Method for manufacturing synthesis gas
A composite oxide catalyst with controlled transition metal content enhances methane partial oxidation selectivity, addressing hot spot issues and catalyst deterioration, ensuring efficient production of carbon monoxide and hydrogen.
Patent Information
- Application Number
- JP2023052410
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
AI Technical Summary
Existing catalysts for methane partial oxidation suffer from rapid heating due to hot spots, leading to complete oxidation and catalyst deterioration, reducing the yield of carbon monoxide and hydrogen.
A composite oxide catalyst containing specific elements from Groups 4 to 6 of the periodic table, aluminum, silicon, and phosphorus, with limited amounts of transition metals, is used to suppress complete oxidation and enhance partial oxidation selectivity.
The catalyst effectively suppresses complete oxidation, maintaining high selectivity for partial oxidation of methane, preventing hot spots and catalyst degradation, thereby improving the yield of carbon monoxide and hydrogen.
Smart Images

Figure 2024140996000004 
Figure 2024140996000005 
Figure 2024140996000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing synthesis gas, and more particularly to a method for producing carbon monoxide and hydrogen (synthesis gas) using methane as a raw material and a catalyst. [Background technology]
[0002] Methane (CH4) reforming is a technology that is often used to produce a mixed gas (synthetic gas) of carbon monoxide (CO) and hydrogen (H2). Among the methane reforming reactions, steam reforming of methane (CH4+H2O→3H2+CO, ΔH0=+206kJ) is the most commonly used technology, but this reaction is a large endothermic reaction, and the large energy consumption in the process is an issue. On the other hand, the partial oxidation of methane (2CH4 + O2 → 4H2 + 2CO, ΔH0 = -36 kJ) is an exothermic reaction, and therefore is attracting attention as a highly energy-efficient process that does not require external energy supply once the reaction begins.
[0003] For such partial oxidation of methane, catalytic materials containing transition metals such as Co, Ni, Ru, Rh, Pd, and Pt as active sites, particularly those containing zeolites, have been used. For example, Patent Document 1 discloses a partial oxidation catalyst for light hydrocarbons containing cobalt- and rhodium-supported zeolite. Patent Document 2 discloses a partial oxidation catalyst for light hydrocarbons in which zeolite supports at least one element selected from transition metals in Groups 8 to 11 of the periodic table and at least one element selected from metals in Groups 1 to 3 of the periodic table. Patent Document 4 discloses a catalytic partial oxidation catalyst for hydrocarbons in which rhodium, iridium or ruthenium is supported on a carrier. Patent Document 5 discloses a supported catalyst for oxidative reforming of organic compounds such as methane, which is made of at least one metal selected from the group consisting of rhodium, ruthenium, iridium, palladium and platinum. Nickel is also used in the oxidative reforming of methane, as described in Patent Document 6, in the form of a supported nickel catalyst. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2019-181375 A [Patent Document 2] Patent Publication No. 2021-45722 [Patent Document 3] China Publication No. 101597030 [Patent Document 4] Japanese Patent Application Publication No. 7-10503 [Patent Document 5] JP 2008-136907 A [Patent Document 6] Special Publication No. 9-502414 Summary of the Invention [Problem to be solved by the invention]
[0005] When the catalytic materials disclosed in Patent Documents 1 and 2 are used, a part of methane is likely to be completely oxidized (CH4+2O2→2H2O+CO2, ΔH0=-803 kJ) simultaneously with the partial oxidation of methane. Since the heat generated by the complete oxidation is much larger than that generated during partial oxidation, the catalyst bed is rapidly heated as soon as the reaction starts, forming a hot spot. The formation of such a hot spot not only reduces the yield of carbon monoxide, but also causes aggregation of active metal species at the hot spot. When a hot spot is formed, even if the reaction is stopped and the partial oxidation reaction is resumed, the complete oxidation reaction is likely to occur again, and the aggregation of metals can also cause catalyst deterioration. Therefore, there is a demand for the development of a catalyst that suppresses the complete oxidation of methane and partially oxidizes methane highly selectively by reaction with oxygen. Partial oxidation of methane using a dual catalyst bed system has also been proposed. In a dual catalyst bed system, a metal oxide catalyst is placed in the front stage of the catalyst bed, and a metal catalyst is placed in the rear stage. The oxide catalyst in the front stage oxidizes methane with O2 and converts it to CO, H2, CO2, and H2O. In the rear stage, where O2 has been consumed, methane is reformed with CO2 and H2O by a supported metal catalyst, and converted to CO and H2. In order to control the reaction heat in the front stage of the catalyst bed, the CO and H2 selectivity of the oxide catalyst is the key. Y-stabilized ZrO2 and Cr2O3 have been reported as oxide catalysts for oxidizing methane (for example, Patent Document 3), but their CO and H2 selectivity is not very high.
[0006] The present invention is devised to solve the above-mentioned problems, and has an object to provide a catalyst that suppresses complete oxidation of methane and partially oxidizes methane with high selectivity in the reaction of methane with oxygen. [Means for solving the problem]
[0007] As a result of investigations conducted by the present inventors to solve the above problems, they found that composite oxides or supported oxides having a heterogeneous oxide-oxide interface exhibit high CO yields in the partial oxidation of CH4. In particular, they found that oxides of Groups 1, 2, and 3 are basic and therefore favor the oxidative coupling of methane (OCM) reaction, that oxides of transition metals of Groups 7 to 11 have excellent redox properties and therefore favor the complete oxidation of methane, and that composite oxides or supported oxide catalysts combining two or more of elements of Groups 4 to 6 of the periodic table and Al, Si, and P are highly active in the partial oxidation of methane. The present invention was completed based on these findings.
[0008] The present invention includes the following gist. [1] A method for producing synthesis gas by partially oxidizing methane using a composite oxide catalyst that contains at least two of the elements of Groups 4 to 6 of the periodic table, or aluminum, silicon, and phosphorus, and has a Co, Ni, and Fe content of less than 0.1 mass%, and a Ru, Rh, Pd, Ir, and Pt content of less than 0.05 mass% each. [2] A composite oxide catalyst for partial oxidation of methane containing at least two of the elements of Groups 4 to 6 of the periodic table, or aluminum, silicon, and phosphorus, with the Co, Ni, and Fe contents each being less than 0.1 mass%, and the Ru, Rh, Pd, Ir, and Pt contents each being less than 0.05 mass%. [3] A method for producing synthesis gas by partially oxidizing methane using a supported oxide catalyst in which at least one of elements from Groups 4 to 6 of the periodic table, aluminum, or silicon is supported on an oxide support, and the supported oxide catalyst contains less than 0.1 mass% Co, Ni, and Fe, and less than 0.05 mass% Ru, Rh, Pd, Ir, and Pt. [4] The method for producing a synthesis gas according to the above [3], wherein the oxide support is at least one selected from the group consisting of Al2O3, ZrO2, TiO2, SiO2 and zeolite. [5] A composite oxide catalyst for partial oxidation of methane, comprising an oxide support and at least two of elements from Groups 4 to 6 of the periodic table, aluminum, and silicon, with the Co, Ni, and Fe contents each being less than 0.1 mass%, and the Ru, Rh, Pd, Ir, and Pt contents each being less than 0.05 mass%. [6] The method for producing a synthesis gas according to the above [4], wherein the crystal structure of the zeolite includes at least one selected from the group consisting of AEI, CHA, MFI, and BEA in the IZA code. Effect of the Invention
[0009] According to the present invention, it is possible to provide a catalyst which suppresses complete oxidation of methane in the reaction of methane with oxygen and highly selectively partially oxidizes methane. [Brief description of the drawings]
[0010] [Figure 1] 1 shows the results of a partial oxidation reaction test of methane using the catalyst produced in Example 1. [Diagram 2] 1 shows the results of a partial oxidation reaction test of methane using the catalyst produced in Example 2. [Diagram 3] 1 shows the results of a partial oxidation reaction test of methane using the catalyst produced in Example 3. [Figure 4] 1 shows the results of a partial oxidation reaction test of methane using the catalyst produced in Example 4. [Diagram 5] 1 shows the results of a partial oxidation reaction test of methane using the catalyst produced in Example 5. [Figure 6] 1 shows the results of a partial oxidation reaction test of methane using the catalyst produced in Example 6. [Figure 7] 1 shows the results of a partial oxidation reaction test of methane using the catalyst produced in Comparative Example 1. [Figure 8] 1 shows the results of a partial oxidation reaction test of methane using the catalyst produced in Comparative Example 2. [Figure 9] 1 shows the results of a partial oxidation reaction test of methane using the catalyst produced in Comparative Example 3. [Figure 10] 1 shows the results of a partial oxidation reaction test of methane using the catalyst produced in Comparative Example 4. [Figure 11] 1 shows the results of a partial oxidation reaction test of methane using the catalyst produced in Comparative Example 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The present invention will be described in detail below. However, the description of the constituent elements described below is one example (representative example) of an embodiment of the present invention, and the present invention is not limited to these contents, and can be implemented in various modifications within the scope of the gist of the present invention.
[0012] [Method of producing synthetic gas] The first synthesis gas production method of the present invention is a method for producing synthesis gas by a partial oxidation reaction of methane, and is characterized by using a composite oxide catalyst containing at least two of elements from Groups 4 to 6 of the periodic table, or aluminum, silicon, and phosphorus, and having a Co, Ni, and Fe content of less than 0.1 mass% and a Ru, Rh, Pd, Ir, and Pt content of less than 0.05 mass%. The second synthesis gas production method of the present invention is characterized in that at least one of elements from Groups 4 to 6 of the periodic table, aluminum, and silicon is supported on an oxide support, and methane is partially oxidized using a supported oxide catalyst having a Co, Ni, and Fe content of less than 0.1 mass% and a Ru, Rh, Pd, Ir, and Pt content of less than 0.05 mass%. In the first synthesis method and the second synthesis method, the first synthesis method is a perspective in which the present invention is understood as a composite oxide including the support, while the second synthesis method is a perspective in which the present invention is understood with a focus on the supported oxide.
[0013] <Composite oxide catalyst> The catalyst used in the present invention is a composite oxide containing at least two of elements from Groups 4 to 6 of the periodic table, or aluminum, silicon, and phosphorus, with a Co, Ni, and Fe content of less than 0.1 mass% and a Ru, Rh, Pd, Ir, and Pt content of less than 0.05 mass%. Here, the content of Co, Ni, and Fe must be less than 0.1% by mass, and more preferably, the total content of Co, Ni, and Fe in the composite oxide must be less than 0.1% by mass. The content of Ru, Rh, Pd, Ir, and Pt must be less than 0.05% by mass, and more preferably, the total content of Co, Ni, and Fe in the composite oxide must be less than 0.1% by mass. By making these elements less than a specific amount, as described above, it is difficult to cause a complete oxidation reaction of methane, and it is possible to proceed with a partial oxidation reaction with high selectivity. Therefore, it is preferable because it is possible to suppress the possibility of localized heat generation that causes catalyst deterioration in the reaction process.
[0014] The advantage of using composite oxides is that acid sites appear when two oxides are mixed to create a composite oxide, and it is generally believed that the cause of the appearance of acid sites is a partial excess or deficiency of electric charge. For example, zeolite is based on a framework structure made of silicon dioxide (SiO2), and some of the silicon has been replaced with aluminum, making part of the framework negatively charged. This excess charge is replenished by protons (H + ) coordinates and exhibits Brønsted acidity. In addition, as a result of the complexation, the cationic site of the oxide that is deficient in charge exhibits Lewis acidity to accept electrons. It is known that the Lewis acidity of this oxide functions as a site for activating CH of alkanes including methane. These mechanisms are described in detail, for example, in Otroshchenko, T.; Jiang, G.; Kondratenko, VA; Rodemerck, U.; Kondratenko, EV Chem. Soc. Rev. 2021, 50, 473-527. or Wischert, R.; Laurent, P.; Coperet, C.; Delbecq, F.; Sautet, PJ Am. Chem. Soc. 2012, 134, 14430-14449. Therefore, it is expected that the compounding of oxides will improve the partial oxidation activity of oxide catalysts for methane.
[0015] Specifically, the elements used as the main components of the composite oxide are preferably selected from Zr, V, W, Al, Si and P, and more preferably combinations of W-Zr, W-Al, V-Zr, Si-Zr, Si-Al, Al-P and Si-P.
[0016] The particle size of the composite oxide is not particularly limited, but may be appropriately determined taking into consideration the size of the reactor used, reaction efficiency, residence time, strength to prevent crushing, air resistance, ease of handling, etc.
[0017] The method for synthesizing the composite oxide is not particularly limited, and a complex polymerization method, a solid-phase precipitation method, a sol-gel method, a hydrothermal synthesis method, or the like may be appropriately used. In the complex polymerization method, an oxide precursor is dissolved in pure water as a starting material to prepare a precursor ion-containing aqueous solution (aqueous solution A). A solution of a chelating agent (aqueous solution B) is also prepared separately. Next, aqueous solution B is added to aqueous solution A under stirring, and the resulting mixed solution is heated (primary baking) to obtain a metal complex as a precursor. This resulting precursor is then heated to burn the organic matter to obtain a complex oxide (powder form). Examples of oxide precursors used to obtain the aqueous solution A include chlorides, oxides, nitrates, sulfates, oxalates, salicylates, acetates, carbonates, hydroxides, etc., and from the viewpoint of controlling the composition of the product, chlorides, nitrates, sulfates, and acetates are preferred, and nitrates are particularly preferred. When the metal-containing raw material is one of these salts, the by-products accompanying the production of the composite oxide are gases or water containing nitrogen, oxygen, chlorine, carbon, sulfur, etc., and can be easily removed from the system. Examples of the solution of the chelating agent include an aqueous solution of citric acid, an ammonia solution of ethylenediaminetetraacetic acid, an aqueous solution of nitrilotriacetic acid, etc. Among these, an aqueous solution of citric acid is preferred because of its low cost and low environmental impact.
[0018] In the solid-state reaction method, the powder of an oxide precursor is mixed as a starting material, and the mixture is calcined to obtain the desired composite oxide (powdered). Examples of oxide precursors used in the solid-state reaction method include hydroxides, oxides, and carbonates. Among these, oxides are preferred because they suppress the generation of impurity phases and can be synthesized at low temperatures. In general, when synthesizing by the solid phase method, the composition distribution of each element is more likely to be biased in the precursor stage and the stage after firing than in the solution method, so it is important to control the particle size of the raw material powder and to mix the powder uniformly. For example, it is effective to use raw material powder with a small particle size and little aggregation, and to mix it using a ball mill, etc.
[0019] The firing temperature and firing time in the synthesis of the composite oxide are not particularly limited, but from the viewpoint of reducing impurity phases, the firing temperature and firing time are preferably set so that the target phase is generated as a main phase or a single phase. On the other hand, from the viewpoint of suppressing the decrease in specific surface area due to sintering and reducing side reactions with the crucible, treatment at a temperature 400° C. lower than the melting point of the target phase and lower than the melting point is preferred. The firing atmosphere is not particularly limited and can be appropriately selected depending on the target composite oxide. The final firing atmosphere may be, for example, an oxygen-inert gas mixed atmosphere or an inert gas atmosphere.
[0020] The composition of the elements of the composite oxide is not particularly limited, but from the viewpoint of reducing impurity phases, it is preferable that the composition be such that the target phase is generated as a main phase or a single phase. In addition, the constituent elements may include, in addition to the elements of Groups 4 to 6 of the periodic table, Si, Al, and P, one or more elements selected from, for example, magnesium (Mg), calcium (Ca), boron (B), yttrium (Y), lanthanum (La), and cerium (Ce).
[0021] The BET specific surface area of the composite oxide is not particularly limited as long as the effects of the present invention are achieved. For example, 2 The BET specific surface area of the composite oxide is preferably 10 m 2 / g or more, sufficient active sites for the raw material methane are secured, improving the reaction efficiency. The BET specific surface area of the composite oxide is 10m 2 / g or more is preferable, and 30m 2 / g or more is more preferable. The above composite oxides may be used alone or in combination of two or more kinds physically mixed in a mortar or ball mill.
[0022] <Supported oxide> The second synthesis method of the present invention also has the same advantages as the first synthesis method. This is because, even in the case of a supported oxide in which elements are not composited at the atomic level like a composite oxide, an interface is formed between the supported species and the oxide, so that the acidic properties can be expected to be expressed. Another advantage of using a supported oxide catalyst is that it is easy to increase the surface area of the catalyst and control its mechanical strength by selecting the support. The combination of the constituent elements is the same as in the first invention. The oxide support is preferably at least one selected from the group consisting of Al2O3, ZrO2, TiO2, SiO2, and zeolite. Hereinafter, a more detailed explanation will be given by taking the case of using zeolite as the supported oxide as an example.
[0023] <Zeolite> In the synthesis gas production method of the present invention, the zeolite used as the catalyst contains silicon (Si) and aluminum (Al) as constituent elements. In addition to Si and Al, the constituent elements may contain one or more elements selected from boron (B), titanium (Ti), vanadium (V), phosphorus (P), zinc (Zn), gallium (Ga), germanium (Ge), zirconium (Zr), and tin (Sn). Note that Al and the like forming the zeolite framework become acid sites and act as reaction sites for catalytic activity. The molar ratio of silicon to aluminum (Si / Al) of these zeolites is not particularly limited as long as it is within the range in which the effects of the present invention can be achieved, but is preferably 3 or more and 100 or less. When the Si / Al ratio is 100 or less, the amount of acid becomes appropriate, and the partial oxidation reaction of methane can be promoted. From the above viewpoint, it is more preferable that the Si / Al ratio is 80 or less. On the other hand, when the Si / Al ratio is 3 or more, dealumination in the partial oxidation reaction of methane can be suppressed, and high activity can be maintained. From the above viewpoint, it is more preferable that the Si / Al ratio is 8 or more. The contents of Si, Al, etc. in the zeolite produced by the method of the present invention can usually be measured by inductively coupled plasma atomic emission spectrometry (ICP-AES) or the like, and are values measured for the produced zeolite, not the ratios of the raw materials charged.
[0024] The Si / Al ratio can be controlled by the SiO2 / Al2O3 ratio used in the production of zeolite, and can also be controlled by the production conditions. Furthermore, after the production of zeolite, the Si / Al ratio can also be controlled by desorbing Al and the like through a steaming process or the like.
[0025] The crystal structure of the zeolite according to the present invention is not particularly limited as long as it exhibits the effects of the present invention, and examples of the codes set by the International Zeolite Association (IZA) include AEI, AEL, AFI, AFX, APC, ATO, BEA, BRE, CDO, CHA, CON, DDR, EAB, EPI, ERI, ESV, EUO, FAU, FER, GIS, GME, HEU, ITH, KFI, LEV, LTA, LTL, MER, MEL, MFI, MON, MOR, MSE, MTF, MTT, MTW, MWW, NES, OFF, PAU, PHI, RHO, RTE, RTH, SOD, STI, STT, SZR, TON, TSC, TUN, UFI, VNI, WEI, YUG, etc. Among these, it is preferable to include one or more types selected from CHA, MFI, and BEA. These zeolites are suitable as reaction sites for the partial oxidation of methane because extra-framework Al species that can exhibit Lewis acidity are generated during the partial oxidation of methane, and therefore show better activity than MOR and FAU. The above zeolites may be used alone or in combination of two or more kinds. The formation of extraskeletal Al species can be confirmed by IR from the OH stretching vibration of Al-OH.
[0026] The pore size of the zeolite is not particularly limited, but is preferably 0.3 nm or more, more preferably 0.35 nm or more. It is also preferably 0.9 nm or less, more preferably 0.8 nm or less, and even more preferably 0.6 nm or less. The pore size referred to here indicates the crystallographic channel diameter defined by the International Zeolite Association (IZA). When the pore size of the zeolite is within the above range, the raw materials methane and oxygen easily enter the zeolite pores, and the reaction easily proceeds at the active sites in the pores. In addition, the product is easily desorbed, and there is no problem such as coking caused by excessive reaction in the pores.
[0027] The ion exchange sites of the zeolite are not particularly limited, and may be either H-type or those exchanged with alkali metal ions, alkaline earth metal ions, etc., with the H-type being preferred.
[0028] The BET specific surface area of the zeolite is not particularly limited as long as the effects of the present invention are achieved. For example, 2 The BET specific surface area of the zeolite is preferably 200 m 2 / g or more, sufficient active sites for the raw material methane are secured, and the reaction efficiency can be improved. From the above viewpoints, the BET specific surface area of the zeolite is 250 m 2 / g or more is more preferable, and 300m 2 On the other hand, the BET specific surface area of the zeolite is preferably 2000 m 2 The BET specific surface area of the zeolite is preferably 2000 m 2 From the above viewpoints, the BET specific surface area of the zeolite is 1500 m 2 / g or less is more preferable, and 2 It is more preferable that the molecular weight is not more than 1 / g. The BET specific surface area can be measured by a nitrogen adsorption method.
[0029] In addition, the pore volume of the zeolite according to the present invention is not particularly limited as long as the effects of the present invention are achieved, but is preferably 0.1 mL / g or more. When the pore volume of the zeolite is 0.1 mL / g or more, sufficient adsorption sites for the raw material methane are secured, and the reaction efficiency can be improved. From the above viewpoints, the pore volume of the zeolite is more preferably 0.2 mL / g or more, and even more preferably 0.3 mL / g or more. On the other hand, the pore volume of the zeolite is preferably 3 mL / g or less, and more preferably 2 mL / g or less. The average pore size of the zeolite may be the pore size value of each crystal structure published by IZA, and the pore volume can be measured by a nitrogen adsorption method.
[0030] The average primary particle size of the zeolite according to the present invention is not particularly limited as long as the effects of the present invention are achieved, but is preferably 10 μm or less. If the average primary particle size of the zeolite is 10 μm or less, it is advantageous in terms of the diffusion of the reaction substrate and the reaction product. From the above viewpoint, the average primary particle size of the zeolite is more preferably 3 μm or less, and further preferably 700 nm or less. On the other hand, the lower limit is not particularly limited as long as it is within the range in which the effects of the present invention can be obtained, and is usually 20 nm or more, preferably 40 nm or more.
[0031] The "average primary particle size" can be measured using a scanning electron microscope (SEM). Here, the term "primary particle" refers to the smallest particle in which no grain boundary is observed. In the present invention, an SEM image of the zeolite catalyst is obtained, and the smallest particle in which no grain boundary is observed and which is a part corresponding to zeolite contained in the SEM image is determined as the "primary particle". In the present invention, the primary particle does not have to exist as a single particle, and may form a secondary particle by aggregation or the like. Even if a secondary particle is formed, the primary particle on the surface of the secondary particle can be distinguished in the SEM image. The "average primary particle diameter" refers to a measurement made as follows. That is, 50 primary particles contained in an SEM image of a zeolite catalyst are randomly selected, and the major axis (the longest straight line length when connecting one end of a primary particle with the other end of a straight line) is measured for each of the selected 50 primary particles, and the arithmetic mean of the major axes of the 50 particles measured is taken as the "average primary particle diameter." However, if the entire zeolite catalyst contains fewer than 50 primary particles, the major axis of each of the primary particles contained in the zeolite catalyst is measured, and the average value is taken as the "average primary particle diameter."
[0032] The average primary particle size can be set within a specific range, for example, by using zeolite having a small particle size as seed crystals, or by adding a surfactant to the raw material gel for zeolite synthesis in the zeolite production process.
[0033] The zeolite according to the present invention has a Co, Ni, and Fe content of less than 0.1 mass% and a Ru, Rh, Pd, Ir, and Pt content of less than 0.05 mass%, so that hot spots are not formed by the complete oxidation reaction of methane. Therefore, the carbon monoxide yield is not reduced due to the formation of hot spots, which is preferable.
[0034] <Zeolite manufacturing method> The method for producing a zeolite of the present invention includes a step of hydrothermally synthesizing a raw material composition. More specifically, the method includes a step of preparing a raw material gel containing a silica source, an aluminum source, and an alkali metal, and a step of hydrothermally synthesizing the raw material gel at 10 to 240°C.
[0035] (Preparation of raw gel) The raw gel is prepared using a silica source, an aluminum source, and a compound containing an alkali metal. In the preparation of the raw gel, other components such as a compound containing an alkaline earth metal, an organic structure directing material, and a seed crystal may be further used as long as they do not significantly impair the effects of the present invention.
[0036] <<Raw materials>> The silica source refers to a raw material compound that becomes silicon atoms that constitute zeolite. Examples of silica sources include fumed silica, silica sol, colloidal silica, water glass, ethyl silicate, methyl silicate, etc., and one or more of these are used. Among these, fumed silica and colloidal silica are preferred because they are easy to handle and highly reactive.
[0037] The aluminum source refers to a raw material compound that becomes the aluminum atoms that constitute the zeolite. The aluminum source is usually an aluminum alkoxide such as pseudoboehmite, gibbsite, aluminum isopropoxide, aluminum triethoxide, etc.; aluminum hydroxide; alumina sol, sodium aluminate, etc., and one or more of these are used. Among these, aluminum hydroxide, aluminum isopropoxide, and pseudoboehmite are preferred because they are easy to handle and highly reactive.
[0038] The compound containing an alkali metal may be a hydroxide of an alkali metal such as NaOH or KOH. The type of alkali metal is not particularly limited, and typically includes Na, K, Li, and Rb, and preferably Na and K. Two or more types of compounds containing an alkali metal may be used in combination. In addition, a compound containing an alkaline earth metal may be used. As the compound containing an alkaline earth metal, Ca(OH)2 or the like may be used. The type of alkaline earth metal is not particularly limited, and typically includes Ca, Mg, Sr, and Ba. In addition, two or more types of compounds containing an alkaline earth metal may be used in combination.
[0039] The organic structure directing agent used in the synthesis of zeolite is usually amines, quaternary ammonium salts, etc. For example, when synthesizing CHA-type aluminosilicate, the organic templates described in U.S. Patent No. 4,544,538 and U.S. Patent Publication No. 2008 / 0075656 are preferred. Note that, depending on the composition of the obtained zeolite, the organic structure directing agent is not necessarily required.
[0040] A seed crystal may be used in the preparation of the raw material gel. As the seed crystal, a zeolite is usually used. If the zeolite to be produced is an aluminosilicate, the seed crystal is preferably an aluminosilicate zeolite, and more preferably an aluminosilicate zeolite containing d6r as the CBU. The seed crystal may contain an amorphous component as a part thereof. The zeolite used as the seed crystal may or may not contain an organic structure-directing material. The method for producing the zeolite to be used as the seed crystal is not particularly limited, and may be produced by the zeolite production method of the present invention, or may be produced by other methods, such as a general batch method using an autoclave. The amount of the seed crystal is preferably large in terms of the effect of promoting crystallization as the seed crystal. On the other hand, it is preferable that the amount of the seed crystal is small in terms of the ease of dissolving the seed crystal and the ease of functioning as the seed crystal. Therefore, the amount of the seed crystal is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, even more preferably 1.0% by mass or more, and particularly preferably 2% by mass or more, relative to the silica source contained in the raw material composition. On the other hand, it is preferably 30% by mass or less, more preferably 20% by mass or less, further preferably 15% by mass or less, and particularly preferably 10% by mass or less.
[0041] (Hydrothermal synthesis of raw gel) The zeolite of the present invention can be produced by hydrothermal synthesis of the raw material gel described above. The hydrothermal synthesis temperature of the raw material gel is usually 10°C or higher, preferably 50°C or higher, and more preferably 70°C or higher. A high temperature is preferable in terms of facilitating the reaction. There is no particular upper limit to the temperature of the hydrothermal synthesis, and it is usually 240°C or lower, preferably 220°C or lower, and more preferably 200°C or lower.
[0042] <<Cation exchange>> The method for producing a zeolite of the present invention may further include a step of exchanging the cation type of the zeolite obtained by the above-mentioned hydrothermal synthesis. Zeolite obtained by hydrothermal synthesis can be cation-exchanged to a desired cation type as necessary. The cation exchange can be performed using, but is not limited to, nitrates such as NH4NO3, LiNO3, NaNO3, KNO3, RbNO3, CsNO3, Be(NO3)2, Ca(NO3)2, Mg(NO3)2, Sr(NO3)2, Ba(NO3)2, or salts of halide ions, sulfate ions, carbonate ions, hydrogen carbonate ions, acetate ions, phosphate ions, and hydrogen phosphate ions instead of the nitrate ions contained in these nitrates, and acids such as nitric acid and hydrochloric acid. The temperature of the cation exchange is not particularly limited as long as it is a general cation exchange temperature, but is usually 10°C or higher and 100°C or lower. Ammonium-type zeolite can also be converted to proton-type zeolite by calcining the zeolite.
[0043] After the raw gel is crystallized, the crystallized raw gel is filtered and washed, and the solid content is dried at 100 to 200°C and then calcined at 400 to 900°C to obtain zeolite powder. Furthermore, zeolite powder can be impregnated with an oxide precursor solution of a prescribed concentration, the solvent is evaporated to dryness, and then the mixture is fired at 400 to 900° C. to obtain a powder of oxide supported on zeolite.
[0044] <Reaction conditions> The reaction conditions using the partial oxidation of methane are common to both the first and second inventions. The reaction temperature in the synthesis gas production method of the present invention is preferably 650° C. or higher. By setting the reaction temperature at 650° C. or higher, the partial oxidation of methane progresses, and synthesis gas can be efficiently obtained. On the other hand, there is no particular upper limit to the reaction temperature, but it is preferably 1000° C. or lower in order to suppress complete oxidation of methane. From the above viewpoints, the reaction temperature in this reaction is preferably in the range of 650°C to 1000°C, and more preferably in the range of 650°C to 800°C. Since this reaction is an exothermic reaction, even if the reaction start temperature is 500°C, it may reach 650°C or higher if an adiabatic reaction vessel is used. Therefore, the reaction temperature here refers not to the inlet temperature of the reaction gas but to the temperature of the catalyst layer of the reactor. The temperature of the catalyst layer can usually be considered to be the same as the internal temperature (not the inlet temperature) of the reactor.
[0045] In the partial oxidation process of methane in the present invention, the ratio of methane to oxygen (CH4 / O2) in the raw material is preferably 1 or more. When this ratio is 1 or more, complete oxidation of methane can be easily suppressed, and partial oxidation of methane can be promoted. Furthermore, when the ratio of methane to oxygen (CH4 / O2) is 1 or more, a sufficient reaction rate can be obtained. From the above viewpoints, the ratio of methane to oxygen (CH4 / O2) in the raw material is preferably 1 or more, more preferably 1.5 or more, and most preferably 2 or more. On the other hand, there is no particular upper limit to the ratio of methane to oxygen (CH4 / O2), but from the standpoint of reaction efficiency, it is preferably 6 or less, and more preferably 3 or less.
[0046] As the reaction mode in this embodiment, a known gas phase reaction process using a fluidized bed reactor, a moving bed reactor, or a fixed bed reactor can be applied. A fixed bed reactor is advantageous in terms of the equipment cost including auxiliary equipment, catalyst cost, and operation management. The process may be carried out in any of a batch, semi-continuous or continuous manner, but is preferably carried out in a continuous manner, and may be a process using a single reactor or a process using multiple reactors arranged in series or parallel.
[0047] When the above-mentioned catalyst is packed into the fluidized bed reactor, in order to minimize the temperature distribution in the catalyst layer, granular materials inactive to the reaction, such as quartz sand, alumina, silica, silica-alumina, etc., may be mixed with the catalyst and packed. In this case, there is no particular restriction on the amount of granular materials inactive to the reaction, such as quartz sand, used. In addition, it is preferable that the granular materials have a particle size similar to that of the catalyst, from the viewpoint of uniform mixing with the catalyst. Furthermore, the reaction substrates (reaction raw materials) may be divided and fed to the reactor for the purpose of dispersing heat generated by the reaction.
[0048] In addition to methane and oxygen, other gases that can be present in the reactor include helium, argon, nitrogen, carbon monoxide, carbon dioxide, hydrogen, water, paraffins, aromatic compounds, and mixtures of these. Of these, the coexistence of water (water vapor) and / or carbon dioxide is preferred because it is expected to have the effect of suppressing carbon deposition on the catalyst. As such a diluent, impurities contained in the reaction raw materials may be used as they are, or a separately prepared diluent may be mixed with the reaction raw materials. The diluent may also be mixed with the reaction raw materials before being placed in the reactor, or may be supplied to the reactor separately from the reaction raw materials.
[0049] The lower limit of the reaction temperature is preferably 650°C or higher. The upper limit of the reaction temperature is not limited as long as the effects of the present invention are achieved, but is preferably 800°C or lower. If the reaction temperature is 650°C or higher, a sufficient reaction rate can be obtained. On the other hand, if the reaction temperature is 800°C or lower, the activity of the catalyst becomes stable.
[0050] The upper limit of the reaction pressure is preferably 3 MPa (absolute pressure, the same applies below). If the reaction pressure is 3 MPa or less, the production of undesirable by-products can be suppressed. From the above viewpoint, the reaction pressure is preferably 1 MPa or less. The lower limit of the reaction pressure is not particularly limited, but is usually 0.1 kPa or more, preferably 1 kPa or more, and more preferably 10 kPa or more. By keeping the reaction pressure at or above these lower limits, a sufficient reaction rate can be obtained.
[0051] The weight space velocity of the reactants is 0.1hr -1 It is preferable that the time is 0.5 hours or more. -1 On the other hand, the weight hourly space velocity is preferably 10 hr -1 It is preferable that the time is less than 5 hours. -1It is more preferable that the weight hourly space velocity is within this range, which is advantageous for the partial oxidation reaction of methane.
[0052] According to the method of the present invention, the reaction products include, in addition to syngas (CO + H2), hydrocarbons having 2 carbon atoms such as ethane and ethylene (by-products), carbon dioxide, and water. Among these reaction products, the selectivity of carbon dioxide with respect to methane as the reaction raw material can be 25% or less. In the present invention, the conversion rate of methane is 8 to 100%, and the selectivities of carbon monoxide and hydrogen are 60 to 90% and 8 to 25%, respectively. In addition, the mixed gas containing unreacted raw materials, by-products, and diluents in the reactor outlet gas can be introduced into known separation and purification equipment, and recovery, purification, recycling, and discharge treatments can be performed according to the respective components.
Examples
[0053] Hereinafter, the present invention will be described in more detail with reference to examples, but the scope of the present invention is not limited by the following examples. (Evaluation method) (1) Physical properties of zeolite <Elemental analysis> Elemental analysis was performed by inductively coupled plasma atomic emission spectrometry (ICP - AES). <X - ray diffraction measurement> The crystal structure of each zeolite was determined by X - ray diffraction measurement (XRD). The measurement was performed using "D2PHASER" manufactured by BRUKER. The elemental analysis results of the oxides used in each example and comparative example are shown in Table 1. The numerical values in Table 1 are the metal semi - quantitative results [μg / g] in the sample, and 200 μg / g corresponds to 0.02 mass%.
[0054]
Table 1
[0055] (2) Reaction evaluation Using a fixed-bed gas-phase flow reactor, 100 mg of the catalyst of each example and comparative example was filled in the middle of a quartz glass reaction tube (catalyst layer part: outer diameter 8.0 mm, inner diameter 6.0 mm, other: outer diameter 6.0 mm, inner diameter 4.0 mm, total length 260 mm). The electric furnace was heated to 500 ° C. under N2 flow (10 ml / min). Then, CH4 was introduced at a flow rate of 5.0 ml / min, O2 at a flow rate of 2.5 ml / min, and N2 at a flow rate of 12.5 ml / min, and a partial oxidation reaction test of methane was performed at a reaction temperature range of 500 ° C. to 800 ° C. Downstream of the reactor, condensation of the generated water was prevented by heating at 100 ° C. with a ribbon heater and diluting the reaction gas with N2 (100 ml / min). The analysis of the product was performed with a two-channel online Micro-GC (FUSION, INFICON). In channel 1 of the Micro-GC, H2, O2, N2, CH4, and CO were quantified using a capillary column Molecular Sieve 5A (trade name) with Ar as the carrier gas. In channel 2, CO2, C2H4, C2H6, and H2O were quantified using a capillary column Porapak (trade name) with He as the carrier gas. A TCD was used as the detector.
[0056] The conversion rate of the reactants and the yield of the products were calculated as follows. In the following formula, F means flow rate, in means inlet, and out means outlet. For example, F CH4,in means the inlet CH4 flow rate.
[0057]
number
[0058] In addition, the following relationship holds in the above formula:
[0059]
number
[0060] Example 1 The above reaction evaluation was carried out using a catalyst in which tungsten oxide was supported on ZrO2 as the support.
[0061] Examples 2 to 6 and Comparative Examples 1 to 5 In Example 1, the support was changed to alumina (Example 2), and the supported oxide was changed to vanadium oxide (VO x ) (Example 3), the supported oxide was changed to silicon oxide (SiO2) (Example 4), the MFI type zeolite (Si / Al=15) (Example 5), the SAPO-34 zeolite (Si / (Al+P+Si)=0.13) (Example 6), zirconium oxide alone (Comparative Example 1), aluminum oxide alone (Comparative Example 2), tungsten oxide (WO3) alone (Comparative Example 3), the supported oxide was changed to nickel oxide (NiO x ) (Comparative Example 4), the support was changed to silicon oxide, and the supported oxide was changed to nickel oxide (NiO x ), a partial oxidation reaction test of methane was carried out in the same manner as in Example 1. The results are shown in Figures 1 to 11, respectively.
[0062] In Example 1, a combination of tungsten and zirconium was used. As shown in FIG. 1, the methane conversion rate was 20% at 600°C, but increased to 80% at 700°C and 100% at 800°C. Meanwhile, the amount of CO gas produced increased, and the selectivity was always high at 60% or more.
[0063] In Example 2, a combination of tungsten and aluminum was used. As shown in FIG. 2, the methane conversion rate was a few percent at 600°C, but increased to 40% at 700°C and 90% or more at 800°C. Meanwhile, the amount of CO gas produced increased, and the selectivity was always high at 60% or more.
[0064] Example 3 is a combination of vanadium and zirconium, and as shown in Figure 3, the methane conversion rate was 60% at 600°C, but increased to nearly 100% at 700°C or higher. On the other hand, the amount of CO gas produced increased, and the selectivity also increased, with water and carbon dioxide (meaning complete oxidation) decreasing at 800°C and the selectivity for CO and hydrogen increasing.
[0065] Example 4 is a combination of silicon and zirconium, and as shown in Figure 4, the methane conversion rate was over 20% at 600°C, but dropped to just under 80% at 700°C or higher, and to 90% at 800°C. On the other hand, the amount of CO gas produced increased, and CO was obtained with a selectivity of approximately 60%.
[0066] Example 5 is an MFI-type zeolite (Si / Al=15), which is a composite oxide of silicon and aluminum. As shown in FIG. 5, the methane conversion rate increased with increasing temperature, while the amount of CO gas produced increased, and the CO selectivity was maintained at a high level of approximately 80%.
[0067] Example 6 is a composite oxide of silicon, aluminum and phosphorus, SAPO-34 (Si / (Al+P+Si)=0.13). As shown in FIG. 6, the methane conversion rate increases with increasing temperature, while the amount of CO gas produced increases, and the CO selectivity can be maintained at a high level of approximately 70%.
[0068] In Comparative Example 1, synthesis gas is produced using zirconium oxide alone. As shown in FIG. 7, as the reaction temperature increases, the CO yield and selectivity of ZrO2 decrease due to the progressive oxidation of CO.
[0069] In Comparative Example 2, synthesis gas is produced using aluminum oxide alone. As shown in FIG. 8, like Comparative Example 1, the CO selectivity is high at low temperatures, but decreases in the high temperature range where the methane conversion rate increases.
[0070] In Comparative Example 3, synthesis gas is produced using tungsten oxide alone. As shown in FIG. 9, even if the reaction temperature increases, the conversion rate itself does not increase.
[0071] Comparative Example 4 is a synthesis gas production using a catalyst in which nickel oxide is supported on zirconium oxide, but as shown in Figure 10, it can be seen that only the combustion reaction proceeds at 500-600°C during the temperature rise (i.e., complete oxidation occurs). This shows that it is better not to include metal species such as Ni as a catalyst for directly partially oxidizing methane.
[0072] Comparative Example 5 is a synthesis gas production using a catalyst in which nickel oxide is supported on silicon oxide as a carrier, but as shown in Figure 11, when the temperature rises from 600°C to 700°C, it can be seen that only the combustion reaction proceeds (i.e., complete oxidation occurs). Even with this combination, it can be seen that it is better not to include metal species such as Ni as a catalyst for direct partial oxidation of methane. [Industrial Applicability]
[0073] According to the production method of the present invention, methane can be partially oxidized with high selectivity, and synthesis gas (CO+H2) can be efficiently produced. Since synthesis gas is important as a raw material for various reactions, the present invention is a technology that can contribute to industry.
Claims
1. A method for producing a synthesis gas by partially oxidizing methane using a composite oxide catalyst that contains at least two of elements from Groups 4 to 6 of the periodic table, or aluminum, silicon, and phosphorus, and has a Co, Ni, and Fe content of less than 0.1 mass%, and a Ru, Rh, Pd, Ir, and Pt content of less than 0.05 mass%, respectively.
2. A composite oxide catalyst for partial oxidation of methane, comprising at least two of elements from Groups 4 to 6 of the periodic table, or aluminum, silicon and phosphorus, and having a Co content, Ni content and Fe content each of less than 0.1 mass%, and a Ru content, Rh content, Pd content, Ir content and Pt content each of less than 0.05 mass%.
3. A method for producing a synthesis gas, comprising the steps of: supporting at least one of elements from Groups 4 to 6 of the periodic table, aluminum, and silicon on an oxide support; and carrying out partial oxidation of methane using a supported oxide catalyst having a Co, Ni, and Fe content each of less than 0.1 mass% and a Ru, Rh, Pd, Ir, and Pt content each of less than 0.05 mass%.
4. The oxide support is Al 2 O 3 , ZrO 2 , TiO 2 , SiO 2 4. The method for producing a synthesis gas according to claim 3, wherein the catalyst is at least one selected from the group consisting of zeolites and zeolites.
5. A composite oxide catalyst for partial oxidation of methane, comprising an oxide support and at least two of elements from Groups 4 to 6 of the periodic table, aluminum, and silicon, the contents of Co, Ni, and Fe being each less than 0.1 mass%, and the contents of Ru, Rh, Pd, Ir, and Pt being each less than 0.05 mass%.
6. The method for producing a synthesis gas according to claim 4, wherein the crystal structure of the zeolite includes at least one selected from the group consisting of AEI, CHA, MFI, and BEA, as determined by the IZA code.
Citation Information
Patent Citations
Hydrocarbon reforming catalyst, hydrocarbon decomposition apparatus, and reformer for fuel cell
JP2004202425A
Fuel reformer and fuel reforming method
JP2006056748A
Partial oxidation catalyst for hydrocarbon, and method and apparatus for manufacturing hydrogen-containing gas using the same
JP2009066520A
Chromium-based catalysts and processes for converting hydrocarbons to synthesis gas
US20020006374A1
Method for preparing H* and CO synthesis gas by using methane partial oxidation device
CN101597030A