Manufacturing method and manufacturing system for recycled material
By using aqueous ammonia to form an ammonia complex and reduce adhesive force, the method effectively separates electrode composite materials from the base material, ensuring minimal crystal structure changes and cost-effective recycling.
Patent Information
- Application Number
- JP2023052935
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2043-03-29
AI Technical Summary
The challenge in recycling electrodes is the difficulty in separating the electrode composite material from the base material without causing significant changes in the active material's crystal structure, which can lead to the need for resynthesis and increased carbon dioxide emissions.
A method involving contacting the electrode with aqueous ammonia to form an ammonia complex at the interface, reducing adhesive force, allowing the electrode composite material to be peeled off without heating, thus preserving the crystal structure.
This approach enables efficient separation of the electrode composite material from the base material while minimizing structural changes, facilitating easy recycling and reducing processing costs and environmental impact.
Smart Images

Figure 2024141344000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to methods and systems for producing recycled materials. [Background technology]
[0002] JP 2017-084681 A discloses a method for recovering positive electrode materials. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2017-084681 A Summary of the Invention [Problem to be solved by the invention]
[0004] The electrodes contain various renewable materials, and it is being considered to produce renewable materials by recovering the renewable materials from the electrodes.
[0005] The electrode includes a substrate and an electrode mixture. The electrode mixture is attached to the substrate. In the initial stage of the regeneration process, it is required to separate the electrode mixture from the substrate. However, since the electrode mixture is firmly attached to the substrate, it is not easy to separate the electrode mixture from the substrate.
[0006] For example, it has been proposed to promote separation of the electrode mixture from the substrate by heating the electrode (see, for example, Patent Document 1). The electrode mixture may contain an active material and a binder, etc. When the electrode mixture is exposed to high temperatures, components such as the binder may dissolve in the active material. As a result, for example, the crystal structure of the active material may change. If the change in the crystal structure is significant, it may be necessary to resynthesize the active material after the active material is returned to its raw materials (sulfates, oxides, bullion, etc.). The synthesis process of the active material is traced back in the order of sulfates, oxides, and bullion. The further back the synthesis process is traced back, the greater the amount of carbon dioxide generated that may be required to regenerate the active material.
[0007] On the other hand, when the change in the crystal structure is minor, the active material can be regenerated by a simple treatment. This regeneration process is also called "direct recycling." Direct recycling is desirable from the viewpoint of reducing the environmental load.
[0008] Therefore, an object of the present disclosure is to separate an electrode mixture from a substrate while suppressing changes in the crystal structure of the active material. [Means for solving the problem]
[0009] The technical configuration and effects of the present disclosure will be described below. However, the mechanism of action in this specification includes assumptions. The mechanism of action does not limit the technical scope of the present disclosure.
[0010] 1. A method for producing recycled materials includes the following steps (a) to (d) in this order: (a) Providing an electrode including a substrate and an electrode mix. (b) The electrode is placed in contact with ammonia water. (c) Separating the electrode mixture from the substrate. (d) Drying the electrode mixture. In the above (a), the electrode mixture is attached to at least a part of a substrate. The substrate contains aluminum. The electrode mixture contains an active material.
[0011] The surface of the substrate is covered with an oxide film (anodized aluminum). The oxide film may be formed by natural oxidation of Al. The electrode mixture is attached to the surface (oxide film) of the substrate. The electrode has many penetration paths leading to the interface between the electrode mixture and the substrate. When the electrode comes into contact with ammonia water, the ammonia water may penetrate to the interface between the electrode mixture and the substrate. At the interface, ammonia acts on the anodized aluminum, and an ammonia complex may be formed. When an ammonia complex is formed, the adhesive force between the substrate and the electrode mixture may be significantly reduced. Due to the reduction in adhesive force, the electrode mixture may be peeled off from the substrate without heating. That is, the electrode mixture may be separated from the substrate while suppressing changes in the crystal structure of the active material.
[0012] Furthermore, due to the reduced adhesion, the electrode mixture can be peeled off from the substrate in a short time. The short treatment time can also reduce the reaction between ammonia water and Al (dissolution of Al, generation of hydrogen gas, etc.). In other words, the substrate can be recovered in a state that is easy to regenerate.
[0013] If a strong alkaline aqueous solution such as a sodium hydroxide solution is used instead of ammonia water, there is a possibility that dissolution of Al will proceed even for a short period of time.
[0014] 2. The method for producing a recycled material described in "1" above may include, for example, the following configuration: The ammonia water contains 1 to 28% ammonia by mass fraction.
[0015] Hereinafter, unless otherwise specified, the concentration of ammonia water refers to the mass fraction of ammonia. Ammonia water in the concentration range of 1 to 28% is easy to obtain or prepare. Furthermore, in the concentration range of 1 to 28%, undesirable reactions tend not to occur easily. Possible undesirable reactions include, for example, dissolution of Al, generation of hydrogen gas, and elution of Li.
[0016] 3. The method for producing a recycled material according to the above item "1" or "2" may include, for example, the following configuration: The active material includes a lithium metal composite oxide.
[0017] For example, when the electrode mixture contains a water-soluble binder, it is possible to separate the electrode mixture from the substrate in water. However, when the active material (lithium metal composite oxide) comes into contact with a large amount of water, Li may be eluted into the water. That is, the composition of the active material may change. Furthermore, the elution of Li causes an alkaline aqueous solution to be formed. For example, the processing costs may increase due to the recovery of Li from the alkaline aqueous solution and the disposal of the alkaline aqueous solution.
[0018] Ammonia water is inherently alkaline. It is believed that the driving force for the Li elution reaction is small in ammonia water. In other words, it is believed that the Li elution reaction does not proceed easily in ammonia water. Therefore, it is expected that active materials with small composition changes can be recovered. Furthermore, it is expected that the processing cost can be reduced.
[0019] 4. The method for producing a recycled material according to any one of the above items "1" to "3" may include, for example, the following configuration: The above step (b) includes immersing the electrode in ammonia water.
[0020] The electrode and the ammonia water can be brought into contact with each other by any method, including, for example, immersion, coating, spraying, and the like.
[0021] 5. The method for producing a recycled material according to any one of the above items "1" to "4" may include, for example, the following configuration: The above (b) includes applying ammonia water to the electrode.
[0022] 6. The method for producing a recycled material according to any one of the above items "1" to "5" may include, for example, the following configuration: The above (b) includes spraying ammonia water onto the electrode.
[0023] 7. The method for producing a recycled material according to any one of the above items "1" to "6" may include, for example, the following configuration: The above (c) includes imparting momentum to the electrode mixture.
[0024] Since the adhesive force between the electrode mixture and the substrate is reduced, the electrode mixture can be peeled off from the substrate by simply applying a momentum (for example, applying vibration, etc.).
[0025] 8. The method for producing a recycled material according to any one of the above items "1" to "7" may include, for example, the following configuration: The above (d) includes recovering ammonia from gas generated during drying.
[0026] Ammonia water may be regenerated from the recovered ammonia, and the ammonia water may be reused in (b) above.
[0027] 9. The method for producing a recycled material according to any one of the above items "1" to "8" may further include the following (e) and (f) in this order: (e) Separating the active material from the electrode mixture. (f) Regenerating active materials.
[0028] For example, the active material may be isolated from the electrode mixture. After isolation, the active material may be subjected to a regeneration process. In other words, a regenerated material may be produced. Compared to the initial state of the active material, the change in the crystal structure is small, so it is expected that the active material can be regenerated by a simple process. For example, the active material may be regenerated by supplying Li to the active material.
[0029] 10. A manufacturing system produces a regenerated material from an electrode including a substrate and an electrode composite. The manufacturing system includes a contacting device, a separating device, and a drying device. The contacting device is configured to contact the electrode with ammonia water. The separating device is configured to separate the electrode composite from the substrate after the electrode is contacted with the ammonia water. The drying device is configured to dry the electrode composite after the substrate is separated from the electrode composite.
[0030] 11. The production system according to the above item "10" may further include, for example, a recovery device. The recovery device is configured to recover ammonia from the gas generated in the drying device.
[0031] Hereinafter, an embodiment of the present disclosure (hereinafter, may be abbreviated as "the present embodiment") will be described. However, this embodiment does not limit the technical scope of the present disclosure. This embodiment is illustrative in all respects. This embodiment is non-restrictive. The technical scope of the present disclosure encompasses all modifications within the meaning and scope equivalent to the description of the claims. For example, it is also intended from the beginning that any configuration may be extracted from this embodiment and this embodiment, and that they may be combined in any manner. [Brief description of the drawings]
[0032] [Figure 1] FIG. 1 is a schematic flow chart of a method for producing recycled materials in this embodiment. [Diagram 2] FIG. 2 is a conceptual diagram showing a manufacturing system in this embodiment. [Diagram 3] FIG. 3 is a conceptual diagram showing the first system. [Figure 4] FIG. 4 is a conceptual diagram showing the second system. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0033] <Terminology explanation> The terms used in this specification are explained. Terms not explained here may be explained at each use in this specification.
[0034] The words "comprise," "include," "have," and variations thereof (e.g., "consisting of") are open-ended. The open-ended form may or may not include additional elements in addition to the required elements. The words "consisting of" are closed-ended. However, the closed form does not exclude additional elements that are normally associated with the technology or that are unrelated to the technology disclosed. The words "consisting essentially of..." are semi-closed. The semi-closed form allows for the addition of elements that do not substantially affect the basic and novel characteristics of the technology disclosed.
[0035] Expressions such as "may" and "may" are used in the permissive sense, meaning "to have the possibility," rather than in the obligatory sense, meaning "to have to."
[0036] Unless otherwise specified, the order of execution of the steps, operations, and the like included in various methods is not limited to the order described. For example, the steps may proceed simultaneously. For example, the steps may be performed in sequence.
[0037] Elements expressed in the singular form include the plural form unless otherwise specified. For example, "particle" includes not only "one particle" but also "multiple particles (particle group)" and "aggregate of particles (powder, powder)."
[0038] Geometric terms (e.g., "parallel," "perpendicular," "orthogonal," etc.) should not be interpreted in a strict sense. For example, "parallel" may deviate slightly from the strict meaning of "parallel." Geometric terms may include, for example, tolerances, errors, etc. in design, work, manufacturing, etc. The dimensional relationships in each drawing may not match the actual dimensional relationships. To aid the reader's understanding, the dimensional relationships (length, width, thickness, etc.) in each drawing may be changed. Furthermore, some configurations may be omitted.
[0039] Numerical ranges such as "m to n%" include the upper and lower limits unless otherwise specified. That is, "m to n%" indicates a numerical range of "m% or more and n% or less". Furthermore, "m% or more and n% or less" includes "more than m% and less than n%". Furthermore, a numerical value arbitrarily selected from within the numerical range may be set as a new upper or lower limit. For example, a new numerical range may be set by arbitrarily combining a numerical value within the numerical range with a numerical value described in another part of this specification, in a table, in a figure, or the like.
[0040] All numerical values are modified by the term "about". The term "about" may mean, for example, ±5%, ±3%, ±1%, etc. All numerical values may be approximations that may vary depending on the application of the disclosed technology. All numerical values may be expressed in significant figures. Measurements may be average values of multiple measurements unless otherwise specified. The number of measurements may be three or more, five or more, or ten or more. In general, the more measurements are made, the more reliable the average value is expected to be. Measurements may be rounded off based on the number of significant figures. Measurements may include errors associated with, for example, the detection limit of the measurement device.
[0041] The stoichiometric composition formula shows a representative example of a compound. The compound may have a non-stoichiometric composition. For example, "Al2O3" is not limited to a compound having a substance amount ratio (molar ratio) of "Al / O=2 / 3". "Al2O3" indicates a compound containing Al and O in any substance amount ratio unless otherwise specified. Furthermore, for example, the compound may be doped with a trace element. A part of Al and O may be replaced with another element.
[0042] The term "derivative" refers to a compound in which a part of a parent compound has been modified by at least one method selected from the group consisting of introduction of a substituent, substitution of an atom, oxidation, reduction, and other chemical reactions. The modification may be at one or more locations. The "substituent" may include at least one selected from the group consisting of, for example, an alkyl group, an alkenyl group, an alkynyl group, a cycloalkyl group, an unsaturated cycloalkyl group, an aromatic group, a heterocyclic group, a halogen atom (F, Cl, Br, I, etc.), an OH group, an SH group, a CN group, an SCN group, an OCN group, a nitro group, an alkoxy group, an unsaturated alkoxy group, an amino group, an alkylamino group, a dialkylamino group, an aryloxy group, an acyl group, an alkoxycarbonyl group, an acyloxy group, an aryloxycarbonyl group, an acylamino group, an alkoxycarbonylamino group, an aryloxycarbonylamino group, a sulfonylamino group, a sulfamoyl group, a carbamoyl group, an alkylthio group, an arylthio group, a sulfonyl group, a sulfinyl group, a ureido group, a phosphoric acid amide group, a sulfo group, a carboxy group, a hydroxamic acid group, a sulfino group, a hydrazino group, an imino group, and a silyl group. These substituents may be further substituted. When there are two or more substituents, the substituents may be the same or different. A plurality of substituents may be bonded to each other to form a ring. The derivative of the polymer compound (resin material) may also be called a "modified product."
[0043] The "copolymer" includes at least one type selected from the group consisting of an unspecified type, a statistical type, a random type, an alternating type, a periodic type, a block type, and a graft type.
[0044] "D50" refers to the particle size at which the cumulative distribution becomes 50% in the volume-based particle size distribution (cumulative distribution). The particle size distribution can be measured by a laser diffraction method.
[0045] "Recycled materials" refers to materials that can be recovered from electrodes in general. Recycled materials are not limited to active materials. For example, a substrate (e.g., Al foil, etc.) is also a recycled material. An electrode mixture is also a recycled material. Applications of recycled materials are not limited to batteries. Recycled materials may be used for applications other than batteries.
[0046] "Electrode" is a general term for positive electrodes, negative electrodes, and bipolar electrodes. That is, an electrode may be a positive electrode, a negative electrode, or a bipolar electrode. An electrode may be, for example, an electrode of a lithium ion battery. A lithium ion battery may be, for example, a liquid battery, a polymer battery, or an all-solid-state battery. Note that the battery is not limited to a lithium ion battery as long as the substrate of the electrode contains Al.
[0047] The term "lithium metal composite oxide" refers to a compound containing Li, a metal (other than Li), and oxygen. The lithium metal composite oxide may contain, for example, a layered oxide, a polyanion compound, or the like.
[0048] <Manufacturing methods for recycled materials> FIG. 1 is a schematic flow chart of the method for producing a recycled material in this embodiment. Hereinafter, the "method for producing a recycled material in this embodiment" may be abbreviated as "this production method". This production method includes "(a) preparation of an electrode", "(b) contact with ammonia water", "(c) separation" and "(d) drying". This production method may further include, for example, "(e) isolation of an active material" and "(f) regeneration of an active material".
[0049] <(a) Preparation of electrodes> This manufacturing method includes preparing an electrode. The electrode may be obtained from any route. For example, the electrode may be collected from within the battery by dismantling the battery in a discharged state. The battery may be, for example, waste or a defective product. The cause of disposal or defect of the battery may be any. The cause of disposal may be, for example, capacity deterioration, voltage drop, micro-short circuit, resistance increase, etc. For example, an electrode discharged as a defective product in the manufacturing process of the battery may be collected. The cause of defect of the electrode may be any. The cause of defect may be, for example, impurity contamination, poor weight, etc.
[0050] The electrode includes a substrate and an electrode mixture. The substrate may have any shape. The substrate may be, for example, a sheet or plate. The substrate may include, for example, a metal foil, a metal porous body, or the like. The substrate includes Al. The substrate may include, for example, a pure Al foil, an Al alloy foil, or the like. The substrate may include, for example, at least one selected from the group consisting of a 1000-series material, a 2000-series material, a 3000-series material, a 4000-series material, a 5000-series material, a 6000-series material, a 7000-series material, and an 8000-series material. For example, the "1000-series material" refers to an Al material having an alloy number in the 1000s according to "JIS H 4000". The substrate may have a thickness of, for example, 5 to 50 μm. The substrate may have a single-layer structure or a multi-layer structure. For example, the substrate may include a clad material. For example, a Cu foil may be attached to an Al foil to form a clad material.
[0051] The electrode mixture is attached to at least a part of the substrate. The electrode mixture may be attached to the entire surface of the substrate. The electrode mixture may be attached to a part of the surface of the substrate. The electrode mixture may be attached to only one surface of the substrate. The electrode mixture may be attached to both the front and back surfaces of the substrate. The electrode mixture may form a layer. That is, an electrode mixture layer may be formed on the surface of the substrate. The electrode mixture layer may have a thickness of, for example, 10 to 1000 μm.
[0052] The electrode mixture includes an active material. The active material may include, for example, a lithium metal composite oxide. The electrode mixture may further include a conductive material, a binder, a solid electrolyte, and the like. The active material is a particle group. The gaps between the particles serve as a permeation path for the liquid. The active material may have a D50 of, for example, 1 to 30 μm. Details of various materials that may be included in the electrode mixture will be described later.
[0053] <(b) Contact with ammonia water> The manufacturing method includes contacting the electrode with ammonia water. The contact between the electrode and ammonia water allows at least a portion of the ammonia water to penetrate into the interface between the electrode mixture and the substrate. This is because the electrode includes a path for liquid penetration. The penetration of the ammonia water is expected to proceed quickly. An ammonia complex can be formed on the surface of the substrate by the action of the ammonia water on the oxide film (anodized aluminum). The formation of the ammonia complex can significantly reduce the adhesive force between the substrate and the electrode mixture.
[0054] The contact method is arbitrary. For example, the electrode may be immersed in the ammonia water. For example, the electrode may be put into the ammonia water. To promote the contact, for example, the electrode may be shredded and then put into the ammonia water. To promote the contact, for example, the ammonia water may be stirred.
[0055] For example, ammonia water may be applied to the electrode. For example, ammonia water may be applied by a roll coater or the like. For example, a sponge roll or the like may be impregnated with ammonia water. A rotating sponge roll may be pressed against the surface of the electrode (electrode mixture), thereby applying ammonia water to the electrode. Application by a roll coater may be suitable, for example, when the electrode is in a hoop shape.
[0056] For example, ammonia water may be sprayed onto the electrodes using a spray coater or the like.
[0057] Ammonia water includes ammonia and water. Ammonia is dissolved in water. The concentration of a saturated solution at room temperature (20±5°C) is about 35%. Ammonia water may have a concentration of, for example, 0.1 to 35%. Ammonia water may have a concentration of, for example, 1 to 28%. Ammonia water in the concentration range of 1 to 28% is easy to obtain or prepare. Furthermore, in the concentration range of 1 to 28%, undesirable reactions tend not to occur easily. Possible undesirable reactions include, for example, dissolution of Al, generation of H2 gas, and elution of Li. Ammonia water may include, for example, 1 to 28% ammonia, and the balance water. The balance may include, in addition to water, for example, any additive, inevitable impurities, etc. The concentration of ammonia water may be, for example, 3% or more, 5% or more, 10% or more, 15% or more, or 20% or more. The concentration of the aqueous ammonia may be, for example, 25% or less, 20% or less, 15% or less, 10% or less, 5% or less, or 3% or less.
[0058] <(c) Separation> The method includes separating the electrode mixture from the substrate, and since the adhesive strength is reduced by contact with the ammonia water, it is expected that the electrode mixture will be peeled off smoothly from the substrate.
[0059] The separation method is arbitrary. For example, momentum may be imparted to the electrode mixture to promote separation. Momentum may be imparted by any method. For example, at least one selected from the group consisting of vibration, contact, liquid transfer, stirring, and sound waves may be imparted to the mixture (ammonia water and electrodes). "Contact" here refers to physically contacting an object with the target object. Contact includes, for example, an operation of scraping off the electrode mixture with a scraper.
[0060] After separation, the electrode mixture and the substrate may be recovered. Any recovery method may be used. For example, two-stage filtration may be performed. For example, the substrate may be recovered by filtering the first mixture (electrode mixture, substrate, and ammonia water) with, for example, a screen filter. A second mixture (electrode mixture and ammonia water) is formed by separation of the substrate. The electrode mixture may be recovered by filtering the second mixture with, for example, a cakeless filter.
[0061] The filtrate (ammonia water) may be reused. That is, the filtrate may be used as ammonia water in "(b) contact with ammonia water". The filtrate may contain, for example, ammonium carbonate, ammonium fluoride, etc. The ammonium carbonate, ammonium fluoride, etc. may be derived from, for example, a binder, an electrolyte, etc. Ammonium carbonate, ammonium fluoride, etc. may also form a complex with Al. That is, it is expected that ammonium carbonate, ammonium fluoride, etc. may also promote separation of the substrate and the electrode mixture.
[0062] The recovery method is not limited to filtration using a filter. For example, the electrode mixture, the base material, and the ammonia water may be recovered separately using a cyclone separator, a gravity separator, or the like. By separating the base material from the ammonia water in a short time, the reaction between Al and the ammonia water may be reduced. For example, the base material may be separated from the ammonia water (bulk) within 5 minutes.
[0063] <(d) Drying> The present manufacturing method includes drying the electrode mixture. The drying can be performed so that the ammonia water adhering to the electrode mixture is completely volatilized. By completely removing the ammonia water, a cleaning operation such as washing with water can be reduced or simplified.
[0064] The drying method is arbitrary. For example, drying may be performed by at least one selected from the group consisting of hot air, infrared rays, and reduced pressure. The lower the drying temperature, the less change in the crystal structure is expected. The drying temperature may be, for example, 200°C or less, 150°C or less, or 120°C or less. The drying temperature may be, for example, 60°C or more, 80°C or more, or 100°C or more. The "drying temperature" refers to the maximum temperature of the workpiece during drying.
[0065] The production method may include recovering ammonia from the gas generated during drying. The recovered ammonia may be dissolved in water to regenerate ammonia water. For example, high-concentration ammonia water may be recovered by reflux. The high-concentration ammonia water may be diluted to adjust the concentration. The ammonia water may be reused in "(b) contact with ammonia water". Reusing the ammonia water is expected to reduce processing costs.
[0066] <(e) Isolation of active material> The manufacturing method may include separating the active material from the electrode mixture. For example, the active material may be isolated by oxidative decomposition of the binder, conductive material, etc.
[0067] <(f) Regeneration of active materials> The present manufacturing method may include regenerating the active material. In the present manufacturing method, since the change in the crystal structure is small, it is expected that the active material can be regenerated by a simple treatment. For example, a mixture of the active material and a lithium compound (lithium source) may be heated to supply Li to the active material. The lithium compound may include, for example, lithium hydroxide, lithium carbonate, etc.
[0068] <Manufacturing System> FIG. 2 is a conceptual diagram showing a manufacturing system in this embodiment. Hereinafter, "the manufacturing system in this embodiment" may be abbreviated as "this system." This system 100 includes a contact device 110, a separation device 120, and a drying device 130. This system 100 may further include, for example, a recovery device 140, a conveying device (not shown), and the like. Each device constituting this system 100 may be separate and independent. Within this system 100, a plurality of devices may be integrated to form a single device.
[0069] The contact device 110 brings the electrode 10 into contact with the ammonia water 20. The contact device 110 may include, for example, a liquid tank and an agitator. The liquid tank stores the ammonia water 20. The agitator agitates the ammonia water 20. The contact device 110 may include, for example, a coating device. The contact device 110 may include, for example, a roll coater, a spray coater, or the like.
[0070] The separator 120 separates the electrode mixture 12 from the substrate 11 after the electrode 10 comes into contact with the ammonia water 20. The separator 120 may include, for example, a screen filter, a disk filter, a rotary filter, a doctor blade, a scraper, a cyclone separator, a gravity separator, or the like.
[0071] After the substrate 11 and the electrode mixture 12 are separated, the drying device 130 dries the electrode mixture 12. The drying device 130 may include, for example, a hot air drying device, an infrared drying device, a pressure reducing device, or the like.
[0072] The recovery device 140 recovers ammonia from the gas generated in the drying device 130. The recovery device 140 may include, for example, a reflux device or the like. The recovery device 140 may prepare ammonia water from the recovered ammonia. The recovery device 140 may include a circulation device or the like. The circulation device may supply ammonia water to the contact device 110.
[0073] The conveying device may convey the workpiece between each of the devices. For example, the conveying device may convey the workpiece by a roll-to-roll method.
[0074] <First System> Fig. 3 is a conceptual diagram showing the first system. This system 100 (see Fig. 2) may include a first system 101. The first system 101 includes a liquid tank 111, an agitator 112, a screen filter 121, and a filtration device 122. The liquid tank 111 and the agitator 112 constitute a contact device 110 (see Fig. 2). The screen filter 121 and the filtration device 122 constitute a separation device 120 (see Fig. 2).
[0075] The first system 101 may be operated as follows. For example, a discharged battery may be disassembled to recover the electrode 10. The electrode 10 includes a substrate 11 and an electrode mixture 12.
[0076] Ammonia water 20 is stored in the liquid tank 111. The electrode 10 is immersed in the ammonia water 20 in the liquid tank 111, thereby bringing the electrode 10 into contact with the ammonia water 20. The agitator 112 agitates the mixture, thereby promoting the penetration of the ammonia water 20 (contact with the substrate 11). Furthermore, the agitator 112 can impart momentum to the workpiece. The agitator 112 agitates the mixture, thereby promoting the peeling of the electrode mixture 12. The peeled electrode mixture 12 may be pulverized in the liquid. The finely divided electrode mixture 12 may be dispersed in the liquid to form a slurry.
[0077] After the electrode mixture 12 is peeled off from the substrate 11, the screen filter 121 may filter out the substrate 11. Furthermore, the filtration device 122 may filter out the electrode mixture 12. The filtration device 122 may be, for example, of a total amount filtration type or a cross-flow filtration type. The electrode mixture 12 may be dried by a drying device (not shown), so that the total amount of the ammonia water may volatilize.
[0078] <Second System> 4 is a conceptual diagram showing the second system. The system 100 (see FIG. 2) may include the second system 102. The second system 102 includes a coating device 113, a peeling device 123, and a winding device.
[0079] The second system 102 may operate as follows. For example, in a battery manufacturing process, the electrode 10 that is rejected as a defective product is collected. The electrode 10 forms a hoop. The electrode 10 may be wound around a bobbin, for example.
[0080] The winding device corresponds to the conveying device. The winding device conveys the work. The winding device can impart momentum to the work. The winding device includes a delivery roll 151, a first touch roll 152, a second touch roll 153, and a winding roll 154. The delivery roll 151 delivers the electrode 10, and the winding roll 154 winds up the substrate 11. Power may be imparted to both the delivery roll 151 and the winding roll 154. Power may be imparted only to the winding roll 154. The first touch roll 152 and the second touch roll 153 can adjust the difference in tension between the delivery side and the winding side.
[0081] The coating device 113 constitutes the contact device 110 (see FIG. 2). The coating device 113 may include, for example, a sponge roll and a fountain. The sponge roll is impregnated with ammonia water. The fountain may supply the ammonia water to the sponge roll so that the amount of ammonia water impregnated in the sponge roll is maintained within a certain range. The sponge roll comes into contact with the electrode 10, whereby the ammonia water is applied to the surface of the electrode 10. The pair of sponge rolls may simultaneously apply the ammonia water to both the front and back surfaces of the electrode 10.
[0082] The peeling device 123 constitutes the separation device 120 (see FIG. 2). The peeling device 123 may include, for example, a doctor blade or the like. The peeling device 123 may peel off the electrode mixture 12 by contact (external force). For example, a pair of doctor blades may simultaneously scrape off the electrode mixture 12 from both the front and back surfaces. After being scraped off, the electrode mixture 12 may be dried by a drying device (not shown). The entire amount of ammonia water may volatilize due to the drying. After the electrode mixture 12 is peeled off, the substrate 11 may be collected by a winding roll 154.
[0083] <Electrode composite material> The various materials that may be included in the electrode mixture are described in detail below. The electrode material may include, for example, 0.1 to 10% by mass of a binder, 0 to 10% by mass of a conductive material, and the remainder being an active material. The remainder may include, in addition to the active material, a solid electrolyte, various additives, inevitable impurities, and the like. The solid electrolyte may include, for example, Li, sulfur, phosphorus, and the like.
[0084] <Active material> The active material causes an electrode reaction. The active material may be a positive electrode active material or a negative electrode active material. The electrode mixture may contain one type of active material alone or may contain multiple types of active materials. The active material may contain, for example, a lithium metal composite oxide. The lithium metal composite oxide may have any crystal structure.
[0085] The lithium metal composite oxide may have, for example, a crystal structure belonging to the space group R-3m. For example, a compound represented by the general formula "LiMO2" may have a crystal structure belonging to the space group R-3m. The lithium metal composite oxide may have, for example, a composition represented by the following formula (1).
[0086] Li 1-a Ni x M 1-x O2…(1) In the formula, the relationships −0.5≦a≦0.5 and 0≦x≦1 are satisfied. M may include, for example, at least one selected from the group consisting of Co, Mn, and Al.
[0087] In the above formula (1), for example, the relationships of 0 < x ≤ 0.1, 0.1 ≤ x ≤ 0.2, 0.2 ≤ x ≤ 0.3, 0.3 ≤ x ≤ 0.4, 0.4 ≤ x ≤ 0.5, 0.5 ≤ x ≤ 0.6, 0.6 ≤ x ≤ 0.7, 0.7 ≤ x ≤ 0.8, 0.8 ≤ x ≤ 0.9, or 0.9 ≤ x ≤ 1 may be satisfied. For example, the relationships of -0.4 ≤ a ≤ 0.4, -0.3 ≤ a ≤ 0.3, -0.2 ≤ a ≤ 0.2, or -0.1 ≤ a ≤ 0.1 may be satisfied.
[0088] LiMO₂ may include, for example, at least one selected from the group consisting of LiCoO₂, LiMnO₂, LiNi 0.9 Co 0.1 O₂, LiNi 0.9 Mn 0.1 O₂, and LiNiO₂.
[0089] The lithium metal composite oxide may have, for example, the composition of the following formula (2). The compound having the composition of the following formula (2) may also be referred to as "NCM".
[0090] Li 1-a Ni x Co y Mn z O₂…(2) In the formula, the relationships of -0.5 ≤ a ≤ 0.5, 0 < x < 1, 0 < y < 1, 0 < z < 1, and x + y + z = 1 are satisfied.
[0091] In the above formula (2), for example, the relationships of 0 < x ≤ 0.1, 0.1 ≤ x ≤ 0.2, 0.2 ≤ x ≤ 0.3, 0.3 ≤ x ≤ 0.4, 0.4 ≤ x ≤ 0.5, 0.5 ≤ x ≤ 0.6, 0.6 ≤ x ≤ 0.7, 0.7 ≤ x ≤ 0.8, 0.8 ≤ x ≤ 0.9, or 0.9 ≤ x < 1 may be satisfied.
[0092] In the above formula (2), for example, the relationship of 0 < y ≤ 0.1, 0.1 ≤ y ≤ 0.2, 0.2 ≤ y ≤ 0.3, 0.3 ≤ y ≤ 0.4, 0.4 ≤ y ≤ 0.5, 0.5 ≤ y ≤ 0.6, 0.6 ≤ y ≤ 0.7, 0.7 ≤ y ≤ 0.8, 0.8 ≤ y ≤ 0.9, or 0.9 ≤ y < 1 may be satisfied.
[0093] In the above formula (2), for example, the relationship of 0 < z ≤ 0.1, 0.1 ≤ z ≤ 0.2, 0.2 ≤ z ≤ 0.3, 0.3 ≤ z ≤ 0.4, 0.4 ≤ z ≤ 0.5, 0.5 ≤ z ≤ 0.6, 0.6 ≤ z ≤ 0.7, 0.7 ≤ z ≤ 0.8, 0.8 ≤ z ≤ 0.9, or 0.9 ≤ z < 1 may be satisfied.
[0094] NCM is, for example, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, LiNi 0.4 Co 0.3 Mn 0.3 O2, LiNi 0.3 Co 0.4 Mn 0.3 O2, LiNi 0.3 Co 0.3 Mn 0.4 O2, LiNi 0.5 Co 0.2 Mn 0.3 O2, LiNi 0.5 Co 0.3 Mn 0.2 O2, LiNi 0.5 Co 0.4 Mn 0.1 O2, LiNi 0.5 Co 0.1 Mn 0.4 O2, LiNi 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.6 Co 0.3 Mn 0.1 O2, LiNi 0.6 Co 0.1 Mn 0.3 O2, LiNi 0.7 Co 0.1 Mn 0.2 O2, LiNi 0.7 Co 0.2 Mn 0.1 O2, LiNi0.8 Co 0.1 Mn 0.1 O2, and LiNi 0.9 Co 0.05 Mn 0.05 It may contain at least one selected from the group consisting of O2.
[0095] The lithium metal composite oxide may have, for example, the composition of the following formula (3). A compound having the composition of the following formula (3) may also be referred to as "NCA".
[0096] Li 1-a Ni x Co y Al z O2…(3) In the formula, the relationships of -0.5 ≤ a ≤ 0.5, 0 < x < 1, 0 < y < 1, 0 < z < 1, and x + y + z = 1 are satisfied.
[0097] In the above formula (3), for example, the relationships of 0 < x ≤ 0.1, 0.1 ≤ x ≤ 0.2, 0.2 ≤ x ≤ 0.3, 0.3 ≤ x ≤ 0.4, 0.4 ≤ x ≤ 0.5, 0.5 ≤ x ≤ 0.6, 0.6 ≤ x ≤ 0.7, 0.7 ≤ x ≤ 0.8, 0.8 ≤ x ≤ 0.9, or 0.9 ≤ x < 1 may be satisfied.
[0098] In the above formula (3), for example, the relationships of 0 < y ≤ 0.1, 0.1 ≤ y ≤ 0.2, 0.2 ≤ y ≤ 0.3, 0.3 ≤ y ≤ 0.4, 0.4 ≤ y ≤ 0.5, 0.5 ≤ y ≤ 0.6, 0.6 ≤ y ≤ 0.7, 0.7 ≤ y ≤ 0.8, 0.8 ≤ y ≤ 0.9, or 0.9 ≤ y < 1 may be satisfied.
[0099] In the above formula (3), for example, the relationships of 0 < z ≤ 0.1, 0.1 ≤ z ≤ 0.2, 0.2 ≤ z ≤ 0.3, 0.3 ≤ z ≤ 0.4, 0.4 ≤ z ≤ 0.5, 0.5 ≤ z ≤ 0.6, 0.6 ≤ z ≤ 0.7, 0.7 ≤ z ≤ 0.8, 0.8 ≤ z ≤ 0.9, or 0.9 ≤ z < 1 may be satisfied.
[0100] NCA is, for example, LiNi 0.7 Co 0.1 Al 0.2 O2, LiNi0.7 Co 0.2 Al 0.1 O2, LiNi 0.8 Co 0.1 Al 0.1 O2, LiNi 0.8 Co 0.17 Al 0.03 O2, LiNi 0.8 Co 0.15 Al 0.05 O2 and LiNi 0.9 Co 0.05 Al 0.05 O2.
[0101] The lithium metal composite oxide may include, for example, a crystal structure belonging to the space group C2 / m. The lithium metal composite oxide may have, for example, a composition represented by the following formula (4).
[0102] Li2MO3…(4) In the formula, M may include, for example, at least one selected from the group consisting of Ni, Co, Mn, and Fe.
[0103] The lithium metal composite oxide may include, for example, a crystal structure belonging to the space group Fd-3m. The lithium metal composite oxide may have, for example, a composition represented by the following formula (5) or (6).
[0104] LiMn 2-x M x O4…(5) In the formula, the relationship 0≦x≦2 is satisfied. M may include, for example, at least one selected from the group consisting of Ni, Fe, and Zn.
[0105] Li 4+x Ti5O 12 …(6) In the formula, the relationship −1≦x≦3 is satisfied.
[0106] The lithium metal composite oxide may contain, for example, a polyanion compound. The polyanion compound may contain, for example, a phosphate (e.g., LiFePO4, etc.), a silicate, a borate, etc. The polyanion compound may have, for example, a composition represented by the following formula (7), (8), (9), or (10).
[0107] LiMPO4…(7) Li 2-x MPO4F...(8) Li2MSiO4…(9) LiMBO3…(10) In the above formulas (7) to (10), M may, for example, include at least one selected from the group consisting of Fe, Mn, and Co. In the above formula (8), for example, the relationship 0≦x≦2 may be satisfied.
[0108] A dopant may be added to the lithium metal composite oxide. The dopant may be diffused throughout the particle or distributed locally. For example, the dopant may be unevenly distributed on the particle surface. The dopant may be a substitutional solid solution atom or an interstitial solid solution atom. The amount of dopant added (molar fraction relative to the entire active material) may be, for example, 0.01 to 5%, 0.1 to 3%, or 0.1 to 1%. One type of dopant may be added, or two or more types of dopants may be added. Two or more types of dopants may form a complex.
[0109] The dopant may include at least one selected from the group consisting of, for example, B, C, N, halogens, Si, Na, Mg, Al, Mn, Co, Cr, Sc, Ti, V, Cu, Zn, Ga, Ge, Se, Sr, Y, Zr, Nb, Mo, In, Pb, Bi, Sb, Sn, W, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, and actinides.
[0110] <Conductive material> The conductive material can form an electronic conduction path in the electrode mixture. The conductive material can include any component. The conductive material can include at least one selected from the group consisting of graphite, acetylene black (AB), Ketjen Black (registered trademark), vapor grown carbon fiber (VGCF), carbon nanotube (CNT), and graphene flake (GF).
[0111] <Binder> The binder can fix the electrode mixture to the substrate. The binder can include any component. The binder can include at least one selected from the group consisting of, for example, polyvinylidene fluoride (PVdF), vinylidene fluoride-hexafluoropropylene copolymer (PVdF-HFP), polytetrafluoroethylene (PTFE), carboxymethyl cellulose (CMC), alginic acid, polyacrylic acid (PAA), polyacrylonitrile (PAN), polyvinyl alcohol (PVA), polyvinylpyrrolidone (PVP), polyoxyethylene alkyl ether, styrene butadiene rubber (SBR), acrylate butadiene rubber (ABR), acrylic resin, methacrylic resin, and derivatives thereof. [Explanation of symbols]
[0112] 10 electrode, 11 substrate, 12 electrode composite, 20 ammonia water, 100 main system, 101 first system, 102 second system, 110 contact device, 111 liquid tank, 112 stirring device, 113 coating device, 120 separation device, 121 screen filter, 122 filtration device, 123 peeling device, 130 drying device, 140 recovery device, 151 delivery roll, 152 first touch roll, 153 second touch roll, 154 take-up roll.
Claims
1. (a) providing an electrode comprising a substrate and an electrode mix; (b) contacting the electrode with aqueous ammonia; (c) separating the electrode mixture from the substrate; and (d) drying the electrode mixture; in that order, In the above (a), the electrode mixture is adhered to at least a part of the base material, The substrate comprises aluminum, and The electrode mixture includes an active material, How recycled materials are produced.
2. The ammonia water contains 1 to 28% ammonia by mass fraction. A method for producing the recycled material according to claim 1.
3. The active material includes a lithium metal composite oxide. A method for producing the recycled material according to claim 1.
4. The step (b) includes immersing the electrode in the ammonia water. A method for producing a recycled material according to any one of claims 1 to 3.
5. The step (b) includes applying the ammonia water to the electrode. A method for producing a recycled material according to any one of claims 1 to 3.
6. The step (b) includes spraying the ammonia water onto the electrode. A method for producing a recycled material according to any one of claims 1 to 3.
7. The step (c) includes imparting momentum to the electrode mixture; A method for producing a recycled material according to any one of claims 1 to 3.
8. The step (d) includes recovering ammonia from a gas generated during drying. A method for producing a recycled material according to any one of claims 1 to 3.
9. (e) separating the active material from the electrode mix; and (f) regenerating the active material; Further comprising, in this order: A method for producing a recycled material according to any one of claims 1 to 3.
10. 1. A manufacturing system for producing recycled materials from an electrode comprising a substrate and an electrode mix, comprising: A contactor, a separator and a dryer, the contactor is configured to contact the electrode with aqueous ammonia; the separation device is configured to separate the electrode mixture from the substrate after contacting the electrode with the ammonia water; and The drying device is configured to dry the electrode mixture after separation of the substrate and the electrode mixture. Manufacturing system.
11. a recovery device; and The recovery device is configured to recover ammonia from the gas generated in the drying device. The manufacturing system of claim 10.
Citation Information
Patent Citations
Method for efficiently separating metal current collector of positive electrode material of waste lithium ion battery
CN106997972A
Extraction method of metal lithium
CN115744932A
Manufacture of non-sintered type cadmium electrode
JP1991127450A
Method for reprocessing and synthesizing metal oxide positive electrode active material for lithium secondary battery
JP2012064557A
Method for recovering positive electrode material of used lithium ion secondary battery