Method for producing asphalt mixture

By separating and classifying recycled aggregates to reduce old asphalt content and mixing with foamed asphalt and additives, the method produces high-quality asphalt mixtures with enhanced flexibility and durability.

JP2024141753APending Publication Date: 2024-10-10NIPPO CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023053568
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Conventional asphalt mixtures using recycled aggregates often lack sufficient quality due to the degradation of old asphalt, which affects the performance of the mixtures.

Method used

A method involving the separation of old asphalt from recycled aggregates using a separator, followed by classification into different particle sizes, and mixing with foamed asphalt and additives to enhance the quality of the mixture.

Benefits of technology

The method enables the production of high-quality asphalt mixtures with improved flexibility and durability by reducing the amount of old asphalt and maintaining a foamed state, using recycled aggregates effectively.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141753000001_ABST
    Figure 2024141753000001_ABST
Patent Text Reader

Abstract

To provide a method for producing an asphalt mixture containing new asphalt and a recycled aggregate, with which the sufficient quality can be easily obtained.SOLUTION: A method for producing an asphalt mixture of the present invention includes: an old asphalt separation step (S2) of peeling off old asphalt from a surface of a recycled aggregate containing the old asphalt by a separator; and a new asphalt mixing step (S6) of mixing the recycled aggregate after the separation step with new asphalt. Preferably, the new asphalt is foamed asphalt, and the method includes a first classification step (S1) of classifying the recycled aggregate as a base material into a first recycled aggregate having a relatively large particle size and a second recycled aggregate having a relatively small particle size before the separation step (S2), and the separation step (S2) is performed on the first recycled aggregate.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing an asphalt mixture containing a novel asphalt and recycled aggregate. [Background technology]

[0002] Asphalt pavement uses an asphalt mixture made by mixing aggregates such as crushed stone and sand with asphalt as a binder.

[0003] In recent years, as part of efforts to prevent global warming, there has been a demand for lowering (medium-temperature) the manufacturing temperature of asphalt mixtures and the construction temperature during paving. In addition, there is a demand for the density ratio (degree of compaction) at a lower construction temperature to be equal to or greater than the density (standard density) of asphalt pavement when mixed at a normal manufacturing temperature and constructed at a normal construction temperature.

[0004] One of the warm-air technologies is a technology that uses foamed asphalt, which is made by mixing heated asphalt with water to foam it, thereby lowering the manufacturing temperature and construction temperature. For example, Patent Document 1 proposes a method of extending the foaming time of air bubbles by adding an antifoaming agent to the foamed asphalt to make the bubbles finer.

[0005] In recent years, recycled aggregate has been produced by crushing and reusing waste asphalt mixtures applied to the surface and base layers of asphalt pavement. This recycled aggregate is used as a material for asphalt mixtures, and is widely used in asphalt pavement roads by mixing it with new asphalt and new aggregate to produce asphalt mixtures.

[0006] For example, in a conventional method for producing an asphalt mixture, recycled aggregate 100 is heated in a dryer 101 as shown in Fig. 5. The heated recycled aggregate 100 is then charged into a mixer 105 together with heated new fine aggregate 102, coarse aggregate 103, and new asphalt 104, and stirred and mixed to produce an asphalt mixture, which is then laid on the road surface as recycled asphalt pavement.

[0007] Recycled aggregate 100 is made by coating the surface of old aggregate that has become waste with old asphalt. By repeatedly recycling recycled aggregate 100 for asphalt pavement, the old asphalt also repeatedly deteriorates due to reheating during production and ultraviolet rays during use, and so recycled aggregate with poor performance has been increasing in recent years. This causes a problem of the performance of the asphalt mixture using recycled aggregate also decreasing.

[0008] To solve this problem, for example, the recycled aggregate described in Patent Document 2 heats the oil-covered surface with hot air and radiant heat in a rotating drum to promote combustion and deterioration, thereby reducing the amount of oil adhering to the old asphalt. Then, in the subsequent heating process, a recycling additive is added to the recycled aggregate and mixed with new asphalt, improving the performance of the asphalt mixture. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Patent No. 6026035 [Patent Document 2] JP 2009-102883 A Summary of the Invention [Problem to be solved by the invention]

[0010] However, conventional asphalt mixtures using recycled aggregates often do not provide sufficient quality. Therefore, the present invention provides a new asphalt that is likely to provide sufficient quality, and a method for producing an asphalt mixture containing recycled aggregate. [Means for solving the problem]

[0011] The method for producing an asphalt mixture according to the present invention is characterized by including an old asphalt separation step in which the old asphalt is peeled off from the surface of recycled aggregate containing the old asphalt by a separator, and a new asphalt mixing step in which the recycled aggregate after the separation step is mixed with new asphalt.

[0012] According to the present invention, the amount of old asphalt can be reduced by using a separator to peel off the old asphalt on the surface of the recycled aggregate, and the amount of new asphalt can be increased by the amount of the reduced amount of old asphalt.

[0013] That is, since recycled aggregate contains old asphalt, in order to produce an asphalt mixture using recycled aggregate, it is necessary to reduce the amount of newly added asphalt according to the amount of old asphalt contained in the recycled aggregate. In contrast, the method of the present invention can increase the amount of new asphalt and / or effectively regenerate old asphalt, making it easier to obtain an asphalt mixture of sufficient quality.

[0014] In the process of the present invention, the novel asphalt is preferably a foamed asphalt.

[0015] In the past, the use of recycled aggregate has been considered in asphalt mixtures using foamed asphalt. However, when recycled aggregate is used in asphalt mixtures using foamed asphalt, it is difficult to maintain the foamed state, making production difficult.

[0016] Specifically, when using recycled aggregate in producing an asphalt mixture using foamed asphalt, it is necessary to reduce the amount of new asphalt added as foamed asphalt, and there are cases where the amount of foamed asphalt is too small. In contrast, in the production method of the present invention, the amount of old asphalt contained in the recycled aggregate can be reduced, so that a larger amount of foamed asphalt can be contained, and an asphalt mixture containing foamed asphalt and recycled aggregate that is relatively easy to produce and has sufficient quality can be obtained.

[0017] In the method of the present invention, it is preferable to include a first classification step prior to the separation step, in which the base material, recycled aggregate, is classified into a first recycled aggregate having a relatively large particle size and a second recycled aggregate having a relatively small particle size, and the separation step is performed on the first recycled aggregate.

[0018] By classifying the first recycled aggregate from the base material recycled aggregate using a separator, the first recycled aggregate with a relatively large particle size can be reused as aggregate. The first recycled aggregate with a relatively large particle size is easy to peel off the old asphalt, and the amount of old asphalt contained per unit weight is smaller than that of the second recycled aggregate with a relatively small particle size, so it is preferable to pass the first recycled aggregate through a separator and mix it with the foamed asphalt.

[0019] In the method of the present invention, it is preferable to include a second classification step of classifying the recycled aggregate after the separation step into a third recycled aggregate having a relatively large particle size and a fourth recycled aggregate having a relatively small particle size, prior to the mixing step of the new asphalt. It is also preferable to carry out the mixing step of the new asphalt using the third recycled aggregate.

[0020] By using the third recycled aggregate, which contains a smaller amount of old asphalt per unit weight, a larger amount of foamed asphalt can be mixed into the new asphalt, making it easier to maintain the foamed state and resulting in a higher quality asphalt mixture.

[0021] In the present invention, it is preferable to include an aggregate mixing step of mixing the second recycled aggregate with the fourth recycled aggregate.

[0022] Mixing the second recycled aggregate and the fourth recycled aggregate, which have relatively small particle sizes, results in high fluidity because the particle sizes are similar, and when a recycling additive is mixed, the efficiency of recycling the old asphalt can be increased. Substantially all or a part of these can be mixed with the foamed asphalt together with other aggregates from which the old asphalt has been stripped by a separator.

[0023] In the present invention, it is preferable that the aggregate mixing step further includes a step of preparing asphalt mortar in which a recycling additive is mixed, and that the asphalt mortar is further mixed in the new asphalt mixing step.

[0024] The second recycled aggregate and the fourth recycled aggregate have a small particle size and contain a relatively large amount of old asphalt per unit weight, so when the recycling additive is used with these recycled aggregates, the recycling additive works very effectively.

[0025] In the present invention, the regenerating additive preferably contains a fatty acid compound.

[0026] It was found that the use of fatty acid compounds as recycling additives significantly increased the recycling effect of recycled aggregate. Effect of the Invention

[0027] According to the present invention, it is possible to provide a method for producing an asphalt mixture containing foamed asphalt and recycled aggregate, which is relatively easy to produce and has sufficient quality. [Brief description of the drawings]

[0028] [Figure 1] FIG. 1 is a schematic diagram showing a flow of a method for producing an asphalt mixture according to one embodiment of the present invention. [Diagram 2] FIG. [Diagram 3] FIG. 1 is a flow diagram showing a process for producing an asphalt mixture based on recycled aggregate containing old asphalt. [Figure 4] FIG. 1 is a diagram showing a test example of a method for producing an asphalt mixture according to an embodiment. [Diagram 5] FIG. 1 is a schematic diagram showing an apparatus and method for producing an asphalt mixture according to a conventional example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0029] Hereinafter, an apparatus and method for producing an asphalt mixture according to an embodiment of the present invention will be described with reference to the accompanying drawings, FIGS. 1 to 4. FIG.

[0030] First, recycled aggregate is produced by crushing waste asphalt excavated during repair or replacement of existing asphalt pavement to an appropriate size as recycled aggregate to be added to produce asphalt mixture A. The crushed recycled aggregate is used as a base material having an appropriate range of particle size, for example, a particle size (R) of 13 mm to 0 mm. In this specification, the particle size refers to the particle size determined by sieving, which is commonly used in this field as the particle size of aggregate.

[0031] The production apparatus 1 for the asphalt mixture A will be described with reference to Figs.

[0032] 1 shows an apparatus 1 for manufacturing an asphalt mixture A according to an embodiment of the present invention. In the apparatus 1 for manufacturing an asphalt mixture A, recycled aggregate containing old asphalt is used as a base material, and the base material asphalt recycled aggregate B is classified by a classification device consisting of a sieve 2 into a first recycled aggregate (coarse aggregate) a having a particle size of more than 2 mm (for example, a particle size of 13 mm or less and more than 2 mm), i.e., a particle size of more than 2 mm, and a second recycled aggregate (fine aggregate) b having a particle size of 2 mm or less (for example, a particle size of 2 mm or less and more than 0 mm).

[0033] This classification separates the first recycled aggregate from the second recycled aggregate at a particle size of 2 mm, but the particle size at the boundary does not have to be 2 mm and can be, for example, 1 mm, 3 mm, 4 mm, 5 mm, or 6 mm.

[0034] In addition, when the particle size of the boundary is 2 mm, the first recycled aggregate a may contain aggregates with a particle size of 2 mm or less. The first recycled aggregate a contains old asphalt, for example, about 3 mass %, and the second recycled aggregate b contains old asphalt, for example, about 7 mass %.

[0035] The first recycled aggregate a is processed in a separator 5 equipped with a sieve 4 as a classification means and is classified again. The sieve 3 is a device that inputs the first recycled aggregate a and strips off a part of the old asphalt located on its outer periphery. As shown in FIG. 2, the first recycled aggregate a is input into an opening 8 of the sieve 3 from a raw material input port 7, and is rotated at an appropriate speed by a rotating rotor 9. The first recycled aggregate a is scattered into a crushing chamber 10 by centrifugal force through a discharge port 9a of the rotating rotor 9.

[0036] The scattered first recycled aggregate a is dead-stocked on the inner wall of the crushing chamber 10, and when it collides with the next scattered first recycled aggregate a, the old asphalt on the surface is crushed and peeled off, and the particle size is adjusted to a shape close to a sphere. The peeled old asphalt becomes small-diameter granules or powder. In addition, not only the old asphalt on the surface of the first recycled aggregate a but also part of the aggregate part may be crushed and separated as stone powder, etc. By passing through the granulator 3, part of the old asphalt on the surface of the first recycled aggregate a is crushed, peeled off, or stripped away, and separated.

[0037] In order to separate a part of the old asphalt on the surface without crushing the first recycled aggregate a by the granulator 3, the rotor 9 is adjusted to an appropriate peripheral speed, for example, in the range of 10 to 60 m / sec. Preferably, the granulator 3 is set to a peripheral speed of about 20 to 50 m / sec. By selecting an appropriate speed from low to high, the crushing ratio of the first recycled aggregate a can be adjusted. If the time spent in the granulator 3 is long, the fourth recycled aggregate (fine aggregate) bb having a particle size of, for example, 2 mm or less will relatively increase, so the operating time must be adjusted as necessary.

[0038] The first recycled aggregate a that has passed through the sieve 3 is classified again by the sieve 4 into a third recycled aggregate (coarse aggregate) ab having a particle size of more than 2 mm and a fourth recycled aggregate (fine aggregate) bb having a particle size of 2 mm or less. The asphalt content of the third recycled aggregate ab and the fourth recycled aggregate bb is, for example, 2 to 8 mass %, preferably 3 to 6 mass %.

[0039] The manufacturing apparatus 1 for the asphalt mixture A is also equipped with an asphalt storage silo 13 capable of storing and heating new asphalt c, and a mixing kettle 14 for heating and mixing the new asphalt c, the regenerative additive d, the second recycled aggregate b, and the fourth recycled aggregate bb. The mixing kettle 14 has a built-in stirring blade 15. Note that a workability improving agent e may be added in place of the regenerative additive d, or together with the regenerative additive d.

[0040] In the present invention, the asphalt mixed in the mixing vessel 14 is, for example, foamed asphalt, and foaming of the foamed asphalt may be performed in the mixing vessel 14, or may be performed in a foaming device or the like installed in the silo 13 or in the supply pipe connecting the silo 13 and the mixing vessel 14. Foamed asphalt can be produced by a well-known method, and can be obtained, for example, by adding water and, optionally, a foaming auxiliary to heated asphalt and foaming the asphalt.

[0041] When preparing foamed asphalt in the mixing vessel 14, recycled aggregate, etc. can be added after the new asphalt c is mixed with water, etc. to prepare foamed asphalt in the mixing vessel 14. Also, when foamed asphalt is charged into the mixing vessel 14, recycled aggregate, etc. can be added to the foamed asphalt.

[0042] The foamed asphalt foamed in the silo 13 may be fed into the mixer 18 without going through the mixing kiln 14 and mixed with the coarse aggregate and asphalt mortar.

[0043] The manufacturing apparatus 1 is also provided with a mixer 18 that mixes the asphalt mortar produced by mixing in the mixing tank 14 with the third recycled aggregate ab using a mixing blade 19. The mixer 18 produces an asphalt mixture A. In this specification, the asphalt mortar refers to the asphalt mixture before the coarse aggregate is mixed therein.

[0044] Next, a method for producing the asphalt mixture A using the production apparatus 1 for producing the asphalt mixture A will be described with reference to a flow diagram using blocks shown in FIG. 1 and FIG.

[0045] In Fig. 3, asphalt recycled aggregate B is classified by sieve 2 into first recycled aggregate (coarse aggregate) a with a particle size of more than 2 mm and second recycled aggregate (fine aggregate) b with a particle size of 2 mm or less (step S1: first classification step). The first recycled aggregate a may contain particles with a particle size of 2 mm or less. The first recycled aggregate a contains old asphalt at, for example, about 3% by mass, and the second recycled aggregate b contains old asphalt at, for example, about 7% by mass.

[0046] Next, in FIG. 3, the first recycled aggregate a is processed and classified in a separator 5 equipped with a granulator 3 and a sieve 4. First, the first recycled aggregate a is fed into the granulator 3 to crush and peel off the old asphalt part on the surface (step S2: separation process). For example, if the first recycled aggregate a has sharp asphalt parts, it is likely to crack or chip, so the particle size can be smoothed by feeding it into the granulator 3 to peel off the sharp parts and corners. The peeled old asphalt on the surface becomes powder or fine particles and is separated from the first recycled aggregate a, and the first recycled aggregate a is sized so that the corners and sharp parts are scraped off to approximate a smooth curved shape. In addition, some of the aggregate exposed on the surface may be crushed together with the old asphalt to become fine aggregate, stone powder, etc.

[0047] The first recycled aggregate a crushed by the granulator 3 is classified again by the sieve 4 (step S3: second classification step) into third recycled aggregate ab with a particle size of over 2 mm from which the old asphalt has been stripped, and fourth recycled aggregate bb with a particle size of 2 mm or less. In this case, the third recycled aggregate ab contains less old asphalt than the first recycled aggregate a.

[0048] Next, in the mixing tank 14, the second recycled aggregate b and the fourth recycled aggregate bb, which have been classified to the same degree (grain size 2 mm or less), are mixed (step S4: aggregate mixing process). In this case, the fourth recycled aggregate bb contains old asphalt powder and the like because the old asphalt has been peeled off from the first recycled aggregate a by the granulator 3. Therefore, the mixture of the second recycled aggregate b and the fourth recycled aggregate bb has a fine grain size, improved fluidity, and high asphalt regeneration efficiency. In addition, since these contain a relatively large amount of old asphalt, the old asphalt can be effectively regenerated when a regeneration additive is used. On the other hand, the final asphalt mixture may be produced without using the entire amount of the fourth recycled aggregate bb obtained by this classification.

[0049] Next, foamed asphalt, for example new asphalt c, is fed from the asphalt storage silo 13 into the mixing vessel 14 and mixed with the mixture of the second recycled aggregate b and the fourth recycled aggregate bb (step S5: asphalt mortar preparation process). This allows for the production of high-quality asphalt mortar with high fluidity. As described above, the foamed asphalt may be prepared in the mixing vessel 14 before mixing with the recycled aggregate, or may be prepared in a foaming device or the like installed in the supply pipe and then mixed into the mixing vessel 14.

[0050] In addition to the new asphalt c, one or both of the regeneration additive d and the workability improving agent e can be added and mixed. By adding these oily components, a high-quality asphalt mortar with fine grain size, high flexibility and fluidity can be produced (step S5).

[0051] The old asphalt in the base material, recycled asphalt aggregate B, has hardened due to aging, but the mixture of second recycled aggregate b and fourth recycled aggregate bb contains fine-grained old asphalt, sand, stone powder, etc. Therefore, by mixing new asphalt c, recycling additive d, and / or workability improvement agent e, a high-quality asphalt mortar with fine grain size and improved fluidity and flexibility can be produced. This can be used as a finished product or by adding other materials for paving and repair work.

[0052] Any regenerating additive known in the art can be used, but it is particularly preferred to use one containing a fatty acid compound.

[0053] The fatty acid compound is preferably a compound represented by the following formula (I) (hereinafter also referred to as compound (I)). R 11 -COO-(AO)mR 12 (I) (In the formula, R 11 is a linear, branched or cyclic hydrocarbon group having 1 to 24 carbon atoms which may have a substituent; R 12represents a hydrogen atom or a methyl group, AO represents a linear or branched oxyalkylene group having 2 to 4 carbon atoms, and m represents the number of moles of the oxyalkylene group added, which is 0 or a number from 1 to 30. In formula (II), R 11 The number of carbon atoms is preferably 6 to 24, more preferably 8 to 20, further preferably 10 to 18, and particularly preferably 12 to 16. In formula (II), m is preferably 0 or an integer of 1 to 25, more preferably 0 or an integer of 1 to 20, and further preferably 0 or an integer of 1 to 15. In formula (II), AO is preferably an oxyethylene group.

[0054] As the fatty acid compound, for example, a fatty acid compound having an iodine value of 50 to 110, 60 to 100, or 70 to 90 can be used. These may be a combination of a plurality of fatty acid compounds, and in this case, the above iodine value refers to the value of the fatty acid compound in which a plurality of compounds are combined. The iodine value of the fatty acid compound is the iodine value measured in accordance with JIS K0070-1992.

[0055] The fatty acid compound represented by formula (I) is preferably a fatty acid, a fatty acid alkyl ester, a fatty acid polyoxyalkylene alkyl ester, or a polyoxyalkylene fatty acid ester, which may be used alone or in combination of two or more selected from these.

[0056] The molecular weight (g / mol) of the fatty acid compound may be, for example, 100 or more, 150 or more, 200 or more, 250 or more, 270 or more, or 280 or more, and may be 500 or less, 450 or less, 400 or less, 350 or less, 330 or less, or 320 or less. When the fatty acid compound is used in combination with multiple compounds, these molecular weights may be weight average molecular weights.

[0057] Compound (I) includes fatty acids: R 11 COOH, fatty acid methyl ester: R 11 COOCH3, fatty acid (poly)oxyethylene methyl ester: R 11COO(CH2CH2O) m CH3, (poly)oxyethylene fatty acid ester: R 11 COO(CH2CH2O m Examples include H.

[0058] Specific examples include palmitic acid, palmitic acid methyl ester, palmitic acid (poly)oxyethylene methyl ester (average number of moles added: 1 to 15), (poly)oxyethylene palmitic acid ester (average number of moles added: 1 to 15), stearic acid, stearic acid methyl ester, stearic acid (poly)oxyethylene methyl ester (average number of moles added: 1 to 15), (poly)oxyethylene stearic acid ester (average number of moles added: 1 to 15), oleic acid, oleic acid methyl ester, oleic acid (poly)oxyethylene methyl ester ester (average number of moles added: 1 to 15), (poly)oxyethylene oleate (average number of moles added: 1 to 15), linoleic acid, linoleic acid methyl ester, linoleic acid (poly)oxyethylene methyl ester (average number of moles added: 1 to 15), (poly)oxyethylene linoleate (average number of moles added: 1 to 15), linolenic acid, linolenic acid methyl ester, linolenic acid (poly)oxyethylene methyl ester (average number of moles added: 1 to 15), (poly)oxyethylene linolenate (average number of moles added: 1 to 15).

[0059] Next, the produced asphalt mortar is fed from the mixing tank 14 into the mixer 18, and the third recycled aggregate ab having a particle size of more than 2 mm is fed into the mixer 18 and mixed to produce the asphalt mixture A (step S6: new asphalt mixing step). The third recycled aggregate ab is a coarse aggregate containing a small amount of old asphalt, and by mixing it with the high-quality produced asphalt mortar, an asphalt mixture A that is less likely to crack and has high fatigue durability can be obtained. Note that a workability improving agent may be added during the production of the asphalt mixture A.

[0060] The asphalt mixture A obtained by mixing for a predetermined time with the mixing blades 19 in the mixer 18 is, for example, dropped into a dump truck 20 and transported to an asphalt pavement construction site. Alternatively, the asphalt mixture A may be discharged directly from the mixer 18 at the construction site and used for construction.

[0061] In the present invention, since foamed asphalt is used to produce an asphalt mixture, the temperature inside the mixer 18 can be lower than usual, i.e., 160°C or less, 155°C or less, 150°C or less, or 140°C or less, and can be 100°C or more, 120°C or more, 130°C or more, or 140°C or more.

[0062] As described above, according to the manufacturing method of the asphalt mixture A of this embodiment, the old asphalt on the surface can be partially peeled off from the first recycled aggregate a, which is a relatively large particle size obtained by classifying the base material, the recycled asphalt aggregate B, by the granulator 3. This allows classification into the third recycled aggregate ab, which has a particle size of more than 2 mm, and the fourth recycled aggregate bb, which contains a large amount of fine old asphalt having a particle size of 2 mm or less. Therefore, by mixing the fourth recycled aggregate bb with the second recycled aggregate b, an asphalt mortar with high flexibility and durability can be manufactured.

[0063] Furthermore, by mixing it with the third recycled aggregate ab, which contains almost no old asphalt, a high-quality asphalt mixture A with high flexibility and fatigue resistance can be produced.

[0064] Next, test examples carried out on the manufacturing method of the asphalt mixture A according to the above-mentioned embodiment will be described with reference to FIG.

[0065] In FIG. 4, the recycled aggregate B as the base material has a particle size of, for example, 13 mm to 0 mm, and contains 5.4% asphalt by mass. Here, the particle size that is the boundary between classification is 5 mm instead of 2 mm, and this recycled aggregate is classified by sieve 2 into a first recycled aggregate a (particle size 13 mm to over 5 mm) with a large particle size and a second recycled aggregate b (particle size 5 mm to 0 mm) with a small particle size. The first recycled aggregate a with a large particle size is 40% by mass, and the second recycled aggregate b with a small particle size is 60% by mass. The ratio of the amount of old asphalt to the amount of the second recycled aggregate b is 6.5% by mass, and 3.9% by mass with respect to the entire recycled aggregate. Since the amount of old asphalt in the recycled aggregate before classification is 5.4% by mass, the content ratio is 72%.

[0066] The amount of old asphalt in the first recycled aggregate a with a large particle size is 3.8% by mass, and 1.5% by mass in the total recycled aggregate. The first recycled aggregate a is fed into the granulator 3 of the separator 5 to be peeled off, and is further classified into the third recycled aggregate ab with a large particle size (particle size 13 mm to over 5 mm) and the fourth recycled aggregate bb with a small particle size (particle size 5 mm to 0 mm) using the sieve 4 of the separator 5. Moreover, the ratio of the amount of asphalt in the second recycled aggregate b and the fourth recycled aggregate bb (particle size 5 mm to 0 mm) with a small particle size classified using the sieve 4 of the separator 5 to the asphalt recycled aggregate B of the base material is 4.7% by mass / 5.4% by mass x 100 = 87%.

[0067] As a result, the large particle size was 25% by mass, and the small particle size was 75% by mass. The large particle size had an old asphalt content of 2.7% by mass, and the amount of old asphalt was 0.7% by mass relative to the entire recycled asphalt aggregate B. The small particle size had an old asphalt content of 6.3% by mass, and the amount of old asphalt was 4.7% by mass relative to the entire recycled aggregate.

[0068] The change in asphalt amount in this test example is shown in Table 1 below. The asphalt amount is indicated by the As amount.

[0069] [Table 1]

[0070] The method for producing asphalt mixture A according to the present invention is not limited to the above-mentioned embodiment, and the configuration of the above-mentioned embodiment can be appropriately replaced or modified without departing from the gist of the present invention. Below, the asphalt mixture A according to this embodiment and a modified example of the method for producing the same will be described, but the same reference numerals will be used to describe the same or similar parts as those in the above-mentioned embodiment.

[0071] For example, in the method for producing an asphalt mixture according to the present embodiment, the produced asphalt mortar can be used as a surface treatment material for pavement surfaces. This makes it possible to extend the life of the pavement surface at low cost. The asphalt mortar is included in the asphalt mixture.

[0072] In addition, in the above-described embodiment, the first recycled aggregate a is separated by peeling off the old asphalt on the surface using a granulator 3, but the means for separating the old asphalt is not limited to the granulator 3 and any appropriate separator such as a crusher or crusher can be used.

[0073] In this embodiment, the asphalt recycled aggregate B as the base material and the first recycled aggregate a are classified into relatively large recycled aggregates with a particle size of 13 mm to over 2 mm and relatively small recycled aggregates with a particle size of 2 mm to 0 mm by the sieves 2 and 4 as classification means. However, the classification of the particle size is not limited to the above embodiment, and the recycled aggregates can be classified into appropriate particle sizes. [Explanation of symbols]

[0074] 1. Asphalt mixture manufacturing equipment 2, 4 sieves 3 Graining machine 5 Separation device 13 Asphalt storage silo 14 Mixing pot 18 Mixer A Asphalt mixture a. First recycled aggregate B. Recycled asphalt aggregate b. Secondary recycled aggregate ab The third recycled aggregate bb The fourth recycled aggregate c New asphalt d. Regeneration additives e. Workability improvement agent

Claims

1. A separation process of the old asphalt, in which the old asphalt is peeled off from the surface of the recycled aggregate containing the old asphalt by a separator; and A new asphalt mixing step of mixing the recycled aggregate after the separation step with new asphalt. A method for producing an asphalt mixture comprising the steps of:

2. The method for producing an asphalt mixture according to claim 1, wherein the novel asphalt is foamed asphalt.

3. 3. The method for producing an asphalt mixture according to claim 2, further comprising a first classification step of classifying the base material, recycled aggregate, into a first recycled aggregate having a relatively large particle size and a second recycled aggregate having a relatively small particle size prior to the separation step, and the separation step is performed on the first recycled aggregate.

4. The method for producing an asphalt mixture according to claim 3, further comprising a second classification step of classifying the recycled aggregate after the separation step into a third recycled aggregate having a relatively large particle size and a fourth recycled aggregate having a relatively small particle size, prior to the mixing step of the new asphalt.

5. The method for producing an asphalt mixture according to claim 4, wherein the mixing step of the new asphalt is carried out using the third recycled aggregate.

6. The method for producing an asphalt mixture according to claim 4, further comprising an aggregate mixing step of mixing the second recycled aggregate with the fourth recycled aggregate.

7. The method for producing an asphalt mixture according to claim 6, further comprising the step of preparing an asphalt mortar by further mixing a regenerating additive in the aggregate mixing step, and further mixing the asphalt mortar in the new asphalt mixing step.

8. The method for producing an asphalt mixture according to claim 7, wherein the rejuvenating additive comprises a fatty acid compound.

Citation Information

Patent Citations

  • Production of acrylonitrile polymer powder

    JP1985026035A

  • Method of manufacturing asphalt mixture

    JP2009102883A