Antifogging agent composition, and antifogging article with antifogging coating formed from that composition
The antifogging agent composition with a (meth)acrylate copolymer, sulfonic acid catalyst, and aromatic surfactants forms a durable coating that maintains antifog properties and minimizes drip marks in high-temperature, high-humidity environments, addressing the limitations of previous technologies.
Patent Information
- Application Number
- JP2023054599
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Existing antifogging agent compositions fail to maintain antifog properties in harsh high-temperature, high-humidity environments and are prone to water drip marks.
An antifogging agent composition comprising a (meth)acrylate copolymer, a sulfonic acid compound as an acid catalyst, and a combination of anionic and cationic surfactants, including a surfactant with an aromatic ring, to form a coating film that retains ion pairs and prevents surfactant outflow.
The composition maintains antifogging properties and reduces noticeable water drip marks in extreme conditions, ensuring effective performance in vehicle lamps.
Smart Images

Figure 2024142457000001 
Figure 2024142457000002 
Figure 2024142457000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an antifogging agent composition and an antifogging article having an antifogging coating film formed from the composition. [Background technology]
[0002] In vehicle lighting such as automobile headlamps, when high-humidity air enters the lamp chamber, the lens is cooled by the outside air or rainfall, and moisture condenses on the inner surface, causing fogging. As a result, the brightness of the vehicle light decreases and the aesthetic appearance of the lens surface is impaired, which may cause discomfort to the user. In order to prevent such fogging of the lens, a method is known in which an anti-fogging agent is applied to the area where fogging occurs (the inner side of the lens) to form an anti-fogging coating film (dried coating film or hardened coating film) (Patent Document 1).
[0003] Patent Document 1 discloses an antifogging agent composition containing a specific copolymer (A), an acid catalyst (B), and a surfactant (C). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2019-006881 A Summary of the Invention [Problem to be solved by the invention]
[0005] Because the interior of a lamp chamber is subject to high temperatures and humidity, there is a demand for an anti-fog coating that can maintain its anti-fogging properties even in such a harsh environment and in which any traces of dripping water are not easily noticeable.
[0006] Patent Document 1 discloses an antifogging agent composition that has the performance required for vehicle lighting fixtures and is capable of forming an antifogging coating film that is particularly excellent in antifogging durability.
[0007] However, the antifogging agent composition disclosed in the above Patent Document 1 cannot maintain antifogging properties in a harsh high-temperature and high-humidity environment, and there is concern that water drip marks that occur will be noticeable.
[0008] The present invention has been made in consideration of the above-mentioned circumstances, and has an object to provide an anti-fog agent composition capable of forming an anti-fog coating film whose anti-fog properties do not decrease even in a severe high-temperature and high-humidity environment and on which any traces of dripping water are not easily noticeable, and an anti-fog article having the anti-fog coating film. [Means for solving the problem]
[0009] That is, the present invention provides an antifogging agent composition comprising a copolymer (A), an acid catalyst (B), and a surfactant (C), wherein the copolymer (A) is a (meth)acrylate copolymer obtained from a monomer mixture, and the monomer mixture is a (meth)acrylate copolymer represented by the general formula (1): [ka] (In general formula (1), R 1 is a hydrogen atom or a methyl group, and R 2 is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.), the acid catalyst (B) contains a sulfonic acid compound, and the surfactant (C) contains an anionic surfactant (C-1) and a cationic surfactant (C-2) having an aromatic ring.
[0010] The present invention also relates to an anti-fogging article having an anti-fogging coating film formed from the anti-fogging agent composition. Effect of the Invention
[0011] The details of the mechanism of action of the antifogging agent composition, antifogging coating film, and antifogging article of the present invention are presumed to be as follows, although the present invention is not necessarily limited to this mechanism of action.
[0012] The copolymer (A) containing the monomer (A-1) and the aromatic cationic surfactant (C-2) have good compatibility and are highly retained in the coating film. In addition, the anionic surfactant (C-1) and the cationic surfactant (C-2) having an aromatic ring form an ion pair in the coating film. As described above, the copolymer (A) retains the ion pair of the anionic surfactant (C-1) and the cationic surfactant (C-2) having an aromatic ring in the coating film, preventing the surfactant from leaking out of the coating film, so that the anti-fogging properties do not decrease under harsh high-temperature and high-humidity environments, and water drip marks are less noticeable. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The antifogging agent composition of the present invention contains a copolymer (A), an acid catalyst (B), and a surfactant (C).
[0014] <Copolymer (A)> The copolymer (A) of the present invention is a (meth)acrylate copolymer obtained from a monomer mixture, and the monomer mixture contains at least the following monomer (A-1):
[0015] <Monomer (A-1)> The monomer (A-1) of the present invention is represented by the general formula (1): [ka] (In general formula (1), R 1 is a hydrogen atom or a methyl group, and R 2 is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.
[0016] The monomer (A-1) mainly functions to form a crosslinked structure in the copolymer by crosslinking between molecules through a dehydration condensation reaction between N-methylol groups or N-methylol ether groups, and a dealcoholization condensation reaction between N-methylol groups or N-methylol ether groups and a hydroxyl group. This condensation reaction is accelerated by an acid catalyst.
[0017] Examples of the monomer (A-1) include N-methylol (meth)acrylamide, N-methoxymethyl (meth)acrylamide, N-propoxymethyl (meth)acrylamide, N-butoxymethyl (meth)acrylamide, and N-isobutoxymethyl (meth)acrylamide. The monomer (A-3) is preferably N-methylol (meth)acrylamide from the viewpoint of excellent water resistance and excellent heat curing of the coating film. At least one type of the monomer (A-1) may be used, or two or more types may be used in combination.
[0018] By using the monomer (A-2) having an aromatic ring in combination with the monomer (A-1), excellent adhesion can be achieved and the elution of the surfactant can be further suppressed.
[0019] Examples of the monomer (A-2) include vinyl monomers having a hydrocarbon aromatic ring, such as styrene, phenyl (meth)acrylate, hydroxyphenyl (meth)acrylate, benzyl (meth)acrylate, polyalkylene glycol monophenyl ether (meth)acrylate, polyalkylene glycol monophenyl phenyl ether (meth)acrylate, and phenoxybenzyl (meth)acrylate; vinyl monomers having a nitrogen-containing aromatic ring, such as 2-vinylpyridine, 4-vinylpyridine, and 2-vinylpyrrole; vinyl monomers having an oxygen-containing aromatic ring, such as 2-vinylfuran; and vinyl monomers having a sulfur-containing aromatic ring, such as 3-vinylthiophene. The monomer (A-2) is preferably a vinyl monomer having a hydrocarbon aromatic ring, from the viewpoint of excellent water resistance and excellent adhesion of the coating film. The monomer (A-2) may be used in combination of two or more kinds.
[0020] The proportions of the individual monomer components in the monomer mixture forming the copolymer (A) of the present invention will be described below.
[0021] The proportion of the monomer (A-1) in the monomer mixture is preferably 1 to 30% by weight, more preferably 3% by weight or more and even more preferably 5% by weight or more from the viewpoints of improving water resistance and suppressing water drip marks, and more preferably 20% by weight or less and even more preferably 15% by weight or less from the viewpoints of improving adhesion.
[0022] When the monomer (A-2) is used, the proportion of the monomer (A-2) in the monomer mixture is preferably 0.1 to 15% by weight. From the viewpoints of improving adhesion and suppressing water drip marks, the proportion of the monomer (A-2) in the monomer mixture is more preferably 1% by weight or more, and even more preferably 3% by weight or more, and from the viewpoints of improving anti-fogging properties, it is more preferably 10% by weight or less, and even more preferably 8% by weight or less.
[0023] In addition, the monomer mixture may contain, as another monomer (A-3) other than the monomer (A-1) and the monomer (A-2), for example, methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, cyclohexyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, oleyl (meth)acrylate, vinyl monomers containing a hydrocarbon group such as acrylate; N-methyl(meth)acrylamide, N-ethyl(meth)acrylamide, Nn-propyl(meth)acrylamide, N-isopropyl(meth)acrylamide; N,N-dialkyl(meth)acrylamide monomers such as N,N-dimethyl(meth)acrylamide and N,N-diethyl(meth)acrylamide; vinyl monomers containing a quaternary ammonium salt such as (meth)acryloyloxyethyltrimethylammonium chloride and (meth)acryloylaminopropyltrimethylammonium chloride; Carboxy group-containing vinyl monomers such as methacrylic acid, itaconic acid, crotonic acid, and maleic acid, and their ammonium salts, organic amine salts, and alkali metal salts; sulfonic acid group-containing vinyl monomers such as vinyl sulfonic acid, methallyl sulfonic acid, 2-(meth)acrylamido-2-methylpropanesulfonic acid, and 3-sulfopropyl(meth)acrylate, and their ammonium salts, organic amine salts, and alkali metal salts; phosphoric acid group-containing vinyl monomers such as 2-(meth)acryloyloxyethyl acid phosphate, and their ammonium salts, organic amine salts, and alkali metal salts; functional amine salts, alkali metal salts; bifunctional (meth)acrylates such as 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol (meth)acrylate, 1,10-decanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, glycerin di(meth)acrylate, and N,N'-methylenebis[(meth)acrylamide]; polyfunctional vinyl monomers such as trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, and pentaerythritol tetra(meth)acrylate;Vinyl monomers having an alkoxysilyl group, such as γ-(meth)acryloxypropyltrimethoxysilane, γ-(meth)acryloxypropyltriethoxysilane, and vinyltrimethoxysilane; and epoxy group-containing vinyl monomers, such as glycidyl (meth)acrylate, vinyl glycidyl ether, and allyl glycidyl ether, can be used. From the viewpoint of excellent anti-fogging properties of the coating film, the monomer (A-3) is preferably an N,N-dialkyl (meth)acrylamide monomer, and from the viewpoint of excellent water resistance of the coating film, a hydrocarbon group-containing vinyl monomer is preferred. The monomer (A-3) may be used in combination of two or more kinds.;
[0024] When an N,N-dialkyl(meth)acrylamide monomer is used as the monomer (A-3), the ratio of the N,N-dialkyl(meth)acrylamide monomer in the monomer mixture is preferably 10% by weight or more and 60% by weight or less, more preferably 20% by weight or more and 50% by weight or less. When a hydrocarbon group-containing vinyl monomer is used as the monomer (A-3), the ratio of the hydrocarbon group-containing vinyl monomer in the monomer mixture is preferably 20% by weight or more and 70% by weight or less, more preferably 30% by weight or more and 60% by weight or less.
[0025] In the monomer mixture, the total proportion of the monomers (A-1) to (A-3) is preferably 85% by weight or more, more preferably 90% by weight or more, and even more preferably 95% by weight or more.
[0026] <Method for producing copolymer (A)> The copolymer (A) of the present invention is obtained by copolymerizing the monomer mixture. The copolymer structure may be any of random copolymers, alternating copolymers, block copolymers and graft copolymers, but a random copolymer is preferred from the viewpoint of improving the effects of the antifogging agent composition, including antifogging properties, and easily preparing the antifogging agent composition. As a polymerization method for obtaining the copolymer, various known polymerization methods such as radical polymerization, cationic polymerization, living anionic polymerization and living cationic polymerization are adopted, but the radical polymerization method is preferred from the viewpoint of ease of industrial productivity and wide-ranging performance. As the radical polymerization method, a normal bulk polymerization method, suspension polymerization method, solution polymerization method, emulsion polymerization method and the like are adopted, but the solution polymerization method is preferred from the viewpoint of being able to be used as an antifogging agent composition as it is after polymerization.
[0027] Examples of the polymerization solvent used in the solution polymerization method include alcohol-based solvents such as methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, s-butanol, t-butanol, and diacetone alcohol; alcohol ether-based solvents such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, 3-methoxy-1-butanol, and 3-methoxy-3-methyl-1-butanol; ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; cyclic ether-based solvents such as tetrahydrofuran and dioxane; ester-based solvents such as methyl acetate, ethyl acetate, n-butyl acetate, isobutyl acetate, t-butyl acetate, methyl lactate, and ethyl lactate; aromatic solvents such as benzene, toluene, and xylene; amide-based solvents such as formamide and dimethylformamide; and water. At least one of the polymerization solvents may be used, and two or more of them may be used in combination.
[0028] In addition, the polymerization solvent preferably has a boiling point of less than 180°C at 1 atmosphere, since solvents with extremely high boiling points may impair the adhesion of the coating film to the substrate when the coating film is dried or heat-cured due to residual solvent.
[0029] The radical polymerization initiator may be a commonly used organic peroxide, an azo compound, or the like. Examples of the organic peroxide include benzoyl peroxide, 3,5,5-trimethylhexanoyl peroxide, t-butylperoxy-2-hexanoate, t-butylperoxypivalate, and t-hexylperoxypivalate. Examples of the azo compound include 2,2'-azobisisobutyronitrile and 2,2'-azobis-2-methylbutyronitrile. At least one type of the radical polymerization initiator may be used, and two or more types may be used in combination.
[0030] The amount of the radical polymerization initiator added is preferably 0.01 to 5 parts by weight based on 100 parts by weight of the monomer mixture. The radical polymerization initiator is preferably added dropwise to a reaction vessel while polymerization is carried out, since this makes it easier to control heat generated by polymerization. The temperature at which the polymerization reaction is carried out is appropriately changed depending on the type of radical polymerization initiator used, but is preferably 30 to 150°C, more preferably 40 to 100°C, in terms of industrial production.
[0031] The weight average molecular weight (Mw) of the copolymer (A) is preferably 20,000 or more, more preferably 30,000 or more, from the viewpoint of imparting water resistance to the anti-fog coating film, and is preferably 120,000 or less, more preferably 110,000 or less, from the viewpoint of improving the coatability and handleability of the anti-fog agent composition.
[0032] The weight average molecular weight (Mw) of the copolymer (A) can be determined by a GPC method using a sample that is dissolved in dimethylformamide to prepare a 0.2 wt% solution and filtered through a 0.45 μm membrane filter, and can be measured under the following conditions. <Measurement of weight average molecular weight (Mw)> Analytical equipment: HLC-8320GPC (Tosoh Corporation) Column: KD-802.5 (Showa Denko K.K.), KD-803 (Showa Denko K.K.), KD-80M (Showa Denko K.K.) connected in series Column size: 8.0 x 300 mm Eluent: dimethylformamide Flow rate: 1.0mL / min Detector: Differential refractometer Column temperature: 40℃ Standard sample: polystyrene
[0033] <Acid catalyst (B)> The acid catalyst (B) of the present invention is a sulfonic acid compound, and functions as a catalyst for promoting the crosslinking reaction caused by the monomer (A-1).
[0034] Examples of the acid catalyst (B) include alkylsulfonic acid compounds such as methanesulfonic acid, ethanesulfonic acid, and 1-propanesulfonic acid; and sulfonic acid compounds having an aromatic ring such as benzenesulfonic acid, styrenesulfonic acid, dodecylbenzenesulfonic acid, p-toluenesulfonic acid, 4-ethylbenzenesulfonic acid, p-chlorobenzenesulfonic acid, m-xylene-4-sulfonic acid, 3-pyridinesulfonic acid, dinonylnaphthalenesulfonic acid, dinonylnaphthalenedisulfonic acid, 1-pyrenesulfonic acid, and polystyrenesulfonic acid.
[0035] The acid catalyst (B) is preferably a sulfonic acid compound having an aromatic ring, from the viewpoints of excellent curability and less noticeable water drip marks. At least one type of the acid catalyst (B) may be used, or two or more types may be used in combination.
[0036] The amount of the acid catalyst (B) is preferably 0.1 to 10 parts by weight based on 100 parts by weight of the copolymer (A). From the viewpoints of improving water resistance and antifogging performance and suppressing water drip marks, the amount of the acid catalyst (B) is more preferably 0.5 parts by weight or more, even more preferably 1 part by weight or more, and more preferably 8 parts by weight or less, even more preferably 7 parts by weight or less based on 100 parts by weight of the copolymer (A).
[0037] <Surfactant (C)> The surfactant (C) of the present invention contains at least an anionic surfactant (C-1) and a cationic surfactant having an aromatic ring (C-2).
[0038] As the anionic surfactant (C-1), any of the conventionally known surfactants can be used, including, for example, fatty acid salts such as sodium oleate and potassium oleate; higher alcohol sulfates such as sodium lauryl sulfate and ammonium lauryl sulfate; alkylbenzene sulfonates and alkylnaphthalene sulfonates such as sodium dodecylbenzene sulfonate and sodium alkylnaphthalene sulfonate; and polyoxyethylene sulfates such as dialkyl naphthalene sulfonate, marine condensates, dialkyl sulfosuccinates, dialkyl phosphates, and sodium polyoxyethylene alkylphenyl ether sulfate. As the anionic surfactant (C-1), for example, fluorine-containing anionic surfactants such as perfluoroalkyl carboxylates, perfluoroalkyl sulfonates, and perfluoroalkyl phosphates can be used. As the anionic surfactant (C-1), from the viewpoint of excellent anti-fogging performance and anti-fogging durability, dialkyl sulfosuccinates are preferred, and perfluoroalkyl sulfonates are more preferred. As the anionic surfactant (C-1), at least one type may be used, and two or more types may be used in combination.
[0039] As the cationic surfactant (C-2) having an aromatic ring, any of the conventionally known surfactants can be used. For example, a surfactant represented by the general formula (2): [ka] (In general formula (2), R 3 is a phenyl or benzyl group, and R 4 is an alkyl group having 1 to 18 carbon atoms or an alkenyl group having 2 to 18 carbon atoms, and X is a chlorine atom, a bromine atom, or an iodine atom. The cationic surfactant (C-2) having an aromatic ring is a compound represented by the formula: 3 is a benzyl group, R 4 is preferably a benzalkonium salt compound in which the alkyl group is a linear alkyl group having a carbon number of 8 to 18. At least one type of the anionic surfactant (C-2) may be used, and two or more types may be used in combination.
[0040] The anionic surfactant (C-1) is preferably 0.5 to 15 parts by weight relative to 100 parts by weight of the copolymer (A). From the viewpoint of improving anti-fogging properties, the anionic surfactant (C-1) is more preferably 1 part by weight or more, and even more preferably 2 parts by weight or more, relative to 100 parts by weight of the copolymer (A), and from the viewpoint of suppressing drip marks, it is more preferably 12 parts by weight or less, and even more preferably 10 parts by weight or less.
[0041] The amount of the cationic surfactant (C-2) having an aromatic ring is preferably 0.05 to 3 parts by weight relative to 100 parts by weight of the copolymer (A). From the viewpoint of improving the anti-fogging durability and the anti-fogging property after a humidity resistance test, the amount of the cationic surfactant (C-2) is more preferably 0.1 parts by weight or more, and even more preferably 0.2 parts by weight or more, relative to 100 parts by weight of the copolymer (A), and from the viewpoint of improving the water resistance and suppressing the formation of water drip marks, the amount is more preferably 2 parts by weight or less, and even more preferably 1.5 parts by weight or less.
[0042] The weight ratio ((C-2) / (C-1)) of the cationic surfactant having an aromatic ring to the anionic surfactant (C-1) is preferably 0.01 to 2.0, and more preferably 0.02 to 1.5, from the viewpoint of suppressing outflow of the surfactant and making the resulting water drip marks less noticeable.
[0043] The antifogging agent composition of the present invention may further comprise a diluent solvent.
[0044] The dilution solvent is used for the purpose of adjusting the solid content and viscosity suitable for coating of the antifogging agent composition. As the dilution solvent, it is preferable to use a polymerization solvent of the copolymer (A). The solid content and viscosity suitable for coating vary depending on the coating method, but in the case of a spray coating method, the copolymer (A) is preferably 3% by weight or more, more preferably 5% by weight or more, and preferably 30% by weight or less, more preferably 20% by weight or less in the antifogging agent composition.
[0045] The antifogging agent composition of the present invention may contain, as other components, various conventional additives such as leveling agents, antioxidants, ultraviolet absorbers, light stabilizers, etc. The amount of the other components added may be the conventional amount for each additive, and is usually 10 parts by weight or less per 100 parts by weight of the copolymer (C).
[0046] <Anti-fog articles> The anti-fog article of the present invention is produced by applying the anti-fog agent composition to an object to be coated by a coating method typically used for coating materials, and then heat-curing the composition to form an anti-fog coating film on the surface of the object to be coated.
[0047] The substrate to be coated can be any known resin substrate, regardless of its type, and examples thereof include polymethyl methacrylate resin, polycarbonate resin, polystyrene resin, acrylonitrile-styrene copolymer resin, polyvinyl chloride resin, acetate resin, ABS resin, polyester resin, and polyamide resin.
[0048] When applying the antifogging agent composition to the substrate, it is preferable to remove any foreign matter adhering to the substrate surface before application in order to increase the wettability of the antifogging agent composition to the substrate and prevent repellency. Examples of the method include dust removal using high-pressure air or ionized air, ultrasonic cleaning using a detergent solution or an alcoholic solvent, wiping using an alcoholic solvent, and cleaning using ultraviolet light and ozone. Examples of the application method include immersion, flow coating, roll coating, bar coating, and spray coating.
[0049] From the viewpoint of obtaining good anti-fogging properties and good coating appearance, the thickness of the anti-fogging coating is preferably about 0.5 to 10 μm, and more preferably about 1 to 5 μm.
[0050] The antifogging article is not limited in its application, but can be used, for example, in vehicle lighting devices for automobiles, such as headlights, auxiliary headlights, vehicle width lights, license plate lights, tail lights, parking lights, back-up lights, turn signals, auxiliary turn signals, and emergency flashers. EXAMPLES
[0051] The present invention will be described below with reference to examples, but the present invention is not limited to these.
[0052] <Example 1> <Production of Copolymer (A)> In a reaction vessel equipped with a thermometer, a stirrer, a nitrogen inlet tube and a cooling tube, 30 parts by weight of n-propyl alcohol and 100 parts by weight of n-butyl acetate were charged as a polymerization solvent, and heated to 70°C while blowing in nitrogen gas. Next, 15 parts by weight of N-methylolacrylamide as monomer (A-1), 5 parts by weight of styrene as monomer (A-2), 30 parts by weight of N,N-dimethylacrylamide as monomer (A-3), 50 parts by weight of methyl methacrylate, and 1.5 parts by weight of t-hexylperoxypivalate (manufactured by NOF Corp., trade name "Perhexyl ND" (active ingredient 70% by weight)) as a radical polymerization initiator were dissolved in 20 parts by weight of n-propyl alcohol, and the solution was dropped over 3 hours. After the dropwise addition, the mixture was stirred for 1 hour and then cooled to produce a solution of copolymer (A). The polymerization conversion rate of the charged monomer of copolymer (A) was measured by gas chromatography and found to be 100%. Furthermore, the weight average molecular weight of the copolymer (A) was measured by gel permeation chromatography and found to be 70,000. The solid content of the solution of this copolymer (A) was 40.1% by weight.
[0053] <Production of antifogging agent composition> An antifogging agent composition was produced by mixing 250 parts by weight of the solution of 100 parts by weight of the copolymer (A) obtained above with 450 parts by weight of propylene glycol monomethyl ether, 300 parts by weight of ethylene glycol monobutyl ether, 5 parts by weight of methanesulfonic acid as the acid catalyst (B), 4 parts by weight of sodium di(2-ethylhexyl)sulfosuccinate (manufactured by NOF Corp., trade name "Rapisol A80" (active ingredient 80% by weight)) as the anionic surfactant (C-1), 0.5 parts by weight of alkyl (C12-C16) benzyl dimethyl ammonium chloride (manufactured by Kao Corp., trade name "Sanisol C" (active ingredient 50% by weight)) as the cationic surfactant (C-2), and 0.05 parts by weight of polyether-modified polydimethylsiloxane (manufactured by BYK-Chemie, trade name "BYK333") as a leveling agent.
[0054] <Preparation of anti-fogging article> In an environment set at 25°C and a relative humidity of 30%, the anti-fog composition obtained above was spray-coated on a polycarbonate (PC) resin plate so that the coating film thickness after curing would be approximately 2 to 3 μm, and the plate was heat-cured at 120°C for 15 minutes to produce an anti-fog article (test piece) having an anti-fog coating film.
[0055] The test pieces obtained above were used to carry out the evaluation methods (1) to (6) below, and the results are shown in Table 1.
[0056] <(1) Steam anti-fogging properties> The test piece was placed 5cm above the water surface in a hot water bath kept at 80℃, with the coating surface facing down, and the coating was continuously irradiated with steam from the hot water bath. The presence or absence of cloudiness 10 seconds after irradiation was visually evaluated on the following three-point scale. A rating of B or above is satisfactory for practical use, and A is preferable. A: A water film is formed immediately after steam irradiation and the glass does not become cloudy. B: Clouding is observed immediately after steam irradiation, but a water film is formed and the clouding does not occur. C: Clouding was observed immediately after steam irradiation, and no water film was formed.
[0057] <(2) Adhesion> According to JIS K 5400 8.5.1, the process of applying tape to the coating film and peeling it off was repeated 30 times, and the coating film was visually evaluated for peeling according to the following four-point scale: A rating of C or higher is acceptable for practical use, B is preferable, and A is more preferable. A: No peeling was observed at all. B: Very slight peeling is observed. C: Partially peeled off. D: Completely peeled off.
[0058] <(3) Water drip marks> The test piece was placed 5 cm above the water surface of a hot water bath kept at 80°C, with the coating surface facing down, and the coating was exposed to steam from the hot water bath for 10 seconds. The test piece was then allowed to stand vertically and dried at room temperature for 1 hour. After drying, the presence or absence of dripping marks was visually evaluated on the following three-point scale. A rating of B or higher is acceptable for practical use, and A is more preferable. A: Water drip marks are not noticeable. B: Water drip marks are barely noticeable. C: Water dripping marks are noticeable.
[0059] <(4) Anti-fogging properties after high temperature and humidity test and steam test> The test piece was left to stand for 500 hours under conditions of 80°C and 85% RH, and then left to stand for 24 hours at room temperature. The test piece was then placed 5 cm above the water surface of a hot water bath kept at 80°C, with the coating surface facing down, and the coating was continuously irradiated with steam from the hot water bath. The presence or absence of cloudiness 10 seconds after irradiation was visually evaluated on the following four-point scale. Note that if the evaluation is B or higher, there is no practical problem, and if it is A, it is more preferable. A: A water film is formed immediately after steam irradiation and the glass does not become cloudy. B: Clouding is observed immediately after steam irradiation, but a water film is formed and the clouding does not occur. C: Clouding was observed immediately after steam irradiation, and no water film was formed.
[0060] <(5) Adhesion after high temperature and high humidity test> The test piece was left to stand for 500 hours under conditions of 80°C and 85% RH, and then left to stand for 24 hours at room temperature. After that, in accordance with JIS K 5400 8.5.1, the process of attaching tape to the coating film and peeling it off was repeated 30 times, and the presence or absence of peeling of the coating film was visually evaluated according to the following four stages. Note that if the evaluation is C or higher, there is no problem in practical use, if it is B, it is preferable, and if it is A, it is more preferable. A: No peeling was observed at all. B: Very slight peeling is observed. C: Partially peeled off. D: Completely peeled off.
[0061] <(6) Water drip marks after high temperature and high humidity test> The test piece was left to stand for 500 hours under conditions of 80°C and 85% RH, and then left to stand for 24 hours at room temperature. The test piece was then placed 5 cm above the water surface of a hot water bath kept at 80°C, with the coating surface facing down, and the coating was continuously exposed to steam from the hot water bath for 10 seconds. The test piece was then stood upright and dried at room temperature for 1 hour. After drying, the presence or absence of water dripping marks was visually evaluated on the following three-point scale. Note that if the evaluation was B or higher, there is no practical problem, and if it was A, it is more preferable. A: Water drip marks are not noticeable. B: Water drip marks are barely noticeable. C: Water dripping marks are noticeable.
[0062] <Examples 2 to 20, Comparative Examples 1 to 2> <Production of Copolymer (A)> Solutions of copolymers (A) of Examples 2 to 20 were produced in the same manner as in Example 1, except that the monomers in Example 1 were changed to the raw materials and their ratios shown in Tables 1 and 2.
[0063] <Production of antifogging agent composition and preparation of antifogging article> Antifogging agent compositions of Examples 2 to 20 and Comparative Examples 1 and 2 were produced in the same manner as in Example 1, except that the raw materials of Example 1 were changed to the raw materials and their ratios shown in Tables 1 and 2. Furthermore, antifogging articles (test pieces) having antifogging coating films of Examples 2 to 20 and Comparative Examples 1 and 2 were produced in the same manner as in Example 1.
[0064] The results obtained by using the test pieces obtained above and the evaluation methods (1) to (6) above are shown in Tables 1 and 2.
[0065] [Table 1]
[0066] [Table 2]
[0067] In Tables 1 and 2, monomers (A-1) to (A-3) are: N-MAA, N-methylolacrylamide; N-MMA, N-methoxymethylacrylamide; St is styrene; BzA, benzyl acrylate; 2VP is 2-vinylpyridine; DMAA is N,N-dimethylacrylamide; DEAA, N,N-diethylacrylamide; MMA, methyl methacrylate; BA represents butyl acrylate.
[0068] In Tables 1 and 2, the acid catalyst (B) is MSA, methanesulfonic acid; pTS, p-toluenesulfonic acid; DBS, dodecylbenzenesulfonic acid; PSS refers to polystyrene sulfonic acid (manufactured by Nouryon, trade name "VERSA-TL72", active ingredient 18% by weight).
[0069] In Tables 1 and 2, surfactant (C) is Rapisol A80 is a dialkyl sulfosuccinate (NOF Corp., active ingredient 80% by weight); Futergent 100 is a fluorine-containing sulfonate (manufactured by Neos, active ingredient 100% by weight); Sanizol C is alkyl (C12-C16) benzyl dimethyl ammonium chloride (Kao Corporation, active ingredient 50% by weight); BTMAC100 is benzyltrimethylammonium chloride (Lion Specialty Chemicals, active ingredient 100% by weight); LipoCard PH100 is phenyltrimethylammonium chloride (Lion Specialty Chemicals, active ingredient 100% by weight); BDAB: benzyldodecyldimethylammonium bromide (Tokyo Chemical Industry Co., Ltd., active ingredient 100% by weight); DTAC stands for dodecyltrimethylammonium chloride (Tokyo Chemical Industry Co., Ltd., active ingredient 100% by weight).
[0070] In Tables 1 and 2, as the leveling agent, BYK-333 refers to polyether-modified polydimethylsiloxane (manufactured by BYK-Chemie, active ingredient 100% by weight).
[0071] The values in each table indicate the amount of active ingredient.
Claims
1. An antifogging agent composition comprising a copolymer (A), an acid catalyst (B), and a surfactant (C), The copolymer (A) is a (meth)acrylate copolymer obtained from a monomer mixture, The monomer mixture is represented by the general formula (1): 【Chemistry 1】 (In general formula (1), R 1 is a hydrogen atom or a methyl group, R 2 is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms; The acid catalyst (B) contains a sulfonic acid compound, The antifogging agent composition is characterized in that the surfactant (C) contains an anionic surfactant (C-1) and a cationic surfactant having an aromatic ring (C-2).
2. 2. The antifogging agent composition according to claim 1, wherein the monomer mixture constituting the copolymer (A) contains a monomer (A-2) having an aromatic ring.
3. The cationic surfactant (C-2) having an aromatic ring is represented by the general formula (2): 【Chemistry 2】 (In general formula (2), R 3 is a phenyl group or a benzyl group, R 4 is an alkyl group having 1 to 18 carbon atoms or an alkenyl group having 2 to 18 carbon atoms, and X is a chlorine atom, a bromine atom or an iodine atom.
4. 3. An anti-fogging article comprising an anti-fogging coating film formed from the anti-fogging agent composition according to claim 1 or 2.
Citation Information
Patent Citations
Coating agent for forming antifogging coated film, antifogging coated film forming article and manufacturing method of antifogging coated film forming article
JP2017019985A
Antifogging agent composition, and antifogging article having antifogging coating film
JP2019006881A
Antifogging agent composition and antifogging article having antifogging coating film
JP2022092158A
Antifogging coating
JP2022127163A
Alkali-soluble hydrophilic polymer coatings
US5093396A