Surface roughening method

The pulsed laser irradiation with overlapping areas forms deep grooves and combined protrusions on the metal surface, effectively improving the bonding strength between metal and resin, addressing the inadequacies of previous methods.

JP2024141262APending Publication Date: 2024-10-10KAYABA CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023052804
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing methods for laser-induced surface roughening to enhance bonding between metal and resin do not adequately address the bonding strength issue, necessitating improvements in laser irradiation techniques.

Method used

A surface roughening treatment method involving pulsed laser irradiation with overlapping areas to form deep grooves and protrusions on the metal surface, enhancing bonding by combining protrusions across multiple rows.

Benefits of technology

The method significantly improves the bonding strength between metal and resin by forming deep grooves and protrusions that trap the resin, reducing the likelihood of detachment and enhancing the composite's structural integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141262000001_ABST
    Figure 2024141262000001_ABST
Patent Text Reader

Abstract

To improve a joint strength between a metallic component and a resin component.SOLUTION: A surface roughening method for roughening a joint surface 2 where a metal component 1 joins when joining the metal component 1 and a resin component 11, comprises an irradiation process in which pulse laser L is radiated to the joint surface 2 of the metal component 1 while being linearly moved. In the irradiation process, by overlapping an irradiation region P so as to radiate pulse laser L again to a fusion part 2a of the metal component 1, a groove part 3, and a protrusion 4 projecting from the joint surface 2 of the metal component 1 that is provided on both sides of the groove 3 are formed.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a surface roughening method. [Background technology]

[0002] Patent Document 1 discloses a metal-resin composite formed by bonding a metal member and a resin. The surface of the metal member is roughened by, for example, laser irradiation, to form roughness. As a result, the resin penetrates into the recesses of the metal member, solidifies, and is fixed so that it does not come out of the recesses, thereby bonding the metal member and the resin. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2018-58231 A Summary of the Invention [Problem to be solved by the invention]

[0004] A specific method for the roughening treatment by laser irradiation is not described in Patent Document 1. In the roughening treatment described in Patent Document 1, there is room for improving the bonding strength between the metal member and the resin by adjusting the method and conditions of laser irradiation.

[0005] The present invention has been made in consideration of the above problems, and has an object to improve the bonding strength between a metal member and a resin member. [Means for solving the problem]

[0006] The present invention provides a roughening treatment method for roughening a joining surface of a metal member when joining the metal member to a resin member, comprising an irradiation step of irradiating the joining surface of the metal member while moving a pulsed laser, and in the irradiation step, a groove portion and protrusions provided on both sides of the groove portion and protruding from the joining surface of the metal member are formed by overlapping irradiation areas so that the pulsed laser is irradiated again to the molten portion of the metal member.

[0007] In this invention, the molten part of the metal member that has been irradiated once with a pulsed laser is deformed by overlapping the irradiation areas so that the pulsed laser is irradiated again to the molten part. As a result, unlike the case where the pulsed laser is simply moved and irradiated without overlapping the irradiation areas of the pulsed laser, a deep groove is formed and a protrusion protruding from the joining surface is formed. Therefore, the resin member that has entered the groove and solidified is less likely to come out of the groove, and the joining strength between the metal member and the resin member is improved.

[0008] In addition, the present invention is characterized in that in the irradiating step, the pulse laser is irradiated while being moved across a plurality of rows, and the protrusions formed in each of the plurality of rows are combined with each other.

[0009] In this invention, the multiple rows of protrusions are combined to form a composite protrusion that is higher. Also, when the protrusions are combined across the groove, the composite protrusion makes it difficult for the resin material that has entered the groove and solidified to escape from the groove. Therefore, the bonding strength between the metal member and the resin member is improved. Effect of the Invention

[0010] According to the present invention, the bonding strength between the metal member and the resin member is improved. [Brief description of the drawings]

[0011] [Figure 1] FIG. 2 is a schematic cross-sectional view of a composite body. [Diagram 2]FIG. 2 is a schematic diagram showing an irradiation step of the surface roughening method according to the embodiment of the present invention. [Diagram 3] 1 is a top view of a joining surface of a metal member, showing an irradiated region of a pulsed laser in an irradiation step of a surface roughening method. [Figure 4] FIG. 2 is a schematic cross-sectional view showing irradiation of a first row of pulsed laser. [Diagram 5] FIG. 13 is a schematic cross-sectional view showing irradiation of a second row of pulsed laser. [Figure 6] 10 is a schematic cross-sectional view showing a state in which a groove portion is covered with a synthetic protrusion portion to form a tunnel shape. FIG. [Figure 7] 13 shows optical microscope photographs of the surfaces of metal members that were subjected to a surface roughening treatment method with different numbers of irradiations. [Figure 8] Electron microscope (SEM) photographs of the surfaces of metal members that were subjected to a surface roughening treatment method with different irradiation times. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, a surface roughening method according to an embodiment of the present invention will be described with reference to the drawings.

[0013] The surface roughening method of this embodiment is carried out when forming a composite body 100 in which a metal member 1 and a resin member 11 are joined together, as shown in FIG.

[0014] In this embodiment, the composite 100 is a so-called multi-material formed by combining a metal member 1 and a resin member 11 for the purpose of weight reduction, high strength, etc. The metal member 1 is, for example, iron or aluminum, and the resin member 11 is, for example, any thermoplastic resin that can be injection molded. The surface roughening method of this embodiment is performed to combine the metal member 1 and the resin member 11 to form a multi-material. Note that the materials of the metal member 1 and the resin member 11 are not limited to those mentioned above. In addition, the composite 100 is not limited to a multi-material, and the surface roughening method may be performed when forming a composite 100 that is not a multi-material.

[0015] The roughening treatment method is carried out when the metal member 1 and the resin member 11 are directly joined without using screws, adhesives, etc., and roughens the joining surface 2 of the metal member 1. After the roughening treatment method is carried out on the joining surface 2 of the metal member 1, the molten resin member 11 is poured onto the joining surface 2 of the metal member 1, thereby joining the metal member 1 and the resin member 11 to form a composite 100. The details of the joining of the metal member 1 and the resin member 11 will be described later.

[0016] 2, the surface roughening method is performed using a pulsed laser L that outputs a laser beam at a constant repetition rate. The surface roughening method includes an irradiation step of irradiating a rectangular joining surface 2 of a metal member 1 with the pulsed laser L while moving it linearly.

[0017] FIG. 2 shows a schematic diagram of an irradiation area P of the pulsed laser L. In the irradiation process, first, as shown in FIG. 2(a), the end of the joining surface 2 of the metal member 1 (the back side in FIG. 2) is irradiated with the pulsed laser L while moving it in a straight line. Next, the pulsed laser L is moved in parallel, and as shown in FIG. 2(b), the pulsed laser L is irradiated while moving it in a straight line adjacent to the row irradiated with the pulsed laser L in FIG. 2(a) at a distance so as not to overlap (in other words, so that the irradiation area P does not overlap). Then, the pulsed laser L is moved in parallel, and as shown in FIG. 2(c), the pulsed laser L is irradiated while moving it in a straight line adjacent to the row irradiated with the pulsed laser L in FIG. 2(b) so as not to overlap. In this way, the operation of irradiating while moving the pulsed laser L in a straight line is repeated, and the entire joining surface 2 of the metal member 1 is irradiated with the pulsed laser L. As a result, the joining surface 2 of the metal member 1 is irradiated with the pulsed laser L in multiple parallel rows. As described above, in the irradiation step, the pulsed laser L is irradiated while moving linearly in a plurality of rows in sequence (in sequence from the end of the joining surface 2 of the metal member 1).

[0018] In this specification, the "number of times of irradiation with the pulsed laser L" refers to the number of sets of a series of operations in which the pulsed laser L is irradiated while moving the pulsed laser L in a linear manner, and the entire joining surface 2 of the metal member 1 is irradiated with the pulsed laser L. In other words, the series of operations in Fig. 2(a) to (c) is one set. When the number of times of irradiation with the pulsed laser L is two sets, the pulsed laser L is irradiated while moving the pulsed laser L in a linear manner, and the entire joining surface 2 of the metal member 1 is irradiated with the pulsed laser L, and then the pulsed laser L is irradiated again while moving the pulsed laser L in the same linear manner, and the entire joining surface 2 of the metal member 1 is irradiated with the pulsed laser L. In the irradiation step, the number of times of irradiation with the pulsed laser L is one set or multiple sets.

[0019] 3, in the irradiation step, when the pulsed laser L is moved linearly while irradiating, the irradiation area P of each pulse of the laser irradiated at a constant repetition frequency is made to overlap. In other words, in the irradiation step, the pulsed laser L is moved linearly so that the irradiation areas P of adjacent laser pulses on the joining surface 2 of the metal member 1 partially overlap.

[0020] In addition, when the pulse laser L is irradiated in multiple sets, the irradiation area P of the pulse laser L of the second or subsequent sets may be in the same position as the irradiation area P of the first set of pulse laser L, or may be shifted in the movement direction of the pulse laser L relative to the irradiation area P of the first set of pulse laser L.

[0021] 4 and 5 are schematic cross-sectional views showing how the pulsed laser L is irradiated in a cross section perpendicular to the movement direction of the pulsed laser L. FIG. 4 is a cross-sectional view showing how the first row (the top row in FIG. 3) of pulsed laser L is irradiated, and FIG. 5 is a cross-sectional view showing how the second row (the middle row in FIG. 3) of pulsed laser L is irradiated adjacent to the first row. FIGS. 4(a)-(d) and 5(a)-(d) sequentially show cross sections along the movement direction of the pulsed laser L, and the direction perpendicular to the paper surface in FIGS. 4 and 5 is the movement direction of the pulsed laser L.

[0022] First, the manner in which the first row of pulsed laser L is irradiated will be described. When the joining surface 2 of the metal member 1 is first irradiated with the pulsed laser L as shown in FIG. 4(a), the irradiated irradiation area P is melted by the energy of the pulsed laser L as shown in FIG. 4(b), and a molten part 2a is formed. In the irradiation process, the irradiation area P of each pulse of the pulsed laser L is overlapped, so that the molten part 2a is irradiated with the pulsed laser L again before the molten part 2a solidifies as shown in FIG. 4(c). When the molten part 2a is irradiated with the pulsed laser L again, the molten part 2a is deformed by the impact of the irradiation. Then, the molten part 2a solidifies, and as shown in FIG. 4(d), a groove part 3 and a protrusion part 4 that is provided on both sides of the groove part 3 and protrudes from the joining surface 2 of the metal member 1 are formed. In the irradiation process, a plurality of areas where the irradiation areas P of the pulsed laser L overlap are formed, so that a plurality of shapes shown in FIG. 4(d) are formed. Furthermore, since the interval between the overlapping irradiation regions P in the moving direction of the pulsed laser L is small, the grooves 3 and the protrusions 4 are formed so as to extend in the moving direction of the pulsed laser L.

[0023] Next, the manner in which the second row of pulsed laser L is irradiated will be described. When the second row of pulsed laser L is irradiated first as shown in FIG. 5(a), the irradiated irradiation area P is melted by the energy of the pulsed laser L as shown in FIG. 5(b), and a molten part 2a is formed. When the molten part 2a is irradiated again with the pulsed laser L before it solidifies as shown in FIG. 5(c), the molten part 2a is deformed by the impact of irradiation. The molten part 2a is deformed so as to climb onto the protrusion 4 of the adjacent row (first row). Then, the molten part 2a is solidified, and a composite protrusion 4a is formed by combining adjacent protrusions 4 as shown in FIG. 5(d). The composite protrusion 4a is formed higher from the joining surface 2 than the protrusion 4 that is not combined. In the irradiation process, multiple regions where the irradiated area P of the pulsed laser L overlap are formed, and thus multiple shapes shown in FIG. 5(d) are formed. In addition, since the interval between overlapping irradiated regions P in the moving direction of the pulsed laser L is small, the grooves 3, the protrusions 4, and the composite protrusions 4a are formed to extend in the moving direction of the pulsed laser L.

[0024] Moreover, when the number of times of irradiation with the pulse laser L is increased, the groove portion 3 is formed deeper, and the protrusion 4 and the composite protrusion 4a are formed higher. Furthermore, when the composite protrusion 4a is tilted from the state shown in (d) of FIG. 5, as shown in FIG. 6, it goes over the groove portion 3 and is combined with another protrusion 4 and the composite protrusion 4a. As a result, the groove portion 3 is covered with the composite protrusion 4a, and a tunnel shape is formed. In addition, when the number of times of irradiation with the pulse laser L is multiple sets, it is preferable to perform the second and subsequent sets of irradiation with the pulse laser L before the melted portion 2a formed by the first set of irradiation is solidified. This makes it easier to form the groove portion 3 deeper than when the melted portion 2a is solidified, and makes it easier to form the protrusion 4 and the composite protrusion 4a higher. However, the second and subsequent sets of irradiation with the pulse laser L may be performed after the melted portion 2a formed by the first set of irradiation is solidified.

[0025] In this embodiment, the interval (irradiation interval) between the rows irradiated with the pulsed laser L is set so that a composite protrusion 4a can be formed by combining the protrusions 4 as described above. As shown in Fig. 3, the interval D between the rows irradiated with the pulsed laser L is the interval between the centers of the irradiation regions P of adjacent pulsed lasers L. For example, the interval D is 1 µm to 100 µm, and 50 µm is preferable.

[0026] In this manner, the surface roughening method of this embodiment is carried out. Figures 7 and 8 are optical microscope photographs and scanning electron microscope (SEM) photographs of the joining surface 2 of the metal member 1 subjected to the surface roughening method under the treatment conditions shown below using a pulsed laser L having the specifications shown below. The number of irradiations was three: 1 set, 5 sets, and 15 sets. In Figure 7, the movement direction of the pulsed laser L is the up-down direction of the paper, and in Figure 8, the movement direction of the pulsed laser L is the direction perpendicular to the paper.

[0027] <Pulse laser specifications> - Sales company name and product name: OMRON "MX-Z2000G" Type: MOPA fiber laser Average power output: 20W ·Wavelength: 1.062nm Repetition rate: 10~1000kHz Pulse width: 7.5nsec Spot diameter: approx. 50μm ·Moving speed: 1~12000mm / sec Maximum energy density: approx. 50MW / cm2

[0028] <Processing conditions> Repetition rate: 100kHz Pulse width: 5 ·Moving speed: 100mm / sec ·Irradiation interval: 50μm Energy density: 0.11MW / cm2 Number of irradiations: 1 set, 5 sets, 15 sets

[0029] As shown in Fig. 7 and Fig. 8, it was confirmed that grooves 3 and protrusions 4 were formed by irradiating the joining surface 2 of the metal members 1 with a pulsed laser L. It was confirmed that when the number of irradiations of the pulsed laser L was one set, the grooves 3 and protrusions 4 were formed so as to extend in the moving direction of the pulsed laser L. It was also confirmed that when the number of irradiations of the pulsed laser L was increased to five sets or fifteen sets, the joining surface 2 of the metal members 1 became rougher, and the protrusions 4 (composite protrusions 4a) went beyond the grooves 3 and were combined with other protrusions 4 to extend perpendicularly to the moving direction of the pulsed laser L. It was also confirmed that the grooves 3 were covered with the composite protrusions 4a, and a tunnel shape as shown by A in Fig. 8 was formed.

[0030] After the roughening treatment method is performed in this manner, the molten resin member 11 is poured onto the joining surface 2 of the metal member 1, thereby joining the metal member 1 and the resin member 11 to form a composite body 100. Specifically, when the molten resin member 11 is poured onto the joining surface 2 of the roughened metal member 1, the resin member 11 penetrates into the grooves 3 of the metal member 1 and solidifies as it is. As a result, the resin member 11 is fixed in place so that it does not come out of the grooves 3 of the metal member 1, and the metal member 1 and the resin member 11 are joined together.

[0031] Here, in the roughening treatment method, in the case where the pulsed laser L is simply moved and irradiated without overlapping the irradiation area P of the pulsed laser L, the metal member 1 is only melted, and the molten metal member 1 is removed to form the groove portion 3, as shown in Fig. 4(b). Therefore, a relatively shallow groove portion 3 is formed on the joining surface 2 of the metal member 1, and a protrusion 4 is not formed. In this case, the resin member 11 that has entered the groove portion 3 of the metal member 1 and solidified is likely to come out of the groove portion 3, and the joining strength (specifically, shear joining strength) between the metal member 1 and the resin member 11 may be insufficient.

[0032] In contrast, in the surface roughening method of the present embodiment, the molten portion 2a of the metal member 1 that has been irradiated once with the pulsed laser L is irradiated again with the pulsed laser L, thereby deforming the molten portion 2a. As a result, unlike the case where the pulsed laser L is simply moved and irradiated without overlapping the irradiation area P of the pulsed laser L, the groove portion 3 is formed deep and a protrusion 4 protruding from the joining surface 2 is formed. Therefore, the resin member 11 that has entered the groove portion 3 and solidified is less likely to come out of the groove portion 3, and the joining strength (shear joining strength) between the metal member 1 and the resin member 11 is improved. Furthermore, the surface roughening method of the present embodiment does not require a step of removing the molten portion 2a, thereby reducing the manufacturing cost of the composite 100.

[0033] In addition, in the surface roughening method of this embodiment, the protrusions 4 formed in each of the multiple rows are combined with each other, so that the combined protrusions 4a are formed higher. Therefore, the resin member 11 that has entered the groove portion 3 and solidified is less likely to come out of the groove portion 3, and the bonding strength between the metal member 1 and the resin member 11 is improved. Furthermore, when the protrusions 4 (composite protrusions 4a) are combined with each other beyond the groove portion 3, the groove portion 3 is covered with the composite protrusions 4a, so that the resin member 11 that has entered the groove portion 3 and solidified is less likely to come out of the groove portion 3 due to the composite protrusions 4a. Therefore, the bonding strength between the metal member 1 and the resin member 11 is improved. In other words, in the surface roughening method of this embodiment, the pulse laser L is irradiated while moving (specifically, while moving in parallel) over the multiple rows so that the protrusions 4 formed in each of the multiple rows are combined with each other.

[0034] Furthermore, the roughening treatment method of this embodiment makes it possible to directly bond the metal member 1 and the resin member 11 to form the composite member 100 without using screws, adhesives, etc., thereby improving the strength, airtightness, and design freedom of the composite member 100 and reducing the manufacturing costs of the composite member 100.

[0035] According to the above embodiment, the following advantageous effects are achieved.

[0036] In the roughening method of the present embodiment, the molten portion 2a of the metal member 1, which has been irradiated once with the pulsed laser L and melted, is deformed by overlapping the irradiation regions P so that the molten portion 2a is irradiated again with the pulsed laser L. As a result, the grooves 3 are formed deeply and protrusions 4 protruding from the joining surface 2 are formed, so that the resin member 11 which has entered the grooves 3 and solidified is less likely to come out of the grooves 3, and the joining strength (shear joining strength) between the metal member 1 and the resin member 11 is improved.

[0037] In the roughening method of the present embodiment, the protrusions 4 formed in each of the multiple rows are combined with each other, so that the combined protrusions 4a are formed higher. Furthermore, when the protrusions 4 are combined with each other beyond the grooves 3, the combined protrusions 4a make it more difficult for the resin member 11 that has entered the grooves 3 and solidified to come out of the grooves 3. Therefore, the bonding strength between the metal member 1 and the resin member 11 is improved.

[0038] Next, modified examples of the present embodiment will be described. The following modified examples are also within the scope of the present invention, and it is possible to combine the following modified examples with each of the configurations of the above embodiment, or to combine the following modified examples with each other.

[0039] <Variation 1> In the above embodiment, in the irradiation step, a plurality of rows of the pulsed laser L are irradiated. However, the present invention is not limited to this, and in the irradiation step, only one row of the pulsed laser L may be irradiated while moving linearly. Even with this configuration, the same effects as those of the above embodiment can be achieved.

[0040] <Variation 2> In the above embodiment, in the irradiation step, when the pulse laser L is irradiated while moving linearly, the irradiation regions P of the laser irradiated at a constant repetition frequency are overlapped. In addition, in the moving direction of the pulse laser L, a plurality of regions where the irradiation regions P overlap are formed with a gap. Not limited to this, in the moving direction of the pulse laser L, the regions where the irradiation regions P overlap may be formed continuously without a gap. Furthermore, when the pulse laser L is irradiated while moving linearly, the pulse laser L may be irradiated so that the irradiation regions P are adjacent or separated without overlapping. Even with this configuration, the surface of the metal member 1 can be roughened, and the bonding strength between the metal member 1 and the resin member 11 is improved.

[0041] <Variation 3> In the above embodiment, in the irradiation step, the pulsed laser L is irradiated while moving linearly so as to be adjacent to and spaced apart from the row irradiated immediately before with the pulsed laser L. This is not limited to the above, and in the irradiation step, the pulsed laser L may be irradiated while moving linearly so as to partially overlap the row irradiated immediately before with the pulsed laser L. Also, the pulsed laser L may be irradiated while moving linearly so as to be in contact with the row irradiated immediately before with the pulsed laser L without any space.

[0042] <Variation 4> In the above embodiment, in the irradiation step, the rectangular joining surface 2 of the metal members 1 is irradiated with the pulsed laser L while moving it in a linear manner. However, in the irradiation step, the pulsed laser L does not necessarily have to be irradiated while moving it in a linear manner. For example, the circular joining surface 2 of the metal members 1 may be irradiated with the pulsed laser L while moving it in an arc. In other words, in the irradiation step, the moving direction of the pulsed laser L may be changed depending on the shape of the joining surface 2 of the metal members 1.

[0043] <Variation 5> In the above embodiment, the resin member 11 is, for example, any thermoplastic resin that can be injection molded. Here, in order to improve the bonding strength between the metal member 1 and the resin member 11, the resin member 11 may have a filler. The filler is provided between the protrusions 4 of the metal member 1.

[0044] The configuration, operation, and effects of the embodiment of the present invention will be described below.

[0045] This is a roughening treatment method for roughening a joining surface 2 of a metal member 1 when joining the metal member 1 and a resin member 11, and includes an irradiation step of irradiating the joining surface 2 of the metal member 1 while moving a pulsed laser L, and in the irradiation step, the irradiation area P is overlapped so that the molten portion 2a of the metal member 1 is irradiated with the pulsed laser L again, thereby forming a groove portion 3 and protrusions 4 provided on both sides of the groove portion 3 and protruding from the joining surface 2 of the metal member 1.

[0046] In this configuration, the molten portion 2a of the metal member 1 that has been irradiated once with the pulsed laser L is irradiated again with the pulsed laser L, thereby deforming the molten portion 2a. As a result, unlike the case where the pulsed laser L is simply moved and irradiated without overlapping the irradiation area P of the pulsed laser L, the groove portion 3 is formed deeply and a protrusion 4 protruding from the joining surface 2 is formed. Therefore, the resin member 11 that has entered the groove portion 3 and solidified is less likely to come out of the groove portion 3, and the joining strength between the metal member 1 and the resin member 11 is improved.

[0047] In the irradiation step of the roughening treatment method, the pulsed laser L is moved over a plurality of rows while being irradiated, so that the protrusions 4 formed in each of the plurality of rows are combined with each other.

[0048] In this configuration, the protrusions 4 in multiple rows are combined together to form a higher combined protrusion 4a. In addition, when the protrusions 4 are combined across the grooves 3, the combined protrusions 4a make it difficult for the resin member 11 that has entered the grooves 3 and solidified to come out of the grooves 3. This improves the bonding strength between the metal member 1 and the resin member 11.

[0049] Although the embodiments of the present invention have been described above, the above-mentioned embodiments merely show some of the application examples of the present invention, and it is not intended that the technical scope of the present invention be limited to the specific configurations of the above-mentioned embodiments. [Explanation of symbols]

[0050] 1...metal member, 2...joint surface, 2a...melted portion, 3...groove portion, 4...projection portion, 4a...composite projection portion, 11...resin member, P...irradiation area

Claims

1. A method for roughening a joining surface of a metal member when joining a metal member and a resin member, comprising: An irradiation step of irradiating the joining surface of the metal member with a pulse laser while moving the pulse laser, A roughening treatment method characterized in that in the irradiation process, a groove portion and protrusions provided on both sides of the groove portion and protruding from the joining surface of the metal member are formed by overlapping the irradiation area positions so that the pulse laser is irradiated again to the molten portion of the metal member.

2. The surface roughening method according to claim 1, A surface roughening method, characterized in that in the irradiation step, a pulsed laser is moved across multiple rows while being irradiated, thereby combining the protrusions formed in each of the multiple rows.

Citation Information

Patent Citations

  • Metal-resin composite and method for producing the same

    JP2018058231A