Polyurethane resin composition, sealant and electric and electronic parts

JP2024142474AActive Publication Date: 2024-10-11SANYU REC
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023054621
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
2043-03-30

AI Technical Summary

Benefits of technology

【0011】 本発明のポリウレタン樹脂組成物は、バイオマス由来の原料を用いていても、柔軟性が高く、伸び率が高く、耐湿性に優れた樹脂製品を製造することができる。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142474000001
    Figure 2024142474000001
  • Figure 2024142474000002
    Figure 2024142474000002
  • Figure 2024142474000003
    Figure 2024142474000003
Patent Text Reader

Abstract

To provide a resin composition that enables the production of a resin product with high flexibility, high elongation, and superior moisture resistance even when employing biomass-derived raw materials.SOLUTION: A polyurethane resin composition comprises (A) an isocyanate group-containing compound, (B) a polyetherpolyol made from biomass-derived glycol, and (C) an epoxy group-containing compound, where the glycol is 1,3 propanediol and / or 1,4 butanediol.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyurethane resin composition, a sealing material, and an electric / electronic part. [Background technology]

[0002] In recent years, the density and integration of electric and electronic components has increased, and there is a demand for improved reliability for each component.

[0003] In order to protect these electric and electronic components, they are sealed with a sealant, and polyurethane resins are used as such sealants (see, for example, Patent Document 1).

[0004] In recent years, various problems have been raised, such as an increase in the amount of waste resin products such as plastic materials, and concerns about global warming caused by carbon dioxide generated during the incineration of resin products. For this reason, from the viewpoint of consideration for the global environment and the human body, the production of resin products from resin compositions using raw materials derived from biomass has attracted much attention.

[0005] However, resin products manufactured using resin compositions using raw materials derived from biomass have a problem that their flexibility is reduced, resulting in a low elongation rate. When such resin products are used in electrical and electronic components, etc., there is a problem that the breaking elongation is insufficient when stress is applied. A moderate elongation rate is required for polyurethane resins. When a polyurethane resin is used to resin-seal the entire printed circuit board of an electrical and electronic component, for example, it is required to follow the deformation of the printed circuit board and maintain high sealing properties. In addition, in thermal shock tests and the like, it is required to have excellent crack resistance at low temperatures and to follow the cast parts and cases, and further, moisture resistance is also required.

[0006] Therefore, there is a demand for the development of a resin composition that can be used to produce resin products that have high flexibility, high elongation, and excellent moisture resistance, even when using raw materials derived from biomass. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2020-35640 A Summary of the Invention [Problem to be solved by the invention]

[0008] An object of the present invention is to provide a resin composition that can be used to produce a resin product having high flexibility, high elongation, and excellent moisture resistance even when a raw material derived from biomass is used. [Means for solving the problem]

[0009] Means for Solving the Problems The present inventors have conducted intensive research and have found that the above-mentioned object can be achieved by a polyurethane resin composition containing an isocyanate group-containing compound, a polyether polyol made from a biomass-derived glycol, and an epoxy group-containing compound, in which a specific glycol is used, and have thus completed the present invention.

[0010] That is, the present invention relates to the following polyurethane resin composition, sealing material, and electric / electronic part. 1. A polyurethane resin composition comprising (A) an isocyanate group-containing compound, (B) a polyether polyol made from a biomass-derived glycol, and (C) an epoxy group-containing compound, The glycol is 1,3 propanediol and / or 1,4 butanediol; A polyurethane resin composition comprising: 2. The polyurethane resin composition according to item 1, wherein the content of the (B) polyether polyol made from a biomass-derived glycol is 25 to 80 mass % relative to 100 mass % of the polyurethane resin composition. 3. The polyurethane resin composition according to item 1 or 2, wherein the content of the (C) epoxy group-containing compound is 0.5 to 60 parts by mass per 100 parts by mass of the (B) polyether polyol made from a biomass-derived glycol. 4. The polyurethane resin composition according to item 1 or 2, wherein the content of the (C) epoxy group-containing compound is 0.5 to 35 parts by mass per 100 parts by mass of the (B) polyether polyol made from a biomass-derived glycol. 5. The polyurethane resin composition according to any one of items 1 to 4, wherein the (A) isocyanate group-containing compound is at least one selected from the group consisting of diphenylmethane diisocyanate and modified products thereof, and hexamethylene diisocyanate and modified products thereof. 6. The polyurethane resin composition according to any one of items 1 to 5, wherein the content of the (A) isocyanate group-containing compound is 10 to 40 parts by mass per 100 parts by mass of the (B) polyether polyol made from a biomass-derived glycol. 7. The polyurethane resin composition according to any one of items 1 to 6, further comprising (D) a castor oil-based polyol. 8. The polyurethane resin composition according to item 7, wherein the content of the castor oil-based polyol (D) is 50 parts by mass or less, based on 100 parts by mass of the polyurethane resin composition. 9. An encapsulant comprising the polyurethane resin composition according to any one of items 1 to 8. 10. An electric / electronic component resin-encapsulated using the encapsulant according to item 9. Effect of the Invention

[0011] Even when a biomass-derived raw material is used, the polyurethane resin composition of the present invention makes it possible to produce a resin product that has high flexibility, high elongation, and excellent moisture resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The polyurethane resin composition, the sealing material, and the electric / electronic part of the present invention will be described in detail below.

[0013] 1. Polyurethane resin composition The polyurethane resin composition of the present invention is a polyurethane resin composition containing (A) an isocyanate group-containing compound (hereinafter also referred to as "(A) component"), (B) a polyether polyol (hereinafter also referred to as "(B) component") made from a biomass-derived glycol, and (C) an epoxy group-containing compound (hereinafter also referred to as "(C) component"), in which the glycol is 1,3-propanediol and / or 1,4-butanediol. The polyurethane resin composition of the present invention uses the above-mentioned (B) component as a raw material of a biomass-derived glycol, and uses 1,3-propanediol and / or 1,4-butanediol as the glycol. The polyurethane resin composition of the present invention contains an epoxy group-containing compound as the component (C) in addition to the above-mentioned (A) and (B) components. The polyurethane resin composition of the present invention uses a specific glycol as the raw material of the (B) component and contains an epoxy group-containing compound as the (C) component, so that even if a biomass-derived raw material is used, a resin product with high flexibility and high elongation can be produced.

[0014] The biomass degree of the polyurethane resin composition of the present invention is preferably 10% or more, more preferably 20% or more, and even more preferably 30% or more. The upper limit of the biomass degree of the polyurethane resin composition of the present invention is preferably as high as possible, and may be 100%, 90%, or 80%.

[0015] In this specification, the biomass degree of the polyurethane resin composition and each raw material is measured by the following measurement method.

[0016] How to measure biomass content The biomass degree of each raw material is measured from the C14 content using an accelerator mass spectrometer. The measured biomass degree (%) of each raw material is multiplied by the blending ratio of each raw material and the sum is calculated to calculate the biomass degree of the polyurethane resin composition.

[0017] ((A) Isocyanate Group-Containing Compound) The (A) isocyanate group-containing compound used in the polyurethane resin composition of the present invention is not particularly limited, and various compounds that have been conventionally used as isocyanate group-containing compounds in polyurethane resin compositions can be used. Examples of the isocyanate group-containing compound include aliphatic polyisocyanate compounds, alicyclic polyisocyanate compounds, aromatic polyisocyanate compounds, and aromatic aliphatic polyisocyanate compounds.

[0018] Examples of the aliphatic polyisocyanate compound include tetramethylene diisocyanate, dodecamethylene diisocyanate, hexamethylene diisocyanate (HDI), 2,2,4-trimethylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, lysine diisocyanate, 2-methylpentane-1,5-diisocyanate, and 3-methylpentane-1,5-diisocyanate.

[0019] Examples of the alicyclic polyisocyanate compound include isophorone diisocyanate, hydrogenated xylylene diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, 1,4-cyclohexane diisocyanate, methylcyclohexylene diisocyanate, and 1,3-bis(isocyanatemethyl)cyclohexane.

[0020] Examples of aromatic polyisocyanate compounds include tolylene diisocyanate, 2,2'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 4,4'-diphenylmethane diisocyanate (MDI), 4,4'-dibenzyl diisocyanate, 1,5-naphthylene diisocyanate, xylylene diisocyanate, 1,3-phenylene diisocyanate, and 1,4-phenylene diisocyanate.

[0021] Examples of the aromatic aliphatic polyisocyanate compound include dialkyldiphenylmethane diisocyanate, tetraalkyldiphenylmethane diisocyanate, α,α,α,α-tetramethylxylylene diisocyanate, and the like.

[0022] The isocyanate group-containing compound may contain an isocyanurate-modified product and / or an allophanate-modified product of the polyisocyanate compound. When the isocyanate group-containing compound contains an isocyanurate-modified product and / or an allophanate-modified product of the polyisocyanate compound, the polyurethane resin composition can exhibit better heat resistance.

[0023] As the component (A), at least one selected from the group consisting of diphenylmethane diisocyanate, modified products of diphenylmethane diisocyanate, hexamethylene diisocyanate, and modified products of hexamethylene diisocyanate can be suitably used.

[0024] The above isocyanate group-containing compounds may be used alone or in combination of two or more kinds.

[0025] The content of the (A) component is preferably 10 to 40 parts by mass, and more preferably 15 to 35 parts by mass, based on 100 parts by mass of the (B) polyether polyol made from biomass-derived glycol. When the upper limit of the (A) component content is within the above range, the curability of the polyurethane resin composition is further improved. When the lower limit of the (A) component content is within the above range, the hydrolysis resistance and curability of the cured polyurethane resin composition are further improved.

[0026] ((B) Polyether polyol made from biomass-derived glycol) In the polyurethane resin composition of the present invention, the component (B) is a polyether polyol made from a biomass-derived glycol, and the biomass-derived glycol is 1,3-propanediol and / or 1,4-butanediol. The glycol is 1,3-propanediol and / or 1,4-butanediol, and any known glycol may be used as long as it is derived from biomass.

[0027] The above-mentioned biomass-derived glycol refers to 1,3 propanediol and / or 1,4 butanediol, which can be synthesized using natural components such as plants as starting materials.

[0028] The component (B) is not particularly limited as long as it is a polyether polyol containing a biomass-derived glycol in the raw material, and may be a copolymer containing other glycols in the raw material other than the biomass-derived glycol, but it is preferable that the raw material does not contain other glycols. Such other glycols are not particularly limited, and various types of glycols that have been conventionally used as polyol components in polyurethane resin compositions can be used.

[0029] Examples of the other glycols include polybutadiene polyol, ethylene glycol, 1,3-propanediol, 1,2-propanediol, 2-methyl-1,3-propanediol, 1,4-butanediol, 1,3-butanediol, 1,4 pentanediol, 1,5-pentanediol, 1,6-hexanediol, 1,5-hexanediol, 1,2-hexanediol, 2,5-hexanediol, octanediol, nonanediol, decanediol, diethylene glycol, triethylene glycol, dipropylene glycol, cyclohexanediol, trimethylolpropane, glycerin, and 2-methylpropane. Examples of suitable polyols include 1,2,3-triol, 1,2,6-hexanetriol, pentaerythritol, polylactone diol, polylactone triol, ester glycol, castor oil-based polyol, polyolefin polyol, polyester polyol, polyether polyol, polycarbonate polyol, acrylic polyol, silicone polyol, fluorine polyol, polytetramethylene glycol, polytetramethylene ether glycol, polypropylene glycol, polyethylene glycol, polycaprolactone polyol, hydrogenated hydroxyl group-containing liquid polyisoprene, and hydrogenated hydroxyl group-containing liquid polybutadiene.

[0030] The content of the (B) component is preferably 25 to 80% by mass, and more preferably 40 to 75% by mass, based on 100% by mass of the polyurethane resin composition of the present invention. When the upper limit of the (B) component content is within the above range, the flexibility and elongation of a resin product produced using the polyurethane resin composition are further improved. When the (B) component content is within the above range, the hardness of a resin product produced using the polyurethane resin composition is further improved.

[0031] In the polyurethane resin composition of the present invention, the NCO / OH ratio between the (A) component and the (B) component is preferably 0.6 to 2.0, and more preferably 0.7 to 1.5. When the lower limit of the NCO / OH ratio is within the above range, the heat resistance of the polyurethane resin composition is further improved. When the upper limit of the NCO / OH ratio is within the above range, the curability of the polyurethane resin composition is further improved.

[0032] ((C) Epoxy Group-Containing Compound) The epoxy group-containing compound (C) used in the polyurethane resin composition of the present invention is not particularly limited, and various compounds conventionally used in resin compositions can be used.

[0033] The component (C) may be any compound having an epoxy group in the molecule, and is not particularly limited, but preferably has an average of two or more epoxy groups in one molecule. As the epoxy group-containing compound, for example, a glycidyl ether type epoxy compound, a glycidyl amine type epoxy compound, a glycidyl ester type epoxy compound, or a cyclic aliphatic (alicyclic) epoxy compound can be used.

[0034] Examples of the glycidyl ether type epoxy compound include bisphenol A type epoxy compounds, bisphenol F type epoxy compounds, bisphenol S type epoxy compounds, bisphenol AD ​​type epoxy compounds, cresol novolac type epoxy compounds, phenol novolac type epoxy compounds, α-naphthol novolac type epoxy compounds, bisphenol A type novolac type epoxy compounds, dicyclopentadiene type epoxy compounds, tetrabromobisphenol A type epoxy compounds, brominated phenol novolac type epoxy compounds, tris(glycidyloxyphenyl)methane, and tetrakis(glycidyloxyphenyl)ethane.

[0035] Examples of the glycidylamine type epoxy compound include tetraglycidyldiaminodiphenylmethane, triglycidyl paraaminophenol, triglycidyl meta-aminophenol, and tetraglycidyl meta-xylylenediamine.

[0036] Examples of the glycidyl ester type epoxy compound include diglycidyl phthalate, diglycidyl hexahydrophthalate, and diglycidyl tetrahydrophthalate.

[0037] Examples of cyclic aliphatic (alicyclic) epoxy compounds include epoxycyclohexylmethyl-epoxycyclohexanecarboxylate and bis(epoxycyclohexyl)adipate.

[0038] As the component (C), a bisphenol A type epoxy compound or a bisphenol F type epoxy compound is preferable, and a bisphenol A type epoxy compound is more preferable.

[0039] The component (C) may be used alone or in combination of two or more kinds.

[0040] The content of the (C) component is preferably 0.5 to 35 parts by mass, more preferably 1 to 55 parts by mass, and even more preferably 5 to 40 parts by mass, based on 100 parts by mass of the (B) polyether polyol made from biomass-derived glycol. When the upper limit of the (C) component content is within the above range, the curability of the polyurethane resin composition is further improved. When the lower limit of the (C) component content is within the above range, the moisture resistance, flexibility, and elongation of a resin product produced by curing the polyurethane resin composition are further improved.

[0041] ((D) Castor oil-based polyol) The polyurethane resin composition of the present invention may contain (D) a castor oil-based polyol (hereinafter, also referred to as "component (D)"). When the polyurethane resin composition of the present invention contains component (D), the moisture resistance and insulating properties of a resin product produced using the polyurethane resin composition of the present invention are further improved.

[0042] As the above-mentioned (D) component, castor oil, castor oil fatty acid, and hydrogenated castor oil or polyols produced using hydrogenated castor oil fatty acid can be used. Examples of such polyols include castor oil, ester exchange products of castor oil and other natural fats and oils, reaction products of castor oil and polyhydric alcohols, esterification products of castor oil fatty acid and polyhydric alcohols, and polyols obtained by addition polymerization of alkylene oxides to these.

[0043] The component (D) may be used alone or in combination of two or more kinds.

[0044] The content of the (D) component is preferably 120 parts by mass or less, more preferably 80 parts by mass or less, even more preferably 50 parts by mass or less, and particularly preferably 40 parts by mass or less, based on 100 parts by mass of the polyether polyol (B) made from biomass-derived glycol. The content of the (D) component is preferably 1 part by mass or more, more preferably 5 parts by mass or more, even more preferably 10 parts by mass or more, and particularly preferably 20 parts by mass or more, based on 100 parts by mass of the polyether polyol (B) made from biomass-derived glycol. When the upper limit of the content of the (D) component is within the above range, the moisture resistance of the resin product produced using the polyurethane resin composition of the present invention is further improved. When the lower limit of the content of the (D) component is within the above range, the moisture resistance and insulating properties of the resin product produced using the polyurethane resin composition of the present invention are further improved.

[0045] ((E) Plasticizer) The polyurethane resin composition of the present invention may further contain a plasticizer (E) (hereinafter also referred to as "component (E)") in addition to the above components (A) to (D). However, it is preferable that the polyurethane resin composition does not contain a plasticizer in order to exhibit higher moisture resistance.

[0046] Examples of the plasticizer include phthalate esters such as dioctyl phthalate, diisononyl phthalate, and diundecyl phthalate; adipic acid esters such as dioctyl adipate and diisononyl adipate; trimellitic acid esters such as trioctyl trimellitate and triisononyl trimellitate; and pyromellitic acid esters such as tetraoctyl pyromellitate and tetraisononyl pyromellitate.

[0047] When the polyurethane resin composition of the present invention contains the (E) component, the content of the (E) component is preferably 70 parts by mass or less, more preferably 60 parts by mass or less, based on 100 parts by mass of the (B) polyether polyol made from biomass-derived glycol. The lower limit of the content of the (E) component is not particularly limited, and may be 1 part by mass or more, or 5 parts by mass or more, based on 100 parts by mass of the (B) polyether polyol made from biomass-derived glycol.

[0048] (Other additives) The polyurethane resin composition of the present invention may contain other additives in addition to the above components (A) to (E), such as a catalyst, an antioxidant, a moisture absorbent, an antifungal agent, a silane coupling agent, etc.

[0049] The catalyst is not particularly limited, and may be a conventionally known catalyst used in polyurethane resin compositions. Examples of such catalysts include tin catalysts such as dioctyltin dilaurate, dibutyltin dilaurate, and dioctyltin diacetate; lead catalysts such as lead octylate, lead octenate, and lead naphthenate; bismuth catalysts such as bismuth octylate and bismuth neodecanoate; and amine catalysts such as diethylenetriamine. In addition, organometallic compounds, metal complex compounds, and the like may be used as the catalyst.

[0050] The amounts of the above other additives used may be appropriately determined according to the intended use from the ranges specified by the usual amounts added so as not to impair the desired properties of the polyurethane resin composition.

[0051] (Polyurethane resin composition) The polyurethane resin composition of the present invention may be either a one-component type or a two-component type, but the polyurethane resin composition of the present invention containing the components (A), (B), and (C) is usually a two-component type resin composition. In the production method described below, the two-component type resin composition will be described.

[0052] 2. Method for producing polyurethane resin composition The method for producing the polyurethane resin composition of the present invention is not particularly limited, and the composition can be produced by any known method used for producing polyurethane resin compositions.

[0053] An example of such a production method is a method of producing the resin composition of the present invention by preparing (B) a component containing a polyether polyol component made from a biomass-derived glycol as a raw material to serve as a first component, preparing (A) a component containing an isocyanate group-containing compound to serve as a second component, and mixing the first and second components to cause a reaction to form a polyurethane resin.

[0054] As long as the first component contains the component (B) and the second component contains the component (A), the other component may be contained in either the first component or the second component.

[0055] Specific examples of the configuration of the first and second components include a configuration in which the first component contains the components (B) and (C), and the second component contains the component (A). Alternatively, the first component may contain the components (B) and (C), and optionally the components (D) and (E), and the second component may contain the component (A).

[0056] The method for preparing the first component and the second component is not particularly limited, and for example, they can be prepared by a preparation method having a step 1 of mixing and stirring the components constituting the first component and the second component in a kneader.

[0057] In the above step 1, the temperature for mixing and stirring is preferably from 60° C. to 120° C., and the stirring time may be from about 30 minutes to 3 hours.

[0058] By the above-described step 1, the first component and the second component are prepared.

[0059] The polyurethane resin composition of the present invention is produced in step 2 by mixing the first component and the second component prepared in step 1. The mixing temperature is not particularly limited, and is preferably 23° C. or higher and 60° C. or lower. The mixing time is not particularly limited, and may be appropriately set according to the pot life of the polyurethane resin composition.

[0060] The polyurethane resin composition of the present invention is produced by the step 2 described above.

[0061] 3.Cured resin material The polyurethane resin composition of the present invention can be cured to obtain a cured resin product. The cured resin product has high flexibility and high elongation, making it useful as a resin product for use in the field of electric and electronic parts.

[0062] The cured resin preferably has an initial hardness A of 0 or more, more preferably 5 or more, even more preferably 10 or more, and particularly preferably 15 or more, when the polyurethane resin composition is left to stand at a temperature of 60° C. for 16 hours to cure and obtain a cured resin. When the lower limit of the initial hardness A is within the above range, the cured resin can be more usefully used as a resin product used in the field of electric and electronic parts. In addition, the initial hardness A is preferably 70 or less, more preferably 65 or less. When the upper limit of the initial hardness A is within the above range, the flexibility and elongation of the cured resin are further improved. In this specification, the initial hardness A of the cured resin is measured by the method described in the Examples below.

[0063] The hardness of the cured resin after the moisture resistance test is preferably 0 or more, more preferably 5 or more. By setting the lower limit of the hardness after the moisture resistance test in the above range, the cured resin can be more usefully used as a resin product used in the field of electrical and electronic components. Even if the hardness of the cured resin is low, for example 0, it is preferable that the shape of the cured resin is maintained. Furthermore, the hardness of the cured resin after the moisture resistance test is preferably 70 or less, more preferably 60 or less. By setting the lower limit of the hardness after the moisture resistance test in the above range, the flexibility and elongation of the cured resin are further improved. In this specification, the method for measuring the hardness of the cured resin after the moisture resistance test is the method described in the Examples below.

[0064] 4. Sealing materials and electrical and electronic parts The present invention is also a sealant made of the polyurethane resin composition. The sealant is required to have a moderate elongation rate. When the polyurethane resin composition is used to resin seal the entire printed circuit board of an electric / electronic component, for example, it is required to follow the deformation of the printed circuit board and maintain high sealing properties. In addition, in a thermal shock test or the like, it is required to have excellent crack resistance at low temperatures and follow the cast parts and cases. The sealant made of the polyurethane resin composition can be suitably used for electric / electronic components and electric / electronic components that generate heat. Examples of such electric / electronic components include transformers such as transformer coils, choke coils, and reactor coils, device control boards, and various sensors. Such electric / electronic components resin-sealed using the sealant of the present invention are also one of the present inventions. The electric / electronic components of the present invention can be used in electric washing machines, toilet seats, water heaters, water purifiers, baths, dishwashers, power tools, automobiles, motorcycles, battery packs, and the like. EXAMPLES

[0065] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the examples.

[0066] The raw materials used in the examples and comparative examples are shown in Table 1 below.

[0067] [Table 1]

[0068] (Preparation of Polyurethane Resin Composition) The raw materials for the first component shown in Table 2 were charged into a reaction vessel and stirred at room temperature and pressure for 1 hour to prepare the first component.

[0069] The raw materials for the second component shown in Table 2 were placed in a reaction vessel equipped with heating, cooling, and pressure reduction devices, and dehydration and reaction were carried out at 60°C and a pressure of 10 mmHg or less for 1 hour to prepare the second component.

[0070] A polyurethane resin composition was obtained by adding the second component to the first component, stirring, defoaming and mixing according to the formulation shown in Table 2. The first and second components were mixed by adjusting the temperature of the first component to 23°C, then adding the second component adjusted to 23°C, and mixing at 2000 rpm for 1 minute using a planetary centrifugal mixer (Thinky Corporation, Awatori Rentaro).

[0071] Preparation of test specimens The polyurethane resin composition was poured into a molding die (test piece 1) of 130×130×3 mm and a molding die (test piece 2) of 30 mm inner diameter and 10 mm height. The polyurethane resin composition was then heated at 60° C. for 16 hours and then left at room temperature for 1 day to harden, producing a test piece.

[0072] The following tests were carried out using test pieces prepared using the polyurethane resin compositions of the Examples and Comparative Examples as described above.

[0073] Hardness A (initial hardness A) Using test piece 2 (inner diameter 30 mm, height 10 mm), the hardness (Type A) was measured at a temperature of 23°C using a hardness meter (Asker Rubber Hardness Meter Type A, manufactured by Kobunshi Keiki Co., Ltd.) according to the measurement method in accordance with JIS K6253.

[0074] Volume resistivity The volume resistivity of the test piece 1 (130×130×3 mm) was measured using a resistance measuring device (DSM-8104, manufactured by HIOKI Corporation).

[0075] Elongation (flexibility) Using test piece 1 (130×130×3 mm), the gauge length at break was measured according to a measurement method in accordance with JIS K6251, and the elongation (flexibility) was calculated according to the following formula. The elongation was also defined as the initial elongation. Elongation (%) = [(gauge length at break - gauge length) / gauge length] x 100

[0076] Hardness after moisture resistance test A pressure cooker test (PCT test) was carried out using test piece 2 (inner diameter 30 mm, height 10 mm) under conditions of 121°C, 100% RH, 2 atm, and 140 hours. After the test, the hardness of test piece 2 was measured by the above-mentioned hardness A measurement method.

[0077] Change in elongation (flexibility) after moisture resistance test Using test piece 1 (130×130×3 mm), a moisture resistance test (pressure cooker test (PCT test)) was performed under conditions of 121°C, 100% RH, 2 atm, and 140 hours. Using test piece 1 after the moisture resistance test, the elongation after the moisture resistance test was measured by the above-mentioned method for measuring elongation (flexibility), and the rate of change in elongation after the moisture resistance test was calculated according to the following formula. Change in elongation (%) = [(elongation after moisture resistance test - initial elongation) / initial elongation)] x 100

[0078] The results are shown in Tables 2 and 3.

[0079] [Table 2]

[0080] [Table 3]

Claims

1. A polyurethane resin composition comprising (A) an isocyanate group-containing compound, (B) a polyether polyol made from a biomass-derived glycol, and (C) an epoxy group-containing compound, The glycol is 1,3 propanediol and / or 1,4 butanediol; A polyurethane resin composition comprising:

2. 2. The polyurethane resin composition according to claim 1, wherein the content of the polyether polyol (B) made from a biomass-derived glycol is 25 to 80 mass% relative to 100 mass% of the polyurethane resin composition.

3. 2. The polyurethane resin composition according to claim 1, wherein a content of the epoxy group-containing compound (C) is 0.5 to 60 parts by mass relative to 100 parts by mass of the polyether polyol (B) made from a biomass-derived glycol.

4. 2. The polyurethane resin composition according to claim 1, wherein a content of the epoxy group-containing compound (C) is 0.5 to 35 parts by mass relative to 100 parts by mass of the polyether polyol (B) made from a biomass-derived glycol.

5. 2. The polyurethane resin composition according to claim 1, wherein the (A) isocyanate group-containing compound is at least one selected from the group consisting of diphenylmethane diisocyanate and modified products thereof, and hexamethylene diisocyanate and modified products thereof.

6. The polyurethane resin composition according to claim 1, wherein the content of the isocyanate group-containing compound (A) is 10 to 40 parts by mass relative to 100 parts by mass of the polyether polyol (B) made from a biomass-derived glycol.

7. The polyurethane resin composition according to claim 1, further comprising (D) a castor oil-based polyol.

8. The polyurethane resin composition according to claim 7, wherein the content of the castor oil-based polyol (D) is 50 parts by mass or less, based on 100 parts by mass of the polyurethane resin composition.

9. A sealing material comprising the polyurethane resin composition according to any one of claims 1 to 8.

10. An electric / electronic component resin-sealed with the sealing material according to claim 9 .

Citation Information

Patent Citations

  • Polyurethane sponge waterproof film

    CN114456698A

  • Bio-polyurethane resin

    JP2014037552A

  • Urethane-modified epoxy resin composition and cured product thereof

    JP2017078125A

  • Curable composition, cured product, and adhesive

    JP2021155673A

  • Self-repairing polyurethane resin raw material, self-repairing polyurethane resin, self-repairing coating material, self-repairing elastomeric material, self-repairing polyurethane resin raw material production method and self-repairing polyurethane resin production method

    WO2016098771A1