Evaluation method and operation method
By evaluating and controlling the sulfidation reaction of metallic copper within the reaction shaft using temperature and partial pressure data, the method enhances the efficiency of copper smelting by improving the matting reaction rate.
Patent Information
- Application Number
- JP2023054105
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2043-03-29
AI Technical Summary
The behavior of metallic copper within the reaction shaft of a copper smelting flash smelting furnace is not fully understood thermodynamically and kinetically, making it difficult to efficiently matte metallic copper.
An evaluation method that acquires temperature distribution, partial pressure of sulfur gas, and trajectory and flow rate of metallic copper particles to calculate reaction rates in multiple regions, and an operation method that controls reactor conditions based on these calculations to enhance the sulfidation reaction of metallic copper.
Enables efficient evaluation and control of the sulfidation reaction of metallic copper, increasing the matting reaction rate and overall efficiency of copper smelting processes.
Smart Images

Figure 00000000_0000_ABST 
Figure 00000000_0001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an evaluation method and an operating method. [Background technology]
[0002] In the reaction shaft of a copper smelting flash furnace, starting materials such as copper concentrate, recycled materials, and solvents are fed from a concentrate burner along with reaction gas. The reaction gas causes an oxidation reaction of the starting materials, producing matte and slag at the bottom of the reaction shaft. It is necessary to understand what reactions are occurring in the starting materials in this reaction shaft (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2011-075228 A Summary of the Invention [Problem to be solved by the invention]
[0004] In recent years, the ratio of recycled materials to raw materials has been increasing. Copper exists mainly as metallic copper in recycled materials. It is preferable that metallic copper is sulfided in the reaction shaft and becomes matte. However, the behavior of metallic copper in the reaction shaft has not been fully elucidated in terms of thermodynamics and reaction kinetics. For this reason, it has been difficult to efficiently turn metallic copper into matte.
[0005] The present invention has been made in view of the above problems, and has an object to provide an evaluation method and an operating method capable of evaluating the sulfidation reaction of metallic copper. [Means for solving the problem]
[0006] The evaluation method according to the present invention is characterized by comprising the steps of: acquiring the temperature distribution, the partial pressure of the sulfur gas, and the trajectory and flow velocity of metallic copper particles inside a reactor that sulfurizes metallic copper by reacting the metallic copper with sulfur gas; dividing the reactor into a plurality of regions based on the temperature distribution and the partial pressure of the sulfur gas, and acquiring the reaction rate per unit time of the sulfurization of the metallic copper for each of the plurality of regions; calculating the reaction rate of the metallic copper particles for each region through which the metallic copper particles pass based on the trajectory and flow rate of each of the metallic copper particles, and integrating the reaction rates of the metallic copper particles to calculate the final reaction rate of each of the metallic copper particles after passing through the reactor; and calculating the final reaction rate of the entire reactor from the results of the final reaction rates of the plurality of metallic copper particles charged into the reactor.
[0007] In the above evaluation method, the step of acquiring the reaction rate for each of the multiple regions includes a step of acquiring the reaction rate per unit time for each of the multiple regions and for each particle size of the metallic copper, and the step of calculating the final reaction rate for each metallic copper particle may include a step of calculating the reaction rate of the metallic copper particle according to the particle size of the metallic copper particle when calculating the reaction rate for each region through which the metallic copper particle passes based on the trajectory and flow velocity of each metallic copper particle, and a step of calculating the final reaction rate for each metallic copper particle by integrating the reaction rates of the metallic copper particles.
[0008] In the above evaluation method, the step of acquiring the reaction rate for each of the multiple regions includes a step of acquiring a particle size distribution of the metallic copper charged into the reactor, and the step of calculating the final reaction rate for each of the metallic copper particles includes a step of determining multiple representative particles representative of the metallic copper particles charged into the reactor, a step of calculating the reaction rate of each of the representative particles in accordance with a ratio of the particle size distribution when calculating the reaction rate for each region through which each of the representative particles passes based on the trajectory and flow velocity of each of the representative particles, and a step of calculating the final reaction rate of each of the representative particles after passing through the reactor by integrating the reaction rates of each of the representative particles, and the step of calculating the final reaction rate in the entire reactor may be a step of determining the final reaction rate of the entire reactor from a result of the final reaction rates of each of the multiple representative particles charged into the reactor.
[0009] In the above evaluation method, the step of acquiring the temperature distribution, the partial pressure of the sulfur gas, and the trajectory and flow velocity of the metallic copper particles may be a step of acquiring the temperature distribution, the partial pressure, and the trajectory and flow velocity by simulation.
[0010] In the above evaluation method, the step of acquiring the response rate for each of the plurality of regions may include the step of acquiring the response rate for each of the plurality of regions by a test.
[0011] In the above evaluation method, the step of calculating the final reaction rate in the entire reactor may be a step of calculating the final reaction rate in the entire reactor from the result of the final reaction rates of all of the metallic copper particles charged into the reactor.
[0012] In the above evaluation method, the reaction apparatus may be a reaction shaft of a flash smelting furnace, the metallic copper is matted in the reaction shaft by sulfidation, the step of acquiring the reaction rate for each of the plurality of regions may be a step of acquiring a reaction rate at which the metallic copper mattes per unit time for each of the plurality of regions of the reaction shaft, the step of calculating the final reaction rate for each metallic copper particle may be a step of calculating a matte rate for each metallic copper particle, and the step of calculating the final reaction rate in the entire reaction apparatus may be a step of calculating a matte rate in the entire reaction apparatus.
[0013] The operating method according to the present invention is characterized by comprising the steps of: acquiring the temperature distribution, the partial pressure of the sulfur gas, and the trajectory and flow velocity of metallic copper particles inside a reactor that sulfurizes metallic copper by reacting the metallic copper with sulfur gas; dividing the reactor into a plurality of regions based on the temperature distribution and the partial pressure of the sulfur gas, and acquiring the reaction rate per unit time of the sulfurization of the metallic copper for each of the plurality of regions; calculating the final reaction rate of each metallic copper particle after passing through the reactor by calculating and integrating the reaction rate for each region through which the metallic copper particle passes based on the trajectory and flow rate of each metallic copper particle; calculating the final reaction rate of the entire reactor from the result of the final reaction rates of the plurality of metallic copper particles charged into the reactor; and controlling the operating conditions of the reactor based on the final reaction rate of the entire reactor.
[0014] In the above operating method, the step of controlling the operating conditions may include a step of controlling a partial pressure of the sulfur gas in the reaction apparatus.
[0015] In the above operating method, the step of controlling the operating conditions may include a step of controlling the particle size of the raw material fed into the reactor based on a final reaction rate in the entire reactor.
[0016] In the above operation method, the reactor may be a reaction shaft of a flash smelting furnace, and the step of controlling the operating conditions may be a step of controlling the operating conditions of the flash smelting furnace. Effect of the Invention
[0017] According to the present invention, it is possible to provide an evaluation method and an operating method capable of evaluating the sulfidation reaction of metallic copper. [Brief description of the drawings]
[0018] [Figure 1] FIG. 1 is a diagram showing a schematic configuration of a flash furnace for copper smelting according to an embodiment. [Diagram 2] FIG. 2 is a diagram illustrating details of a concentrate burner. [Diagram 3] FIG. 3 is a flowchart illustrating a process according to the embodiment. [Figure 4] 4(a) and 4(b) are flow charts illustrating the process according to the embodiment. [Diagram 5] FIG. 5 is a diagram illustrating the results of the simulation. [Figure 6] FIG. 6 is a diagram illustrating the results of the simulation. [Figure 7] FIG. 7 is a diagram illustrating the results of the simulation. [Figure 8] FIG. 8 is a diagram illustrating the results of the simulation. [Figure 9] FIG. 9 is a diagram illustrating the results of the simulation. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] (Embodiment) FIG. 1 is a diagram showing a schematic configuration of a flash smelting furnace 100 for copper smelting according to an embodiment. As shown in FIG. 1, the flash smelting furnace 100 includes a reaction shaft 1 in which concentrate and reaction gas are mixed, a settler 2, and an uptake 3. A concentrate burner 4 is provided on the ceiling of the reaction shaft 1. The concentrate burner 4 supplies a reaction main blast gas, a reaction auxiliary gas, and a dispersion gas (which also contributes to the reaction) into the reaction shaft 1 together with copper concentrate, solvent, recycled raw materials, etc. (hereinafter, these solid raw materials are referred to as starting materials). For example, the reaction main blast gas and the reaction auxiliary gas are oxygen-enriched air, and the dispersion gas is air or oxygen-enriched air.
[0020] When the starting material is fed into the reaction shaft 1 from the concentrate burner 4, the copper concentrate containing sulfides undergoes an oxidation reaction according to the following reaction formula (1) and separates into matte 5 and slag 6 at the bottom of the reaction shaft 1. In the following reaction formula (1), Cu2S·FeS corresponds to the main component of matte 5, and FeO·SiO2 corresponds to the main component of slag 6. Silica ore is used as the solvent. CuFeS2+SiO2+O2→Cu2S·FeS+FeO·SiO2+SO2+ Reaction heat (1) The matte 5 is processed, for example in a converter, to produce metallic copper.
[0021] FIG. 2 is a diagram illustrating the details of the concentrate burner 4, and is an explanatory diagram showing the input section 10 that inputs the starting material, the main reaction gas, the auxiliary reaction gas, and the dispersion gas into the reaction shaft 1.
[0022] The input section 10 of the concentrate burner 4 is provided with a lance 16, and a first passage 11 through which the dispersion gas passes and a fourth passage 14 through which the reaction auxiliary gas passes are formed in the lance 16. The fourth passage 14 is provided in the center of the lance 16, and the first passage 11 is provided around the fourth passage 14. The input section 10 is also provided with a second passage 12 as a raw material flow path provided on the outside of the lance 16, more specifically on the outer periphery of the lance 16. The input section 10 further includes a third passage 13 provided on the outside of the second passage 12, more specifically on the outer periphery of the second passage 12, through which the reaction main blast gas passes. The third passage 13 is formed by a tubular portion provided so as to surround the second passage 12, and communicates with a funnel-shaped air chamber 17 provided above it. The second passage 12 and the third passage 13 are separated by a cylindrical partition wall 21.
[0023] The first passage 11 supplies the dispersion gas into the reaction shaft 1. The second passage 12 supplies the concentrate into the reaction shaft 1. The third passage 13 supplies the main reaction blast gas from the air chamber 17 into the reaction shaft 1. The fourth passage 14 supplies the auxiliary reaction gas into the reaction shaft 1.
[0024] A hollow truncated cone-shaped dispersion cone 15 is formed at the tip (lower end) of the lance 16. A plurality of supply holes 152 are formed in a lower side portion 151 of the dispersion cone 15 to discharge the dispersion gas that has passed through the first passage 11 into the reaction shaft 1. The supply holes 152 are provided so that the gas is discharged in the normal direction to the bottom circle of the dispersion cone 15.
[0025] The raw materials fed into the flash smelting furnace 100 include copper concentrate and recycled raw materials. The main component of copper concentrate is sulfide (e.g., CuFeS2). On the other hand, recycled raw materials contain a lot of metallic copper (simple Cu). In recent years, the proportion of recycled raw materials in the raw materials has been increasing. For this reason, a lot of metallic copper is fed into the flash smelting furnace 100.
[0026] The copper concentrate undergoes an oxidation reaction in the reaction shaft 1, generating sulfur. Metallic copper reacts with sulfur and is sulfided. A portion of the metallic copper is sulfided in the reaction shaft 1 to become matte 5 (mattification). The remaining metallic copper is matted in the settler 2. It is preferable to matte a large amount of metallic copper in the reaction shaft 1. In order to promote mattification, it is effective to increase the reaction rate of metallic copper mattification in the reaction shaft 1.
[0027] 3 to 4(b) are flow charts illustrating the process in the embodiment, including the steps of the evaluation method and the operation method. As shown in FIG. 3, the reaction rate of the reaction in which metallic copper is matted in the reaction shaft 1 is evaluated (step S10). Based on the evaluation result, the operation conditions of the flash smelting furnace 100 are controlled (step S12). By controlling the operation conditions, the reaction rate is increased, and metallic copper is efficiently matted. The reaction rate indicates the proportion of metallic copper that is matted within a certain period of time.
[0028] FIG. 4(a) is a flow chart showing the process of evaluating the reaction rate, which corresponds to step S10 in FIG. 3. As shown in FIG. 4(a), a simulation is performed to obtain the partial pressure of sulfur gas (S2), the partial pressure of oxygen (O2), the partial pressure of sulfur dioxide (SO2), the temperature distribution, and the trajectory of particles in the reaction shaft 1 (step S20). The parameters of the simulation are adjusted so that the simulated temperature distribution matches the temperature distribution in the reaction shaft 1 during operation. The partial pressure and the trajectory are calculated using the parameters. As described later, the reaction shaft 1 is set into a plurality of regions based on the temperature distribution and the partial pressure of sulfur gas.
[0029] A test is carried out using an experimental furnace (step S22). From the test, the reaction rate per unit time for each of the multiple regions in the reaction shaft 1 is obtained (step S24). Based on the reaction rate for each region and the trajectory and speed of the metallic copper particles charged into the reaction shaft, the matte reaction rate for the entire reaction shaft 1 is obtained (step S26). Specifically, based on the trajectory and flow rate of each metallic copper particle, the final reaction rate is calculated for each metallic copper particle from the region it has passed through and the time it has been present in each region. The reaction rate of the entire reaction shaft 1 can be calculated based on the final reaction rates of all the metallic copper particles.
[0030] FIG. 4(b) is a flow chart showing the process of controlling the operating conditions, which corresponds to step S12 in FIG. 3. As shown in FIG. 4(b), the recycled material is pre-treated before being fed into the flash smelting furnace 100 (step S30). For example, the recycled material is powdered by the pre-treatment, and the particle size of the powder is adjusted to a desired size. The partial pressure of sulfur gas in the reaction shaft 1 of the flash smelting furnace 100 is controlled (step S32). For example, the partial pressure of sulfur gas can be increased by reducing the concentration of oxygen blown. The partial pressure of sulfur gas is adjusted to a desired value. The reaction rate is increased and matting of the recycled material is promoted by controlling the operating conditions.
[0031] 5 to 9 are diagrams illustrating the results of a simulation, showing the inside of the reaction shaft 1 of a flash smelting furnace 100. FIG.
[0032] Figure 5 shows the partial pressure of sulfur gas. As the temperature of the copper concentrate rises, sulfur volatilizes from the copper concentrate, generating sulfur gas. The partial pressure on the side of reaction shaft 1 farther from settler 2 is higher than the partial pressure on the side closer to settler 2.
[0033] Figure 6 shows the partial pressure of oxygen. Oxygen is supplied from the concentrate burner 4 into the reaction shaft 1 at an initial speed of, for example, 120 m / s. The oxygen reacts with sulfur on the outer periphery of the reaction shaft 1 and is consumed. The partial pressure is high near the concentrate burner 4 and low at positions away from the concentrate burner 4. Figure 7 shows the partial pressure of sulfur dioxide. Sulfur dioxide is generated by oxidation of sulfur.
[0034] Figure 8 shows the temperature distribution. The temperature rises as sulfur reacts with oxygen. There is a lot of unreacted oxygen near the concentrate burner 4, so the temperature is low. The temperature rises at positions away from the concentrate burner 4. In particular, in the center of the reaction shaft 1, oxygen is blown in from the concentrate burner 4, and there is a large mass of copper concentrate, so sulfur is likely to be generated. Therefore, a reaction between sulfur and oxygen is likely to occur, and the temperature rises. Figure 9 shows the trajectory of particles. The trajectory for each particle size is shown. The specific gravity of the particles is assumed to be constant. The volume of the region is obtained based on the simulation.
[0035] Based on the results of the simulation, the reaction shaft 1 is divided into multiple regions. Specifically, the multiple regions are determined based on the temperature distribution and the partial pressure of sulfur gas. For example, the regions are those with a temperature of 1100°C or higher and lower than 1200°C, and a partial pressure of 0.04 Pa or higher and lower than 0.05 Pa. Tests are performed to determine the reaction rate per unit time for each region (steps S22 and S24 in FIG. 4(b)).
[0036] Tables 1 and 2 show examples of reaction rates per unit time. Table 1 is an example where the temperature is T1. Table 2 is an example where the temperature is T2, which is different from T1. [Table 1] [Table 2]
[0037] In Table 1, reaction shaft 1 is divided into a region R1 where the partial pressure of sulfur gas (S2 partial pressure) is equal to or greater than X1 (X1~), a region R2 where the partial pressure of sulfur gas is equal to or greater than X2 but less than X1 (X2~X1), a region R3 where the partial pressure of sulfur gas is equal to or greater than X3 but less than X2 (X3~X2), a region R4 where the partial pressure of sulfur gas is equal to or greater than X4 but less than X3 (X4~X3), and a region R5 where the partial pressure of sulfur gas is less than X4 (~X4).
[0038] In region R1, the reaction rate per unit time of metallic copper with a particle size of less than 50 μm (up to 50 μm) is A11, the reaction rate per unit time of metallic copper with a particle size of 50 μm to 100 μm (50 μm to 100 μm) is A12, and the reaction rate per unit time of metallic copper with a particle size of 100 μm or more (100 μm or more) is A13. The volume of region R1 is B1. In region R2, the reaction rate per unit time of metallic copper with a particle size of less than 50 μm is A21, the reaction rate per unit time of metallic copper with a particle size of 50 μm to 100 μm is A22, and the reaction rate per unit time of metallic copper with a particle size of 100 μm or more is A23. The volume of region R1 is B2. Similarly as above, reaction rates per unit time A31, A32, and A33 in region R3, volume B3 of region R3, reaction rates per unit time A41, A42, and A43 in region R4, volume B4 of region R4, reaction rates per unit time A51, A52, and A53 in region R5, and volume B5 of region R5 are obtained.
[0039] In Table 2, reaction shaft 1 is divided into a region R6 where the partial pressure of sulfur gas is equal to or greater than X1, a region R7 where the partial pressure of sulfur gas is equal to or greater than X2 but less than X1, a region R8 where the partial pressure of sulfur gas is equal to or greater than X3 but less than X2, a region R9 where the partial pressure of sulfur gas is equal to or greater than X4 but less than X3, and a region R10 where the partial pressure of sulfur gas is less than X4.
[0040] In region R6, the reaction rate per unit time for particle diameters less than 50 μm is A61, the reaction rate per unit time for particle diameters between 50 μm and 100 μm is A62, and the reaction rate per unit time for particle diameters equal to or greater than 100 μm is A63. The volume of region R6 is B6. In region R7, the reaction rate per unit time for particle diameters less than 50 μm is A71, the reaction rate per unit time for particle diameters between 50 μm and 100 μm is A72, and the reaction rate per unit time for particle diameters equal to or greater than 100 μm is A73. The volume of region R7 is B7. Reaction rates per unit time A81-A103 and volumes B8-B10 in regions R8-R10 are also obtained.
[0041] Next, based on the trajectory and speed of the metallic copper particles charged into the reaction shaft 1, the area through which each metallic copper particle passes and the time it remains in that area are determined. For example, assume that a metallic copper particle with a particle size of less than 50 μm remains in area R1 at temperature T1 for time t1, and then in area R6 at temperature T2 for time t2, where it completes its reaction. In this case, the final reaction rate Y1 (%) after the metallic copper particle passes through the reaction shaft can be calculated using the following method. First, the reaction rate Y1' in area R1 is calculated. Y1' = A11 × t1 Next, calculate the reaction rate Y1" in region R6. Since it is necessary to calculate the unreacted portion of the particle in region R6, the reaction rate Y1" is calculated using the following formula. Y1“=(1-Y1')×A61×t2 From the above calculations, the reaction rate for each region is calculated. The final reaction rate for one metallic copper particle is calculated by integrating the reaction rates for each region. In other words, the final reaction rate Y1 (%) is as follows: Y1=Y1'+Y1“ In this way, calculations are performed for each metallic copper particle to determine the final reaction rate of each metallic copper particle. Then, the reaction rate of the entire reaction shaft 1 can be calculated based on the final reaction rates of all metallic copper particles.
[0042] In the examples of Tables 1 and 2, the number of regions is 10, but it may be less than 10 or more than 10. The number of particle size classifications is 3, but it may be less than 3 or more than 3. Tables 1 and 2 show examples of two temperatures, but the regions may be defined based on two or more temperatures.
[0043] The above calculation can be performed for all metallic copper particles charged into the reaction shaft 1, and the final reaction rate for each metallic copper particle can be calculated. The final reaction rate for the entire reaction shaft 1 can be calculated by accumulating the final reaction rates for all metallic copper particles. The final reaction rate for the entire reaction shaft 1 may be calculated by calculating the final reactions of multiple metallic copper particles, rather than all of the charged metallic copper particles, and accumulating the results for those particles to calculate the final reaction rate for the entire reaction shaft 1.
[0044] The reaction rate may be calculated, for example, by the following method. When performing a simulation, a representative particle representing multiple particles is defined. Multiple representative particles are determined so as to correspond to all particles charged into the reaction shaft 1, and their trajectories and speeds are obtained by simulation. In addition, the particle size distribution of the metallic copper particles to be charged into the reaction shaft 1 is determined. From the trajectory and speed of each representative particle, the area through which each representative particle passes and the time spent in the area are obtained. The representative particle may also be determined randomly without using any particular regular selection method. Alternatively, in order to prevent bias in the reaction rate per unit time and trajectory due to particle size, the representative particle may be determined so as to match as closely as possible to the particle size distribution of the metallic copper particles to be charged into the reactor.
[0045] For example, suppose that the particle size distribution of the metallic copper particles charged into the reaction shaft 1 is α% less than 50 μm in particle size, β% between 50 μm and 100 μm, and γ% 100 μm or more. Suppose that a representative particle exists in region R1 at temperature T1 for time t1, and then in region R6 at temperature T2 for time t2, where it terminates its reaction. In this case, the reaction rate Y2 (%) of this representative particle can be calculated as follows. First, the reaction rate Y2' in region R1 is calculated. Y2'={A11×(α / 100)+A12×(β / 100)+A13×(γ / 100}×t1 Next, calculate the reaction rate Y1" in region R6. Since it is necessary to calculate the unreacted portion in region R6, the following formula is used. Y2“=(1-Y2')×[{A61×(α / 100)+A62×(β / 100)+A63×(γ / 100)}×t2] From the above results, the final reaction rate Y2 (%) is as follows: Y2=Y2'+Y2“
[0046] In this way, calculations are performed for each representative particle to determine the final reaction rate of each metallic copper particle, and then the reaction rate of the entire reaction shaft 1 can be calculated based on the final reaction rates of all metallic copper particles.
[0047] According to this embodiment, since the reaction rate in the reaction shaft 1 is known, it is possible to estimate the amount of metallic copper that will be matted in the reaction shaft 1. The metallic copper that has not been matted in the reaction shaft 1 is matted in the settler 2. By operating the flash smelting furnace 100 so that the metallic copper is matted in the reaction shaft 1 and the settler 2, the efficiency of matting the metallic copper can be increased.
[0048] For example, the amount of gas such as oxygen injected into the reaction shaft 1 is adjusted to control the partial pressure of sulfur gas in the reaction shaft 1. In pre-treatment of the recycled material before feeding into the flash smelting furnace 100, the recycled material is pulverized to form a powder. The particle size of the powder is controlled. By setting the partial pressure and particle size to the desired size, the reaction rate of matte formation can be increased. Among the operating conditions of the flash smelting furnace 100, conditions other than the partial pressure and particle size of the gas may be controlled.
[0049] As shown in Figures 5 to 9, the simulation can obtain the temperature distribution, partial pressure of sulfur gas, partial pressure of oxygen gas, partial pressure of sulfur dioxide, and particle trajectories. Heat is generated by the reaction between sulfur gas and oxygen gas. The temperature distribution can be estimated from the partial pressures of sulfur gas and oxygen gas. In locations where the partial pressure of sulfur gas is high and the temperature is high, metallic copper is easily sulfurized. Regions are defined based on the distribution of partial pressure and temperature gas.
[0050] The reaction rates for each region can be obtained, for example, by testing or calculated using software such as fact sage. Simulations are suitable for calculating reaction rates in equilibrium, but are difficult to calculate reaction rates in non-equilibrium. Metallic copper is thought to pass through reaction shaft 1 in a matter of seconds, and it is assumed that the reaction is not in equilibrium. By testing particles in a non-equilibrium state using an experimental furnace, it is possible to obtain highly accurate reaction rates.
[0051] The above embodiment can be applied to a reactor in which metallic copper reacts with sulfur gas and is sulfurized. The reaction shaft 1 of the flash smelting furnace 100 is an example of a reactor. Matte formation is an example of sulfurization of metallic copper.
[0052] The above-described embodiment is a preferred example of the present invention, but the present invention is not limited to this embodiment and can be modified in various ways without departing from the scope of the present invention. [Explanation of symbols]
[0053] 1 Reaction shaft 2 Setra 3. Uptake 4 Concentrate burner 5. Matt 6. Slug 10 Input section 11 1st aisle 12 2nd aisle 13 3rd aisle 14 4th aisle 16. Lance 100 Flash furnace
Claims
1. A step of acquiring a temperature distribution inside a reactor in which metallic copper is sulfurized by reacting metallic copper with sulfur gas, a partial pressure of the sulfur gas, and a trajectory and flow velocity of metallic copper particles; A step of dividing the reaction device into a plurality of regions based on the temperature distribution and the partial pressure of the sulfur gas, and acquiring a reaction rate per unit time of the sulfurization of the metallic copper for each of the plurality of regions; calculating a reaction rate of the metallic copper particles for each region through which the metallic copper particles pass based on the trajectory and flow rate of each metallic copper particle, and integrating the reaction rates of the metallic copper particles to calculate a final reaction rate of each metallic copper particle after passing through the reactor; and calculating a final reaction rate in the entire reactor from the final reaction rates of the plurality of metallic copper particles charged into the reactor.
2. The step of acquiring the reaction rate for each of the plurality of regions includes a step of acquiring the reaction rate per unit time for each of the plurality of regions and for each particle diameter of the metallic copper, 2. The evaluation method according to claim 1, wherein the step of calculating the final reaction rate for each metallic copper particle includes the steps of: calculating the reaction rate of the metallic copper particle according to the particle size of the metallic copper particle when calculating the reaction rate for each region through which the metallic copper particle passes based on the trajectory and flow velocity of each metallic copper particle; and calculating the final reaction rate for each metallic copper particle by integrating the reaction rates of the metallic copper particles.
3. The step of acquiring the reaction rate for each of the plurality of regions includes a step of acquiring a particle size distribution of metallic copper to be charged into the reaction apparatus, The step of calculating the final reaction rate for each metallic copper particle includes a step of determining a plurality of representative particles representative of the metallic copper particles to be charged into the reactor, a step of calculating the reaction rate of each representative particle in accordance with the ratio of the particle size distribution when calculating the reaction rate for each region through which each representative particle passes based on the trajectory and flow velocity of each representative particle, and a step of calculating the final reaction rate of each representative particle after passing through the reactor by integrating the reaction rate of each representative particle, 2. The evaluation method according to claim 1, wherein the step of calculating the final reaction rate in the entire reactor is a step of determining the final reaction rate of the entire reactor from the results of the final reaction rates of each of the plurality of representative particles charged into the reactor.
4. The evaluation method according to claim 1 or 2, characterized in that the process of acquiring the temperature distribution, the partial pressure of the sulfur gas, and the trajectory and flow velocity of the metallic copper particles is a process of acquiring the temperature distribution, the partial pressure, and the trajectory and flow velocity by simulation.
5. 3. The evaluation method according to claim 1, wherein the step of acquiring the response rate for each of the plurality of regions includes the step of acquiring the response rate for each of the plurality of regions by a test.
6. 3. The evaluation method according to claim 1, wherein the step of calculating the final reaction rate in the entire reactor is a step of calculating the final reaction rate in the entire reactor from the result of the final reaction rates of all the metallic copper particles charged into the reactor.
7. The reactor is a reaction shaft of a flash smelting furnace; In the reaction shaft, the metallic copper is sulfurized to form a matte. The step of acquiring the reaction rate for each of the plurality of regions is a step of acquiring a reaction rate at which the metallic copper turns into matte per unit time for each of the plurality of regions of the reaction shaft, The step of calculating the final reaction rate for each metallic copper particle is a step of calculating a matte rate for each metallic copper particle, The evaluation method according to claim 1 or 2, wherein the step of calculating a final reaction rate in the entire reaction apparatus is a step of calculating a matte rate in the entire reaction apparatus.
8. A step of acquiring a temperature distribution inside a reactor in which metallic copper is sulfurized by reacting metallic copper with sulfur gas, a partial pressure of the sulfur gas, and a trajectory and flow velocity of metallic copper particles; A step of dividing the reaction device into a plurality of regions based on the temperature distribution and the partial pressure of the sulfur gas, and acquiring a reaction rate per unit time of the sulfurization of the metallic copper for each of the plurality of regions; calculating a final reaction rate of each metallic copper particle after passing through the reactor by calculating and integrating a reaction rate for each region through which the metallic copper particle passes based on the trajectory and flow rate of each metallic copper particle; Calculating the final reaction rate in the entire reactor from the final reaction rate of the plurality of metallic copper particles charged into the reactor; and controlling the operating conditions of the reactor based on the final reaction rate in the entire reactor.
9. 9. The method of claim 8, wherein the step of controlling the operating conditions includes the step of controlling a partial pressure of the sulfur gas in the reactor.
10. 10. The operating method according to claim 8 or 9, wherein the step of controlling the operating conditions includes a step of controlling the particle size of the raw material fed into the reactor based on a final reaction rate in the entire reactor.
11. The reactor is a reaction shaft of a flash smelting furnace; The operating method according to claim 8 or 9, wherein the step of controlling the operating conditions is a step of controlling the operating conditions of the flash smelting furnace.
Citation Information
Patent Citations
Raw copper air refining process based on mathematical model
CN101435024A
Recycle method of valuable metals from scraps
JP1997078151A
Flash furnace and its operation method
JP2019183202A
A system and method for monitoring and optimizing smelting operations of a furnace.
WO2011089622A2
Operation method of flash smelting furnace, and raw material supply apparatus
JP2011075228A