 μm. The material of the abrasive is, for example, alumina. The abrasive has, for example, acute-angled protrusions.

[0030] The blast control unit 19 of the blast processing device 10 acquires blast processing conditions as a preparation step (S10). The blast control unit 19 acquires the blast processing conditions based on the operation of an operator or information stored in the memory unit. The blast processing conditions include the injection pressure, injection speed, nozzle distance, and scanning conditions of the work (speed, feed pitch, number of scans). The injection pressure is, for example, 0.5 MPa or more and 2.0 MPa or less. The smaller the injection pressure, the lower the inertial force. Therefore, when the injection pressure is less than 0.5 MPa, it is difficult to form the irregularities 2b of the desired shape. The higher the injection pressure, the higher the inertial force. Therefore, the abrasives are more likely to be crushed by collision with the aluminum member 2. As a result, problems such as (1) poor processing efficiency because the energy of the collision is dispersed to other than the formation of the irregularities 2b, and (2) the abrasives are worn out significantly, making it uneconomical, etc. occur. Such problems become more pronounced when the injection pressure exceeds 2.0 MPa. The blast control unit 19 manages the blast processing conditions to precisely control the size, depth, density, etc. of the irregularities 2b on the surface 2a of the aluminum member 2 on the micro- or nano-order. The blast processing conditions may include conditions for specifying the region to be blasted. In this case, selective surface treatment is possible.

[0031] Next, the blast processing device 10 performs the following series of processes as a blast processing step (S20). First, the aluminum member 2 to be blasted is set on the processing table 18 in the processing chamber 11. The aluminum member 2 does not substantially contain magnesium and sodium. Next, the blast control unit 19 operates a dust collector (not shown). The dust collector reduces the pressure inside the processing chamber 11 to a negative pressure state based on a control signal from the blast control unit 19. Next, the injection nozzle 12 injects the abrasives as a two-phase solid-gas flow of compressed air at an injection pressure in the range of 0.5 MPa to 2.0 MPa based on a control signal from the blast control unit 19. Next, the blast control unit 19 operates the processing table 18 to move the aluminum member 2 into the injection flow of the two-phase solid-gas flow (below the injection nozzle in FIG. 3). FIG. 7 is a conceptual diagram of the blast processing. As shown in FIG. 7, the abrasives are injected from the injection nozzle 12 to a partial region 2f of the surface 2a of the aluminum member 2. Here, the blast control unit 19 continues the operation of the processing table 18, and operates it so that the jet flow draws a preset trajectory on the aluminum member 2. FIG. 8 is a diagram explaining the scanning of the blast processing. As shown in FIG. 8, the blast control unit 19 operates the processing table 18 according to a scanning trajectory L at a feed pitch P. FIG. 9 is a cross-sectional view taken along line IX-IX in FIG. 1, explaining the manufacturing process of the composite member. As shown in FIG. 9(A), the aluminum member 2 before the blast processing has no unevenness 2b formed. By the above-mentioned operation of the processing table 18, the desired micro-order unevenness 2b is formed on the surface 2a of the aluminum member 2, as shown in FIG. 9(B).

[0032] By performing blast processing using abrasives having a particle diameter of 30 μm or more and 710 μm or less at a spray pressure range of 0.5 MPa or more and 2.0 MPa or less, desired micro-order irregularities 2b are formed on the surface 2a of the aluminum member 2. Hereinafter, the surface 2a of the aluminum member 2 refers to the outermost surface layer of the aluminum member 2 regardless of whether the surface is processed or modified. Note that the surface 2a of the aluminum member 2 is also referred to as the surface 2c of the irregularities 2b when specifically explaining the surface layer of the irregularities 2b. The micro-order irregularities are irregularities having a height difference of 1 μm or more and less than 1000 μm. FIG. 10 is a conceptual diagram of the aluminum member shown in FIG. 9. As shown in FIG. 10, the irregularities 2b have an inclined portion 2e that is inclined from the convex portion to the concave portion of the irregularities 2b. The inclined portion 2e contributes to the joining with the resin member 4 and serves as a stress concentration portion that contributes to the shear resistance. The arithmetic mean roughness Ra of the unevenness 2b as defined in JIS B0601 (1994) may be 0.7 μm or more and 5.0 μm or less by the blasting process. The arithmetic mean slope RΔa of the unevenness 2b as defined in JIS B0601 (1994) may be 0.17 or more and 0.50 or less by the blasting process, as calculated by the formula shown in FIG. 10. The root mean square slope RΔq of the unevenness 2b as defined in JIS B0601 (1994) may be 0.27 or more and 0.60 or less by the blasting process. Furthermore, the natural oxide film on the surface 2a of the aluminum member 2 is, for example, a film having a thickness of about 9 nm or less. After the operation of the blasting device 10 is stopped, the aluminum member 2 is taken out, and the blasting process is completed. As shown in FIG. 9B, the unevenness 2b of the surface 2a of the aluminum member 2 after the blasting process has acute projections.

[0033] Next, in the surface hydroxylation step (S30), the processing unit 30 of the inspection system 100 described later modifies the surface 2a of the aluminum member 2 to aluminum hydroxide to form a surface nanostructure 2d. For example, the processing unit 30 performs hydrothermal treatment on the surface 2a of the aluminum member 2 on which the irregularities 2b are formed, and modifies the surface 2c of the irregularities 2b to aluminum hydroxide. As a result, the processing unit 30 forms a surface nanostructure 2d formed of aluminum hydroxide on the surface 2c of the irregularities 2b. Aluminum hydroxide is an aluminum hydroxide and is an aluminum compound having a hydroxyl group. In the hydrothermal treatment in the surface hydroxylation step (S30), the surface 2a of the aluminum member 2 is reacted with heated water. In the hydrothermal treatment, the aluminum member 2 on which the irregularities 2b are formed is immersed in pure water heated to 70°C or higher and 100°C or lower for a predetermined period of time. As a result, the surface 2c of the irregularities 2b is modified mainly to boehmite, and the surface nanostructure 2d is formed. By using the pure water, it is possible to suppress impurities other than aluminum hydroxide from remaining on the surface 2a of the aluminum member 2. The aluminum hydroxide formed on the surface 2a of the aluminum member 2 is not limited to boehmite, and may be any one of diaspore, pseudo-boehmite, bayerite, nostrandite, gibbsite, and doillite. The aluminum hydroxide formed on the surface 2a of the aluminum member 2 may be formed of a plurality of types of aluminum hydroxide selected from diaspore, boehmite, pseudo-boehmite, bayerite, nostrandite, gibbsite, and doillite. As shown in (C) of FIG. 9, the surface nanostructure 2d is formed on the surface 2c of the unevenness 2b, and the surface nanostructure 2d is exposed on the surface 2a of the aluminum member 2. The surface nanostructure 2d is a film made of aluminum hydroxide and is sponge-like (porous). A plurality of pores having a pore size of 10 nm or more and less than 1000 nm are formed in the surface nanostructure 2d. The thickness of the surface nanostructure 2d is not less than 0.01 μm and not more than 1 μm.As a result, a spongy (porous) surface nanostructure 2d is formed on the sharp portions (acute-angled protrusions) of the unevenness 2b formed by the blasting process (S20) and is modified into aluminum hydroxide, which has the additional effect of making it less likely that the resin member 4 penetrating the unevenness 2b will break starting from the sharp portions.

[0034] Next, a molding machine (not shown) performs molding using the above-mentioned mold 20 as a joining step (S40). First, the mold 20 is opened, the aluminum member 2 modified to aluminum hydroxide (with the surface nanostructure 2d formed) is mounted in the space 22, and the mold 20 is closed. Then, the molding machine injects molten resin having a set resin temperature into the inside of the mold 20 from the resin injection port. The injected resin passes through the sprue 24, the runner 25, and the gate 26 and fills the space 23. The molding machine controls the filling pressure and injection rate of the resin based on the detection result of the pressure sensor 27. Based on the detection result of the temperature sensor 28, the molding machine controls the mold temperature to be a set value. Also, based on the detection result of the pressure sensor 27, the molding machine controls the pressure to be a set value during a set retention time. After that, the molding machine performs heat treatment based on the set heat treatment temperature and heat treatment time. At this time, as shown in FIG. 9(D), functional groups contained in the aluminum member 2 and functional groups in the resin member 4 bond to each other, thereby bonding the aluminum member 2 and the resin member 4. For example, an oxygen atom of a hydroxyl group in the surface nanostructure 2d forms a hydrogen bond with a hydrogen atom contained in the resin member 4. Thereafter, the molding machine opens the mold 20 and removes the composite member 1 in which the aluminum member 2 and the resin member 4 are integrated. When the bonding step (S40) is completed, the flowchart shown in FIG. 6 ends. Note that the bonding step (S40) may be performed by bonding the resin member 4 to the surface 2a of the aluminum member 2 by thermocompression molding, press molding, or ultrasonic bonding.

[0035] As described above, according to the manufacturing method MT of the composite member 1, the surface 2a of the aluminum member 2 is blasted. In the blasting process (S20), the natural oxide film formed on the surface 2a of the aluminum member 2 is thinned (removed) by the blasting process. The surface 2a of the aluminum member 2 (the surface exposed by the blasting process) is formed with micro-order irregularities 2b by the blasting process. In the surface hydroxylation process (S30), the surface 2a of the aluminum member 2 on which the irregularities 2b are formed (surface 2c of the irregularities 2b) is modified to aluminum hydroxide. As a result, a surface nanostructure 2d is formed on the surface 2c of the irregularities 2b. The surface nanostructure 2d is formed of aluminum hydroxide. As a result of this modification, functional groups of aluminum hydroxide (e.g., hydroxyl groups) are imparted to the irregularities 2b of the aluminum member 2. The resin member 4 penetrates into the unevenness 2b of the surface 2a of the aluminum member 2 and solidifies; the surface nanostructure 2d on the surface layer of the unevenness 2b increases the contact surface area between the aluminum member 2 and the resin member 4, and the resin member 4 penetrates into the surface nanostructure 2d and solidifies; and the functional groups present on the surface 2c of the unevenness 2b and the functional groups present on the resin member 4 are bonded. By organically bonding these three components, a synergistic effect is created that cannot be achieved by simply adding the anchor effect or molecular bond effect of each component, and a strong bond is realized. Then, in the bonding process (S40), the resin member 4 is bonded to the surface of the aluminum member 2. The functional groups present on the surface of the resin member 4 are bonded to the aluminum member 2 by molecular bonding between the functional groups present on the surface and the functional groups contained in the aluminum member 2. The sharp parts of the unevenness 2b formed by the blasting process (S20) are scraped off by the surface hydroxylation process (S30). Therefore, this manufacturing method MT has the additional effect of making it difficult for the resin member 4 to break from sharp parts (acute-angled protrusions). As described above, a composite member 1 is manufactured in which the aluminum member 2 and the resin member 4 are joined together with more effective joining characteristics by chemical bonding through molecular bonds and mechanical bonding through the anchor effect over a wide surface area. The joining characteristics include at least the joining strength.

[0036] According to manufacturing method MT, in the blasting process step (S20), abrasives having a particle size of 30 μm or more and 710 μm or less and having acute protrusions are sprayed at a spray pressure of 0.5 MPa or more and 2.0 MPa or less to perform blasting. As a result, this manufacturing method MT can properly remove the natural oxide film formed on the surface 2a of the aluminum member 2 and then form the irregularities 2b on the surface 2a of the aluminum member 2, so that in the surface hydroxylation process (S30), a uniform surface nanostructure 2d can be formed on the surface 2a of the aluminum member 2 and the anchor effect can be properly exerted.

[0037] [Aluminum component inspection equipment] Fig. 11 is a conceptual diagram of an inspection system for an aluminum member according to an embodiment. An inspection system 100 for an aluminum member 2 shown in Fig. 11 (hereinafter referred to as "inspection system 100") is provided in a manufacturing system in which a manufacturing method MT for a composite member 1 is executed. The inspection system 100 inspects the aluminum member 2 before bonding with the resin member 4, of the composite member 1 obtained by bonding a resin member 4 to a surface 2a of the irregularities 2b of the aluminum member 2 that has been modified to aluminum hydroxide (having a surface nanostructure 2d formed thereon).

[0038] The inspection system 100 includes a processing section 30, a transport section 40, an inspection unit 50, and an inspection control section 60. The processing section 30 modifies the surface 2a of the aluminum member 2 to aluminum hydroxide. The processing section 30 forms a surface nanostructure 2d on the surface 2a of the aluminum member 2. That is, the processing section 30 executes processing related to the surface hydroxylation step (S30) in the manufacturing method MT of the composite member 1 described above. The processing section 30 includes a storage section 31 that stores the aluminum member 2 on which the blast processing step (S20) is performed and on which the unevenness 2b is formed, and a heater 32 that can heat the storage section 31. The storage section 31 is a water tank in which hydrothermal treatment can be performed. The storage section 31 immerses the aluminum member 2 in heated water. The storage section 31 reacts the aluminum member 2 on which the unevenness 2b is formed with the heated water. The heater 32 heats the storage section 31 so that the temperature of the water in the storage section 31 is 70°C or higher and 100°C or lower. The processing section 30 may have a temperature sensor. The processing section 30 may control the heater 32 so that the temperature of the accommodation section 31 acquired by the temperature sensor is 70° C. or higher and 100° C. or lower.

[0039] The transport section 40 transports the aluminum member 2 from the processing section 30. The transport section 40 is provided, for example, close to the processing section 30. The transport section 40 includes, for example, a transport robot 41 and a belt conveyor 42. The transport robot 41 takes out the aluminum member 2 for which the surface hydroxylation step (S30) has been completed from the storage section 31 of the processing section 30, and places the aluminum member 2 on the belt conveyor 42. The transport robot 41 is, for example, a robot arm. The belt conveyor 42 places and moves the aluminum member 2 with the surface 2a facing upward. The belt conveyor 42 can repeatedly transport (move) and stop the aluminum member 2. The belt conveyor 42 transports the aluminum member 2, for example, to the position of the mold 20 where the joining step (S40) is performed.

[0040] The inspection unit 50 inspects whether or not aluminum hydroxide is formed on the surface 2a of the aluminum member 2. The inspection unit 50 is, for example, a Fourier Transform Infrared Spectroscopy. The inspection unit 50 performs an FT-IR method and measures the infrared spectrum (intensity) of the aluminum member 2.

[0041] The inspection unit 50 has an irradiation section 51, an optical fiber 52, a prism 53, a shielding section 54, and a detection section 55. The irradiation section 51 irradiates the aluminum member 2 with infrared light. The optical fiber 52 is provided below the irradiation section 51 (on the belt conveyor 42 side) and extends toward the belt conveyor 42. The optical fiber 52 guides the infrared light irradiated from the irradiation section 51 to the prism 53. The optical fiber 52 guides the infrared light refracted from the prism 53 to the detection section 55.

[0042] The prism 53 is provided at the lower end of the optical fiber 52. The prism 53 extends downward from the optical fiber 52 to a position where the prism 53 can contact or approach the aluminum member 2 placed on the belt conveyor 42. The prism 53 refracts the infrared light guided from the optical fiber 52 and guides it to the irradiation target range of the aluminum member 2. The prism 53 refracts the infrared light reflected by the aluminum member 2 and guides it to the optical fiber 52. The shielding portion 54 covers at least the lower end of the optical fiber 52 and the prism 53, and shields at least the lower end of the optical fiber 52 and the prism 53 from light from outside. The shielding portion 54 is, for example, a cylindrical member.

[0043] The detection unit 55 detects the wave number and intensity of the reflected light of the infrared light irradiated by the irradiation unit 51. Detecting the wave number includes at least one of obtaining the wave number directly from the reflected light and calculating the wave number based on the wavelength of the reflected light. The wave number is the reciprocal of the wavelength. The detection unit 55 receives, from the optical fiber 52, the infrared light irradiated from the irradiation unit 51 to the aluminum member 2 and reflected by the aluminum member 2. The detection unit 55 is, for example, an optical sensor.

[0044] The inspection unit 50 is provided close to the aluminum member 2 so that no gap is formed between at least the prism 53 and the aluminum member 2. The position of the inspection unit 50 is adjusted with respect to the transport section 40 so that, for example, external light such as lighting does not enter between at least the prism 53 and the aluminum member 2 to be inspected.

[0045] The inspection control unit 60 is connected to the inspection unit 50. The inspection control unit 60 is configured as, for example, a PLC (Programmable Logic Controller). The inspection control unit 60 may be configured as a computer system including a processor such as a CPU (Central Processing Unit), memories such as a RAM (Random Access Memory) and a ROM (Read Only Memory), input / output devices such as a touch panel, a mouse, a keyboard, and a display, and a communication device such as a network card. The inspection control unit 60 realizes the function of the inspection control unit 60 by operating each piece of hardware under the control of the processor based on a computer program stored in the memory.

[0046] The inspection control unit 60 includes an acquisition unit 61, an irradiation control unit 62, a storage unit 63, an estimation unit 64, a determination unit 65, and a notification unit 66. The acquisition unit 61 acquires the wave number and intensity of the reflected infrared light detected by the detection unit 55. The irradiation control unit 62 controls the irradiation unit 51 of the inspection unit 50. The irradiation control unit 62 acquires the position of the aluminum component 2 on the transport unit 40. The irradiation control unit 62 causes the irradiation unit 51 to irradiate infrared light when the aluminum component 2 is located directly below the inspection unit 50.

[0047] The memory unit 63 stores the association between the wave number and intensity of the reflected infrared light and the joining characteristics. The joining characteristics include at least the joining strength. The association includes information that associates the wave number and intensity of the reflected infrared light with the joining characteristics of the composite material 1 when the composite material 1 is manufactured by the manufacturing method MT. The association includes, for example, a table, a formula, a graph, etc. that associates the wave number and intensity of the reflected infrared light with the joining characteristics. The wave number and intensity of the reflected infrared light in the association includes the wave number and intensity corresponding to the peak of aluminum hydroxide. In other words, the association includes a table, a formula, a graph, etc. that associates the wave number and intensity corresponding to the peak of aluminum hydroxide with the joining characteristics of the composite material 1. The formula includes an approximation calculated based on a table that associates the wave number and intensity corresponding to the peak of aluminum hydroxide with the joining characteristics of the composite material 1.

[0048] The wave number corresponding to the peak of aluminum hydroxide is, for example, 3340 cm -1 , and 1075cm -1 Including 3340cm -1 The peak at 3340 cm in this embodiment is a peak detected in response to the bond of a hydroxyl group. -1 The peak at 1075 cm is detected when aluminum hydroxide (e.g., Al(OH)3) and water (H2O) are present in the area to be examined. -1 The peak at 1075 cm in this embodiment is a peak detected in response to a bond between an aluminum atom and a hydroxyl group. -1A peak in is detected when aluminum hydroxide (e.g., Al(OH)3) is present in the inspection target area. In the surface hydroxylation step (S30), the longer the treatment time of the hydrothermal treatment on the aluminum member 2, the greater the intensity at the wave number corresponding to the aluminum hydroxide peak on the surface 2a of the aluminum member 2. Furthermore, in the surface hydroxylation step (S30), the longer the treatment time of the hydrothermal treatment on the aluminum member 2, the better the bonding characteristics of the composite member 1 in which the aluminum member 2 and the resin member 4 are bonded together. Therefore, there is a correlation between the intensity at the wave number corresponding to the aluminum hydroxide peak and the bonding characteristics. For example, the greater the intensity at the wave number corresponding to the aluminum hydroxide peak, the greater the bonding strength.

[0049] The estimation unit 64 estimates the bonding characteristics of the composite member based on the wavenumber and intensity of the reflected light detected by the detection unit 55 and the above-mentioned correlation. The estimation unit 64 estimates the bonding characteristics corresponding to the wavenumber and intensity of the reflected infrared light detected by the detection unit 55 in the above-mentioned correlation. The estimation unit 64 estimates the bonding characteristics (e.g., bonding strength) by substituting, for example, the intensity for the wavenumber of the reflected infrared light detected by the detection unit 55 corresponding to the wavenumber of the peak of aluminum hydroxide into a mathematical formula.

[0050] The determination unit 65 determines whether or not the intensity of the wave number of the peak of aluminum hydroxide among the wave numbers of the reflected infrared light detected is less than a predetermined threshold value. The threshold value is stored in advance in the storage unit 63. The threshold value is set for each wave number of the reflected infrared light. For example, the threshold value is set for each wave number corresponding to the peak of aluminum hydroxide. For example, the threshold value is set so that the bonding strength of the composite material 1 is equal to or greater than a predetermined strength.

[0051] The notification unit 66 notifies of an abnormality when the determination unit 65 determines that the intensity of the reflected infrared light detected by the detection unit 55 relative to the wave number is less than a predetermined threshold. The inspection system 100 includes, for example, an abnormality display unit, a buzzer, etc., which are not shown. The abnormality display unit is, for example, a display. The notification unit 66 outputs a signal to the abnormality display unit to visually display that an abnormality exists. The notification unit 66 outputs a signal to the buzzer to emit a sound or voice indicating that an abnormality exists.

[0052] Next, a series of steps of the inspection method for the aluminum member 2 will be described. FIG. 12 is a flowchart of the inspection method for the aluminum member according to the embodiment. The inspection method CT for the aluminum member 2 is executed by the inspection system 100. The inspection method CT for the aluminum member 2 is executed, for example, after the surface hydroxylation step (S30) and before the joining step (S40) in the manufacturing method MT for the composite member 1. The inspection method CT for the aluminum member 2 is executed, for example, after the hydrothermal treatment is performed for a predetermined time by the processing unit 30. As shown in FIG. 12, first, as a conveying step (S31), the aluminum member 2 is conveyed from the processing unit 30 by the conveying unit 40. The conveying robot 41 of the conveying unit 40 takes out the aluminum member 2 from the storage unit 31 of the processing unit 30, and places it on the belt conveyor 42 so that the surface 2a (surface nanostructure 2d) of the aluminum member 2 faces the inspection unit 50. The belt conveyor 42 conveys the aluminum member 2 directly under the inspection unit 50.

[0053] Next, in an irradiation step (S32: an example of an irradiating step), the irradiation section 51 of the inspection unit 50 irradiates infrared light onto the aluminum member 2 transported by the transport section 40. Note that the belt conveyor 42 may continue to transport (move) the aluminum member 2 even during the irradiation step (S32). The belt conveyor 42 may stop transporting the aluminum member 2 during the irradiation step (S32).

[0054] Subsequently, in a detection step (S33: an example of a detection step), the detection section 55 of the inspection unit 50 detects the wave number and intensity of the reflected light of the infrared light irradiated onto the aluminum member 2 by the irradiating section 51.

[0055] Next, as a determination step (S34: an example of a determination step), the determination unit 65 determines whether or not the intensity of the detected reflected infrared light at a wave number is less than a predetermined threshold. In this embodiment, the determination unit 65 determines whether or not the intensity of the detected reflected infrared light at a wave number of an aluminum hydroxide peak is less than a predetermined threshold. If the intensity is less than the predetermined threshold, the inspection system 100 proceeds to a notification step (S35). If the intensity is equal to or greater than the predetermined threshold, the inspection system 100 proceeds to an estimation step (S36).

[0056] In the determination step (S34), when the determination unit 65 determines that the intensity of the aluminum hydroxide peak relative to the wave number is less than the predetermined threshold, the notification unit 66 notifies of an abnormality in the notification step (S35: an example of a notification step). The notification unit 66 outputs a signal to an abnormality display unit, a buzzer, or the like to notify of the abnormality. In the determination step (S34), when the determination unit 65 determines that the intensity of the aluminum hydroxide peak relative to the wave number is less than the predetermined threshold, the aluminum member 2 to be determined may be excluded from the transport unit 40.

[0057] In the determination step (S34), when the determination unit 65 determines that the intensity of the aluminum hydroxide peak relative to the wave number is not less than the predetermined threshold value, or when the notification step (S35) is executed, an estimation step (S36: an example of an estimation step) is executed. In the estimation step (S36), the estimation unit 64 estimates the joining characteristics of the composite material 1 based on the wave number and intensity of the reflected light detected by the detection unit 55 and the previously acquired correlation between the wave number and intensity of the reflected light of the infrared light and the joining characteristics. In the estimation step (S36), the estimation unit 64 estimates the joining characteristics when the composite material 1 is manufactured using the aluminum member 2 irradiated with infrared light based on the intensity of the reflected light relative to the wave number detected by the detection unit 55 corresponding to the wave number of the aluminum hydroxide peak, the wave number, and the above-mentioned correlation. When the estimation step (S36) is completed, the flowchart of the inspection method CT shown in FIG. 12 is completed.

[0058] For example, if the judgment unit 65 judges in the judgment step (S34) that the intensity of the aluminum hydroxide peak versus wave number is not less than a predetermined threshold, the aluminum member 2 is transported to the position of the mold 20 where the joining step (S40) in the manufacturing method MT of the composite member 1 is performed.

[0059] As described above, the inspection method CT for the aluminum member 2 and the inspection system 100 for the aluminum member 2 are applied to the aluminum member 2 before the aluminum member 2 and the resin member 4 are joined to obtain the composite member 1. In the irradiation step (S32), the irradiation unit 51 irradiates the aluminum member with infrared light, and in the detection step (S33), the wave number and intensity of the reflected light of the irradiated infrared light are detected by the detection unit 55. Here, the tendency of the wave number and intensity of the reflected light of the infrared light reflects the formation state of the compound on the surface of the aluminum member. The formation state of the compound includes, for example, the modified state of the aluminum hydroxide on the surface of the aluminum member. In the reflected light of the infrared light, the intensity corresponding to the peak of the aluminum hydroxide is related to the modified state of the aluminum hydroxide on the surface 2a of the aluminum member 2. In addition, the modified state of the aluminum hydroxide in the aluminum member is related to the joining characteristics between the aluminum member 2 and the resin member 4. Therefore, in the estimation unit 64, the bonding characteristics of the composite member 1 are estimated based on the wave number and intensity of the detected reflected light and the previously acquired correlation between the wave number and intensity of the reflected infrared light and the bonding characteristics. The wave number and intensity of the reflected infrared light in this correlation includes the wave number and intensity corresponding to the peak of aluminum hydroxide. Therefore, according to the inspection method CT for the aluminum member 2 and the inspection system 100 for the aluminum member 2, the bonding characteristics of the composite member 1 can be estimated without performing a destructive inspection on the composite member 1. Since the bonding characteristics of this embodiment include at least the bonding strength, according to the inspection method CT for the aluminum member 2 and the inspection system 100 for the aluminum member 2, at least the bonding strength of the bonding characteristics of the composite member 1 can be estimated without performing a destructive inspection on the composite member 1.

[0060] Here, in the inspection unit 50, the shielding section 54 covers at least the lower end of the optical fiber 52 and the prism 53 to block external light. In addition, the positions of the prism 53 and the aluminum member 2 are adjusted so that external light does not enter at least between the detection section 55 and the inspection target. This suppresses the effect of noise on the detected reflected light, and the detection section 55 can appropriately detect the modified state of the aluminum hydroxide on the surface 2a of the aluminum member 2, i.e., the wave number and intensity of the reflected infrared light.

[0061] In the above-described embodiment, the FT-IR method is performed in the irradiation step (S32) by the irradiation unit 51 and the detection step (S33) by the detection unit 55. Compared to the case where a measurement method using Raman spectroscopy or a hyperspectral camera is performed, the inspection system 100 performs the FT-IR method, so that the surface nanostructure 2d having a small thickness formed on the surface 2a of the aluminum member 2 can be detected with high accuracy. Compared to the case where X-ray diffraction measurement method (XRD) or Auger electron spectroscopy (AES) is performed, the inspection system 100 performs the FT-IR method, so that even if the aluminum member 2 has been subjected to the blast processing step (S20) and has the unevenness 2b formed thereon, the surface nanostructure 2d can be detected with high accuracy without being significantly affected by the unevenness. In addition, when X-rays are irradiated to the aluminum member 2 being transported by the transport unit 40, additional equipment is required to prevent the X-rays from scattering to the outside, which is costly. Furthermore, while Auger electron spectroscopy (AES) allows elemental analysis, it is difficult to detect compounds, whereas the FT-IR method in the inspection system 100 can adequately detect the characteristics of the compound aluminum hydroxide.

[0062] In the inspection method CT for the aluminum member 2 and the inspection system 100 for the aluminum member 2, the judgment unit 65 executes a judgment step (S34). In the inspection method CT for the aluminum member 2 and the inspection system 100 for the aluminum member 2, when it is judged in the judgment step (S34) that the intensity of the reflected light of the detected infrared light corresponding to the wave number of the peak of the aluminum hydroxide is less than a predetermined threshold, the notification unit 66 executes a notification step (S35). In this case, an abnormality is notified when the intensity of the reflected light of the detected infrared light corresponding to the wave number of the peak of the aluminum hydroxide is less than the threshold, so that an aluminum member 2 having inappropriate joining characteristics of the composite member 1 can be detected before the manufacturing of the composite member 1, and the worker can grasp the aluminum member 2. The worker who recognizes the notification by the notification unit 66 can, for example, remove the aluminum member 2 from the belt conveyor 42, so that the manufacturing of a composite member 1 whose joining characteristics are estimated to not satisfy a predetermined level in the joining step (S40) can be suppressed.

[0063] The inspection system 100 for the aluminum member 2 includes a processing unit 30 and a transport unit 40, and the irradiation unit 51 is provided on the transport unit 40 and irradiates infrared light onto the aluminum member 2 transported by the transport unit 40. In this case, a plurality of aluminum members 2 can be efficiently inspected on the manufacturing line for the aluminum members 2, which contributes to efficient manufacturing of the composite member 1.

[0064] [Modifications of the inspection method and inspection system] Although the present embodiment has been described above, the present invention is not limited to the present embodiment, and can be implemented in various modifications within the scope of the present embodiment. For example, the estimation step (S36) may be performed after the detection step (S33) regardless of whether or not at least one of the determination step (S34) and the notification step (S35) is performed. The inspection method CT for the aluminum member 2 may not perform the determination step (S34) and the notification step (S35). The inspection method CT for the aluminum member 2 may perform the determination step (S34) and the notification step (S35) without performing the estimation step (S36). The inspection system 100 may not include at least one of the processing unit 30 and the transport unit 40. The inspection control unit 60 may not include at least one of the determination unit 65 and the notification unit 66. The inspection control unit 60 may not include the memory unit 63. In this case, the inspection system 100 may include a storage medium capable of communicating with the inspection control unit 60 as the storage unit 63.

[0065] [Modifications of aluminum and resin materials] Although the aluminum member 2 and the resin member 4 according to the above embodiment are shown as plate-shaped members, the shape is not limited thereto, and any shape that allows them to come into contact with each other can be adopted. The resin member 4 according to the above embodiment is in contact with a part of the surface 2a of the aluminum member 2, but it may be in contact with the entire surface 2a of the aluminum member 2.

[0066] The material of the resin member is not limited to the above-mentioned examples. For example, the material of the resin member may be a thermoplastic fiber reinforced resin or a thermosetting fiber reinforced resin. The thermoplastic fiber reinforced resin includes, for example, aramid fiber reinforced thermoplastic resin (AFRTP: Aromatic polyamide Fiber Reinforced Thermo Plastics), carbon fiber reinforced thermoplastic resin (CFRTP: Carbon Fiber Reinforced Thermo Plastics), and glass fiber reinforced thermoplastic resin (GFRTP: Glass Fiber Reinforced Thermo Plastics). The thermosetting fiber reinforced resin includes, for example, aramid fiber reinforced resin (AFRP: Aromatic polyamide Fiber Reinforced Plastics), carbon fiber reinforced resin (CFRP: Carbon Fiber Reinforced Plastics), and glass fiber reinforced resin (GFRP: Glass Fiber Reinforced Plastics).

[0067] [Modifications of injection molding] The injection molding is not limited to insert molding, but may be outsert molding. EXAMPLES

[0068] [Confirmation of aluminum hydroxide peak] In the following, in order to explain the above-mentioned effects, the present disclosure will be described in more detail with reference to examples. The present disclosure is not limited to these examples. First, Examples 1 and 2 and Comparative Example 1 were prepared to confirm the relationship between the treatment time of the hydrothermal treatment and the wave number and intensity corresponding to the peak of aluminum hydroxide.

[0069] [Example 1] The blasting process step (S20) was carried out using the blasting device shown in FIG. 2 and FIG. 3. The aluminum member was an aluminum plate (JIS: ADC12). For the blasting process, alumina with acute-angled protrusions was used as the material, and the abrasives had a central particle diameter of 106 μm to 125 μm. The blasting pressure was 1.0 MPa. At this time, irregularities with arithmetic mean roughness Ra, arithmetic mean slope RΔa, and root-mean-square slope RΔq of 2.5 μm, 0.35, and 0.42, respectively, as specified in JIS B0601 (1994), were formed on the surface of the aluminum member. Subsequently, a hydrothermal treatment was carried out in the surface hydroxylation process (S30). The time (treatment time) for immersing the blasted aluminum member in pure water at 90° C. was 0.5 minutes. For the hydrothermal treatment, pure water, which is ion-exchanged water and has an electrical conductivity of 0.05 μS / cm, was used.

[0070] [Example 2] In Example 2, the treatment time of the hydrothermal treatment in the surface hydroxylation step (S30) of the production method MT was set to 2 minutes. The other conditions were the same as those of Example 1.

[0071] [Comparative Example 1] In Comparative Example 1, the hydrothermal treatment time in the surface hydroxylation step (S30) of the manufacturing method MT was set to 0 minutes. That is, an aluminum member was prepared that had not been subjected to the hydrothermal treatment in the surface hydroxylation step (S30). The other conditions were the same as those in Example 1.

[0072] [Evaluation of aluminum hydroxide peaks] For Examples 1 and 2 and Comparative Example 1, a Fourier transform infrared spectrophotometer (FT-IR spectrometer ALPHAII manufactured by Bruker Japan) was used as the inspection unit to carry out the FT-IR method and measure the infrared spectrum of the aluminum member. FIG. 13 is a graph showing the measurement results of the infrared spectrum of the surface of the aluminum member according to the example. The vertical axis of FIG. 13 shows the intensity (infrared spectrum), and the horizontal axis shows the wave number (cm -1) are shown. The results of Example 1 are shown by a solid line, the results of Example 2 are shown by a dashed line, and the results of Comparative Example 1 are shown by a dashed line. By comparing the results of Examples 1 and 2 and the results of Comparative Example 1 shown in FIG. 13, it was confirmed that the longer the treatment time of the hydrothermal treatment, the higher the strength across the entire wavenumber. In addition, by comparing the results of Examples 1 and 2 and the results of Comparative Example 1, it was confirmed that by carrying out the hydrothermal treatment, -1 , and 1075cm -1 It was confirmed that there was a peak in the wavenumber band around 3340 cm. -1 The peak at 1075 cm is detected when aluminum hydroxide (e.g., Al(OH)3) and water (HO) are present in the test area. -1 The peak in is detected when aluminum hydroxide (e.g., Al(OH)3) is present in the test area. Therefore, it was shown that the surface of the aluminum component was modified to aluminum hydroxide (a surface nanostructure was formed) by performing the hydrothermal treatment in the surface hydroxylation step (S30).

[0073] [Relationship between aluminum hydroxide peak and bonding strength] Next, Examples 3 to 8 and Comparative Example 2 were prepared, and the relationship between the treatment time of the hydrothermal treatment, the wave number and intensity corresponding to the peak of aluminum hydroxide, and the bonding strength of the composite member was confirmed.

[0074] [Example 3] The blasting process step (S20) was carried out using the blasting device shown in FIG. 2 and FIG. 3. The aluminum member was an aluminum plate (JIS: ADC12). For the blasting process, alumina with acute-angled protrusions was used as the material, and the abrasives had a central particle diameter of 106 μm to 125 μm. The blasting pressure was 1.0 MPa. At this time, irregularities with arithmetic mean roughness Ra, arithmetic mean slope RΔa, and root-mean-square slope RΔq of 2.5 μm, 0.35, and 0.42, respectively, as specified in JIS B0601 (1994), were formed on the surface of the aluminum member. Subsequently, a hydrothermal treatment was carried out in the surface hydroxylation process (S30). The time (treatment time) for immersing the blasted aluminum member in pure water at 90° C. was 0.5 minutes. For the hydrothermal treatment, pure water, which is ion-exchanged water and has an electrical conductivity of 0.05 μS / cm, was used. Next, a joining step (S40) was performed. Using the mold shown in Fig. 4 and Fig. 5, a resin member was joined by injection molding to the aluminum member that had been subjected to the hydrothermal treatment. The material of the resin member was polyphenylene sulfide resin (PPS). During injection, the mold temperature was 150°C, the injection speed was 20 mm / s, the injection pressure was 53 MPa or more and 93 MPa or less, and the injection time was 0.56 s. During holding, the holding pressure was 80 MPa, and the holding time was 8 s. In the shear strength test piece, the area of ​​the joint between the aluminum member and the resin member was 50 mm2 of 5 mm x 10 mm. 2 It was decided.

[0075] [Example 4] In Example 4, the treatment time of the hydrothermal treatment in the surface hydroxylation step (S30) of the production method MT was set to 1 minute, and the other conditions were the same as those of Example 3.

[0076] [Example 5] In Example 5, the treatment time for the hydrothermal treatment in the surface hydroxylation step (S30) of the production method MT was set to 2 minutes, and the other conditions were the same as those of Example 3.

[0077] [Example 6] In Example 6, the treatment time of the hydrothermal treatment in the surface hydroxylation step (S30) of the production method MT was set to 3 minutes, and the other conditions were the same as those of Example 3.

[0078] [Example 7] In Example 7, the treatment time of the hydrothermal treatment in the surface hydroxylation step (S30) of the production method MT was set to 4 minutes, and the other conditions were the same as those of Example 3.

[0079] [Example 8] In Example 8, the treatment time of the hydrothermal treatment in the surface hydroxylation step (S30) of the production method MT was set to 5 minutes, and the other conditions were the same as those of Example 3.

[0080] [Comparative Example 2] In Comparative Example 2, the hydrothermal treatment time in the surface hydroxylation step (S30) of the manufacturing method MT was set to 0 minutes. That is, an aluminum member was prepared that had not been subjected to the hydrothermal treatment in the surface hydroxylation step (S30). The other conditions were the same as those in Example 3.

[0081] [Evaluation of aluminum hydroxide peaks] During the manufacturing process of each composite member according to Examples 3 to 8 and Comparative Example 2, after the surface hydroxylation step (S30) was completed and before the joining step (S40) was performed, the infrared spectrum of the aluminum member was measured by FT-IR method using a Fourier transform infrared spectrophotometer (FT-IR spectrometer: ALPHAII manufactured by Bruker Japan). -1 , and 1075cm -1 A baseline was drawn by connecting the start and end of the waveform with a straight line for the curve containing the infrared spectrum intensity of each peak at 3340 cm. The difference from the apex of each peak to the baseline was calculated as the intensity. -1 In contrast, the strength of Example 3 was 0.125, the strength of Example 4 was 0.173, the strength of Example 5 was 0.219, the strength of Example 6 was 0.262, the strength of Example 7 was 0.293, the strength of Example 8 was 0.32, and the strength of Comparative Example 2 was 0.-1 In contrast, the strength of Example 3 was 0.025, the strength of Example 4 was 0.035, the strength of Example 5 was 0.041, the strength of Example 6 was 0.048, the strength of Example 7 was 0.052, the strength of Example 8 was 0.057, and the strength of Comparative Example 2 was 0.

[0082] After the infrared spectrum measurement, the above-mentioned bonding step (S40) was carried out. The bonding strengths of Examples 3 to 8 and Comparative Example 2 prepared under the above conditions were measured. As an example of the bonding strength, the shear strength was measured. The evaluation device was used for the measurement by a test method conforming to ISO 19095-2 (overlapped test piece (Type B)). The bonding strength of Example 3 was 11 MPa, the shear strength of Example 4 was 21 MPa, the shear strength of Example 5 was 36 MPa, the bonding strength of Example 6 was 34 MPa, the shear strength of Example 7 was 37 MPa, the shear strength of Example 8 was 38 MPa, and the shear strength of Comparative Example 2 was 7 MPa.

[0083] Fig. 14 is a table showing the relationship between the strength corresponding to the wave number of the aluminum hydroxide peak on the surface of the aluminum member according to the embodiment and the bonding strength. Fig. 15 is a graph showing the relationship between the strength corresponding to the wave number of the aluminum hydroxide peak on the surface of the aluminum member according to the embodiment and the bonding strength. Fig. 15(A) shows the strength corresponding to the wave number of the aluminum hydroxide peak on the surface of the aluminum member according to the embodiment, 3340 cm -1 15B is a graph showing the relationship between the strength corresponding to the aluminum hydroxide peak at 1075 cm on the surface of the aluminum member according to the embodiment and the bonding strength. -1 15A and 15B are graphs showing the relationship between the strength corresponding to the bonding strength and the bonding strength, in which the vertical axis in each of (A) and (B) of Fig. 15 shows the bonding strength (MPa), and the horizontal axis shows the intensity of reflected light (infrared spectrum).

[0084] As shown in Figures 14, 15(A) and 15(B), when the intensity corresponding to each wave number of the aluminum hydroxide peak is equal to or less than a predetermined value, it was confirmed that the longer the treatment time of the hydrothermal treatment in the surface hydroxylation step (S30), the higher the intensity corresponding to each wave number of the aluminum hydroxide peak and the higher the bonding strength. For example, -1 In the case where the intensity corresponding to the wave number of the aluminum hydroxide peak is 0.25 or less, the longer the treatment time of the hydrothermal treatment in the surface hydroxylation step (S30), the higher the intensity corresponding to each wave number of the aluminum hydroxide peak and the higher the bonding strength. -1 When the intensity corresponding to each wave number of the aluminum hydroxide peak is 0.045 or less, the longer the treatment time of the hydrothermal treatment in the surface hydroxylation step (S30), the greater the intensity corresponding to each wave number of the aluminum hydroxide peak and the greater the bonding strength. In other words, it was shown that there is a correlation between the intensity corresponding to each wave number of the aluminum hydroxide peak and the bonding strength.

[0085] It was also confirmed that when the bonding strength reached around 35 MPa, the rate of increase in bonding strength decreased even though the strength corresponding to each wave number of the aluminum hydroxide peak increased as the hydrothermal treatment time increased. This suggests that when the hydrothermal treatment time has elapsed for a certain period of time, even if the surface continues to be modified to aluminum hydroxide, the surface nanostructure has already been formed on the surface, so the increase in new surface area due to the surface nanostructure slows down, and the effect on the bonding strength between the aluminum member and the resin member is reduced.

[0086] From this, it was confirmed that when the intensity corresponding to each wave number of the aluminum hydroxide peak is less than a predetermined value, the bonding strength corresponding to that intensity is uniquely determined. Furthermore, it was confirmed that when the intensity corresponding to each wave number of the aluminum hydroxide peak is equal to or greater than a predetermined value, it is suggested that the bonding strength corresponding to that intensity is equal to or greater than a predetermined value. -1 , and 1075cm -1It was confirmed that the intensities of the peaks at wavenumbers of 100 and 150 are correlated with the bonding strength. Therefore, it was suggested that the bonding strength can be estimated by detecting the intensity corresponding to at least one wavenumber of the aluminum hydroxide peaks and inputting the intensity into the relationship. From the above, it is considered that the bonding strength can be appropriately estimated by calculating a relational expression showing the relationship between the intensity corresponding to each wavenumber of the aluminum hydroxide peak and the bonding strength, and inputting the intensity corresponding to each wavenumber of the aluminum hydroxide peak into the relational expression. [Explanation of symbols]

[0087] 1...composite member, 2...aluminum member, 2b...unevenness, 2d...surface nanostructure, 4...resin member, 10...blast processing device, 19...blast control unit, 20...mold, 30...processing unit, 40...transport unit, 50...inspection unit, 51...irradiation unit, 52...optical fiber, 53...prism, 54...shielding unit, 55...detection unit, 60...inspection control unit, 61...acquisition unit, 62...irradiation control unit, 63...memory unit, 64...estimation unit, 65...judgment unit, 66...alarm unit, 100...inspection system, CT...inspection method.

Claims

1. A method for inspecting an aluminum component before bonding with a resin component, the method comprising the steps of: detecting a wave number and an intensity of reflected light of infrared light irradiated onto the aluminum member; estimating the joining characteristics of the composite member based on the detected wave number and intensity of the reflected infrared light and a previously acquired correlation between the wave number and intensity of the reflected infrared light and joining characteristics; 2. A method for inspecting an aluminum component, comprising:

2. The method for inspecting an aluminum member according to claim 1 , wherein the bonding characteristics include at least a bonding strength.

3. The method for inspecting an aluminum member according to claim 1 or 2, wherein the wavenumber and intensity of the reflected infrared light in the correlation include a wavenumber and intensity corresponding to a peak of aluminum hydroxide.

4. determining whether the intensity of the reflected infrared light detected at a wave number corresponding to the wave number of an aluminum hydroxide peak is less than a predetermined threshold value; a step of notifying an abnormality when the intensity is determined to be less than a predetermined threshold in the step of determining; The method for inspecting an aluminum member according to claim 1 or 2, further comprising:

5. A system for inspecting an aluminum component before bonding with a resin member, the system being included in a composite component obtained by bonding a resin member to an uneven surface of an aluminum component modified with aluminum hydroxide, the system comprising: an irradiation unit that irradiates the aluminum member with infrared light; a detection unit that detects a wave number and an intensity of reflected light of the infrared light irradiated by the irradiation unit; an estimation unit that estimates the joining characteristics of the composite material based on a wave number and an intensity of the reflected light detected by the detection unit and a previously acquired correlation between the wave number and the intensity of the reflected light of the infrared light and joining characteristics; An inspection system for an aluminum component comprising:

6. The aluminum component inspection system according to claim 5 , wherein the bonding characteristics include at least bonding strength.

7. 7. The aluminum component inspection system according to claim 5 or 6, wherein the wavenumber and intensity of the reflected infrared light in the correlation include a wavenumber and intensity corresponding to a peak of aluminum hydroxide.

8. a treatment section for modifying a surface of the aluminum member into the aluminum hydroxide; a conveying section that conveys the aluminum member from the processing section; Equipped with 7. The aluminum component inspection system according to claim 5, wherein the irradiation unit irradiates the aluminum component transported by the transport unit with infrared light.

Citation Information

Patent Citations

  • Production method for composite member, and composite member

    WO2017141381A1