Ceramic body and method for producing the same
A ceramic body manufacturing method using specific SiC powder ratios and metal impregnation improves thermal conductivity, addressing the limitations of conventional methods and enhancing performance in heat exchangers.
Patent Information
- Application Number
- JP2023052276
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2043-03-28
AI Technical Summary
Conventional methods face difficulties in stably increasing the proportion of SiC in ceramic bodies, limiting the thermal conductivity of Si-impregnated SiC ceramic bodies, which are used in applications like heat exchangers, and other systems requiring improved thermal conductivity.
A ceramic body manufacturing method involving a molding process with a specific ratio of SiC powders of different average particle sizes (15 to 50 μm and 2 to 8 μm) followed by firing and impregnation with metal Si, optimizing the packing density and thermal conductivity.
The method results in a ceramic body with enhanced thermal conductivity, suitable for applications such as heat exchangers, by increasing the SiC proportion and ensuring high thermal conductivity values.
Smart Images

Figure 2024140909000002 
Figure 2024140909000003 
Figure 2024140909000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a ceramic body and a method for making the same. [Background technology]
[0002] In recent years, there has been a demand for improved fuel economy in automobiles. In particular, to prevent a deterioration in fuel economy when the engine is cold, such as when the engine is started, there are hopes for a system that can quickly warm the coolant, engine oil, automatic transmission fluid (ATF), etc., thereby reducing friction loss. There are also hopes for a system that can heat the exhaust gas purification catalyst in order to quickly activate the catalyst.
[0003] In the above-mentioned system, a heat exchanger having a honeycomb shape and including a ceramic body (honeycomb structure) made of Si-impregnated SiC is used (Patent Document 1). The ceramic body is manufactured by degreasing a ceramic molded body containing silicon carbide (hereinafter referred to as "SiC"), and then impregnating it with metallic silicon (hereinafter referred to as "Si"). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 6763699 Summary of the Invention [Problem to be solved by the invention]
[0005] In recent years, there has been a demand for increasing the thermal conductivity of ceramic bodies made of Si-impregnated SiC in order to improve the performance of heat exchangers (for example, to improve heat recovery). SiC constitutes the skeleton of the ceramic body and has a higher thermal conductivity than Si. Therefore, it is believed that the thermal conductivity of the ceramic body can be improved by increasing the proportion of SiC in the ceramic body. However, with conventional methods, it is difficult to stably increase the proportion of SiC in the ceramic body (skeleton), and there is a problem that the thermal conductivity of the ceramic body is not sufficiently improved. Although the ceramic body used in a heat exchanger has been described above as an example, there is also a need for improved thermal conductivity for ceramic bodies used in applications other than heat exchangers.
[0006] The present invention has been made to solve the above-mentioned problems, and has an object to provide a ceramic body made of Si-impregnated SiC and having high thermal conductivity, and a method for producing the same. [Means for solving the problem]
[0007] As a result of intensive research into ceramic bodies made of Si-impregnated SiC, the inventors have found that the above problems can be solved by using a molding material containing two types of SiC powders having a predetermined average particle size D50 in a predetermined ratio, and have completed the present invention. That is, the present invention is exemplified as follows.
[0008] [1] A molding process in which a molding material containing SiC powder having an average particle size D50 of 15 to 50 μm and SiC powder having an average particle size D50 of 2 to 8 μm in a mass ratio of 3:7 to 7:3 is molded to obtain a molded body; a firing / impregnation step for firing the molded body and impregnating it with metallic Si; A method for producing a ceramic body having the following structure:
[0009] [2] The method for producing a ceramic body according to [1], wherein the firing / impregnation step is carried out by firing the molded body in contact with metallic silicon.
[0010] [3] The method for producing a ceramic body according to [2], wherein the firing is carried out in an inert gas atmosphere or in vacuum at a temperature of 1400 to 1600°C.
[0011] [4] The method for producing a ceramic body according to any one of [1] to [3], wherein the ceramic raw material contained in the molding material is only the SiC powder.
[0012] [5] The method for producing a ceramic body according to any one of [1] to [4], wherein at least one of a drying treatment and a degreasing treatment is carried out on the molded body between the molding step and the firing / impregnation step.
[0013] [6] The method for producing a ceramic body according to any one of [1] to [5], wherein the molded body has a honeycomb shape having an outer peripheral wall and a plurality of partition walls arranged inside the outer peripheral wall and defining a plurality of cells extending from a first end face to a second end face, or a hollow honeycomb shape having an inner peripheral wall, an outer peripheral wall, and partition walls arranged between the inner peripheral wall and the outer peripheral wall and defining a plurality of cells extending from a first end face to a second end face.
[0014] [7] A SiC skeleton including SiC particles having a particle size of 15 to 50 μm and SiC particles having a particle size of 2 to 8 μm in a volume ratio of 3:7 to 7:3; a metal Si impregnated portion formed around at least a part of the SiC skeleton; A ceramic body comprising: Effect of the Invention
[0015] According to the present invention, it is possible to provide a ceramic body having high thermal conductivity made of Si-impregnated SiC and a method for producing the same. [Brief description of the drawings]
[0016] [Figure 1] FIG. 2 is a partially enlarged cross-sectional view of a molded body produced according to a method for producing a ceramic body according to an embodiment of the present invention. [Diagram 2] 2 is a cross-sectional view perpendicular to the cell extension direction of a honeycomb-shaped molded body. FIG. [Diagram 3] 2 is a cross-sectional view perpendicular to the cell extension direction of a hollow honeycomb-shaped molded body. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, the embodiments of the present invention will be described in detail with reference to the drawings. The present invention is not limited to the following embodiments, and it should be understood that modifications and improvements to the following embodiments, which are made based on the ordinary knowledge of a person skilled in the art, fall within the scope of the present invention, without departing from the spirit of the present invention.
[0018] (1) Method for manufacturing ceramic body The method for producing a ceramic body according to an embodiment of the present invention includes a molding step and a firing / impregnation step. These steps will be described in detail.
[0019] <Forming process> The molding process is a process in which a molding material containing SiC powder having an average particle size D50 of 15 to 50 μm (hereinafter abbreviated as "SiC powder A") and SiC powder having an average particle size D50 of 2 to 8 μm (hereinafter abbreviated as "SiC powder B") in a mass ratio of 3:7 to 7:3 is molded to obtain a molded body. Here, a partially enlarged cross-sectional view of the molded body produced under the above conditions is shown in FIG. 1. As shown in FIG. 1, by using two types of SiC powder A and B having average particle diameter D50 in the above mass ratio, SiC powder B having a small average particle diameter D50 is easily filled between SiC powder A having a large average particle diameter D50 in molded body 10, so that the packing density of the SiC powder (SiC powder A and B) constituting molded body 10 can be increased. As a result, the thermal conductivity of the ceramic body obtained by subjecting molded body 10 to the firing and infiltration process is improved. On the other hand, if the conditions are not as described above, the packing density of the SiC particles constituting the molded body cannot be sufficiently increased, and therefore the thermal conductivity of the ceramic body is not sufficiently improved. Here, the "average particle size D50" of the SiC powders A and B used in the molding step refers to the particle size at an integrated value of 50% (D50) in the particle size distribution determined by a laser diffraction / scattering method.
[0020] The SiC powder A may be of a single type or of a combination of two or more types. Specifically, two or more types of SiC powder A having an average particle size D50 in the range of 15 to 50 μm may be used. Similarly, the SiC powder B may be a single type or a combination of two or more types. Specifically, two or more types of SiC powder B having an average particle size D50 in the range of 2 to 8 μm may be used.
[0021] From the viewpoint of stably ensuring the above-mentioned effects, the average particle size D50 of the SiC powder A is preferably 20 to 45 μm, and more preferably 25 to 40 μm. Moreover, from the viewpoint of stably ensuring the above-mentioned effects, the average particle size D50 of the SiC powder B is preferably 3 to 7 μm, and more preferably 4 to 6 μm. Furthermore, from the viewpoint of stably ensuring the above-mentioned effects, the mass ratio of SiC powder A to SiC powder B is preferably 4:6 to 6:4.
[0022] The molding material preferably contains only SiC powders A and B as ceramic raw materials. SiC powders A and B have high thermal conductivity and have a thermal expansion coefficient close to that of metal Si to be impregnated in a process described later, so that a ceramic body having excellent resistance to thermal stress can be obtained. Here, the ceramic raw material means a raw material that constitutes the skeleton of the ceramic body after the firing and impregnation steps.
[0023] The molding material may contain components known in the art as necessary. Examples of known components include a dispersion medium, a binder, a plasticizer, and a dispersant. The content of these components is not particularly limited as long as it does not impair the effects of the present invention.
[0024] The dispersion medium may be water or a mixed solvent of water and an organic solvent such as alcohol, with water being particularly preferred.
[0025] Examples of the binder include organic binders such as methyl cellulose, hydroxypropoxyl cellulose, hydroxyethyl cellulose, carboxymethyl cellulose, and polyvinyl alcohol. In particular, it is preferable to use methyl cellulose and hydroxypropoxyl cellulose in combination. The binder may be a single type, or two or more types may be used in combination.
[0026] Examples of the plasticizer include polyoxyalkylene alkyl ethers, polycarboxylic acid polymers, and alkyl phosphate esters.
[0027] The dispersant may be a surfactant such as polyoxyalkylene alkyl ether, ethylene glycol, dextrin, fatty acid soap, polyalcohol, etc. The dispersant may be a single type or a combination of two or more types.
[0028] The molding method is not particularly limited, and a known method such as extrusion molding can be used. In extrusion molding, a molded body of a desired shape can be obtained by selecting a die and a jig of an appropriate shape. For example, when a molded body of a honeycomb shape is obtained, the shape and density of the cells, the number, length and thickness of the partition walls, the shape and thickness of the outer peripheral wall and the inner peripheral wall, etc. can be controlled by selecting a die and a jig of an appropriate shape.
[0029] The shape of the molded body obtained by the molding step is not particularly limited, but it is preferable that the molded body has a honeycomb shape having an outer peripheral wall and a plurality of partition walls disposed inside the outer peripheral wall and defining a plurality of cells extending from the first end face to the second end face, or a hollow honeycomb shape having an inner peripheral wall, an outer peripheral wall, and partition walls disposed between the inner peripheral wall and the outer peripheral wall and defining a plurality of cells extending from the first end face to the second end face. By making the molded body into such a shape, for example, when used in a heat exchanger, its performance (for example, heat recovery performance) can be improved.
[0030] Here, Figure 2 shows a cross-sectional view perpendicular to the cell extension direction of a honeycomb-shaped formed body (honeycomb formed body), and Figure 3 shows a cross-sectional view perpendicular to the cell extension direction of a hollow honeycomb-shaped formed body (hollow honeycomb formed body). As shown in Fig. 2, the honeycomb formed body 100 has an outer peripheral wall 110 and a plurality of partition walls 130 disposed inside the outer peripheral wall 110 and defining a plurality of cells 120 extending from a first end face to a second end face. Also, as shown in Fig. 3, the hollow honeycomb formed body 200 has an inner peripheral wall 140, the outer peripheral wall 110, and partition walls 130 disposed between the inner peripheral wall 140 and the outer peripheral wall 110 and defining a plurality of cells 120 extending from the first end face to the second end face.
[0031] The shapes (external shapes) of the honeycomb molded body 100 and the hollow honeycomb molded body 200 are not particularly limited and may be, for example, a circular cylinder, an elliptical cylinder, a rectangular prism, or other polygonal prism. That is, the external shapes of the honeycomb molded body 100 and the hollow honeycomb molded body 200 in a cross section perpendicular to the extension direction of the cells 120 may be a circle, an ellipse, a rectangle, or other polygonal shapes. In addition, the hollow portion of the hollow honeycomb molded body 200 may be the same as or different from the external shape of the hollow honeycomb molded body 200, and may be any of the above-mentioned various shapes. The shape of the cells 120 in a cross section perpendicular to the direction in which the cells 120 extend is not limited to the shape shown in the figure, and may be a circle, an ellipse, a polygon such as a triangle, or the like.
[0032] It is preferable that the honeycomb formed body 100 and the hollow honeycomb formed body 200 have a structure that satisfies the following characteristics after the firing and impregnation steps. The honeycomb formed body 100 and the hollow honeycomb formed body 200 after the firing and impregnation steps are called honeycomb structures.
[0033] The cell density (i.e., the number of cells 120 per unit area) in a cross section perpendicular to the extension direction of the cells 120 of the honeycomb structure may be appropriately adjusted depending on the application, etc., but is preferably 4 to 320 cells / cm. 2In a cross section perpendicular to the direction in which the cells 120 extend, the cell density is preferably in the range of 4 cells / cm. 2 By setting the cell density at or above 320 cells / cm, the strength of the partition walls 130, and in turn the strength and effective GSA (geometric surface area) of the honeycomb structure itself can be sufficiently ensured. 2 By satisfying the following, it is possible to prevent an increase in pressure loss when the fluid flows.
[0034] The thickness of the partition walls 130 of the honeycomb structure may be appropriately designed depending on the purpose, but is preferably 50 μm to 2 mm, and more preferably 60 μm to 600 μm. When the thickness of the partition walls 130 is 50 μm or more, the mechanical strength is improved and damage due to impact or thermal stress can be suppressed. On the other hand, when the thickness of the partition walls 130 is 2 mm or less, the proportion of the cell volume in the honeycomb structure increases, thereby reducing the pressure loss of the fluid and improving the heat exchange rate.
[0035] The thickness of the outer peripheral wall 110 and the inner peripheral wall 140 (if present) of the honeycomb structure may be appropriately designed depending on the purpose, but when used for heat exchange, it is preferably more than 0.3 mm and not more than 10 mm, more preferably 0.5 mm to 5 mm, and even more preferably 1 mm to 3 mm. When used for heat storage, the thickness of the outer peripheral wall 110 may be set to 10 mm or more to increase the heat capacity of the outer peripheral wall 110.
[0036] <Firing and impregnation process> The firing / impregnation step involves firing the compact and impregnating it with metallic silicon. The conditions for the calcination / impregnation step are not particularly limited, and the steps can be carried out in accordance with known methods. In addition, the calcination / impregnation step can be carried out in one step, but the calcination and impregnation can also be carried out in separate steps. Specifically, the calcination step and the impregnation step can be carried out as separate steps.
[0037] The firing / impregnation step is preferably carried out by firing the molded body in contact with metallic silicon. By firing in this state, the molten metallic silicon can penetrate into the gaps between the ceramic particles that make up the molded body by capillary action, thereby impregnating the metallic silicon. Furthermore, this method allows firing and impregnation to be carried out in a single step, thereby reducing manufacturing costs.
[0038] The position where the metal Si is contacted in the molded body is not particularly limited, but it is preferable to place the metal Si on the upper surface of the molded body and make the metal Si contact therewith. For example, when the honeycomb molded body 100 and the hollow honeycomb molded body 200 are used as the molded body, the position where the metal Si is contacted may be any of the end face (first end face or second end face), the outer peripheral wall 110, and the inner peripheral wall 140 (if present). In addition, when the direction in which the cells 120 extend is the vertical direction, it is preferable to place the metal Si on the end face (first end face or second end face) located above the honeycomb molded body 100 and the hollow honeycomb molded body 200 and make the metal Si contact therewith. By making the metal Si contact in this way, the metal Si is easily impregnated by gravity.
[0039] The firing is preferably carried out in an inert gas atmosphere or in vacuum at a temperature of 1400 to 1600° C. By carrying out firing under such conditions, it becomes easier to impregnate the metal Si. In addition, it is possible to suppress insufficient sintering due to oxidation and reduce oxides contained in the molding material. The inert gas atmosphere may be a nitrogen gas atmosphere, a rare gas atmosphere such as argon, or a mixed gas atmosphere thereof. From the viewpoint of stably ensuring the above-mentioned effects, the firing temperature is preferably 1450 to 1550° C. The firing time is not particularly limited, but is typically 0.25 to 5 hours. The firing furnace used for firing is not particularly limited, but an electric furnace, a gas furnace, or the like can be used.
[0040] <Other processes> Between the molding step and the firing / impregnation step, the molded body may be subjected to at least one of drying and degreasing treatments. After the firing / impregnation step, the molded body may be subjected to surface treatment such as polishing. The drying process is not particularly limited, and any known method can be used. For example, the drying process can be performed using a microwave dryer, a hot air dryer, a dielectric dryer, a reduced pressure dryer, a vacuum dryer, a freeze dryer, or the like.
[0041] The degreasing treatment is a process for burning and removing components such as binders. The conditions for the degreasing treatment are not particularly limited as long as the binders can be burned, and may be appropriately set according to the type of binders. For example, the molded body can be degreased by heating it at 300 to 600°C for 1 to 10 hours.
[0042] (2) Ceramic body A ceramic body according to an embodiment of the present invention is obtained by the above-mentioned method for producing a ceramic body. This ceramic body has a SiC skeleton and a metal Si-impregnated portion. The SiC skeleton contains SiC particles having a particle size of 15 to 50 μm and SiC particles having a particle size of 2 to 8 μm in a volume ratio of 3:7 to 7:3. By making the SiC skeleton contain two types of SiC particles having predetermined particle sizes in the above volume ratio, the proportion of SiC particles in the ceramic body can be increased, thereby improving the thermal conductivity of the ceramic body.
[0043] Here, the volume ratio of SiC particles having a particle size of 15-50 μm to SiC particles having a particle size of 2-8 μm in the ceramic body can be obtained by observing the cross section of the ceramic body with an SEM. Specifically, in the SEM image of the cross section of the ceramic body, SiC particles having a particle size of 15-50 μm are distinguished from SiC particles having a particle size of 2-8 μm. In this case, the particle size of the SiC particles is taken as the circle equivalent diameter. The ratio of the total area of SiC particles having a particle size of 15-50 μm to the total area of SiC particles having a particle size of 2-8 μm is taken as the volume ratio of SiC particles having a particle size of 15-50 μm to SiC particles having a particle size of 2-8 μm in the ceramic body.
[0044] The metal Si-impregnated portion is formed in at least some of the voids in the SiC skeleton, and by forming the metal Si-impregnated portion, the ceramic body can be made dense, and the thermal conductivity and strength can be increased.
[0045] The thermal conductivity of the ceramic body is not particularly limited, but is preferably 140 W / mK or more, more preferably 150 W / mK or more at 25° C. When the ceramic body is used in a heat exchanger, the thermal conductivity of the ceramic body can be set within the above range to improve the heat recovery performance of the heat exchanger. The thermal conductivity value means a value measured by the laser flash method (JIS R1611:1997).
[0046] Other characteristics of the ceramic body, such as the material constituting the ceramic body and its shape, are the same as those described in the above-mentioned method for producing a ceramic body, and therefore will not be described here. EXAMPLES
[0047] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way.
[0048] (Examples 1 to 4) Three types of SiC powder with average particle sizes D50 of 35 μm, 25 μm, and 5 μm were prepared. Next, two or three of these SiC powders were mixed in the mass ratios shown in Table 1, and 28 parts by mass of water and 7 parts by mass of methyl cellulose were further added and mixed for a total of 100 parts by mass of SiC powder to obtain a molding material. This molding material was extrusion molded to obtain a honeycomb-shaped molded body. The size of the honeycomb molded body was adjusted so that it would become a honeycomb structure of the following shape after the firing and impregnation process. Shape of honeycomb structure in cross section perpendicular to cell extension direction: circular Cell shape in cross section perpendicular to the cell extension direction: Rectangle Length of cell extension: 100mm Outer diameter of honeycomb structure in cross section perpendicular to cell extension direction: 100 mm Cell density: 14 cells / cm 2 Partition thickness: 0.3mm Outer wall thickness: 1.5mm
[0049] Next, the honeycomb formed body was arranged so that the cell extension direction was the vertical direction, metal Si was placed on the upper end face, and then fired at a temperature of 1500°C in a vacuum to obtain a honeycomb structure (ceramic body).
[0050] (Comparative Examples 1 and 2) A honeycomb structure (ceramic body) was obtained in the same manner as in the above-mentioned Examples, except that SiC powder having an average particle size D50 of 35 μm or SiC powder having an average particle size D50 of 5 μm was used alone.
[0051] The thermal conductivity of the honeycomb structure obtained above was measured at 25° C. using a laser flash method (JIS R1611:1997). In the evaluation of thermal conductivity, a thermal conductivity of 150 W / mK or more was indicated as ⊚, a thermal conductivity of 140 W / mK or more but less than 150 W / mK was indicated as ◯, and a thermal conductivity of less than 140 W / mK was indicated as ×. The results are shown in Table 1.
[0052] [Table 1]
[0053] As shown in Table 1, the honeycomb structures (ceramic bodies) of Examples 1 to 4, which were prepared using SiC powder with an average particle size D50 of 15 to 50 μm and SiC powder with an average particle size D50 of 2 to 8 μm in a mass ratio of 3:7 to 7:3, had higher thermal conductivity than the honeycomb structures (ceramic bodies) of Comparative Examples 1 and 2, which were prepared using a single type of SiC powder.
[0054] As can be seen from the above results, the present invention can provide a ceramic body made of Si-impregnated SiC and having high thermal conductivity, and a method for producing the same. [Explanation of symbols]
[0055] 10 Molded body 100 Honeycomb molded body 110 Peripheral wall 120 cells 130 Bulkhead 140 Inner wall 200 Hollow honeycomb molding
Claims
1. A molding process of molding a molding material containing SiC powder having an average particle size D50 of 15 to 50 μm and SiC powder having an average particle size D50 of 2 to 8 μm in a mass ratio of 3:7 to 7:3 to obtain a molded body; a firing / impregnation step of firing the molded body and impregnating it with metal Si; A method for producing a ceramic body having the following structure:
2. The method for producing a ceramic body according to claim 1 , wherein the firing / impregnation step is carried out by firing the molded body in a state of contact with metallic Si.
3. The method for producing a ceramic body according to claim 2, wherein the firing is carried out at a temperature of 1400 to 1600° C. in an inert gas atmosphere or under vacuum.
4. The method for producing a ceramic body according to any one of claims 1 to 3, wherein the ceramic raw material contained in the molding material is only the SiC powder.
5. The method for producing a ceramic body according to any one of claims 1 to 3, wherein at least one of a drying treatment and a degreasing treatment is performed on the molded body between the molding step and the firing / impregnation step.
6. The method for producing a ceramic body according to any one of claims 1 to 3, wherein the molded body has a honeycomb shape having an outer peripheral wall and a plurality of partition walls arranged inside the outer peripheral wall and defining a plurality of cells extending from a first end face to a second end face, or a hollow honeycomb shape having an inner peripheral wall, an outer peripheral wall, and partition walls arranged between the inner peripheral wall and the outer peripheral wall and defining a plurality of cells extending from a first end face to a second end face.
7. a SiC skeleton including SiC particles having a particle size of 15 to 50 μm and SiC particles having a particle size of 2 to 8 μm in a volume ratio of 3:7 to 7:3; a metal Si impregnated portion formed in at least some of the voids of the SiC skeleton; A ceramic body comprising:
Citation Information
Patent Citations
Handotaikakusanro
JP1976085374A
Manufacture of structural member for semiconductor diffusion furnace
JP1988035452A
Sic sintered body
JP1988222086A
Silicon-impregnated silicon carbide-based material for heat treatment of semiconductor, and its production
JP2000103677A
Silicon / silicon carbide composite material and method of producing the same
JP2004018322A