Polyurethane resin composition, sealant and electric and electronic parts
A polyurethane resin composition using biomass-derived glycol and specific additives addresses the flexibility and moisture resistance issues, ensuring high elongation and effective sealing of electronic components.
Patent Information
- Application Number
- JP2023054623
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing polyurethane resin compositions derived from biomass materials suffer from low elongation rates and insufficient flexibility, which compromises their performance in sealing electrical and electronic components, particularly in terms of moisture resistance and thermal shock resistance.
A polyurethane resin composition containing an isocyanate group-containing compound and a polyether polyol made from biomass-derived glycol, specifically 1,3 propanediol and/or 1,4 butanediol, with a biomass content of 15% or more, along with optional additives like polybutadiene polyol and ester plasticizers, to enhance flexibility and moisture resistance.
The composition achieves high flexibility, high elongation, and excellent moisture resistance, making it suitable for sealing electronic components and maintaining sealing performance under thermal stress.
Smart Images

Figure 2024142475000001 
Figure 2024142475000002 
Figure 2024142475000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyurethane resin composition, a sealing material, and an electric / electronic part. [Background technology]
[0002] In recent years, the density and integration of electric and electronic components has increased, and there is a demand for improved reliability for each component.
[0003] In order to protect these electric and electronic components, they are sealed with a sealant, and polyurethane resins are used as such sealants (see, for example, Patent Document 1).
[0004] In recent years, various problems have been raised, such as an increase in the amount of waste resin products such as plastic materials, and concerns about global warming caused by carbon dioxide generated during the incineration of resin products. For this reason, from the viewpoint of consideration for the global environment and the human body, the production of resin products from resin compositions using raw materials derived from biomass has attracted much attention.
[0005] However, resin products manufactured using resin compositions using raw materials derived from biomass have a problem that their flexibility is reduced, resulting in a low elongation rate. When such resin products are used in electrical and electronic components, etc., there is a problem that the breaking elongation is insufficient when stress is applied. A moderate elongation rate is required for polyurethane resins. When a polyurethane resin is used to resin-seal the entire printed circuit board of an electrical and electronic component, for example, it is required to follow the deformation of the printed circuit board and maintain high sealing properties. In addition, in thermal shock tests and the like, it is required to have excellent crack resistance at low temperatures and to follow the cast parts and cases, and further, moisture resistance is also required.
[0006] Therefore, there is a demand for the development of a resin composition that can be used to produce resin products that have high flexibility, high elongation, and excellent moisture resistance, even when using raw materials derived from biomass. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2020-35640 A Summary of the Invention [Problem to be solved by the invention]
[0008] An object of the present invention is to provide a resin composition that can be used to produce a resin product having high flexibility, high elongation, and excellent moisture resistance even when a raw material derived from biomass is used. [Means for solving the problem]
[0009] Means for Solving the Problems The present inventors have conducted intensive research and have found that the above-mentioned object can be achieved by a polyurethane resin composition containing an isocyanate group-containing compound and a polyether polyol made from a biomass-derived glycol, in which a specific glycol is used, and have thus completed the present invention.
[0010] That is, the present invention relates to the following polyurethane resin composition, sealing material, and electric / electronic part. 1. A polyurethane resin composition comprising (A) an isocyanate group-containing compound and (B) a polyether polyol made from a biomass-derived glycol, The glycol is 1,3 propanediol and / or 1,4 butanediol; A polyurethane resin composition comprising: 2. The polyurethane resin composition according to item 1, having a biomass ratio of 15% or more. 3. The polyurethane resin composition according to item 1 or 2, wherein the content of the (B) polyether polyol made from a biomass-derived glycol is 15 to 80 mass % relative to 100 mass % of the polyurethane resin composition. 4. The polyurethane resin composition according to any one of items 1 to 3, wherein the (A) isocyanate group-containing compound is at least one selected from the group consisting of diphenylmethane diisocyanate and modified products thereof, and hexamethylene diisocyanate and modified products thereof. 5. The polyurethane resin composition according to any one of items 1 to 4, wherein the content of the (A) isocyanate group-containing compound is 10 to 35 parts by mass per 100 parts by mass of the (B) polyether polyol made from a biomass-derived glycol. 6. The polyurethane resin composition according to any one of items 1 to 5, further comprising (C) a polybutadiene polyol. 7. The polyurethane resin composition according to item 6, wherein the content of the polybutadiene polyol (C) is 50 to 450 parts by mass per 100 parts by mass of the polyether polyol (B) made from a biomass-derived glycol. 8. The polyurethane resin composition according to any one of items 1 to 7, further comprising (D) a plasticizer. 9. The polyurethane resin composition according to item 8, wherein the plasticizer is an ester-based plasticizer. 10. The polyurethane resin composition according to item 8 or 9, wherein the content of the plasticizer (D) is 20 to 150 parts by mass per 100 parts by mass of the polyether polyol (B) made from a biomass-derived glycol. 11. An encapsulant comprising the polyurethane resin composition according to any one of items 1 to 10. 12. An electric / electronic component resin-encapsulated with the encapsulant according to item 11. Effect of the Invention
[0011] Even when a biomass-derived raw material is used, the polyurethane resin composition of the present invention makes it possible to produce a resin product that has high flexibility, high elongation, and excellent moisture resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The polyurethane resin composition, the sealing material, and the electric / electronic part of the present invention will be described in detail below.
[0013] 1. Polyurethane resin composition The polyurethane resin composition of the present invention is a polyurethane resin composition containing (A) an isocyanate group-containing compound (hereinafter also referred to as "component (A)") and (B) a polyether polyol (hereinafter also referred to as "component (B)") made from a biomass-derived glycol, the glycol being 1,3-propanediol and / or 1,4-butanediol. The polyurethane resin composition of the present invention uses component (B) made from a biomass-derived glycol as a raw material, and 1,3-propanediol and / or 1,4-butanediol is used as the glycol. Since component (B) of the polyurethane resin composition of the present invention uses a specific glycol as a raw material, it is possible to produce a resin product having high flexibility and high elongation even when a biomass-derived raw material is used.
[0014] The biomass degree of the polyurethane resin composition of the present invention is preferably 10% or more, more preferably 20% or more, and even more preferably 30% or more. The upper limit of the biomass degree of the polyurethane resin composition of the present invention is preferably as high as possible, and may be 100%, 90%, or 80%. In this specification, the method for measuring the biomass degree of the polyurethane resin composition and each raw material is the method described in the Examples below.
[0015] ((A) Isocyanate Group-Containing Compound) The (A) isocyanate group-containing compound used in the polyurethane resin composition of the present invention is not particularly limited, and various compounds that have been conventionally used as isocyanate group-containing compounds in polyurethane resin compositions can be used. Examples of the isocyanate group-containing compound include aliphatic polyisocyanate compounds, alicyclic polyisocyanate compounds, aromatic polyisocyanate compounds, and aromatic aliphatic polyisocyanate compounds.
[0016] Examples of the aliphatic polyisocyanate compound include tetramethylene diisocyanate, dodecamethylene diisocyanate, hexamethylene diisocyanate (HDI), 2,2,4-trimethylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, lysine diisocyanate, 2-methylpentane-1,5-diisocyanate, and 3-methylpentane-1,5-diisocyanate.
[0017] Examples of the alicyclic polyisocyanate compound include isophorone diisocyanate, hydrogenated xylylene diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, 1,4-cyclohexane diisocyanate, methylcyclohexylene diisocyanate, and 1,3-bis(isocyanatemethyl)cyclohexane.
[0018] Examples of aromatic polyisocyanate compounds include tolylene diisocyanate, 2,2'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 4,4'-diphenylmethane diisocyanate (MDI), 4,4'-dibenzyl diisocyanate, 1,5-naphthylene diisocyanate, xylylene diisocyanate, 1,3-phenylene diisocyanate, and 1,4-phenylene diisocyanate.
[0019] Examples of the aromatic aliphatic polyisocyanate compound include dialkyldiphenylmethane diisocyanate, tetraalkyldiphenylmethane diisocyanate, α,α,α,α-tetramethylxylylene diisocyanate, and the like.
[0020] The isocyanate group-containing compound may contain an isocyanurate-modified product and / or an allophanate-modified product of the polyisocyanate compound. When the isocyanate group-containing compound contains an isocyanurate-modified product and / or an allophanate-modified product of the polyisocyanate compound, the polyurethane resin composition can exhibit better heat resistance.
[0021] As the component (A), at least one selected from the group consisting of diphenylmethane diisocyanate, modified products of diphenylmethane diisocyanate, hexamethylene diisocyanate, and modified products of hexamethylene diisocyanate can be suitably used.
[0022] The above isocyanate group-containing compounds may be used alone or in combination of two or more kinds.
[0023] The content of the (A) component is preferably 10 to 35 parts by mass, more preferably 15 to 30 parts by mass, based on 100 parts by mass of the (B) polyether polyol made from biomass-derived glycol. When the upper limit of the (A) component content is within the above range, the curability of the polyurethane resin composition is further improved. When the lower limit of the (A) component content is within the above range, the hydrolysis resistance and curability of the polyurethane resin composition are further improved.
[0024] ((B) Polyether polyol made from biomass-derived glycol) In the polyurethane resin composition of the present invention, the component (B) is a polyether polyol made from a biomass-derived glycol, and the biomass-derived glycol is 1,3-propanediol and / or 1,4-butanediol. The glycol is 1,3-propanediol and / or 1,4-butanediol, and any known glycol may be used as long as it is derived from biomass.
[0025] The above-mentioned biomass-derived glycol refers to 1,3 propanediol and / or 1,4 butanediol, which can be synthesized using natural components such as plants as starting materials.
[0026] The component (B) is not particularly limited as long as it is a polyether polyol containing a biomass-derived glycol in the raw material, and may be a copolymer containing other glycols in the raw material other than the biomass-derived glycol, but it is preferable that the raw material does not contain other glycols. Such other glycols are not particularly limited, and various types of glycols that have been conventionally used as polyol components in polyurethane resin compositions can be used.
[0027] Examples of the other glycols include polybutadiene polyol, ethylene glycol, 1,3-propanediol, 1,2-propanediol, 2-methyl-1,3-propanediol, 1,4-butanediol, 1,3-butanediol, 1,4 pentanediol, 1,5-pentanediol, 1,6-hexanediol, 1,5-hexanediol, 1,2-hexanediol, 2,5-hexanediol, octanediol, nonanediol, decanediol, diethylene glycol, triethylene glycol, dipropylene glycol, cyclohexanediol, trimethylolpropane, glycerin, and 2-methylpropane. Examples of suitable polyols include 1,2,3-triol, 1,2,6-hexanetriol, pentaerythritol, polylactone diol, polylactone triol, ester glycol, castor oil-based polyol, polyolefin polyol, polyester polyol, polyether polyol, polycarbonate polyol, acrylic polyol, silicone polyol, fluorine polyol, polytetramethylene glycol, polytetramethylene ether glycol, polypropylene glycol, polyethylene glycol, polycaprolactone polyol, hydrogenated hydroxyl group-containing liquid polyisoprene, and hydrogenated hydroxyl group-containing liquid polybutadiene.
[0028] The content of the (B) component is preferably 15 to 80 mass%, more preferably 20 to 75 mass%, based on 100 mass% of the polyurethane resin composition of the present invention. When the upper limit of the (B) component content is within the above range, the flexibility and elongation of a resin product produced using the polyurethane resin composition are further improved. When the (B) component content is within the above range, the hardness of a resin product produced using the polyurethane resin composition is further improved.
[0029] In the polyurethane resin composition of the present invention, the NCO / OH ratio between the (A) component and the (B) component is preferably 0.6 to 2.0, and more preferably 0.7 to 1.5. When the lower limit of the NCO / OH ratio is within the above range, the heat resistance of the polyurethane resin composition is further improved. When the upper limit of the NCO / OH ratio is within the above range, the curability of the polyurethane resin composition is further improved.
[0030] ((C) Polybutadiene polyol) The polyurethane resin composition of the present invention may contain (C) polybutadiene polyol (hereinafter, also referred to as "component (C)"). When the polyurethane resin composition of the present invention contains component (C), the moisture resistance of a resin product produced using the polyurethane resin composition of the present invention is further improved.
[0031] The component (C) is not particularly limited as long as it is a polybutadiene polyol, and examples thereof include a polyol having a repeating unit composed of polybutadiene having 60 to 90 mol % of 1,4 bonds and 10 to 40 mol % of 1,2 bonds, the repeating number being 10 to 14, and having hydroxyl groups at both ends.
[0032] The molecular weight of the polybutadiene polyol used as the component (C) is preferably 800-4,800, and more preferably 1,200-3,000.
[0033] Commercially available products of component (C) include hydroxyl-containing liquid polybutadiene Poly bd (registered trademark) R-15HT (product name) and R-45HT (product name) manufactured by Idemitsu Kosan Chemical Co., Ltd.
[0034] The component (C) may be used alone or in combination of two or more kinds.
[0035] The content of the (C) component is preferably 50 to 450 parts by mass, more preferably 70 to 300 parts by mass, based on 100 parts by mass of the (B) polyether polyol made from biomass-derived glycol. When the upper limit of the (C) component content is within the above range, the curability of the polyurethane resin composition is further improved. When the lower limit of the (C) component content is within the above range, the moisture resistance of the cured resin obtained by curing the polyurethane resin composition is further improved.
[0036] ((D) Plasticizer) The polyurethane resin composition of the present invention may contain a plasticizer (D) (hereinafter, also referred to as "component (D)"). When the polyurethane resin composition of the present invention contains component (D),
[0037] As the component (D), any known plasticizer used in polyurethane resin compositions can be used, with the use of an ester-based plasticizer being preferred among these.
[0038] Examples of the ester plasticizer include phthalates such as dioctyl phthalate, diisononyl phthalate, and diundecyl phthalate; adipates such as dioctyl adipate and diisononyl adipate; trimellitates such as trioctyl trimellitate and triisononyl trimellitate; and pyromellitates such as tetraoctyl pyromellitate and tetraisononyl pyromellitate. Of these, phthalates are more preferred.
[0039] In addition, the component (D) used in the polyurethane resin composition of the present invention is preferably a plasticizer made of a raw material derived from biomass. By using such a plasticizer as the component (D), the biomass content of the polyurethane resin composition of the present invention is further improved, and the elongation of the cured resin obtained by curing the polyurethane resin composition of the present invention is further improved.
[0040] The content of component (D) is preferably 20 to 150 parts by mass, and more preferably 50 to 120 parts by mass, based on 100 parts by mass of polyether polyol (B) made from biomass-derived glycol as a raw material. By setting the content of the plasticizer within the above range, the mixing viscosity during production of the polyurethane resin composition can be reduced without significantly decreasing the moisture resistance of the polyurethane resin composition.
[0041] (Other additives) The polyurethane resin composition of the present invention may contain other additives in addition to the above components (A) to (D), such as a catalyst, an antioxidant, a moisture absorbent, an antifungal agent, a silane coupling agent, etc.
[0042] The catalyst is not particularly limited, and may be a conventionally known catalyst used in polyurethane resin compositions. Examples of such catalysts include tin catalysts such as dioctyltin dilaurate, dibutyltin dilaurate, and dioctyltin diacetate; lead catalysts such as lead octylate, lead octenate, and lead naphthenate; bismuth catalysts such as bismuth octylate and bismuth neodecanoate; and amine catalysts such as diethylenetriamine. In addition, organometallic compounds, metal complex compounds, and the like may be used as the catalyst.
[0043] The amounts of the above other additives used may be appropriately determined according to the intended use from the ranges specified by the usual amounts added so as not to impair the desired properties of the polyurethane resin composition.
[0044] (Polyurethane resin composition) The polyurethane resin composition of the present invention may be either a one-component type or a two-component type, but the polyurethane resin composition of the present invention containing the components (A), (B), and (C) is usually a two-component type resin composition. In the production method described below, the two-component type resin composition will be described.
[0045] 2. Method for producing polyurethane resin composition The method for producing the polyurethane resin composition of the present invention is not particularly limited, and the composition can be produced by any known method used for producing polyurethane resin compositions.
[0046] An example of such a production method is a method of producing the resin composition of the present invention by preparing (B) a component containing a polyether polyol component made from a biomass-derived glycol as a raw material to serve as a first component, preparing (A) a component containing an isocyanate group-containing compound to serve as a second component, and mixing the first and second components to cause a reaction to form a polyurethane resin.
[0047] As long as the first component contains the component (B) and the second component contains the component (A), the other component may be contained in either the first component or the second component.
[0048] Specific examples of the configuration of the first and second components include a configuration in which the first component contains the components (B) and (C), and the second component contains the component (A). Alternatively, the first component may contain the components (B) and (C), and optionally the component (D), and the second component may contain the component (A).
[0049] The method for preparing the first component and the second component is not particularly limited, and for example, they can be prepared by a preparation method having a step 1 of mixing and stirring the components constituting the first component and the second component in a kneader.
[0050] In the above step 1, the temperature for mixing and stirring is preferably from 60° C. to 120° C., and the stirring time may be from about 30 minutes to 3 hours.
[0051] By the above-described step 1, the first component and the second component are prepared.
[0052] The polyurethane resin composition of the present invention is produced in step 2 by mixing the first component and the second component prepared in step 1. The mixing temperature is not particularly limited, and is preferably 23° C. or higher and 60° C. or lower. The mixing time is not particularly limited, and may be appropriately set according to the pot life of the polyurethane resin composition.
[0053] The polyurethane resin composition of the present invention is produced by the step 2 described above.
[0054] 3.Cured resin material The polyurethane resin composition of the present invention can be cured to obtain a cured resin product. The cured resin product has high flexibility and high elongation, making it useful as a resin product for use in the field of electric and electronic parts.
[0055] The cured resin preferably has an initial hardness A of 0 or more, more preferably 5 or more, even more preferably 10 or more, and particularly preferably 15 or more, when the polyurethane resin composition is left to stand at a temperature of 60° C. for 16 hours to cure and obtain a cured resin. When the lower limit of the initial hardness A is within the above range, the cured resin can be more usefully used as a resin product used in the field of electric and electronic parts. In addition, the initial hardness A is preferably 70 or less, more preferably 65 or less. When the upper limit of the initial hardness A is within the above range, the flexibility and elongation of the cured resin are further improved. In this specification, the initial hardness A of the cured resin is measured by the method described in the Examples below.
[0056] 4. Sealing materials and electrical and electronic parts The present invention is also a sealant made of the polyurethane resin composition. The sealant is required to have a moderate elongation rate. When the polyurethane resin composition is used to resin seal the entire printed circuit board of an electric / electronic component, for example, it is required to follow the deformation of the printed circuit board and maintain high sealing properties. In addition, in a thermal shock test or the like, it is required to have excellent crack resistance at low temperatures and follow the cast parts and cases. The sealant made of the polyurethane resin composition can be suitably used for electric / electronic components and electric / electronic components that generate heat. Examples of such electric / electronic components include transformers such as transformer coils, choke coils, and reactor coils, device control boards, and various sensors. Such electric / electronic components resin-sealed using the sealant of the present invention are also one of the present inventions. The electric / electronic components of the present invention can be used in electric washing machines, toilet seats, water heaters, water purifiers, baths, dishwashers, power tools, automobiles, motorcycles, battery packs, and the like. EXAMPLES
[0057] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the examples.
[0058] The raw materials used in the examples and comparative examples are shown in Table 1 below.
[0059] [Table 1]
[0060] (Preparation of Polyurethane Resin Composition) The raw materials for the first component shown in Table 2 were charged into a reaction vessel and stirred at room temperature and pressure for 1 hour to prepare the first component.
[0061] The raw materials for the second component shown in Table 2 were placed in a reaction vessel equipped with heating, cooling, and pressure reduction devices, and dehydration and reaction were carried out at 60°C and a pressure of 10 mmHg or less for 1 hour to prepare the second component.
[0062] A polyurethane resin composition was obtained by adding the second component to the first component, stirring, defoaming and mixing, according to the formulation shown in Table 2. The first and second components were mixed by adjusting the temperature of the first component to 23°C, then adding the second component, which had also been adjusted to 23°C, and mixing at 2000 rpm for 1 minute using a planetary centrifugal mixer (Thinky Corporation, Awatori Rentaro).
[0063] Preparation of test specimens The polyurethane resin composition was poured into a molding die (test piece 1) of 130×130×3 mm and a molding die (test piece 2) of 30 mm inner diameter and 10 mm height. The polyurethane resin composition was then heated at 60° C. for 16 hours and then left at room temperature for 1 day to harden, producing a test piece.
[0064] The following tests were carried out using test pieces and the like prepared using the polyurethane resin compositions of the Examples and Comparative Examples as described above.
[0065] Viscosity of the first component 200g of the first component was poured into a 225cc mayonnaise bottle to add the sample. The sample temperature was adjusted to 40±0.5°C, and the viscosity was measured after rotating for 60 seconds using a BH type viscometer and a BL type viscometer with a specified rotor and rotation speed.
[0066] Hardness A (initial hardness A) Using test piece 2 (inner diameter 30 mm, height 10 mm), the hardness (Type A) was measured at a temperature of 23°C using a hardness meter (Asker Rubber Hardness Meter Type A, manufactured by Kobunshi Keiki Co., Ltd.) according to the measurement method in accordance with JIS K6253.
[0067] Elongation (flexibility) Using test piece 1 (130×130×3 mm), the gauge length at break was measured according to a measurement method in accordance with JIS K6251, and the elongation (flexibility) was calculated according to the following formula. The elongation was also defined as the initial elongation. Elongation (%) = [(gauge length at break - gauge length) / gauge length] x 100
[0068] Volume resistivity The volume resistivity of the test piece 1 (130×130×3 mm) was measured using a resistance measuring device (DSM-8104, manufactured by HIOKI Corporation). The volume resistivity was defined as the initial volume resistivity.
[0069] Volume resistivity change rate after moisture resistance test A moisture resistance test (pressure cooker test (PCT test)) was conducted for 7 days at 85°C and 85% RH using test piece 1 (130 x 130 x 3 mm). The volume resistivity after the moisture resistance test was measured using test piece 1 after the moisture resistance test by the above-mentioned method for measuring volume resistivity, and the rate of change in volume resistivity after the moisture resistance test was calculated according to the following formula. Volume resistivity change rate (%) = [(initial volume resistivity) / volume resistivity after moisture resistance test)] x 100 The evaluation was performed according to the following evaluation criteria. If the evaluation was ◯ or higher, it was evaluated that there would be no problem in practical use. ◎: The change in volume resistivity is less than 90%. ○: The change rate of volume resistivity is 90 to 95% ×: The rate of change in volume resistivity exceeds 95%
[0070] Time until hardness A becomes 0 in moisture resistance test The time until the hardness A reached 0 at 121°C, 100% RH and 2 atmospheres was measured. The hardness A was measured by the above-mentioned method for measuring hardness A.
[0071] Biomass ratio The biomass ratio of the polyurethane resin composition was measured from the C14 content using an accelerator mass spectrometer.
[0072] The results are shown in Tables 2 and 3.
[0073] [Table 2]
[0074] [Table 3]
Claims
1. A polyurethane resin composition comprising (A) an isocyanate group-containing compound and (B) a polyether polyol made from a biomass-derived glycol, The glycol is 1,3 propanediol and / or 1,4 butanediol; A polyurethane resin composition comprising:
2. The polyurethane resin composition according to claim 1, having a biomass degree of 15% or more.
3. 2. The polyurethane resin composition according to claim 1, wherein the content of the polyether polyol (B) made from a biomass-derived glycol is 15 to 80 mass% relative to 100 mass% of the polyurethane resin composition.
4. 2. The polyurethane resin composition according to claim 1, wherein the (A) isocyanate group-containing compound is at least one selected from the group consisting of diphenylmethane diisocyanate and modified products thereof, and hexamethylene diisocyanate and modified products thereof.
5. The polyurethane resin composition according to claim 1, wherein the content of the isocyanate group-containing compound (A) is 10 to 35 parts by mass relative to 100 parts by mass of the polyether polyol (B) made from a biomass-derived glycol.
6. The polyurethane resin composition according to claim 1 , further comprising (C) a polybutadiene polyol.
7. The polyurethane resin composition according to claim 6, wherein the content of the polybutadiene polyol (C) is 50 to 450 parts by mass per 100 parts by mass of the polyether polyol (B) made from a biomass-derived glycol.
8. The polyurethane resin composition according to claim 1 , further comprising (D) a plasticizer.
9. The polyurethane resin composition according to claim 8 , wherein the plasticizer is an ester-based plasticizer.
10. The polyurethane resin composition according to claim 8, wherein the content of the plasticizer (D) is 20 to 150 parts by mass per 100 parts by mass of the polyether polyol (B) made from a biomass-derived glycol.
11. A sealing material comprising the polyurethane resin composition according to any one of claims 1 to 10.
12. An electric / electronic component resin-sealed with the sealing material according to claim 11.
Citation Information
Patent Citations
Two-component cold-setting liquid urethane composition
JP2006199889A
Bio-polyurethane resin
JP2014037552A
Polyurethane resin composition, sealing material, and electric / electronic component
JP2016098326A
Flame-retardant composition, and flame-retardant polyurethane molding
JP2019099650A
Polyurethane resin composition for electric insulation
JP2019182901A