Surface protective film and optical component
The surface protection film with a specific adhesive composition and stress attenuation rate addresses peeling electrification and pressure marks, improving yield and efficiency in polarizing plate handling.
Patent Information
- Application Number
- JP2023054517
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Polarizing plates with surface protection films face issues of peeling electrification that can damage underlying circuits and leave pressure marks, reducing yield and work efficiency.
A surface protection film comprising a transparent resin base film with an adhesive layer containing poly(meth)acrylic polymer, polyether-modified silicone compound, isocyanate crosslinking agent, and antistatic agent, designed to have a stress attenuation rate of 0.5% to 3.0% to minimize peeling voltage and pressure marks.
The film effectively reduces peeling voltage and suppresses pressure marks, enhancing production efficiency and product yield by protecting underlying components.
Smart Images

Figure 2024142393000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a surface protection film and an optical component. [Background technology]
[0002] Optical films and optical products such as displays using the same are used. Examples of optical films include polarizing plates, retardation plates, lens films for displays, anti-reflection films, hard coat films, transparent conductive films for touch panels, etc. When manufacturing and transporting optical products, a surface protective film can be attached to the surface of the optical film to prevent the surface from being soiled or scratched in later processes.
[0003] The appearance inspection of the optical product can be performed with the surface protection film attached to the optical film. Performing the appearance inspection with the surface protection film attached can improve work efficiency because it is possible to eliminate the need to peel off the surface protection film and reattach it.
[0004] Patent Document 1 discloses a surface protection film using an adhesive composed of an alkyl trimethyl ammonium salt, a hydroxyl group-containing acrylic polymer, and a polyisocyanate. Patent Document 2 discloses an adhesive composition composed of an ionic liquid and an acrylic polymer having an acid value of 1.0 or less, and an adhesive sheet using the same. Patent Document 3 discloses an adhesive composition composed of an acrylic polymer, a polyether polyol compound, and an alkali metal salt treated with an anion-adsorbing compound, and a surface protection film using the same. Patent Document 4 discloses an adhesive composition containing an alkali metal salt and a polyether-modified silicone, and a surface protection film using the same. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2005-131957 A [Patent Document 2] JP 2005-330464 A [Patent Document 3] JP 2005-314476 A [Patent Document 4] JP 2014-125625 A Summary of the Invention [Problem to be solved by the invention]
[0006] When a polarizing plate with a surface protective film is peeled off from an adherend, it is required to prevent the circuit of the adherend (driver IC, etc.) from being adversely affected by peeling static electricity. When a polarizing plate with a surface protective film is gripped by hand or pressed with a roll for handling, pressure marks may be left on the polarizing plate. A polarizing plate with pressure marks has a dent, which deteriorates the appearance of the polarizing plate as a product and causes a decrease in yield.
[0007] An object of one aspect of the present invention is to provide a surface protection film and an optical component that can reduce peeling electrification voltage and suppress the formation of pressure marks. [Means for solving the problem]
[0008] One aspect of the present invention provides a surface protection film comprising a substrate film made of a transparent resin and an adhesive layer formed on one side of the substrate film, the adhesive layer containing a poly(meth)acrylic polymer, a polyether-modified silicone compound, an isocyanate-based crosslinking agent, and an antistatic agent, the stress decay rate of which when laminated to a TAC film is 0.5% or more and 3.0% or less as measured by a loop stiffness tester.
[0009] The surface protection film has a release film attached to the side of the pressure-sensitive adhesive layer opposite to the base film.
[0010] Another aspect of the present invention provides an optical component having the above-mentioned surface protective film attached to an adherend. Effect of the Invention
[0011] One aspect of the present invention can provide a surface protection film and an optical component that can reduce peeling electrification voltage and suppress the formation of pressure marks. [Brief description of the drawings]
[0012] [Figure 1] FIG. 2 is a cross-sectional view of a surface protection film according to an embodiment. [Diagram 2] FIG. 2 is a cross-sectional view of a surface protective film with a release film in which a release film is bonded to the surface protective film of the embodiment. [Diagram 3] 1 is a cross-sectional view of an example optical component. [Figure 4] FIG. 1 is a diagram showing the configuration of a test device for a pressing test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, the present invention will be described in detail based on the embodiments. 1 is a cross-sectional view showing a surface protection film according to an embodiment. As shown in FIG. 1, a surface protection film 10 according to an embodiment includes a base film 1 and a pressure-sensitive adhesive layer 2.
[0014] [Base film] As the base film 1, a film (polyester film) formed of polyester such as polyethylene terephthalate, polyethylene naphthalate, polyethylene isophthalate, polybutylene terephthalate, etc. is preferably used. In addition to polyester films, films made of other resins can also be used as long as they have the necessary strength and optical suitability. The base film 1 may be a non-stretched film, or a uniaxially or biaxially stretched film. The stretching ratio of the stretched film and the orientation angle in the axial direction formed by the crystallization of the stretched film may be controlled to a specific value.
[0015] A substrate film made of a transparent and flexible resin is used as the substrate film 1. This allows for visual inspection of the optical product, which is the adherend, with the surface protection film 10 attached to the optical product.
[0016] "Transparent" means that the visible light transmittance calculated as the average value of the transmittance in the thickness direction in the entire wavelength range when measured within a measurement wavelength range of 380 nm to 780 nm is 50% or more (preferably 70% or more, more preferably 80% or more). The light transmittance can be measured in accordance with "Plastics - Determination of total light transmittance and total light reflectance" as specified in JIS K 7375:2008.
[0017] The thickness of the base film 1 is not particularly limited, but may be, for example, 12 μm to 100 μm. It is more preferable that the thickness of the base film 1 is 20 μm to 50 μm, since the base film 1 is easy to handle. If necessary, the surface of the base film 1 may be subjected to an adhesion enhancing treatment such as surface modification by corona discharge or application of an anchor coating agent.
[0018] [Adhesive layer] It is preferable that the pressure-sensitive adhesive layer 2 adheres to the surface of the adherend, can be easily peeled off after use, and does not easily contaminate the adherend. The pressure-sensitive adhesive layer 2 is formed on one surface of the base film 1 (the lower surface in FIG. 1). The pressure-sensitive adhesive layer 2 contains a poly(meth)acrylic polymer, a polyether-modified silicone compound, an isocyanate-based crosslinking agent, and an antistatic agent.
[0019] The poly(meth)acrylic polymer may be, for example, a polymer obtained by copolymerizing a main monomer, a comonomer, and a functional monomer. Examples of the main monomer include butyl acrylate (for example, n-butyl acrylate), 2-ethylhexyl acrylate, isooctyl acrylate, isononyl acrylate, etc. As the main monomer, one of these may be used, or two or more of them may be used in combination. Examples of the comonomer include acrylonitrile, vinyl acetate, methyl acrylate, methyl methacrylate, ethyl acrylate, butyl acrylate, etc. As the comonomer, one of these may be used, or two or more of them may be used in combination. Examples of the functional monomer include acrylic acid, methacrylic acid, hydroxyethyl acrylate (e.g., 2-hydroxyethyl acrylate), hydroxybutyl acrylate, glycidyl methacrylate, dimethylacrylamide, N-methylol methacrylamide, hydroxyl group-containing acrylic monomer, carboxyl group-containing acrylate, and polyoxyalkylene group-containing acrylic monomer. As the functional monomer, one of these may be used, or two or more may be used in combination. The poly(meth)acrylic polymer may have an appropriate composition selected according to the desired properties.
[0020] The monomer composition constituting the poly(meth)acrylic polymer preferably contains 50% or more (meth)acrylic monomers, and may contain 100% (meth)acrylic monomers.
[0021] A compound containing a polyoxyalkylene group may be copolymerized or mixed with the poly(meth)acrylic polymer. Examples of compounds containing a polyoxyalkylene group include polyethylene glycol (400) monoacrylate, polyethylene glycol (400) monomethacrylate, methoxypolyethylene glycol (400) acrylate, methoxypolyethylene glycol (400) methacrylate, polypropylene glycol (400) monoacrylate, polypropylene glycol (400) monomethacrylate, methoxypolypropylene glycol (400) acrylate, and methoxypolypropylene glycol (400) methacrylate.
[0022] The polyether-modified silicone compound is a siloxane compound in which a polyether group is introduced into a silicone chain. The polyether-modified silicone compound is, for example, a siloxane compound in which an oxyalkylene chain is introduced into a silicone chain. Specific examples of alkylene oxides that are raw materials for oxyalkylene chains include ethylene oxide and propylene oxide. As the alkylene oxide, one of these may be used, or two or more may be used in combination. When two or more alkylene oxides are used, the addition form may be block addition or random addition.
[0023] The polyether group may be introduced into a side chain of the silicone chain, or into a terminal of the silicone chain, or into both the side chain and the terminal of the silicone chain.
[0024] The polyether-modified silicone compound, for example, affects the antistatic effect of the pressure-sensitive adhesive layer 2. For example, the antistatic effect of the pressure-sensitive adhesive layer 2 can be adjusted by selecting the molecular weight of the polyethylene oxide used in the side chain.
[0025] Commercially available polyether-modified silicone compounds include, for example, KF-351A, KF-352A, KF-353, KF-354L, KF-355A, KF-642, KF-644, KF-6012, KF-6017P, KF-6020, and KF-6204 (manufactured by Shin-Etsu Chemical Co., Ltd.); SH3746, SH3771, SH3772, SH3773M, SH8400, SH8700, SF8410, FZ-2110, FZ-2123, L-7001, and L-7002. (manufactured by Dow-Toray); TSF-4440, TSF-4441, TSF-4445, TSF-4446, TSF-4450 (manufactured by Momentive Performance Materials); BYK-300, BYK-306, BYK-307, BYK-320, BYK-325, BYK-330 (manufactured by BYK-Chemie), etc.
[0026] The amount of polyether-modified silicone compound added to the adhesive layer 2 varies depending on the type and the degree of compatibility with the adhesive, but may be set in consideration of the peeling electrification voltage when the surface protection film 10 is peeled off from the adherend, the tendency to contaminate the adherend, the adhesive properties, etc. The greater the amount of silicone surfactant added, the lower the peeling electrification voltage when the surface protection film is peeled off, but since the adherend is more likely to be contaminated, it is necessary to select an appropriate amount to be added.
[0027] The amount of the polyether-modified silicone compound added can be, for example, 0.005 to 0.5 parts by mass (preferably 0.01 to 0.1 parts by mass) relative to 100 parts by mass of the poly(meth)acrylic polymer.
[0028] The isocyanate-based crosslinking agent crosslinks the poly(meth)acrylic polymer. The isocyanate-based crosslinking agent is a curing agent that cures the poly(meth)acrylic polymer. The isocyanate-based crosslinking agent is, for example, a polyisocyanate compound. Examples of the polyisocyanate compound include biuret-modified diisocyanates, isocyanurate-modified diisocyanates, and adducts of diisocyanates. As the polyisocyanate compound, one of these may be used, or two or more may be used in combination.
[0029] Examples of diisocyanates include hexamethylene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, tolylene diisocyanate, xylylene diisocyanate, etc. As the diisocyanates, one of these may be used, or two or more of them may be used in combination. Examples of the adduct include adducts of diisocyanates and trivalent or higher polyols. Examples of the trivalent or higher polyols include trimethylolpropane and glycerin.
[0030] When the poly(meth)acrylic polymer has a functional group capable of undergoing a crosslinking reaction (such as a hydroxyl group), crosslinking proceeds as a result of this functional group reacting with an isocyanate-based crosslinking agent. The amount of the isocyanate-based crosslinking agent added is preferably 0.25 parts by mass or more and 10 parts by mass or less based on 100 parts by mass of the poly(meth)acrylic polymer.
[0031] Commercially available isocyanate crosslinking agents include, for example, Coronate (registered trademark) HX (HDI isocyanurate, manufactured by Tosoh Corporation), Coronate (registered trademark) HL (HDI adduct, manufactured by Tosoh Corporation), and Takenate (registered trademark) D-140N (IPDI adduct, manufactured by Mitsui Chemicals, Inc.).
[0032] As the antistatic agent, an alkali metal salt can be used. Examples of the alkali metal salt include salts of alkali metals such as lithium, sodium, and potassium. Specifically, for example, Li + , Na + , K + One or more of the cations and Cl - , Br - , I - , BF4 - , PF6 -、 SCN - , ClO4 - , CF3SO3 - , (CF3SO2)2N - , (C2F5SO2)2N - , (CF3SO2)3C - Metal salts composed of one or more anions from the above are preferably used. Among them, lithium salts such as LiBr, LiI, LiBF4, LiPF6, LiSCN, LiClO4, LiCF3SO3, Li(CF3SO2)2N, Li(C2F5SO2)2N, and Li(CF3SO2)3C are particularly preferred. These alkali metal salts may be used alone or in combination of two or more. Li(CF3SO2)2N is lithium bis(trifluoromethanesulfonyl)imide.
[0033] Ionic compounds may be used as the antistatic agent. Examples of the ionic compounds include ionic liquids and ionic solids. The ionic compounds are ionic compounds having a cation and an anion. Examples of the cation include cyclic amidine ions such as imidazolium ions, pyridinium ions, ammonium ions, sulfonium ions, phosphonium ions, tri-n-butylmethylammonium ions, and the like. Examples of the anion include C n H 2n+1 COO - , C n F 2n+1 COO - , NO3 - , C n F 2n+1 SO3 - , (C n F2n+1 SO2)2N - , (C n F 2n+1 SO2)3C - , PO4 3- , AlCl4 - , Al2Cl7 - , ClO4 - , BF4 - , PF6 - , AsF6 - , SbF6 - etc. Ionic liquids include (n-C4H9)3(CH3)N + - N(SO2CF3)2" (tri-n-butylmethylammonium bistrifluoromethanesulfonimide).
[0034] Commercially available antistatic agents include FC-4400 (tri-n-butylmethylammonium bistrifluoromethanesulfonimide, manufactured by 3M).
[0035] The antistatic agent can reduce static electricity during transport and handling of optical components. This reduces the adhesion of foreign matter such as dust and dirt during processing. When the surface protection film 10 is peeled off from the optical product 5 (see FIG. 3), the peeling electrification voltage can be reduced. This reduces the risk of damaging the driver IC, TFT element, gate line driving circuit, etc. of the optical product 5. This increases the production efficiency in the process of manufacturing liquid crystal display panels, etc., and increases the reliability of the production process.
[0036] If necessary, a crosslinking catalyst may be added as an additive to the pressure-sensitive adhesive layer 2 in order to promote a crosslinking reaction. If necessary, an adhesion improver such as a silane coupling agent may be added as an additive to the pressure-sensitive adhesive layer 2 in order to improve the adhesion between the base film 1 and the pressure-sensitive adhesive. If necessary, additives such as an antioxidant and an ultraviolet absorbing agent may be added to the pressure-sensitive adhesive layer 2.
[0037] The thickness of the pressure-sensitive adhesive layer 2 is not particularly limited, but is, for example, preferably from 5 μm to 40 μm, and more preferably from 10 μm to 30 μm. The adhesive strength (low-speed adhesive strength) of the surface protection film 10 to the surface of the adherend at a peel speed of 0.3 m / min may be, for example, 0.03 N / 25 mm to 0.1 N / 25 mm. The adhesive strength (low-speed adhesive strength) is preferably 0.05 N / 25 mm to 0.07 N / 25 mm. An example of the adherend is a TAC polarizing plate (a polarizing plate using a TAC film as a polarizer protective film).
[0038] The adhesive strength of the surface protection film 10 to the surface of the adherend at a peeling speed of 30 m / min (high-speed adhesive strength) is preferably 0.8 N / 25 mm or less. If the high-speed adhesive strength exceeds 0.8 N / 25 mm, the workability when peeling off the surface protection film 10 after use may be deteriorated. An example of the adherend is a TAC polarizing plate (a polarizing plate using a TAC film as a polarizer protective film).
[0039] The adhesive strength of the adhesive layer 2 can be adjusted by known methods such as changing the adhesive composition, adjusting the amount of curing agent added, or adjusting the amount of tackifier or adhesive strength regulator added.
[0040] When the surface protection film 10 is attached to a TAC film, the stress decay rate measured by a loop stiffness tester is 0.5% or more and 3.0% or less. When the stress attenuation rate is 0.5% or more, the peeling electrification voltage is easily reduced. If the stress attenuation rate is 3.0% or less, the formation of indentations can be suppressed. The smaller the stress attenuation rate, the greater the effect of suppressing the formation of indentations.
[0041] The stress decay rate can be measured, for example, as follows. A sample (for example, 15 mm wide x 170 mm long) is prepared by bonding a surface protection film to a TAC film (triacetyl cellulose film, 60 μm thick). A sample is set in a Loop Stiffness Tester (registered trademark) (manufactured by Toyo Seiki Seisakusho Co., Ltd.) (loop stiffness tester). The sample is bent into a loop (arc shape) in the thickness direction. The stress (maximum stress) of the sample is measured when the loop part of the sample is pressed so as to be crushed by the measuring probe.
[0042] The stress decay rate is the rate of stress reduction one second after the measurement probe is stopped, relative to the maximum stress mentioned above. The stress reduction rate (%) is expressed as (σ1-σ2) / σ1×100, where σ1 is the maximum stress and σ2 is the stress one second after the measurement probe is stopped. For example, if σ1 is 100 Pa and σ2 is 98 Pa, the stress reduction rate is (100-98) / 100×100=2%.
[0043] A known method can be used to form the pressure-sensitive adhesive layer 2 on the surface of the base film 1. Specifically, known coating methods such as reverse coating, comma coating, gravure coating, slot die coating, Mayer bar coating, and air knife coating can be used.
[0044] Known methods can be used for forming the pressure-sensitive adhesive layer 2 and for laminating the release film 3 to the pressure-sensitive adhesive layer 2. Specific examples include (1) a method in which a resin composition for forming the pressure-sensitive adhesive layer 2 is applied to one side of a base film 1, dried to form the pressure-sensitive adhesive layer 2, and then laminating the release film 3 to the pressure-sensitive adhesive layer 2, and (2) a method in which a resin composition for forming the pressure-sensitive adhesive layer 2 is applied to the surface of the release film 3, dried to form the pressure-sensitive adhesive layer 2, and then laminating the base film 1 to the pressure-sensitive adhesive layer 2.
[0045] Fig. 2 is a cross-sectional view showing a surface protective film 11 with a release film in which a release film 3 is bonded to a surface protective film 10. As shown in Fig. 2, the release film 3 is bonded to the side of the pressure-sensitive adhesive layer 2 opposite to the base film 1 (the lower side in Fig. 2).
[0046] A known release film may be used as the release film 3. As the release film 3, a polyolefin film such as a polyethylene film or a polypropylene film, a fluorine film, or the like may be used alone. The release film 3 may be a release film obtained by treating a resin film with a release agent (also called a release agent). Examples of the resin film include polyester films such as PET (polyethylene terephthalate) and PEN (polyethylene naphthalate), and polyamide films. Examples of the release agent include silicone resins, resins containing long-chain alkyl groups, and fluorine resins. Among them, a release film 3 obtained by treating a PET film with a silicone-based release agent is preferable. The thickness of the release film 3 is not particularly limited, but is preferably 12 μm to 38 μm in terms of workability and cost.
[0047] Fig. 3 is a cross-sectional view showing an optical component 20, which is an example of an optical component. As shown in Fig. 3, the optical component 20 has a surface protection film 10 bonded to the surface of an optical product 5. The optical component 20 is produced as follows. After the release film 3 of the surface protection film 11 with a release film (see Fig. 2) is peeled off to expose the pressure-sensitive adhesive layer 2, the surface protection film 10 is bonded to the optical product 5, which is the adherend, via the pressure-sensitive adhesive layer 2.
[0048] Examples of the optical product 5 include optical films such as a polarizing plate, a retardation plate, a lens film, a polarizing plate that also serves as a retardation plate, and a polarizing plate that also serves as a lens film. Such optical products 5 are used as components of liquid crystal display devices such as liquid crystal display panels and various instruments. Examples of the optical product 5 include optical films such as anti-reflection films, hard coat films, and transparent conductive films for touch panels. EXAMPLES
[0049] The present invention will now be further described with reference to examples. Example 1 An adhesive was prepared from a copolymer of 80 parts by weight of 2-ethylhexyl acrylate, 10 parts by weight of butyl acrylate, 7 parts by weight of methoxypolyethylene glycol (400) methacrylate, and 3 parts by weight of 2-hydroxyethyl acrylate. 100 parts by weight of a 40% ethyl acetate solution of this adhesive was mixed with 0.3 parts by weight of lithium bis(trifluoromethanesulfonyl)imide as an antistatic agent, 0.08 parts by weight of Dowsil (registered trademark) L-7002 (manufactured by Dow-Toray Industries, Inc.) as a polyether-modified silicone compound, and 1 part by weight of Coronate (registered trademark) HX (manufactured by Tosoh Corporation) as an isocyanate-based crosslinking agent, and the mixture was stirred and mixed to prepare an adhesive composition.
[0050] The prepared adhesive composition was applied to the surface of a 38 μm thick polyethylene terephthalate film (base film) using an applicator so that the adhesive layer would have a thickness of 20 μm after drying. The base film to which the adhesive composition was applied was heated and dried in a hot air circulation oven at 100° C. for 3 minutes to obtain an adhesive film. This adhesive film is configured by forming an adhesive layer on one side of a polyethylene terephthalate film. A release film (Diafoil MRF25, manufactured by Mitsubishi Chemical Corporation) was attached to the surface of the adhesive layer of the adhesive film so that the release layer was in contact with the adhesive layer. The resulting adhesive sheet was aged at 40°C for 3 days to obtain the surface protection film of Example 1. The release film was a 25 μm thick polyethylene terephthalate film with the surface treated with a silicone release agent.
[0051] Example 2 A surface protection film of Example 2 was obtained in the same manner as in Example 1, except that the amount of Dowsil L-7002 added was 0.04 parts by mass.
[0052] Example 3 A surface protection film of Example 2 was obtained in the same manner as in Example 1, except that the amount of Dowsil L-7002 added was 0.02 parts by mass.
[0053] Example 4 The surface protection film of Example 4 was obtained in the same manner as Example 1, except that 0.3 parts by mass of tri-n-butylmethylammonium bistrifluoromethanesulfonimide (FC-4400, manufactured by 3M, melting point 27.5°C) was used instead of lithium bis(trifluoromethanesulfonyl)imide as the antistatic agent.
[0054] Example 5 A surface protection film of Example 5 was obtained in the same manner as in Example 4, except that the amount of Dowsil L-7002 added was 0.04 parts by mass.
[0055] Example 6 A surface protection film of Example 6 was obtained in the same manner as in Example 4, except that the amount of Dowsil L-7002 added was 0.02 parts by mass.
[0056] Example 7 The surface protection film of Example 7 was obtained in the same manner as in Example 4, except that the amount of Dowsil L-7002 added was 0.04 parts by mass and the amount of Coronate HX added was 1.5 parts by mass.
[0057] Comparative Example 1 A surface protection film of Comparative Example 1 was obtained in the same manner as in Example 1, except that the amount of Dowsil L-7002 added was 0.32 parts by mass.
[0058] Comparative Example 2 A surface protection film of Comparative Example 2 was obtained in the same manner as in Example 1, except that the amount of Dowsil L-7002 added was 0.16 parts by mass.
[0059] Comparative Example 3 A surface protective film of Comparative Example 3 was obtained in the same manner as in Example 1, except that the amount of Dowsil L-7002 added was 0.
[0060] Comparative Example 4 A surface protection film of Comparative Example 4 was obtained in the same manner as in Example 4, except that the amount of Dowsil L-7002 added was 0.32 parts by mass.
[0061] Comparative Example 5 A surface protection film of Comparative Example 5 was obtained in the same manner as in Example 4, except that the amount of Dowsil L-7002 added was 0.16 parts by mass.
[0062] Comparative Example 6 A surface protective film of Comparative Example 6 was obtained in the same manner as in Example 4, except that the amount of Dowsil L-7002 added was 0.
[0063] The evaluation test methods and results are shown below.
[0064] (Method of measuring adhesive strength to TAC polarizing plate) A polarizing plate using TAC film as a polarizer protective film (TAC polarizing plate) is laminated to the surface of a glass plate using a laminating machine. A surface protective film cut into a strip (width 25 mm) is laminated to the surface of the TAC polarizing plate. The TAC polarizing plate with the surface protective film laminated is stored for one day in a test environment of 23°C x 50% RH. The strength when the surface protective film is peeled off in a 180° direction at a peeling speed of 0.3 m / min using a tensile tester is measured, and this is taken as the adhesive strength (N / 25 mm). The TAC polarizing plate is formed by laminating a TAC film to both sides of the polarizing plate.
[0065] (Method of measuring the peeling charge voltage for TAC polarizing plate) A polarizing plate using a TAC film as a polarizer protective film (TAC polarizing plate) is laminated on the surface of a glass plate using a laminating machine. A surface protective film cut into a strip (width 25 mm) is laminated on the surface of the TAC polarizing plate. The TAC polarizing plate with the surface protective film laminated thereon is stored for one day under a test environment of 23°C x 50% RH. While peeling the surface protective film at a peeling speed of 30 m per minute using a high-speed peeling tester (manufactured by Tester Sangyo), the surface potential of the polarizing plate surface is measured every 10 ms using a surface potential meter (manufactured by Keyence Corporation). The maximum absolute value of the surface potential is defined as the peeling charging voltage (kV).
[0066] (Method of measuring electrostatic charge voltage when peeling off PMMA polarizing plate) The peeling electrification voltage was measured in the same manner as in "Peeling electrification voltage for TAC polarizer" except that a PMMA polarizer was used instead of a TAC polarizer. The PMMA polarizer is a polarizer that uses a PMMA (polymethyl methacrylate) film as a polarizer protective film. The PMMA polarizer is formed by laminating a PMMA film on each side of the polarizer.
[0067] (Stress reduction rate vs. TAC film) The surface protection film is laminated to a TAC film (thickness 60 μm) to obtain a composite film, which is then left to stand for 24 hours. This composite film is then cut into a strip (width 15 mm × length 170 mm) to obtain a sample. A sample is set in a Loop Stiffness Tester (registered trademark) (manufactured by Toyo Seiki Seisakusho). The sample is bent into a loop (arc shape) in the thickness direction. The stress of the sample is measured when the loop portion of the sample is pressed so as to be crushed by the measuring terminal. Specifically, the sample is bent into a loop (arc shape) with an outer circumference of 80 mm. The loop portion is pressed in the diameter direction using the measuring terminal. The measuring terminal presses the loop portion until the inner diameter of the loop portion in the minor axis direction becomes 1.5 mm, and then stops. The speed at which the measuring terminal applies a pressing force to the loop portion is, for example, 3.3 mm / sec. The measuring terminal presses the loop portion, and the stress (maximum stress) is measured when the measuring terminal stops. The stress decay rate is the rate of stress reduction 1 second after the measurement probe is stopped, relative to the maximum stress mentioned above. The stress reduction rate (%) is expressed as (σ1-σ2) / σ1×100, where σ1 is the maximum stress and σ2 is the stress 1 second after the measurement probe is stopped.
[0068] (Pressure test: Pipe method reproduction test) Fig. 4 is a configuration diagram showing a test device for a compression test. As shown in Fig. 4, this test device includes a first pipe 21, a second pipe 22, and a third pipe 23. The pipes 21 to 23 are made of stainless steel, and have a length of 80 mm and an outer diameter of 16 mm. The second pipe 22 and the third pipe 23 are arranged side by side on the left and right and in contact with each other. The first pipe 21 is disposed above the second pipe 22 and the third pipe 23. In a plan view, the central axis of the first pipe 21 is located at the position of the tangent line between the second pipe 22 and the third pipe 23.
[0069] A surface protection film is attached to the surface of a polarizing plate (TAC polarizing plate) using a TAC film (thickness 60 μm) as a polarizer protection film, to obtain an optical component 20 (see FIG. 3). The optical component 20 has a surface protection film 10 attached to the surface of an optical product 5 (polarizing plate).
[0070] The optical component 20 is sandwiched between the pipes 22, 23 and the pipe 21. At a temperature of 23°C, the pipe 21 is brought close to the pipes 22, 23, and a load of 300 g is applied to the optical component 20. The load is applied for 20 seconds. The presence or absence of pressure marks at the points pressed by the pipes 21 to 23 is checked. If no pressure marks are formed, the result is marked as "◯" (Good). If pressure marks are formed, the result is marked as "×" (No Good).
[0071] The measurement results for the surface protection films of Examples 1 to 7 and Comparative Examples 1 to 6 are shown in Table 1.
[0072] [Table 1]
[0073] From Table 1, we can see the following: The surface protection films of Examples 1 to 7 had a stress decay rate against a TAC film of 0.5% or more and 3.0% or less. The surface protection films of Examples 1 to 7 had low peeling electrification voltages against a TAC polarizing plate and a PMMA polarizing plate. No pressure marks were observed in the surface protection films of Examples 1 to 7. Press marks were observed in Comparative Examples 1, 2, 4, and 5, which had high stress attenuation rates. In Comparative Examples 3 and 6, which had low stress attenuation rates, the peeling electrification voltage against the PMMA polarizing plate increased. Thus, it was difficult to simultaneously suppress the formation of the pressing marks in the pressing test and the peeling electrification voltage in Comparative Examples 1 to 6. In contrast, in Examples 1 to 7, by setting the stress decay rate within the above-mentioned range, it was possible to suppress the formation of the pressing marks and reduce the peeling electrification voltage. [Explanation of symbols]
[0074] Reference Signs List 1...base film, 2...adhesive layer, 3...release film, 5...adherend (optical product), 10...surface protection film, 20...optical component.
Claims
1. The present invention comprises a base film made of a transparent resin and a pressure-sensitive adhesive layer formed on one surface of the base film, the pressure-sensitive adhesive layer contains a poly(meth)acrylic polymer, a polyether-modified silicone compound, an isocyanate-based crosslinking agent, and an antistatic agent; When laminated to a TAC film, the stress decay rate measured by a loop stiffness tester is 0.5% or more and 3.0% or less. Surface protection film.
2. The surface protective film according to claim 1 , further comprising a release film attached to the side of the pressure-sensitive adhesive layer opposite to the base film.
3. 3. An optical component comprising the surface protective film according to claim 1 or 2 attached to an adherend.
Citation Information
Patent Citations
Surface protecting film and optical component whereon it is stuck
JP2005131957A
Adhesive composition, adhesive sheet and surface-protective film
JP2005314476A
Pressure sensitive adhesive composition and pressure sensitive adhesive sheet