Method of manufacturing heat exchanger

By softening and hardening the base material of heat exchangers, the method addresses the challenge of forming fins on hard materials, ensuring desired shapes and mechanical strength.

JP2024140660APending Publication Date: 2024-10-10SUMITOMO PRECISION PRODUCTS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023051917
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Conventional methods face difficulties in forming fins on heat exchangers with somewhat hard materials like aluminum or aluminum alloys, as it is challenging to carve them into desired shapes due to their hardness.

Method used

The method involves softening the base material through annealing to reduce its hardness below 40 Vickers, followed by skiving to form fins, and then hardening it back to the required strength using age hardening treatment.

Benefits of technology

This approach allows for the formation of fins with desired shapes and ensures mechanical strength, improving workability and enabling the production of heat exchangers with enhanced performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024140660000001_ABST
    Figure 2024140660000001_ABST
Patent Text Reader

Abstract

To provide a method of manufacturing a heat exchanger, which can form a fin with a desired shape even when a base material with a certain level of hardness is skived.SOLUTION: A method of manufacturing a heat exchanger includes the steps of: softening a base material 10 with a predetermined level of hardness; forming a fin 11 by shaving and raising a surface 10a of the softened base material 10 by skiving; and hardening the base material 10 by applying a heat treatment to the base material 10 after the formation of the fin 11.SELECTED DRAWING: Figure 10
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a heat exchanger, and more particularly to a method for manufacturing a heat exchanger having fins formed on its outer surface by skiving. [Background technology]

[0002] 2. Description of the Related Art Conventionally, a method for manufacturing a heat exchanger having fins formed on its outer surface by skiving is known (see, for example, Patent Document 1).

[0003] The above-mentioned Patent Document 1 discloses a method for manufacturing a heat exchanger by forming fins on the outer surface of the heat exchanger by skiving. Specifically, the above-mentioned Patent Document 1 discloses a method for manufacturing a heat exchanger by forming fins by scraping the surface of a heat sink material made of aluminum or an aluminum alloy having a Vickers hardness of 40 to 65 by skiving. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2001-156224 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, when forming fins by skiving a heat sink material (base material) that is relatively hard, such as aluminum or an aluminum alloy having a Vickers hardness of 40 to 65, there is a problem in that it is difficult to cut the fins into the desired shape.

[0006] The present invention has been made to solve the above-mentioned problems, and one object of the present invention is to provide a method for manufacturing a heat exchanger that is capable of forming fins having a desired shape, even when skiving is performed on a substrate that is relatively hard. [Means for solving the problem]

[0007] In order to achieve the above object, the inventors of the present application conducted intensive research and found that it is possible to soften a base material having a predetermined hardness before skiving the base material, and then perform skiving on the surface of the softened base material, thereby making it possible to carve fins into a desired shape. That is, the manufacturing method of a heat exchanger according to the present invention includes a step of softening a base material having a predetermined hardness, a step of forming fins by carving the surface of the softened base material by skiving, and a step of hardening the base material by performing a heat treatment on the base material after the fins have been formed.

[0008] In the method for manufacturing a heat exchanger according to the present invention, as described above, the step of softening a base material having a predetermined hardness and the step of scraping the surface of the softened base material by skiving to form fins are provided. This makes it possible to perform skiving in a state where the base material is softened to a hardness suitable for forming fins, even when skiving is performed on a base material that is somewhat hard, thereby improving the workability when scraping the fins. As a result, it is possible to provide a method for manufacturing a heat exchanger that can form fins having a desired shape even when skiving is performed on a base material that is somewhat hard. In addition, the method for manufacturing a heat exchanger according to the present invention includes a step of hardening the base material by heat treating the base material after forming the fins, as described above. This makes it possible to harden the softened base material after the fins are formed, so that the hardness of the base material after the fins are formed can be restored to a predetermined hardness. As a result, when manufacturing a heat exchanger having fins having a desired shape by skiving, it is possible to make the hardness of the heat exchanger (fins) a predetermined hardness, so that the mechanical strength required for the heat exchanger can be ensured.

[0009] In the method for manufacturing a heat exchanger according to the above invention, the step of softening the base material preferably includes a step of annealing the base material, and in the step of annealing the base material, the base material is softened by annealing so that its hardness becomes less than Vickers hardness 40. With this configuration, the base material is softened to a hardness of less than Vickers hardness 40, so that when a fin is formed on a relatively hard base material by skiving, the base material can be softened to a hardness that allows the fin to be scraped into a desired shape. As a result, it is possible to improve the processability of a relatively hard base material so that the fin can be scraped into a desired shape, so that even when a fin is formed on a relatively hard base material by skiving, the fin can be easily scraped into a desired shape.

[0010] In this case, preferably, in the step of annealing the substrate, the substrate is softened by annealing so that the substrate has a hardness equivalent to that of an O material. In this manner, the substrate can be reliably softened to a Vickers hardness of less than 40. As a result, the substrate can be reliably softened to a hardness that allows the fin to be cut into a desired shape.

[0011] When the substrate is softened by annealing to a hardness of less than Vickers hardness 40, the heat treatment for hardening the substrate in the step of hardening the substrate preferably includes age hardening. In this manner, the substrate softened to a hardness of less than Vickers hardness 40 can be easily hardened to a predetermined hardness.

[0012] In this case, the base material before softening is preferably aluminum or an aluminum alloy having a Vickers hardness of 58 or more, and in the step of annealing the base material, the base material having a Vickers hardness of 58 or more is softened by annealing to a hardness of less than Vickers hardness 40, and in the step of hardening the base material, the base material is hardened to a hardness of 58 or more by age hardening. With this configuration, it is possible to scrape off fins by skiving after softening an aluminum or aluminum alloy base material having a hardness equivalent to T5 material of Vickers hardness 58 or more to an equivalent to O material of Vickers hardness less than 40, so that fins having a desired shape can be scraped off compared to a configuration in which fins are formed on a base material having a hardness equivalent to T5 material. In addition, since the base material after forming fins by skiving is hardened to a hardness of 58 or more by age hardening, the base material after forming fins can be restored to a hardness equivalent to T5 material. As a result, even when fins are formed by skiving on an aluminum or aluminum alloy substrate having a hardness equivalent to that of T5 material, a method for manufacturing a heat exchanger can be provided that is capable of forming fins having a desired shape while maintaining mechanical strength equivalent to that of T5 material.

[0013] In the method for manufacturing a heat exchanger according to the above invention, the substrate is preferably an extruded material, and is a multi-hole tube including a plurality of through holes extending along the extrusion direction of the substrate, and the method further includes a step of bending the multi-hole tube after forming the fins and before hardening the multi-hole tube. With this configuration, the substrate is softened by the annealing treatment, so that the substrate can be easily curved. As a result, a curved heat exchanger, such as a heat exchanger used as a surface cooler for an aircraft engine, can be easily manufactured.

[0014] In this case, preferably, the method further includes a step of welding a predetermined member to the multi-hole pipe after bending the multi-hole pipe and before hardening the multi-hole pipe. With this configuration, since the predetermined member is welded to the multi-hole pipe before hardening the multi-hole pipe, even if the weld heat affected zone softens during welding, the weld heat affected zone can be hardened at the same time when the multi-hole pipe is hardened. As a result, it is possible to suppress a decrease in the mechanical strength of the weld zone caused by softening of the weld heat affected zone when the predetermined member is welded.

[0015] In the method for manufacturing a heat exchanger according to the above invention, preferably, in the step of forming the fins, the surface of the base material is scraped by skiving so that the fins have a thickness of 0.4 mm to 1.0 mm and the interval between the fins is 2.0 mm to 4.0 mm. In this way, even when manufacturing a heat exchanger in which fins having a thin thickness of 0.4 mm to 1.0 mm are arranged at narrow intervals of 2.0 mm to 4.0 mm, the base material is softened by annealing, making it possible to easily scrape the fins into a desired shape. Effect of the Invention

[0016] According to the present invention, as described above, it is possible to provide a method for manufacturing a heat exchanger that is capable of forming fins having a desired shape even when skiving is performed on a substrate that is relatively hard. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a schematic perspective view showing a heat exchanger according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic vertical cross-sectional view of a heat exchanger. [Diagram 3] FIG. 2 is a schematic diagram for explaining the structure of a base material before fins are formed. [Figure 4] FIG. 2 is a schematic diagram of a top view of a base material before fins are formed. [Diagram 5] FIG. 4 is a schematic diagram for explaining the structure of a base material on which a fin-forming portion is formed. [Figure 6] 1A to 1C are schematic diagrams illustrating a process for forming fins on a substrate by skiving. [Figure 7] FIG. 2 is a schematic perspective view showing a base material on which fins are formed. [Figure 8] FIG. 2 is a schematic perspective view showing a base material on which fins are formed and which has been subjected to bending processing. [Figure 9] FIG. 2 is a schematic perspective view showing a base material that has been bent and to which a predetermined member has been welded. [Figure 10] 4 is a flowchart for explaining a method for manufacturing a heat exchanger. [Figure 11] FIG. 11 is a schematic perspective view showing a heat exchanger according to a modified example. [Figure 12] 10 is a flowchart for explaining a method for manufacturing a heat exchanger according to a modified example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, an embodiment of the present invention will be described with reference to the drawings.

[0019] The configuration of a heat exchanger 100 manufactured by the manufacturing method of a heat exchanger according to the present embodiment will be described with reference to Figures 1 and 2. The heat exchanger 100 of the present embodiment is a heat exchanger that exchanges heat between a fluid 2 flowing inside the heat exchanger 100 and an external fluid 3 flowing outside the heat exchanger 100.

[0020] Specifically, the heat exchanger 100 of this embodiment shown in Fig. 1 is a heat exchanger for an aircraft engine, and is mounted inside the aircraft engine. The heat exchanger 100 is provided as an air-cooled heat exchanger (cooler) that cools a fluid 2 flowing inside the aircraft engine by exchanging heat with an airflow (external fluid 3) passing through the aircraft engine. The aircraft engine is an engine of a type that generates propulsive force by using air taken in from the outside into a cylindrical casing, such as a gas turbine engine, and a high-speed airflow is generated inside the casing. The fluid 2 is an oil used in aircraft, such as a lubricating oil for the aircraft engine, or a lubricating oil for a generator driven by the aircraft engine.

[0021] In this manner, the heat exchanger 100 is configured as a surface cooler for an aircraft engine. The surface cooler is a type of heat exchanger that cools the fluid 2 flowing inside the heat exchanger 100 by airflow flowing along the fins 11 provided on the outer surface of the hollow plate-like heat exchanger 100. As shown in FIG. 2, the heat exchanger 100 has a curved shape that is curved along the longitudinal direction so as to follow a curved surface S formed inside the aircraft engine. The curved surface S inside the aircraft engine is, for example, the inner circumferential surface of a fan casing of the aircraft engine.

[0022] The heat exchanger 100 is provided along the generally cylindrical curved surface S in the circumferential direction (direction C) with a length of about 1 / n circumference (n is a real number equal to or greater than 1). The length of the heat exchanger 100 is formed to be, for example, about 1 / 8 of the entire circumference of the curved surface S, but the heat exchanger 100 may have an annular shape extending substantially over the entire circumference of the curved surface S. The external fluid 3 (air flow) flows generally along direction A (see FIG. 1), which is the axial direction (the direction of the turbine's rotation axis) in the aircraft engine. The curved surface S in the aircraft engine is not necessarily a perfectly cylindrical curved surface, so in that case, the radius of curvature of the heat exchanger 100 varies depending on the position in the axial direction (direction A).

[0023] (Overall configuration of heat exchanger) The following describes the overall configuration of the heat exchanger 100. As shown in Fig. 1, the heat exchanger 100 includes a heat exchanger body 1 on which a plurality of fins 11 are formed.

[0024] As described above, the heat exchanger body 1 has a curved shape along the curved surface S (see FIG. 2). In this embodiment, the heat exchanger body 1 has a shape curved along the longitudinal direction. The heat exchanger body 1 is formed into a curved plate shape as a whole. The heat exchanger body 1 has a width W, a length L in the circumferential direction (direction C), and a thickness t1. The width W is smaller than the length L, and the thickness t1 is smaller than the length L and the width W.

[0025] The heat exchanger body 1 includes an internal flow path 20, a fluid inlet 21 and a fluid outlet 22 each connected to the internal flow path 20, and a plurality of fins 11 formed on the outer surface. The heat exchanger body 1 also includes two port parts 30a, 30b. One end of the port parts 30a, 30b communicates with the outside of the heat exchanger body 1, and the other end communicates with the internal flow path 20 of the heat exchanger body 1. In this embodiment, the port part 30a functions as the fluid inlet 21. The port part 30b functions as the fluid outlet 22. The two port parts 30a, 30b are examples of the "predetermined member" in the claims.

[0026] 2, the internal flow path 20 is a passage through which the fluid 2 flows. The internal flow path 20 is also a space portion formed inside the heat exchanger body 1. One end of the internal flow path 20 communicates with a fluid inlet 21, and the other end communicates with a fluid outlet 22 (see FIG. 1).

[0027] 1, the fluid inlet 21 and the fluid outlet 22 are each a fluid passage that opens to the outside of the heat exchanger body 1. Each of the fluid inlet 21 and the fluid outlet 22 is connected to a fluid circuit outside the heat exchanger body 1. In this embodiment, each of the fluid inlet 21 and the fluid outlet 22 is disposed at one end of the heat exchanger body 1 in the longitudinal direction, and is aligned in the width direction of the heat exchanger body 1.

[0028] The fins 11 are provided on the other surface 1b in the thickness direction of the heat exchanger body 1. The fins 11 are provided so as to rise from the other surface 1b. The fins 11 are arranged along the longitudinal direction of the heat exchanger body 1. The fins 11 are provided substantially parallel to each other and at substantially equal intervals (substantially equal pitch). The fins 11 generally extend along the width direction of the heat exchanger body 1 (axial direction A of the aircraft engine). In each drawing, only a portion of the fins 11 is shown, and the remaining portions are omitted by two-dot chain lines. In this embodiment, the fins 11 are not provided on one surface 1a in the thickness direction of the heat exchanger body 1.

[0029] (base material) Next, the substrate 10 (see FIG. 3) will be described with reference to FIG. 3 and FIG. 4. As shown in FIG. 3, the substrate 10 is aluminum or an aluminum alloy having a thickness t2. The thickness t2 is greater than the thickness t1 (see FIG. 1) of the heat exchanger body 1 (see FIG. 1). The substrate 10 before softening has a hardness of Vickers hardness (HV) 58 or more. Specifically, the substrate 10 before softening is aluminum or an aluminum alloy having a hardness of Vickers hardness 58 or more. In this embodiment, the substrate 10 is an A6000 series aluminum alloy. Specifically, the substrate 10 is an A6063 (JIS standard) material. In "JISH4100", the A6063 material having a hardness of Vickers hardness 58 or more is specified as a T5 material. That is, the substrate 10 according to this embodiment is an A6063 material having a hardness equivalent to a T5 material.

[0030] As shown in FIG. 3, the substrate 10 is an extruded material. Specifically, the substrate 10 is a multi-hole tube including a plurality of through holes 10b extending along the extrusion direction (direction C) of the substrate 10. The through holes 10b function as the internal flow path 20 of the heat exchanger body 1. The multi-hole tube is formed by extrusion molding of aluminum or an aluminum alloy. Therefore, the plurality of through holes 10b as the internal flow path 20 are provided so as to extend linearly from one end to the other end of the multi-hole tube in the direction in which the multi-hole tube extends (direction C (see FIG. 4)). In this specification, the thickness direction of the substrate 10 is defined as direction T.

[0031] 4, the multi-hole pipe has a rectangular shape when viewed from the direction T. That is, the multi-hole pipe is a plate-like member having a thickness t2 (see FIG. 3) and provided with a plurality of through holes 10b penetrating in the direction C.

[0032] In this embodiment, fins 11 (see FIG. 1) are formed on the surface 10a of the multi-hole tube (base material 10). In this embodiment, the fins 11 are formed by skiving the fin-forming portion 10c. The fin-forming portion 10c is formed when the base material 10 is extruded. The fin-forming portion 10c may be formed by cutting both ends of the surface 10a of the base material 10 in the A direction. The thickness t2 of the base material 10 is set to be the sum of the thickness t1 of the heat exchanger body 1 and the thickness t3 of the fin-forming portion 10c. The thickness t3 of the fin-forming portion 10c is set according to the thickness t4 of the fin 11 (see FIG. 6(B)) and the length D1 of the fin 11 (see FIG. 6(B)).

[0033] (Annealing treatment for base material) In this embodiment, as described above, the fin 11 is formed by skiving. Skiving is a processing method for thinly scraping the surface of a material. In this embodiment, the fin 11 is formed by scraping off the fin forming portion 10c formed on the surface 10a of the base material 10.

[0034] Here, when forming the fins 11 by skiving, depending on the hardness of the base material 10, the fins 11 after cutting may have a curved (rolled) shape or a wavy shape, making it difficult to cut the fins 11 into the desired shape.

[0035] Therefore, as a result of intensive research, the inventors of the present invention discovered that it is possible to carve the fins 11 into the desired shape by softening the base material 10 and then forming the fins 11 by skiving.

[0036] Therefore, in this embodiment, the base material 10 is softened by performing an annealing treatment. Furthermore, the surface 10a of the softened base material 10 after the annealing treatment is scraped up by skiving to form the fins 11.

[0037] In this embodiment, the annealing treatment involves heating the substrate 10 at a temperature of 400° C. to 430° C. for 2 to 3 hours.

[0038] After the heating of the substrate 10 is completed, the substrate 10 is cooled to 260°C or less at 30°C / hr or less, and after the temperature reaches 260°C or less, the substrate 10 is naturally cooled to room temperature. Preferably, the hardness of the A6063 material equivalent to the O material is not specified in the JIS standard. Therefore, based on the tensile strength and hardness of the A6063 material, the hardness of the A6063 material equivalent to the O material is calculated to be less than Vickers hardness 40. That is, in this embodiment, the substrate 10 is softened by performing an annealing treatment so that the hardness of the substrate 10 is less than Vickers hardness 40.

[0039] (Fin formation by skiving) Next, with reference to Fig. 6(A) to Fig. 6(C), a configuration in which the substrate 10 is softened by annealing and then the fin 11 is formed by skiving will be described. As shown in Fig. 6(A), a cutting jig 40 is inclined at a predetermined angle θ with respect to the surface 10a of the substrate 10 that has been softened by annealing, and a fin forming portion 10c provided on the surface 10a of the substrate 10 is cut. The angle θ of the cutting jig 40 is set according to the thickness t4 (see Fig. 6(B)) of the fin 11 to be cut and the length D1 (see Fig. 6(B)) of the fin 11.

[0040] Then, by repeating the process of Fig. 6(A), a plurality of fins 11 are cut out from the surface 10a of the base material 10 as shown in Fig. 6(B). After that, as shown in Fig. 6(C), a plurality of fins 11 are cut out from the fin forming portion 10c corresponding to the length L of the base material 10, and the base material 10 is cut to the predetermined length L. This completes the formation of the fins 11 by scraping the surface 10a of the base material 10 by skiving.

[0041] In this embodiment, in the process of forming the fins 11 (the process of FIG. 6(A) to FIG. 6(C)), the surface 10a of the base material 10 is scraped by skiving so that the fins 11 have a thickness t4 of 0.4 mm or more and 1.0 mm or less, and the interval p1 between the fins 11 is 2.0 mm or more and 4.0 mm or less. In this embodiment, the fins 11 are formed on the surface 10a of the base material 10 by skiving so that the fins 11 extend in a direction perpendicular to the direction (direction C) in which the through holes 10b (see FIG. 5) of the multi-hole tube extend. This allows the fins 11 to be formed so that the fins 11 extend along the direction A (see FIG. 1). Therefore, the fins 11 can be formed so that the fins 11 extend in a direction perpendicular to the direction (direction C) in which the through holes 10b (see FIG. 5) extend. Therefore, the efficiency of heat exchange between the fluid 2 flowing through the through holes 10b as the internal flow path 20 (see FIG. 2) and the external fluid 3 can be improved.

[0042] In addition, when the fins 11 are scraped by skiving without annealing an extrusion-molded member such as a multi-hole pipe, the workability of the fins 11 may decrease due to the hardness of the base material 10, and the shape of the fins 11 may not be the desired shape, depending on the direction of the skiving. Therefore, when the fins 11 are scraped by skiving without annealing, the skiving is performed in the direction along the extrusion direction of the multi-hole pipe to suppress the deterioration of the workability of the fins 11. On the other hand, in this embodiment, the base material 10 is softened by performing the annealing treatment on the base material 10, so that the workability when scraping out the fins 11 by skiving can be improved. Therefore, the fins 11 can be scraped out by skiving regardless of the extrusion direction when forming the multi-hole pipe. That is, in this embodiment, the direction in which the skiving is performed on the surface 10a of the multi-hole pipe (base material 10) may be the direction along the extrusion direction of the multi-hole pipe or the opposite direction to the extrusion direction.

[0043] (Bending of base material) Next, with reference to Figs. 7 to 9, a configuration for manufacturing a heat exchanger 100 (see Fig. 1) used as a surface cooler for an aircraft engine by bending the base material 10 will be described.

[0044] Fig. 7 shows a substrate 10 on which a plurality of fins 11 are formed. In this embodiment, the substrate 10 has a plate-like shape. Therefore, as shown in Fig. 7, the substrate 10 on which the fins 11 are formed by skiving also has a plate-like shape. Therefore, in order to use the substrate 10 on which the fins 11 are formed by skiving as a surface cooler for an aircraft engine, the substrate 10 needs to be curved.

[0045] Therefore, as shown in Fig. 8, the substrate 10 on which the multiple fins 11 are formed is curved so as to fit along the curved surface S (see Fig. 2) formed inside the aircraft engine. In this embodiment, the substrate 10 is softened by annealing, and then the substrate 10 is bent before being hardened to a predetermined hardness by heat treatment. That is, the multi-hole pipe is curved so as to fit along the curved surface S inside the aircraft engine while maintaining the hardness equivalent to that of an O material.

[0046] 9, after the multi-hole pipe is curved and before the multi-hole pipe is hardened, the port portions 30a, 30b are welded to the multi-hole pipe. In addition to the port portions 30a, 30b, members (not shown) for fixing the multi-hole pipe to a mounting structure such as a bracket provided on the inner circumferential surface of an aircraft engine are welded to the multi-hole pipe. The welding of the port portions 30a, 30b to the multi-hole pipe and members for fixing the multi-hole pipe to a mounting structure such as a bracket provided on the inner circumferential surface of an aircraft engine is also performed after the base material 10 is softened by annealing the base material 10 and before the base material 10 is hardened to a predetermined hardness.

[0047] (hardening by heat treatment) In this embodiment, a plurality of fins 11 are formed on the surface 10a (see FIG. 5) of the substrate 10 by skiving, the substrate 10 is curved, and predetermined members such as the port portions 30a and 30b are joined by welding, and then the substrate 10 is hardened by heat treatment. The heat treatment for hardening the substrate 10 according to this embodiment includes age hardening.

[0048] Specifically, the substrate 10 softened to a hardness equivalent to O material is subjected to age hardening treatment so as to have a hardness equivalent to T5 material. More specifically, the substrate 10 having a hardness of 58 or more is softened by annealing treatment so as to have a hardness of less than Vickers hardness 40, and in the process of hardening the substrate 10, the substrate 10 is hardened by age hardening treatment so as to have a hardness of 58 or more Vickers hardness. In this embodiment, the substrate 10 is held at a temperature of about 200° C. for 8 to 9 hours to perform age hardening treatment. Thereafter, necessary processing, surface treatment, etc. are performed, and the heat exchanger 100 (see FIG. 1) is assembled, thereby manufacturing the heat exchanger 100.

[0049] (Heat exchanger manufacturing process) Next, with reference to FIG. 10, a method for manufacturing the heat exchanger 100 (see FIG. 1) according to this embodiment will be described.

[0050] In step S1, the substrate 10 (see FIG. 5) having a predetermined hardness is softened. Specifically, in step S1, the substrate 10 is softened by being annealed. In this embodiment, the substrate 10 having a hardness equivalent to a T5 material is softened to a hardness equivalent to an O material by being annealed. In addition, before the substrate 10 is softened in step S1, a fin-forming portion 10c is formed on a surface 10a (see FIG. 5) of the substrate 10. That is, in step S1, the substrate 10 on which the fin-forming portion 10c has been formed is softened by being annealed.

[0051] In step S2, the surface 10a of the base material 10 that has been softened after the annealing treatment is scraped off by skiving to form the fins 11.

[0052] In step S3, after the fins 11 are formed and before the multi-hole pipe (substrate 10) is hardened, the multi-hole pipe is curved. Specifically, the multi-hole pipe is curved in the longitudinal direction so as to fit along a curved surface S (see FIG. 2) formed inside an aircraft engine.

[0053] In step S4, after the multi-hole pipe is curved and before the multi-hole pipe is hardened, the ports 30a, 30b are welded to the multi-hole pipe. Also in step S4, members for fixing to a mounting structure such as a bracket provided on the inner circumferential surface of the aircraft engine are welded.

[0054] In step S5, the base material 10 after the fins 11 are formed is subjected to a heat treatment to harden the base material 10. Thereafter, necessary processing, surface treatment, and the like are performed, and the manufacturing process of the heat exchanger 100 is completed.

[0055] (Effects of this embodiment) In this embodiment, the following effects can be obtained.

[0056] The manufacturing method of the heat exchanger 100 of this embodiment includes a step of softening the base material 10 having a predetermined hardness, a step of scraping the surface 10a of the softened base material 10 by skiving to form the fins 11, and a step of hardening the base material 10 by performing heat treatment on the base material 10 after the fins 11 are formed. As a result, even when skiving is performed on a base material 10 that is somewhat hard, it is possible to perform skiving in a state in which the base material 10 is softened to a hardness suitable for forming the fins 11, so that the workability when scraping the fins 11 can be improved. Therefore, even when the fins 11 are formed by skiving, the fins 11 can be scraped into a desired shape. As a result, it is possible to provide a manufacturing method of a heat exchanger that can form the fins 11 having a desired shape even when skiving is performed on a base material 10 that is somewhat hard. In addition, the manufacturing method of the heat exchanger 100 according to this invention includes a step of hardening the base material 10 by heat treating the base material 10 after the fins 11 are formed, as described above. This allows the softened base material 10 to be hardened, so that the hardness of the base material 10 after the formation of the fins 11 can be restored to a predetermined hardness. As a result, when manufacturing a heat exchanger 100 having fins 11 with a desired shape by skiving, it is possible to set the hardness of the heat exchanger 100 (fins 11) to a predetermined hardness, so that the mechanical strength required for the heat exchanger 100 can be ensured.

[0057] In addition, in this embodiment, as described above, the step of softening the substrate 10 includes a step of performing an annealing treatment on the substrate 10, and in the step of performing an annealing treatment on the substrate 10, the substrate 10 is softened by performing an annealing treatment so that the hardness of the substrate 10 becomes less than Vickers hardness 40. As a result, since the substrate 10 is softened to a hardness less than Vickers hardness 40, when the fin 11 is formed on the substrate 10 having a certain degree of hardness by skiving, the substrate 10 can be softened to a hardness that allows the substrate 10 to be scraped into a desired shape. As a result, it is possible to improve the processability of the substrate 10 having a certain degree of hardness so that the fin 11 can be scraped into a desired shape, so that even when the fin 11 is formed on the substrate 10 having a certain degree of hardness by skiving, the fin 11 can be easily scraped into a desired shape.

[0058] In the present embodiment, as described above, in the step of annealing the substrate 10, the substrate 10 is softened by annealing so that its hardness is equivalent to that of an O-material. This ensures that the substrate 10 is softened to a Vickers hardness of less than 40. As a result, the substrate 10 is softened to a hardness that allows the fin 11 to be cut into a desired shape.

[0059] In the present embodiment, as described above, in the step of hardening the substrate 10, the heat treatment for hardening the substrate 10 includes an age hardening treatment. This makes it possible to easily harden the substrate 10, which has been softened to a hardness of less than Vickers hardness 40, to a predetermined hardness.

[0060] In this embodiment, as described above, the base material 10 before softening is aluminum or an aluminum alloy having a Vickers hardness of 58 or more, and in the step of annealing the base material 10, the base material 10 having a Vickers hardness of 58 or more is softened by annealing to a hardness of less than Vickers hardness 40, and in the step of hardening the base material 10, the base material 10 is hardened by age hardening to a hardness of 58 or more. As a result, it is possible to soften the base material 10 of aluminum or aluminum alloy having a hardness equivalent to T5 material of Vickers hardness 58 or more to an equivalent to O material of Vickers hardness less than 40, and then scrape off the fin 11 by skiving, so that the fin 11 having a desired shape can be scraped off compared to the configuration in which the fin 11 is formed on the base material 10 having a hardness equivalent to T5 material. In addition, since the substrate 10 after the fins 11 are formed by skiving is hardened by age hardening to a Vickers hardness of 58 or more, the substrate 10 after the fins 11 are formed can be restored to a hardness equivalent to that of a T5 material. As a result, even when the fins 11 are formed by skiving on the substrate 10 made of aluminum or an aluminum alloy having a hardness equivalent to that of a T5 material, it is possible to provide a manufacturing method for a heat exchanger that can form the fins 11 having a desired shape while ensuring mechanical strength equivalent to that of a T5 material.

[0061] In the present embodiment, as described above, the substrate 10 is an extruded material, and is a multi-hole tube including a plurality of through holes 10b extending along the extrusion direction (C direction) of the substrate 10, and the method further includes a step of bending the multi-hole tube after forming the fins 11 and before hardening the multi-hole tube. As a result, since the substrate 10 is softened by the annealing treatment, the substrate 10 can be easily curved. As a result, a curved heat exchanger 100, such as a heat exchanger 100 used as a surface cooler for an aircraft engine, can be easily manufactured.

[0062] In addition, in this embodiment, as described above, a step of welding the port portions 30a, 30b to the multi-hole pipe after bending the multi-hole pipe and before hardening the multi-hole pipe is further provided. As a result, since the port portions 30a, 30b are welded to the multi-hole pipe before hardening the multi-hole pipe, even if the weld heat affected zone is softened during welding, the weld heat affected zone can be hardened at the same time when the multi-hole pipe is hardened. As a result, it is possible to suppress a decrease in the mechanical strength of the welded zone caused by softening of the weld heat affected zone when welding the port portions 30a, 30b.

[0063] In the present embodiment, as described above, in the step of forming the fins 11, the surface 10a of the base material 10 is scraped by skiving so that the fins 11 have a thickness t4 of 0.4 mm or more and 1.0 mm or less, and the interval p1 between the fins 11 is 2.0 mm or more and 4.0 mm or less. As a result, even when manufacturing a heat exchanger in which the fins 11 having a thin thickness t4 of 0.4 mm or more and 1.0 mm or less are arranged at a narrow interval p1 of 2.0 mm or more and 4.0 mm or less, the base material 10 is softened by performing an annealing treatment, so that the fins 11 can be easily scraped into a desired shape.

[0064] [Example (Effect Confirmation Experiment)] In order to confirm the effect of the above embodiment, the following experiment was performed. First, the substrate 10 having a Vickers hardness of 77 was annealed to soften the hardness of the substrate 10 to a Vickers hardness of 28. Then, the surface 10a (fin forming portion 10c) of the substrate 10 softened to a Vickers hardness of 28 was scraped up to form the fins 11 so that the thickness t3 of the fins 11 was 0.5 mm and the interval p1 between the fins 11 was 2.1 mm.

[0065] In this way, it was confirmed that by subjecting the substrate 10 having a Vickers hardness of 77 to an annealing treatment to soften it to a Vickers hardness of 28, and then forming the fins 11 by skiving, it is possible to form the fins 11 having the desired shape on the substrate 10 having a Vickers hardness of 77.

[0066] In addition, the substrate 10 after the fins 11 were subjected to an age hardening treatment, and the hardness of the substrate 10 after the fins 11 were formed was returned to a predetermined hardness. This makes it possible to set the hardness of the heat exchanger 100 (fins 11) to a predetermined hardness when manufacturing a heat exchanger 100 having fins 11 with a desired shape by skiving, so that the mechanical strength required for the heat exchanger 100 can be ensured. As described above, it was confirmed by experiment that the effects described in the above embodiment can be obtained.

[0067] [Variations] The embodiments and examples disclosed herein should be considered to be illustrative and not restrictive in all respects. The scope of the present invention is indicated by the claims, not by the description of the embodiments and examples above, and further includes all modifications (variations) within the meaning and scope of the claims.

[0068] For example, in the above embodiment, an example of the heat exchanger 100 that is a surface cooler is shown, but the present invention is not limited to this. The present invention may be applied to a heat exchanger other than a surface cooler as long as it is a heat exchanger having fins 11 formed by skiving. The heat exchanger of the present invention does not need to be provided along the curved surface S inside an aircraft engine. The heat exchanger may be provided in a moving body other than an aircraft, or in a fixedly installed device other than a moving body.

[0069] For example, as in the modified example shown in Fig. 11, a non-curved heat exchanger 200 may be manufactured by forming fins 211 by skiving a plate-shaped substrate 210. The substrate 210 is a plate-shaped aluminum or aluminum alloy without through holes. The non-curved heat exchanger 200 is, for example, a heat sink provided on the surface of an electronic device to exchange heat between heat generated by the electronic device and an external fluid.

[0070] A method for manufacturing the heat exchanger 200 (see FIG. 11) according to the modified example will be described with reference to Fig. 12. Note that the same steps as those in the method for manufacturing the heat exchanger 100 (see FIG. 1) according to the above embodiment are denoted by the same reference numerals, and detailed description thereof will be omitted.

[0071] In step S1, the base material 210 (see FIG. 11) is softened by performing an annealing treatment on the base material 210.

[0072] In step S2, the base material 210, which has been softened by annealing, is subjected to skiving to form fins 211 (see FIG. 11).

[0073] In step S5, the base material 210 after the fins 211 are formed is hardened by heat treatment. Specifically, the base material 210 on which the fins 211 are formed is hardened by age hardening. Thereafter, necessary processing, surface treatment, etc. are performed, and the manufacturing process of the heat exchanger 100 is completed.

[0074] In the above embodiment, an example of a configuration in which the substrate 10 is softened to a Vickers hardness of 28 when the substrate 10 is softened to a hardness equivalent to that of O material has been shown, but the present invention is not limited to this. In the present invention, as long as the substrate 10 has a hardness equivalent to that of O material (a hardness less than Vickers hardness of 40), the hardness of the substrate 10 after being softened does not matter.

[0075] In the above embodiment, the substrate 10 is hardened by age hardening treatment in which the substrate 10 is heated, cooled to 260° C. or less at a rate of 30° C. / hr or less, and then naturally cooled to room temperature, but the present invention is not limited to this. Conditions for the age hardening treatment may be other than those described above as long as the substrate 10 can be hardened to a predetermined hardness.

[0076] In the above embodiment, an example of a configuration in which age hardening is performed in the step of hardening the substrate 10 is shown, but the present invention is not limited to this. In the present invention, the substrate 10 may be hardened by a heat treatment other than age hardening, such as quenching or tempering. Any heat treatment may be used as long as it is possible to harden the substrate 10 to a predetermined hardness.

[0077] In the above embodiment, the port parts 30a and 30b are welded to the base material 10 after the fin 11 is formed and curved, and then the base material 10 is heat-treated to harden the base material 10. However, the present invention is not limited to this. For example, the base material 10 may be configured to be hardened by heat-treating the base material 10 after the fin 11 is formed and curved, and then the port parts 30a and 30b are welded to the base material 10. However, in the case of the configuration in which the port parts 30a and 30b are welded to the base material 10 after the hardening, the mechanical strength of the welded part is reduced due to softening of the welded heat-affected zone caused during welding. Therefore, it is preferable to harden the base material 10 by performing heat treatment on the base material 10 after the fin 11 is formed and curved.

[0078] In the above embodiment, the fins 11 are formed by skiving so that the thickness t4 of the fins 11 is 0.5 mm and the interval p1 between the fins 11 is 2.1 mm, but the present invention is not limited to this. It is preferable that the thickness t4 of the fins 11 is 0.4 mm or more and 1.0 mm or less, and the interval p1 between the fins 11 is 2.0 mm or more and 4.0 mm or less, but the fins 11 may be formed to have any thickness t4 and any interval p1.

[0079] In the above embodiment, the fins 11 are formed by skiving only on the other surface 1b of the heat exchanger body 1, but the present invention is not limited to this. In the present invention, the fins 11 may be formed by skiving only on the one surface 1a of the heat exchanger body 1, or the fins 11 may be formed by skiving on both the other surface 1b and the one surface 1a of the heat exchanger body 1.

[0080] In the above embodiment, the width W of the heat exchanger body 1 is smaller than the length L, but the present invention is not limited to this. For example, the width W of the heat exchanger body 1 may be larger than the length L.

[0081] In the above embodiment, the substrate 10 is made of A6063 T5 material having a Vickers hardness of 58 or more, but the present invention is not limited to this. The type of substrate 10 is not limited as long as it is made of aluminum or an aluminum alloy that is softened by annealing and hardened by heat treatment.

[0082] In the above embodiment, the base material 10 is softened by annealing, but the present invention is not limited to this. The base material 10 may be softened by any process as long as the process softens the base material 10 by heat treatment. [Explanation of symbols]

[0083] 10, 210 base material 10a Surface of the substrate 10b Through hole 11, 211 Fin 30a, 30b Port portion (predetermined member) 100, 200 heat exchanger t4 Thickness (fin thickness) p1 Spacing (spacing between fins)

Claims

1. softening a substrate having a predetermined hardness; A step of scraping the surface of the softened base material by skiving to form a fin; and hardening the base material by performing a heat treatment on the base material after the fins are formed.

2. The step of softening the base material includes a step of subjecting the base material to an annealing treatment, 2. The method for manufacturing a heat exchanger according to claim 1, wherein in the step of annealing the base material, the base material is softened by annealing so that the base material has a hardness of less than 40 in Vickers hardness.

3. 3. The method for manufacturing a heat exchanger according to claim 2, wherein in the step of annealing the base material, the base material is softened by annealing so that its hardness becomes equivalent to that of an O-steel material.

4. The method for manufacturing a heat exchanger according to claim 3 , wherein in the step of hardening the base material, a heat treatment for hardening the base material includes an age hardening treatment.

5. The substrate before being softened is aluminum or an aluminum alloy having a Vickers hardness of 58 or more; In the step of annealing the base material, the base material having a Vickers hardness of 58 or more is softened by annealing so as to have a hardness of less than Vickers hardness of 40; 5. The method for manufacturing a heat exchanger according to claim 4, wherein in the step of hardening the base material, the base material is hardened by the age hardening treatment so as to have a Vickers hardness of 58 or more.

6. The substrate is an extruded shape and is a multi-hole tube including a plurality of through holes extending along an extrusion direction of the substrate, The method of claim 1 further comprising the step of bending the multi-hole tube after forming the fins and before curing the multi-hole tube.

7. 7. The method for manufacturing a heat exchanger according to claim 6, further comprising the step of welding a predetermined member to the multi-hole pipe after bending the multi-hole pipe and before hardening the multi-hole pipe.

8. 2. The method for manufacturing a heat exchanger according to claim 1, wherein in the step of forming the fins, the surface of the base material is scraped by skiving so that the fins have a thickness of 0.4 mm or more and 1.0 mm or less and the spacing between the fins is 2.0 mm or more and 4.0 mm or less.

Citation Information

Patent Citations

  • Manufacture of aluminummsoldered fin heat exchanger

    JP1979061015A

  • Heat Sink and Manufacturing Method

    KR1020010105508A

  • Heat exchanger and fabrication method thereof

    US20080289809A1

  • Heat sink and producing method therefor

    JP2001156224A