Photosensitive coloring resin composition and cured film obtained from the same

A fluororesin-containing photosensitive colored resin composition addresses high reflection issues in display devices by lowering refractive index and enhancing recoatability, improving visibility and jet blackness without additional antireflection layers.

JP2024142553AInactive Publication Date: 2024-10-11TORAY INDUSTRIES INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023054725
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing photosensitive colored resin compositions used in display devices suffer from high reflection intensity due to the difference in refractive indices between the colorant and the device materials, leading to poor visibility and difficulty in post-processing, such as recoatability, despite efforts to incorporate silica particles and fluorine-based surfactants.

Method used

Incorporating a specific fluororesin with a fluorine-containing monomer and a polyalkylene oxide group-containing monomer into the photosensitive colored resin composition, along with a radically polymerizable compound, to lower the refractive index and improve recoatability.

Benefits of technology

The composition achieves reduced light reflection intensity, enhanced visibility, and improved sharpness and jet blackness, while maintaining excellent recoatability and avoiding the need for additional antireflection layers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142553000001
    Figure 2024142553000001
  • Figure 2024142553000002
    Figure 2024142553000002
  • Figure 2024142553000003
    Figure 2024142553000003
Patent Text Reader

Abstract

To provide a photosensitive coloring resin composition which has low reflection intensity on the film surface side of a cured film, and has good recoatability.SOLUTION: A photosensitive coloring resin composition contains a coloring material, an alkali-soluble resin, a photopolymerization initiator, a fluorine-containing resin containing a repeating unit derived from a fluorine-containing monomer having a specific structure and a repeating unit derived from a polyalkylene oxide group-containing monomer represented by general formula (4), and a radical-polymerizable compound. In the formula, R2 represents a group having a carbon-carbon double bond; Y2 represents an alkylene group having 2 to 4 carbon atoms; R3 represents a hydrogen or an alkyl group having 1 to 4 carbon atoms; and n3 represents an integer of 2 or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a photosensitive colored resin composition and a cured film. [Background technology]

[0002] The present invention relates to a photosensitive colored resin composition and a cured film. More specifically, the present invention relates to a photosensitive colored resin composition that is useful in a technology for improving the deterioration of visibility of a display device due to reflection, and a cured film using the photosensitive colored resin composition.

[0003] Conventionally, various ideas have been devised for display devices to prevent deterioration of visibility due to reflection, and examples of such ideas include anti-reflection films such as moth-eye films and circular polarizing plates, as well as those using colored cured films such as color filters.

[0004] In constructing an anti-reflection means for a display device such as a color filter, a colored resin composition in which a colorant is dispersed or dissolved in a binder resin solution is usually used. In particular, a photosensitive colored resin composition in which a pigment is dispersed in a solution in which an alkali-soluble resin, a polymerization initiator, a radical-polymerizable compound, etc. are mixed is widely used because it is possible to form fine patterns in a photolithography process of exposure and development.

[0005] However, since the coloring material used in the colored resin composition generally has a higher refractive index than the materials constituting the display device, such as the substrate, film, sealing material, insulating film, and other structures, the higher the content ratio of the coloring material in the cured film containing the coloring material, the higher the refractive index, and the higher the reflection intensity of light at the boundary with other constituent materials. In other words, the greater the difference in refractive index between the substances forming the boundary, the higher the reflection intensity at the boundary. For example, the refractive index of glass and resin is about 1.5, while the refractive index of carbon black is about 2.0 and that of copper phthalocyanine is about 1.8. However, the higher the content ratio of the coloring material, the greater the difference in refractive index between adjacent layers. Therefore, when the coloring material is used as a color filter or the like to transmit light or when used as a light-shielding material, the reflection of light at the surface of the layer containing the coloring material becomes stronger when light enters the layer, which causes a problem of worsening visibility. In addition, in recent years, with changes in panel configuration, there is a demand to reduce the reflection intensity on the film surface side opposite to the substrate.

[0006] Therefore, efforts have been made to suppress reflection by blending particulate silica or the like in a photosensitive colored resin composition. Patent Document 1 describes that in a colored cured film for a display device, the reflection intensity on the film surface side of the cured film can be reduced by including silica particles and setting the Si element content in a specific range in a surface element composition analysis by X-ray photoelectron spectroscopy (XPS).

[0007] Furthermore, Patent Document 2 describes that it is possible to form partition walls with low reflectance by devising a compounding design of a photosensitive resin composition for black resist, for example, by including an alkali-soluble resin containing an unsaturated group having a specific structure and including a surfactant having a fluorine atom and an ethylenically unsaturated bond in the molecule. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2018-141849 A [Patent Document 2] JP 2022-173086 A Summary of the Invention [Problem to be solved by the invention]

[0009] However, the inventors of the present invention have found that the photosensitive colored resin composition described in Patent Document 1 has a relatively high refractive index of about 1.5 and silica particles are added to reduce the reflection intensity, and therefore the composition does not have a sufficient effect of reducing the refractive index when mixed with a pigment having a higher refractive index. In addition, Patent Document 2 uses a fluorine-based surfactant, but the fluorine-based surfactant used in Patent Document 2 has poor recoatability, making it difficult to handle post-processing such as processing another layer on a layer containing a coloring material.

[0010] Therefore, the present invention aims to provide a photosensitive colored resin composition that has a low reflection intensity on the surface side of a colored cured film and has good recoatability. Another object of the present invention is to provide a cured film using this photosensitive colored resin composition. [Means for solving the problem]

[0011] In order to solve the above problems, the present inventors conducted extensive research and found that the above problems can be solved by including a specific fluorine-containing resin in a photosensitive colored resin composition, and thus completed the present invention. The present invention has the following configuration. That is, the gist of the present invention is as follows: The photosensitive color resin composition includes a colorant, an alkali-soluble resin, a photopolymerization initiator, a fluorine-containing resin containing a repeating unit derived from a fluorine-containing monomer represented by the following general formula (1) and a repeating unit derived from a polyalkylene oxide group-containing monomer represented by the following general formula (4) (such a fluorine-containing resin may be simply referred to as "fluorine-containing resin α"), and a radical polymerizable compound.

[0012] [ka]

[0013] [In the formula, R1 represents a hydrogen atom or a methyl group. Y1 represents a divalent linking group. R f is a structure represented by the following formula (2-1) or (2-2).

[0014] [ka]

[0015] [In the formula, * indicates the point of attachment to the oxygen atom.]

[0016] [ka]

[0017] [In the formula, R2 represents a monovalent group having a carbon-carbon double bond. Y2 represents an alkylene group having 2 to 4 carbon atoms. R3 represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. n3 represents an integer of 2 or more.] Effect of the Invention

[0018] By using the photosensitive color resin composition of the present invention, the reflection intensity of light incident on the cured film can be reduced, and the visibility of the display device and the vividness and jet blackness according to the coloring material used can be improved. In addition, the photosensitive color resin composition of the present invention has excellent recoatability, so it has excellent adaptability to post-processing.

[0019] In addition, since the cured film itself has high antireflection properties, it is expected that the process can be prevented from becoming complicated, such as by providing an additional antireflection layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] The photosensitive color resin composition of the present invention contains a colorant, an alkali-soluble resin, a photopolymerization initiator, a fluorine-containing resin, and a radical-polymerizable compound.

[0021] Hereinafter, each component of the photosensitive color resin composition of the present invention will be described in detail with reference to examples.

[0022] <Coloring material> As the coloring material used in the present invention, pigments, dyes, etc. generally used in display devices can be used. In order to improve the heat resistance, reliability, and light resistance of the cured film, it is preferable to use a pigment. In this case, it is preferable to contain a coloring material with a small crystallite size, since it can reduce the deterioration of jet blackness due to scattering. There is no particular limitation on the pigment, but red pigments, blue pigments, yellow pigments, orange pigments, purple pigments, green pigments, black pigments, white pigments, etc. can be appropriately selected and used. These coloring materials may be used alone or in combination of two or more. As the black pigment, black organic pigments such as carbon black, perylene black, and aniline black are preferable from the viewpoint of low reflection intensity and light blocking properties. Among them, carbon black is particularly preferable.

[0023] The secondary particle diameter of the colorant is preferably 30 nm to 100 nm. If the secondary particle diameter is 30 nm or more, the storage stability after dispersion is excellent. On the other hand, if the secondary particle diameter is 100 nm or less, the diffuse reflection value when made into a film is low, and a vivid color can be obtained, and in particular, in the case of a black pigment, the jet blackness is excellent. The secondary particle diameter of the pigment is determined by the particle diameter (D 50 The secondary particle diameter is measured on a sufficiently diluted photosensitive colored resin composition (usually diluted to a pigment concentration of about 0.005 to 0.2% by mass and then measured. However, if there is a concentration recommended by the measuring device, follow that concentration.) at 25°C.

[0024] Carbon black has an average primary particle size of 1 to 18 nm and a dibutyl phthalate absorption of 30 to 80 cm 3It is preferable to use carbon black having an average primary particle size of 1.0 to 4.0. By setting the average primary particle size of carbon black within the above range, the value of diffuse reflection can be reduced and the jet black appearance can be enhanced. Furthermore, by setting the dibutyl phthalate absorption amount of carbon black within the above range, the value of diffuse reflection can be reduced, the jet black appearance can be enhanced, and dispersibility can be improved. Furthermore, by setting the pH value of carbon black within the above range, dispersibility can be improved.

[0025] The average primary particle diameter of carbon black can be determined by the following method. First, carbon black is ultrasonically dispersed in chloroform, dropped onto a mesh with a collodion film attached, and dried, and a primary particle image of the carbon black is obtained by observation with a transmission electron microscope (TEM). Next, the primary particle diameter of each carbon black particle is converted into the diameter of a circle with the same area as the primary particle diameter of the individual carbon black particles, and the particle diameter of each of multiple carbon black particles (usually about 200 to 300 particles) is determined. Using the obtained primary particle diameter value, the number average value is calculated according to the following formula to determine the average primary particle diameter.

[0026] Particle size of individual carbon black particles: X1, X2, X3, X4, . . ., X i ,···X m Average primary particle diameter = ΣX i / m [m is the number of particles, and Xi is the primary particle diameter of the i-th particle.]

[0027] The dibutyl phthalate absorption amount of carbon black was measured based on JIS K 6221.

[0028] The pH value of the carbon black was measured in accordance with ASTM D1512. Resin-coated carbon black can also be used as the carbon black. Resin-coated carbon black can be obtained by treating known carbon black using the method described in, for example, JP-A-9-26571, JP-A-9-71733, JP-A-9-95625, JP-A-9-238863, or JP-A-11-60989.

[0029] The content of the coloring material such as black pigment in the photosensitive colored resin composition of the present invention is preferably 1% by mass or more and 70% by mass or less, more preferably 10% by mass or more and 60% by mass or less, based on the total amount of solids contained in the resin composition (100% by mass). If the content of the coloring material is too low, the dispersion stability cannot be maintained. On the other hand, if the content of the coloring material is too high, the reflection of light on the cured film surface tends to be strong, so that sufficient color clarity and jet blackness may not be obtained depending on the required level.

[0030] <Alkali-soluble resin> The alkali-soluble resin used in the present invention refers to a resin having an alkali-soluble group, such as a phenolic hydroxyl group or carboxyl group, an acid value of 10 mgKOH / g or more, and a weight average molecular weight (Mw) of 500 to 150,000, and does not contain fluorine atoms in the structure. Here, the weight average molecular weight (Mw) refers to a value measured by gel permeation chromatography using tetrahydrofuran as a carrier and converted using a calibration curve of standard polystyrene.

[0031] Examples of the alkali-soluble resin include cardo resins, acrylic resins, novolac resins, polyimide resins, polyimide precursors, polybenzoxazole resins, polybenzoxazole precursors, polyamide resins, etc., which satisfy the above-mentioned conditions for alkali-soluble resins. Among these, from the viewpoints of pattern processability and coating film reliability, resins selected from cardo resins, acrylic resins, and polyimide resins are preferred, and acrylic resins are more preferred.

[0032] <Photopolymerization initiator> The photopolymerization initiator used in the present invention refers to a compound that generates radicals by exposure. By including a photopolymerization initiator, the radical polymerizable compound can be polymerized by exposure to light, and photocured. Examples of the photopolymerization initiator include a carbazole-based photopolymerization initiator, an acylphosphine oxide-based photopolymerization initiator, an oxime ester-based photopolymerization initiator, and an α-aminoalkylphenone-based photopolymerization initiator. Two or more of these may be included. Among these, a carbazole-based photopolymerization initiator or an oxime ester-based photopolymerization initiator is preferred because of its high sensitivity to a mixed line consisting of an i-line (365 nm), an h-line (405 nm), and a g-line (436 nm) in the exposure step described below. An oxime ester-based photopolymerization initiator is particularly preferred.

[0033] Examples of the oxime ester photopolymerization initiator include 1-phenyl-1,2-propanedione-2-(o-ethoxycarbonyl)oxime, 1,2-octanedione, 1-[4-(phenylthio)-2-(o-benzoyloxime)], 1-phenyl-1,2-butadione-2-(o-methoxycarbonyl)oxime, 1,3-diphenylpropanetrione-2-(o-ethoxycarbonyl)oxime, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethanone(o-acetyloxime), etc. Two or more of these may be contained.

[0034] The content of the photopolymerization initiator in the photosensitive colored resin composition of the present invention is preferably 1 part by mass or more and 60 parts by mass or less, more preferably 3 parts by mass or more and 20 parts by mass or less, relative to 100 parts by mass of the radical polymerizable compound, from the viewpoint of improving the sensitivity to light exposure. When the content of the photopolymerization initiator is 1 part by mass or more, the dissolution of the fluorine-containing resin in the developer can be prevented, and the decrease in the refractive index can be maintained. On the other hand, when the content of the photopolymerization initiator is 60 parts by mass or less, the deep curing property to light exposure can be improved, and the pattern processability can be improved.

[0035] <Fluorine-containing resin (fluorine-containing resin α)> The fluorine-containing resin contained in the photosensitive colored resin composition of the present invention contains a repeating unit derived from a fluorine-containing monomer represented by the following general formula (1) and a repeating unit derived from a polyalkylene oxide group-containing monomer represented by the following general formula (4) described below. By using such a fluorine-containing resin, the refractive index of the surface vicinity of the cured film can be specifically lowered by mass transfer during the process of applying and drying the photosensitive colored resin composition of the present invention, thereby exhibiting the effect of lowering the reflection intensity on the film surface side.

[0036] [ka]

[0037] [In the formula, R1 represents a hydrogen atom or a methyl group. Y1 represents a divalent linking group. R f is a structure represented by the following formula (2-1) or (2-2).

[0038] [ka]

[0039] [In the formula, * indicates the point of attachment to the oxygen atom.] The fluorine-containing monomer that gives the repeating unit of the fluorine-containing resin used in the present invention contains fluorine atoms and also contains double bonds between carbon atoms. The fluorine atoms play a role in lowering the refractive index of the resin composition. In addition, the double bonds between carbon atoms are not dissolved in the developer in the development step by causing a crosslinking reaction in the exposure step during the exposure and development steps when preparing and processing the coating film, and as a result, play a role in maintaining the lowering of the refractive index in the film after exposure.

[0040] Also, R f By having the structure represented by formula (2-1) or formula (2-2), a fine sea-island structure is formed on the surface, which reduces the contact angle of the overcoating composition and improves recoatability.

[0041] Y1 is a divalent linking group, preferably a divalent organic group containing a divalent saturated aliphatic hydrocarbon group having 1 to 50 carbon atoms. The divalent saturated aliphatic hydrocarbon group preferably has 1 to 30 carbon atoms, more preferably 2 to 10 carbon atoms, and most preferably 2 to 4 carbon atoms, and specific examples include linear or branched alkylene groups having the above carbon atoms. A linear alkylene group is preferred. The divalent saturated aliphatic hydrocarbon group may have one or more hydrogen atoms substituted with halogen atoms. Examples of halogen atoms include fluorine atoms, chlorine atoms, bromine atoms, and iodine atoms, and among these, fluorine atoms and chlorine atoms are preferred.

[0042] Y1 is preferably a divalent organic group containing a divalent saturated aliphatic hydrocarbon group having 1 to 50 carbon atoms, but there is no particular limitation on the groups that may be contained other than the divalent saturated aliphatic hydrocarbon group, and examples thereof include an arylene group. Preferred arylene groups are arylene groups having 6 to 15 carbon atoms, such as a phenylene group, a naphthylene group, a tolylene group, a xylylene group, an anthranylene group, and a phenanthrylene group. Among them, a preferred arylene group is a phenylene group, particularly a p-phenylene group. Here, a hydrogen atom bonded to the arylene group may be substituted with a halogen atom. In addition, Y1 may have other groups that link the divalent saturated aliphatic hydrocarbon groups and between the divalent saturated aliphatic hydrocarbon group and the arylene group, and examples of such linking groups include an ether bond (-O-), an ester bond (-COO- or -O-CO-), and an amide bond (-NHCO- or -CONH-).

[0043] Preferred specific examples of Y1 include the divalent organic groups shown below.

[0044] -(CH2)n a -(n a = an integer from 2 to 10, preferably from 2 to 4) -C6H4COO(CH2)n b -(n b = an integer from 2 to 10, preferably from 2 to 4) -C6H4(CH2)nc -(n c = an integer from 1 to 10, preferably from 2 to 4) -CH2CH2(OCH2CH2)n d -(n d = an integer from 1 to 10, preferably from 2 to 4) -C6H4CO(OCH2CH2)n e - (n e = an integer of 1 to 10, preferably 2 to 4).

[0045] Among the above preferred specific examples of Y1, the following groups are particularly preferred.

[0046] -C6H4COO(CH2)n b -(n b = an integer of 2 to 10, preferably 2 to 4).

[0047] The fluorine-containing monomer can be produced by a known method, for example, by adding dropwise an organic solvent solution of an acid chloride to an organic solvent solution of a hydroxyl group-containing alkyl (meth)acrylate at room temperature based on the following reaction formula (3).

[0048] [ka]

[0049] [In the formula, R f and R1 are the same as those explained in the general formula (1). n2 is an integer of 2 to 10. The fluorine-containing monomer may be used alone or in combination of two or more kinds.

[0050] The polyalkylene oxide group-containing monomer represented by the following general formula (4), which provides the repeating unit of the fluorine-containing resin used in the present invention, will now be described.

[0051] [ka]

[0052] [In the formula, R2 represents a monovalent group having a carbon-carbon double bond. Y2 represents an alkylene group having 2 to 4 carbon atoms. R3 represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. n3 represents an integer of 2 or more.] By using the polyalkylene oxide group-containing monomer, the compatibility of the fluorine-containing resin itself with the photosensitive color resin composition can be improved. Specifically, when a coating film made of the photosensitive color resin composition of the present invention is produced, it has the effect of preventing an increase in diffuse reflection caused by insufficient compatibility.

[0053] Examples of R2 include CH2=CH-, CH2=CH-CH2-, CH2=C(CH3)-, CH2=CH-CO-, CH2=C(CH3)-CO-, CH3CH=CH-CO-, and the like.

[0054] Examples of Y2 include -CH2CH2-, -CH(CH3)-, -CH2CH2CH2-, -CH(CH3)CH2-, -CH2CH(CH3)-, -CH2CH2CH2CH2-, -CH2CH(CH3)CH2-, -CH(CH2CH3)CH2-, -CH(CH2CH3)CH2-, and -CH2CH(CH2CH3)-.

[0055] Examples of R3 include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, and a t-butyl group.

[0056] n3 is an integer of 2 or more, preferably 2-50, more preferably 2-30, and further preferably 2-20.

[0057] The polyalkylene oxide group-containing monomer may be used alone or in combination of two or more kinds.

[0058] The fluorine-containing resin may be prepared by copolymerizing an optional monomer in addition to the above-described fluorine-containing monomer and polyalkylene oxide group-containing monomer, such as ethylene, propylene, acrylonitrile, methacrylonitrile, vinyl acetate, (meth)acrylic acid ester, acrylamide, methacrylamide, and a hydrophilic group-containing monomer. Examples of (meth)acrylic acid esters include methyl acrylate (MA), ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, s-butyl acrylate, t-butyl acrylate, pentyl acrylate, hexyl acrylate, octyl acrylate, 2-ethylhexyl acrylate, cyclohexyl acrylate, phenyl acrylate, benzyl acrylate, methyl methacrylate (MMA), ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, pentyl methacrylate, hexyl methacrylate, octyl methacrylate, 2-ethylhexyl methacrylate, cyclohexyl methacrylate, phenyl methacrylate, and benzyl methacrylate.

[0059] Examples of the hydrophilic group-containing monomer include acrylic acid, methacrylic acid, maleic acid, itaconic acid, and a monomer represented by the following general formula (5).

[0060] [ka]

[0061] [In the formula, R4 represents a hydrogen atom or a methyl group, Y3 represents a divalent linking group, and R5 represents a hydrophilic group.] Examples of the hydrophilic group represented by R5 include a hydroxyl group (-OH), a carboxyl group (-COOH) or a salt thereof, and a phosphoric acid (-O-PO-(OH)2) or a salt thereof. Examples of the salt of the carboxyl group or phosphoric acid include an alkali metal (Na, K, Li, Cs) salt and an alkaline earth metal (Ca, Mg, Sr, Ba) salt, with an alkali metal salt being preferred, and a sodium salt or a potassium salt being more preferred.

[0062] The divalent linking group represented by Y3 includes a linear, branched or cyclic alkylene group having 1 to 20 carbon atoms, an arylene group which may be substituted, and an aralkylene group which may be substituted, which may be bonded via an ether bond (-O-), an ester bond (-COO- or -O-CO-), or an amide bond (-NHCO- or -CONH-). For example, examples of butylene groups having the above bonds include -CH2CH2-O-CH2CH2-, -CH2CH2-O-CO-CH2CH2-, -CH2CH2-CO-O-CH2CH2-, -CH2CH2-CONH-CH2CH2-, and -CH2CH2-NHCO-CH2CH2-. Examples of the alkylene group having 1 to 14 carbon atoms include -(CH2)m- (m is an integer of 1 to 20), -CH(CH3)CH2-, -CH2CH(CH3)-, -CH(CH2CH3)CH2-, and -CH2CH(CH2CH3)-. Examples of the aryl group include a phenylene group, a biphenylene group, a phenoxyphenylene group, a naphthylene group, an anthracenylene group, a phenanthrenylene group, and a fluorenylene group. Examples of the arylene group include a benzylene group and a phenethylene group. The number of the substituents of the arylene group and the aralkylene group is preferably 1 to 3, and more preferably 1 to 2. Examples of the substituent include a methoxy group, an ethoxy group, a methyl group, an ethyl group, a chlorine atom, -CN, -NO2, -OH, an acetyl group, an acetylamino group, and a carbamoyl group. Examples of the divalent group represented by Y3 include the following: -(CH2) m1 -, (m1=2~10), -CH(CH3)CH2-, -CH2CH(CH3)-, -CH(CH2CH3)CH2-, -CH2CH(CH2CH3)-, -(CH2CH2O) m2 -CH2CH2-, (m2=1 to 9), -CH2CH2O-CO-(C6H4)-, -CH2CH2-CO-O-(C6H4)-, -CH2CH2O-CO-(CH2CH2)-, -CH2CH2-CO-O-(CH2CH2)-, -CH2CH2O-CO-(cyclohexylene group)-, -CH2CH2-CO-O-(cyclohexylene group)-.

[0063] The hydrophilic group-containing monomer may be used alone or in combination of two or more kinds.

[0064] The fluorine-containing resin used in the photosensitive color resin composition of the present invention may contain a structural unit derived from an isocyanate group-containing compound represented by the following general formula (6).

[0065] [ka]

[0066] [In the formula, R6 represents a monovalent group having a carbon-carbon double bond. Y4 represents a divalent saturated aliphatic hydrocarbon group having 2 to 10 carbon atoms, and the saturated aliphatic hydrocarbon group may have an ether bond.] Examples of R6 include CH2=CH-, CH2=CH-CH2-, CH2=C(CH3)-, CH2=CH-CO-, CH2=C(CH3)-CO-, and CH3CH=CH-CO-.

[0067] In the general formula (6), Y4 is a divalent saturated aliphatic hydrocarbon group having 2 to 10 carbon atoms, which may have an ether bond. Y4 is preferably a divalent saturated aliphatic hydrocarbon group having 2 to 4 carbon atoms, i.e., an alkylene group.

[0068] The structural unit derived from the isocyanate group-containing compound represented by general formula (6) is preferably contained in the fluororesin by reacting the isocyanate group of the isocyanate group-containing compound represented by general formula (6) with a hydroxyl group in the fluororesin.

[0069] The isocyanate group-containing compound represented by the general formula (6) can be obtained as a commercial product, but can also be produced by a known method. Commercially available isocyanate group-containing compounds include compound name: 2-methacryloyloxyethyl isocyanate (Karenz MOI; manufactured by Resonac Co., Ltd.), compound name: 2-acryloyloxyethyl isocyanate (Karenz AOI; manufactured by Resonac Co., Ltd.), compound name: 1,1-bis(acryloyloxymethyl)ethyl isocyanate (Karenz BEI; manufactured by Resonac Co., Ltd.), and the like.

[0070] The isocyanate group-containing compound may be used alone or in combination of two or more kinds.

[0071] The fluorine-containing resin used in the present invention can be produced, for example, by copolymerizing a fluorine-containing monomer and a polyalkylene oxide group-containing monomer as essential components. In addition, a known polymerization method can be used as the polymerization method. In detail, the monomers are mixed in a desired ratio, an appropriate amount of a polymerization initiator is added, and the mixture is reacted in the presence of an organic solvent at a temperature from room temperature to about 100°C for about 1 to 24 hours. This allows the reaction to proceed quantitatively. The order of mixing the monomers is not particularly limited.

[0072] The fluorine-containing resin used in the photosensitive colored resin composition of the present invention can be obtained, for example, by radical polymerization, preferably followed by the action of an isocyanate group-containing compound represented by general formula (6). Examples of the polymerization initiator include t-butyl hydroperoxide, cumene hydroperoxide, 2,5-dimethylhexane-2,5-dihydroperoxide, dicumyl peroxide, di-t-butyl peroxide, t-butylperoxyisobutyrate, t-butyl-α-cumyl peroxide, di-α-cumyl peroxide, α,α'-bis(t-butylperoxy)-p-diisopropylbenzene, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, 2,5-dimethyl-2,5-di(t -butylperoxy)-hexyne-3 acetyl peroxide, succinic acid peroxide, diisobutyryl peroxide, lauroyl peroxide, benzoyl peroxide, t-butyl peroxyacetate, t-butyl peroxyisobutyrate, diisobutyl peroxydicarbonate, t-butyl peroxyisopropyl carbonate, methyl ethyl ketone peroxide, cyclohexanone peroxide, 2,2'-azobisisobutyronitrile, dimethyl 2,2'-azobisisobutyrate, Examples of the azo compounds include 2,2'-azobis(2-methylpropionate)dimethyl (V-601), 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(isobutylamidine) dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane] and its disulfate, and 2,2'-azobis(2-methylamidoxime) dihydrochloride; potassium persulfate, sodium persulfate, ammonium persulfate, potassium persulfate, t-butyl hydroperoxide, benzoyl peroxide, and cumene hydroperoxide. These radical polymerization initiators may be used alone or in combination of two or more. The molecular weight of the copolymerization reaction may be adjusted using a chain transfer agent such as lauryl mercaptan, octyl mercaptan, dodecyl mercaptan, 2-mercaptoethanol, octyl thioglycolate, 3-mercaptopropionic acid, or thioglycerin.The solvent used in the polymerization is not particularly limited as long as the above reaction proceeds, and examples thereof include aprotic solvents.Preferred examples of aprotic solvents include dimethoxyethane, ethyl acetate, methyl ethyl ketone, methyl isobutyl ketone, acetonitrile, tetrahydrofuran, N,N-dimethylformamide, toluene, and propylene glycol monomethyl ether acetate.The solvent used in the polymerization may be used alone or in combination of two or more.The fluorine-containing resin may be a random polymer or block copolymer of a fluorine-containing monomer, a polyalkylene oxide group-containing monomer, and other monomers used as optional components.

[0073] When the fluorine-containing resin used in the photosensitive colored resin composition of the present invention is produced as an embodiment in which an isocyanate group-containing compound is further compounded, in addition to the case where R3 in the polyalkylene oxide group-containing monomer is a hydrogen atom, a monomer containing a hydroxyl group or a carboxyl group, preferably a hydroxyl group, can be used to react with the isocyanate group-containing compound. Specific reaction conditions for reacting the isocyanate group-containing compound include, for example, producing a copolymer with a fluorine-containing monomer, a polyalkylene oxide group-containing monomer, and other monomers used as optional components, and then mixing the isocyanate group-containing compound with the resulting polymer solution in a predetermined ratio and stirring at -20°C to 100°C, preferably 20°C to 90°C, for 1 to 48 hours to produce the copolymer. This allows the hydroxyl group to react with the isocyanate group of the isocyanate group-containing compound to form a urethane bond. At this time, the mixed isocyanate group-containing compound reacts quantitatively. An alkaline catalyst may be used in the reaction. The alkaline catalyst is not particularly limited as long as the reaction proceeds, but preferred alkaline catalysts include organic alkaline catalysts such as triethylamine, tributylamine, pyridine, and 1,4-diazabicyclo[2.2.2]octane. The alkaline catalyst is particularly preferably 1,4-diazabicyclo[2.2.2]octane. The alkaline catalyst may be used alone or in combination of two or more.

[0074] The weight average molecular weight of the fluorine-containing resin used in the photosensitive colored resin composition of the present invention is preferably 2,000 to 20,000, and more preferably 3,000 to 15,000.

[0075] In a preferred embodiment, when the proportions of the fluorine-containing monomer, the polyalkylene oxide group-containing monomer, and the other monomers used as optional components in the polymerization of the fluorine-containing resin are a1, b1, and c1 (mass%), respectively, it is preferable that the following relationship is simultaneously satisfied (wherein a1+b1+c1=100 mass%).

[0076] "a1 is preferably 1 to 50 mass%, more preferably 3 to 40 mass% b1 is preferably 10 to 99 mass%, more preferably 20 to 80 mass% The content of c1 is preferably 0 to 89% by mass, and more preferably 20 to 70% by mass.

[0077] In addition, when the structural unit derived from the polyalkylene oxide group-containing monomer is taken as 100 mol %, and the proportion of the isocyanate group-containing compound combined is taken as d1 (mol %), it is preferable that the following relationship is satisfied.

[0078] "d1 is preferably 5 to 80 mol %, more preferably 10 to 70 mol %, and further preferably 20 to 60 mol %."

[0079] The amount of the fluorine-containing resin used in the photosensitive colored resin composition of the present invention is preferably 0.5% by mass or more and 20% by mass or less, more preferably 1% by mass or more and 10% by mass or less, based on 100% by mass of the total solid content of the resin composition. When the content of the fluorine-containing resin is 0.5% by mass or more, the fluorine-containing resin can sufficiently move to the film surface side during drying, thereby reducing the reflectance. On the other hand, when the content of the fluorine-containing resin is 20% by mass or less, the development processability can be improved.

[0080] <Radical polymerizable compound> The photosensitive color resin composition of the present invention contains a radical polymerizable compound. The radical polymerizable compound is a compound having polymerization activity against the radical generated by the photopolymerization initiator. Note that the radical polymerizable compound does not contain a fluorine atom in the molecular structure.

[0081] The radical polymerizable compound is preferably a compound having two or more radical polymerizable functional groups. The radical polymerizable functional group of the radical polymerizable compound is preferably a (meth)acrylic group from the viewpoint of improving the sensitivity during exposure and the hardness of the cured film. The (meth)acrylic group here refers to a methacryl group or an acrylic group. The molecular weight of the radical polymerizable compound is preferably 100 to 3,000, more preferably 250 to 1,500.

[0082] As the radical polymerizable compound, it is preferable to use a compound containing a fluorene skeleton. Examples of the compound containing a fluorene skeleton include 9,9-bis[4-(3-acryloxy-2-hydroxypropoxy)phenyl]fluorene, 9,9-bis[3-methyl-4-(3-acryloxy-2-hydroxypropoxy)phenyl]fluorene, and a compound having a fluorene skeleton and a condensed polycyclic aromatic ring other than a fluorene skeleton and one or more hydroxyl groups (hereinafter, sometimes referred to as "(E-1A) component").

[0083] It is more preferable to use the (E-1A) component as the radical polymerizable compound used in the photosensitive colored resin composition of the present invention. Examples of the condensed polycyclic aromatic ring other than the fluorene skeleton in the (E-1A) component include pentalene, indene, naphthalene, heptalene, biphenylene, anthracene, phenanthrene, pentacene, pyrene, tetracene, and pentacene. From this viewpoint, it is preferable to use a compound represented by general formula (7-1) as the radical polymerizable compound. By containing a compound containing a fluorene skeleton, it crosslinks with the fluorine-containing resin during exposure, prevents the fluorine-containing resin from dissolving in the developer in the development process, and plays a role in maintaining a low reflectance.

[0084] [ka]

[0085] [In the formula, R 50 and R 51 each independently represents an alkylene group having 1 to 6 carbon atoms; R52 and R 53 each independently represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, a cycloalkyl group having 4 to 10 carbon atoms, or an aryl group having 6 to 15 carbon atoms; R 54 and R 55 R each independently represents a hydrogen atom or a methyl group. 56 ~R 61 R each independently represents a halogen atom, an alkyl group having 1 to 10 carbon atoms, a cycloalkyl group having 4 to 10 carbon atoms, an aryl group having 6 to 15 carbon atoms, a fluoroalkyl group having 1 to 10 carbon atoms, a fluorocycloalkyl group having 4 to 10 carbon atoms, or a fluoroaryl group having 6 to 15 carbon atoms. 62 and R 63 are each independently a hydrogen atom or COR 64 At least one of them represents a hydrogen atom, and R 64 represents an alkyl group having 1 to 12 carbon atoms, a cycloalkyl group having 1 to 12 carbon atoms, an alkenyl group having 1 to 12 carbon atoms, a cycloalkenyl group having 1 to 12 carbon atoms, or an alkynyl group having 1 to 12 carbon atoms. p and q each independently represent an integer of 0 to 3, and r and s each independently represent a natural number of 1 to 3. t and u each independently represent an integer of 0 to 4, and v and w each independently represent an integer of 0 to 3.] Examples of the (E-1A) component include 9,9-bis[5-(3-(meth)acryloxy-2-hydroxypropoxy)naphthyl]fluorene, 9,9-bis[5-{3-methyl-(3-(meth)acryloxy-2-hydroxypropoxy)}naphthyl]fluorene, 9,9-bis[5-{(3-(meth)acryloxy-2-hydroxypropoxy)ethoxy}-1-naphthyl]fluorene, 9,9-bis[5-{(3-(meth)acryloxy-2-hydroxypropoxy)propoxy}-1-naphthyl]fluorene, and 9,9-bis[5-(3-(meth)acryloxy-2-hydroxypropoxy)anthryl]fluorene.

[0086] In addition, the photosensitive color resin composition of the present invention preferably uses a polyfunctional acrylate compound having three or more functional groups as a radical polymerizable compound. By including a polyfunctional acrylate having three or more functional groups, the sensitivity can be improved.

[0087] Examples of the trifunctional or higher polyfunctional acrylate compound include trimethylolpropane tri(meth)acrylate, triacrylformal, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, ε-caprolactone-modified dipentaerythritol hexa(meth)acrylate, δ-valerolactone-modified dipentaerythritol hexa(meth)acrylate, γ-butyrolactone-modified dipentaerythritol hexa(meth)acrylate, β-propiolactone-modified dipentaerythritol hexa(meth)acrylate, and dipentaerythritol hexa(meth)acrylate.

[0088] Examples of radical polymerizable compounds other than compounds containing a fluorene skeleton or trifunctional or higher polyfunctional acrylate compounds include poly(meth)acrylate carbamates, 1,6-hexanediol adipic acid (meth)acrylic acid esters, phthalic anhydride propylene oxide (meth)acrylic acid esters, tripropylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 2-hydroxy-3-(meth)acryloyloxypropyl methacrylate, 2-hydroxy-3-(meth)acryloyloxypropyl acrylate, 1,6-hexanediyl bis(meth)acrylate bis(oxy)bis(2-hydroxy-3,1-propanediyl), and bisphenol A diglycidyl ether di(meth)acrylate.

[0089] The content of the radical polymerizable compound used in the photosensitive colored resin composition of the present invention is preferably 5% by mass or more and 80% by mass or less, more preferably 15% by mass or more and 60% by mass or less, based on the total content of the alkali-soluble resin and the radical polymerizable compound (100% by mass). When the content of the radical polymerizable compound is 5% by mass or more, the dissolution of the fluorine-containing resin in the developer can be prevented, and low reflectance can be maintained. On the other hand, when the content of the radical polymerizable compound is 80% by mass or less, the thickening of the pattern line width relative to the design value can be improved.

[0090] <Solvent> The photosensitive color resin composition of the present invention preferably contains a solvent. Examples of the solvent include ethers, acetates, esters, ketones, aromatic hydrocarbons, amides, and alcohols.

[0091] Examples of the ethers include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol mono-n-propyl ether, ethylene glycol mono-n-butyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol mono-n-propyl ether, diethylene glycol mono-n-butyl ether, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol mono-n-propyl ether, propylene glycol mono-n-butyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol mono-n-propyl ether, dipropylene glycol mono-n-butyl ether, dipropylene glycol dimethyl ether, dipropylene glycol methyl-n-butyl ether, tripropylene glycol monomethyl ether, tripropylene glycol monoethyl ether, diethylene glycol dimethyl ether, diethylene glycol methyl ethyl ether, diethylene glycol diethyl ether, and tetrahydrofuran. Examples of acetates include butyl acetate, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, 3-methoxybutyl acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate (hereinafter, BDG-AC: vapor pressure of 5 Pa at 20° C.), cyclohexanol acetate, propylene glycol diacetate, and propylene glycol monomethyl ether acetate (PGMEA).Examples of suitable acetates include propylene glycol monoethyl ether acetate, dipropylene glycol methyl ether acetate (hereinafter, DPMA: vapor pressure at 20°C of 10 Pa), 3-methoxy-3-methyl-1-butyl acetate, 1,4-butanediol diacetate, 1,3-butylene glycol diacetate, and 1,6-hexanediol diacetate. Examples of esters include alkyl lactate esters such as methyl 2-hydroxypropionate and ethyl 2-hydroxypropionate; ethyl 2-hydroxy-2-methylpropionate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, ethyl ethoxyacetate, ethyl hydroxyacetate, methyl 2-hydroxy-3-methylbutanoate, 3-methoxybutyl acetate, 3-methyl-3-methoxybutyl acetate, 3-methyl-3-methoxybutylpropionate, ethyl acetate, n-propyl acetate, i-propyl acetate, n-butyl acetate, i-butyl acetate, n-pentyl formate, i-pentyl acetate, n-butyl propionate, ethyl butyrate, n-propyl butyrate, i-propyl butyrate, n-butyl butyrate, methyl pyruvate, ethyl pyruvate, n-propyl pyruvate, methyl acetoacetate, ethyl acetoacetate, and ethyl 2-oxobutanoate. Examples of ketones include methyl ethyl ketone, cyclohexanone, 2-heptanone, and 3-heptanone. Examples of aromatic hydrocarbons include toluene and xylene. Examples of amides include N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide. Examples of alcohols include butyl alcohol, isobutyl alcohol, pentanol, 4-methyl-2-pentanol, 3-methyl-2-butanol, 3-methyl-3-methoxybutanol, and diacetone alcohol. Two or more of these may be contained.

[0092] Among these, acetates are preferably used in order to further stabilize the dispersion of the colorant. The content of acetates in 100% by mass of the total solvent is preferably 40% by mass or more and 100% by mass or less, and more preferably 70% by mass or more and 100% by mass or less.

[0093] In addition, it is preferable to use a solvent having a vapor pressure of 0.01 Pa or more and 100 Pa or less at 20° C. When a solvent having a low vapor pressure is used, the drying speed is suppressed, the fluorine-containing resin is easily precipitated on the surface, and the reflection intensity of the film surface can be further reduced. Examples of the solvent having a vapor pressure of 0.01 Pa or more and 100 Pa or less at 20° C. include DPMA and BDG-AC.

[0094] The content of the solvent having a vapor pressure of 0.01 to 100 Pa at 20° C. is preferably 10% by mass or more, and more preferably 20% by mass or more, based on 100% by mass of the total solvent, from the viewpoint of suppressing the observation rate. On the other hand, from the viewpoint of finally drying the coating film, the content is preferably 90% by mass or less, and more preferably 80% by mass or less.

[0095] The content of the solvent is preferably 50% by mass or more, more preferably 70% by mass or more, based on 100% by mass of the photosensitive color resin composition, from the viewpoint of uniformity of the thickness of the coating film in the coating process, while it is preferably 95% by mass or less, more preferably 90% by mass or less, from the viewpoint of suppressing pigment sedimentation.

[0096] <Other ingredients that can be used optionally> The photosensitive color resin composition of the present invention may contain a polymer dispersant. The polymer dispersant is a compound having both a pigment affinity group having a chemical bond or adsorption action to the pigment surface and a polymer chain or group having solvent affinity. The polymer dispersant improves the wettability of the pigment to the dispersion medium in a wet media dispersion process, promotes deagglomeration of the pigment, stabilizes the particle size and viscosity by steric hindrance and / or electrostatic repulsion effect, and further suppresses the occurrence of color separation during storage or application of the photosensitive color resin composition.

[0097] As the polymer dispersant, commercially available ones can be used. For example, polyester-based polymer dispersants, acrylic-based polymer dispersants, polyurethane-based polymer dispersants, polyallylamine-based polymer dispersants, carbodiimide-based dispersants, etc. can be mentioned. Polymer dispersants are classified into polymer dispersants with an amine value of 1 mgKOH / g or more and an acid value of less than 1 mgKOH / g, polymer dispersants with an acid value of 1 mgKOH / g or more and an amine value of less than 1 mgKOH / g, polymer dispersants with an amine value of 1 mgKOH / g or more and an acid value of 1 mgKOH / g or more, and polymer dispersants with an amine value of less than 1 mgKOH / g and an acid value of less than 1 mgKOH / g. Two or more of these may be used. Among these, polymer dispersants with an amine value of 1 mgKOH / g or more are preferred. The content of the polymer dispersant is preferably 10% by mass or more and 100% by mass or less, more preferably 20% by mass or more and 60% by mass or less, relative to 100% by mass of the colorant, and a content of the polymer dispersant of 10% by mass or more can improve the dispersion stability, while a content of the polymer dispersant of 100% by mass or less can improve the heat resistance and adhesion of the colored film.

[0098] The photosensitive colored resin composition of the present invention may contain a blocked isocyanate. A blocked isocyanate is a compound having two or more isocyanate groups blocked by a blocking agent. The blocked isocyanate has a long pot life and a photosensitive colored resin composition containing the blocked isocyanate has excellent viscosity stability because the blocking agent is dissociated by heating and the isocyanate group is regenerated. In the photosensitive colored resin composition of the present invention, the blocked isocyanate can be used as a curing agent. The blocked isocyanate dissociates (deprotects) the blocking agent by heating at a relatively low temperature to regenerate the isocyanate group. The regenerated isocyanate group thermally reacts with a hydroxyl group and / or a carboxyl group in the alkali-soluble resin, thereby curing the photosensitive colored resin composition. The type of blocked isocyanate is not particularly limited, and commercially available ones can be used. The content of the blocked isocyanate is preferably 1% by mass or more and 300% by mass or less with respect to 100 parts by mass of the alkali-soluble resin.

[0099] The photosensitive colored resin composition of the present invention may contain an adhesion improver. Examples of the adhesion improver include silane coupling agents such as vinyltrimethoxysilane, vinyltriethoxysilane, epoxycyclohexylethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, p-styryltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, and N-phenyl-3-aminopropyltrimethoxysilane, titanium chelating agents, aluminum chelating agents, and compounds obtained by reacting aromatic amine compounds with alkoxy group-containing silicon compounds. Two or more of these may be contained. By containing these adhesion improvers, the adhesion to the underlying substrate such as silicon wafers, ITO, SiO2, and silicon nitride can be improved when developing the photosensitive colored resin film. In addition, the resistance to oxygen plasma and UV ozone treatment used for cleaning can be improved. The content of the adhesion improver is preferably 0.1% by mass or more and 10% by mass or less based on 100% by mass of the alkali-soluble resin.

[0100] The photosensitive colored resin composition of the present invention may contain a surfactant for the purpose of improving wettability with the substrate or improving the uniformity of the thickness of the photosensitive colored resin film, if necessary. Even if the fluorine-containing resin has a surface activity, it is not included in the surfactants referred to here. Commercially available compounds can be used as the surfactant. The content of the surfactant is preferably 0.001% by mass or more and 1% by mass or less relative to 100% by mass of the alkali-soluble resin.

[0101] <Method for preparing photosensitive colored resin composition> The method for preparing the photosensitive colored resin composition of the present invention will be described below with reference to an example. However, it goes without saying that the following description is merely an example for the purpose of aiding in the implementation of the present invention, and the present invention is not limited to this example.

[0102] As a method for producing the photosensitive colored resin composition of the present invention, for example, a method is preferred in which a resin solution containing a colorant, a part of an alkali-soluble resin, and optionally a dispersant and a solvent is dispersed using a dispersing machine to prepare a dispersion liquid with a high colorant concentration, and then the remaining alkali-soluble resin, a photopolymerization initiator, a fluorine-containing resin, a radical polymerizable compound, and optionally other components are added and stirred. Filtration may be performed as necessary.

[0103] Examples of the dispersing machine include ball mills, bead mills, sand grinders, three-roll mills, and high-speed impact mills. Among these, bead mills are preferred for improving dispersion efficiency and fine dispersion. Examples of the bead mills include coball mills, basket mills, pin mills, and dyno mills. Examples of the beads used in the bead mills include titania beads, zirconia beads, and zircon beads. The bead diameter of the bead mill is preferably 0.03 mm to 1.0 mm. When the primary particle diameter of the colorant and the particle diameter of the secondary particles formed by the aggregation of the primary particles are small, it is preferable to use minute beads having a diameter of 0.03 mm to 0.10 mm. In this case, it is preferable to use a bead mill equipped with a separator using a centrifugal separation method that can separate the minute beads from the dispersion liquid. On the other hand, when dispersing a colorant containing coarse particles of the submicron order, it is preferable to use beads having a diameter of 0.10 mm or more in order to obtain sufficient crushing force.

[0104] Next, the method of forming a cured film by curing the photosensitive colored resin composition of the present invention will be described. The method of forming a cured film includes the steps of applying the photosensitive colored resin composition to the surface of a substrate to form a colored film, drying the colored film, exposing the colored film, developing the exposed colored film, and post-curing.

[0105] First, the process of applying a photosensitive colored resin composition to form a colored cured film will be described. In this process, the photosensitive colored resin composition of the present invention is applied to a substrate by spin coating, slit coating, dip coating, spray coating, printing, or the like to obtain a colored film. Among these, the slit coating method is preferably used. The coating speed in the slit coating method is generally in the range of 10 mm / sec to 400 mm / sec. The film thickness of the colored film varies depending on the solid content concentration and viscosity of the photosensitive colored resin composition, but it is usually applied so that the film thickness after drying is 0.1 μm to 10 μm, preferably 0.5 μm to 3 μm. Here, the solid content concentration refers to the ratio of the mass of components other than the solvent to the mass of all components at the time of preparing the composition, expressed as %. Examples of the substrate include transparent substrates such as soda glass, alkali-free glass, and quartz glass, silicon wafers, ceramics, and gallium arsenide substrates. A resin layer, an inorganic film, pixels, wiring, and the like may be present on the substrate. Prior to coating, the substrate to which the photosensitive colored resin composition is to be coated may be subjected to a pretreatment such as a UV treatment or a plasma treatment.

[0106] Next, the step of drying the colored film will be described. In this step, after applying the photosensitive colored resin composition, the colored film is dried. The drying method in this step is typically drying under reduced pressure or drying by heating. Both drying under reduced pressure and drying by heating may be performed, or only one of them may be performed. Drying by heating will be described. This step is also called pre-baking. For drying, a hot plate, an oven, infrared rays, etc. are used. The heating temperature varies depending on the type and purpose of the colored film, and it is preferable to perform the heating at a temperature in the range of 50°C to 180°C for one minute to several hours. In the drying step, volatile components such as the solvent are removed.

[0107] Next, the step of exposing the colored film will be described. In this step, in order to form a pattern from the obtained colored film, the colored film is exposed to actinic radiation through a mask having a desired pattern. Actinic radiation used for exposure includes ultraviolet rays, visible light, electron beams, and X-rays, but in the present invention, it is preferable to use i-rays (365 nm), h-rays (405 nm), and g-rays (436 nm) from a mercury lamp, or monochromatic light from a UV-LED light source.

[0108] Next, the process of developing the exposed colored film will be described. In this process, after exposure, the unexposed parts are removed using a developer to form a desired pattern. As the developer, an aqueous solution of an alkaline compound such as tetramethylammonium hydroxide (hereinafter, TMAH), diethanolamine, diethylaminoethanol, sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, triethylamine, diethylamine, methylamine, dimethylamine, dimethylaminoethyl acetate, dimethylaminoethanol, dimethylaminoethyl methacrylate, cyclohexylamine, ethylenediamine, or hexamethylenediamine is preferable. In some cases, polar solvents such as N-methyl-2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethylsulfoxide, γ-butyrolactone, or dimethylacrylamide, alcohols such as methanol, ethanol, or isopropanol, esters such as ethyl lactate or PGMEA, or ketones such as cyclopentanone, cyclohexanone, isobutyl ketone, or methyl isobutyl ketone may be added alone or in combination to these alkaline aqueous solutions. Possible development methods include spray, paddle, immersion, and ultrasonic. Next, it is preferable to rinse the pattern formed by development with distilled water. Here, too, rinsing may be performed by adding alcohols such as ethanol and isopropyl alcohol, or esters such as ethyl lactate and PGMEA to distilled water.

[0109] Next, the curing process of the colored film will be described. The patterned colored film obtained through the development process is subjected to a heat treatment (post-baking) to obtain a cured colored film (cured film). The heat treatment may be carried out in air, in a nitrogen atmosphere, or in a vacuum. The heating temperature is preferably 120 to 300°C, and the heating time is preferably 0.25 to 5 hours. The heating temperature may be changed continuously or stepwise.

[0110] The cured film of the present invention has a low reflection intensity on the film surface side due to the mass transfer effect of the fluorine-containing resin. This is believed to be because, when mass analysis is performed in the thickness direction of the cured film by time-of-flight secondary ion mass spectrometry (TOF-SIMS) using sputtered ions, the intensity profile of the substance derived from the fluorine-containing resin tends to be high near the film surface. Also, when composition analysis is performed in the depth direction by X-ray photoelectron spectroscopy (XPS), the intensity of fluorine atoms tends to be high near the film surface.

[0111] The fluorine-containing resin contained in the photosensitive colored resin composition of the present invention contains a repeating unit derived from a fluorine-containing monomer represented by general formula (1) and a repeating unit derived from a polyalkylene oxide group-containing monomer represented by general formula (4). By using such a fluorine-containing resin, the refractive index of the surface vicinity of the cured film can be specifically lowered by mass transfer during the process of applying and drying the photosensitive colored resin composition of the present invention, thereby exhibiting the effect of lowering the reflection intensity on the film surface side. EXAMPLES

[0112] The present invention will be described in detail below with reference to examples and comparative examples, but the aspects of the present invention are not limited to these.

[0113] <Evaluation method> [Light blocking property] The resin composition as the sample was applied onto an alkali-free glass substrate (AN100) manufactured by AGC Inc. using a spinner (MS-A150) manufactured by Mikasa Co., Ltd. so that the film thickness after post-curing would be 1 μm, and the colored film was heated and dried on a hot plate at 90 °C for 3 minutes. With respect to this colored film, ultraviolet rays were irradiated at 200 mJ / cm 2 and then it was subjected to a development treatment for 60 seconds with an alkaline developer of a 0.045 mass% potassium hydroxide aqueous solution. The obtained substrate was heated and dried in an oven at 170 °C for 30 minutes to obtain a cured film. Regarding the obtained cured film, using an optical densitometer 361TVisual manufactured by X-Rite, the OD value per 1 μm of unit film thickness was calculated and evaluated according to the following criteria. Note that A is the most excellent.

[0114] A: 2.5 or more B: 1.5 or more and less than 2.5 C: Less than 1.5.

[0115] [Brightness of total reflected light, brightness of diffuse reflected light] The resin composition as the sample was applied onto an alkali-free glass substrate (AN100) using a spinner (MS-A150) manufactured by Mikasa Co., Ltd. so that the film thickness after post-curing would be 1 μm, and the colored film was heated and dried on a hot plate at 90 °C for 3 minutes. With respect to this colored film, ultraviolet rays were irradiated at 200 mJ / cm 2 and then it was subjected to a development treatment for 60 seconds with an alkaline developer of a 0.045 mass% potassium hydroxide aqueous solution. The obtained substrate was heated and dried in an oven at 170 °C for 30 minutes to obtain a cured film. The obtained cured film was calibrated with a white calibration plate "CM-A145" manufactured by Konica Minolta Inc., and using a spectrocolorimeter "CM-2600d" manufactured by Konica Minolta Inc., light was made to enter from the surface of the cured film under the measurement conditions of a standard light source D65 (color temperature 6504K), a viewing angle of 10° (CIE1976), atmospheric pressure, and 20 °C, and measurements were performed respectively by the SCI method (detecting all reflected light including specular reflected light) and the SCE method (detecting only diffuse reflected light), and the brightness (L * value) was obtained in each measurement method and evaluated according to the following criteria. Note that A is the most excellent. <L value by measurement by the SCI method * > A: Less than 26.0 B: 26.0 or more and less than 33.5 C: 33.5 or more <L value measured by the SCE method * > A: Less than 0.4 B: 0.4 or more and less than 0.7 C: 0.7 or more.

[0116] [Developability] The resin composition as a sample was applied onto an alkali-free glass substrate (AN100) using a spinner (MS-A150) manufactured by Mikasa Co., Ltd. so that the film thickness after post-curing would be 1 μm, and the colored film was heated and dried on a hot plate at 90 °C for 3 minutes. With respect to this colored film, using a mask aligner (PEM-6M) manufactured by Union Optical Co., Ltd., ultraviolet rays were irradiated through a negative mask (design line & space: 4 locations of 5, 10, 15, 20 μm) manufactured by HOYA Co., Ltd. at 200 mJ / cm 2 exposure, and patterning substrates were obtained by developing with an alkaline developer of 0.045 mass% aqueous potassium hydroxide solution. The obtained patterning substrates were heated and dried in an oven at 170 °C for 30 minutes to obtain cured films.

[0117] For each pattern of line & space, using an optical microscope ("BH3-MJL (trade name)" manufactured by Olympus Sales Co., Ltd.), it was magnified 50 times and observed 100 locations per size, and the developability was evaluated according to the following criteria from the minimum opening pattern in which 90 or more patterns remained. Note that A is the most excellent.

[0118] A: The minimum pattern is less than 10 μm B: The minimum pattern is 10 μm or more and less than 20 μm C: The minimum pattern is 20 μm or more.

[0119] [Recoatability] The resin composition sample was applied onto a non-alkali glass substrate (AN100) using a spinner (MS-A150) manufactured by Mikasa Co., Ltd., so that the film thickness after post-curing would be 1 μm, and the colored film was heated and dried on a hot plate at 90° C. for 3 minutes. The colored film was irradiated with ultraviolet light at 200 mJ / cm 2 The film was exposed to light, developed for 60 seconds with an alkaline developer of 0.045% by weight potassium hydroxide aqueous solution, and then dried by heating in an oven at 170°C for 30 minutes to obtain a cured film. 1 μL of PGMEA was dropped onto the surface of the obtained cured film, and the contact angle was measured. The measurement was performed using a contact angle measuring device (DMs-401; manufactured by Kyowa Interface Science Co., Ltd.) in accordance with JIS-R3257, at 23°C by the sessile drop method.

[0120] The recoatability was evaluated based on the contact angle according to the following criteria, with A being the best.

[0121] A: Contact angle is 10 degrees or less B: Contact angle exceeds 10 degrees In many cases, a coating film of a composition containing a solvent such as PGMEA is formed on the cured film of the photosensitive color resin composition in a later process. If the contact angle of the solvent on the cured film is high, it becomes difficult to form a coating film in the later process.

[0122] (Synthesis Example 1: Synthesis of Alkali-Soluble Resin (P-1)) A methyl methacrylate / methacrylic acid / styrene copolymer (mass ratio 30 / 40 / 30) was synthesized by the method described in Example 1 of Japanese Patent No. 3120476. 40 parts by mass of glycidyl methacrylate was added to 100 parts by mass of the obtained copolymer, and the mixture was reprecipitated with purified water, filtered and dried to obtain an acrylic alkali-soluble resin (P-1) having a weight average molecular weight of 15,000 and an acid value of 110 mgKOH / g. The acid value of the alkali-soluble resin was the amount (mg) of potassium hydroxide required to neutralize 1 g of the alkali-soluble resin (unit: mgKOH / g), and the weight average molecular weight was measured in terms of polystyrene using a gel permeation chromatography (GPC) "HLC-8220GPC" (testing device manufactured by Tosoh Corporation) with tetrahydrofuran as the carrier.

[0123] (Synthesis Example 2: Synthesis of Fluorine-containing Resin (f-1)) In a two-necked eggplant flask, 5.7g of fluorine-containing monomer (a-1) represented by the following structural formula, 37.2g of Blenmar PP-800 (manufactured by NOF Corp.) (b-1), 57.2g of benzyl methacrylate (c-1), 0.6g of V-601 as an initiator, 1.1g of dodecanethiol (LM) as a polymerization regulator, and 203.3g of propylene glycol monomethyl ether acetate (PGMEA) as a solvent were placed, and the reaction mixture was stirred for 30 minutes while bubbling with nitrogen. The reaction mixture was heated to 80°C and stirred at 80°C for 5 hours.

[0124] After the reaction was completed, the reaction mixture was diluted with propylene glycol monomethyl ether acetate (PGMEA) so that the solid content concentration was 30% by mass. 0.3 equivalents of 2-(isocyanateethyl)acrylate (d-1) represented by the following structural formula and 0.01 equivalents of 1,4-diazabicyclo[2.2.2]octane were added to the monomer (b-1), and the reaction solution was stirred at 50°C for 20 hours to obtain a fluorine-containing resin (f-1).

[0125] [ka]

[0126] [In (a-1), R f is a structure represented by the following formula (1a) or (2a).

[0127] [ka]

[0128] [In the formula, * indicates the point of attachment to the oxygen atom.] In addition, the meaning of "≒" in formula (b-1) is an approximation because the used compound is a mixture of compounds with different values ​​of n, and the average value is not an integer (the same applies below).

[0129] (Synthesis Example 3: Synthesis of Fluorine-Containing Resin (f-2)) In a two-necked eggplant flask, 29.5 g of the fluorine-containing monomer (a-1), 64.9 g of Blenmar PP-800 (manufactured by NOF Corp.) (b-1), 5.6 g of HOA-MS (N) (manufactured by Kyoeisha Chemical Co., Ltd.) (c-2) represented by the following structural formula, 0.6 g of V-601 as an initiator, 1.1 g of dodecanethiol (LM) as a polymerization regulator, and 203.3 g of propylene glycol monomethyl ether acetate (PGMEA) as a solvent were placed, and the reaction mixture was stirred for 30 minutes while bubbling with nitrogen. The reaction mixture was heated to 80°C and stirred at 80°C for 5 hours. After the reaction was completed, the reaction mixture was diluted with propylene glycol monomethyl ether acetate (PGMEA) so that the solid content concentration was 30% by mass, to obtain a fluorine-containing resin (f-2).

[0130] [ka]

[0131] (Synthesis Example 4: Synthesis of fluororesin (k-1) not corresponding to fluororesin α) In a glass flask equipped with a stirrer, a thermometer, a cooling tube, and a dropping device, 20 parts by mass of a perfluoropolyether compound having hydroxyl groups at both ends represented by the following formula (ka), 10 parts by mass of diisopropyl ether as a solvent, 0.006 parts by mass of p-methoxyphenol as a polymerization inhibitor, and 3.3 parts by mass of triethylamine as a neutralizing agent were charged, and stirring was started under an air stream, and 3.1 parts by mass of methacrylic acid chloride was dropped over 2 hours while keeping the temperature in the flask at 10 ° C. After the dropwise addition, the mixture was stirred at 10 ° C for 1 hour, heated to 30 ° C and stirred for 1 hour, and then heated to 50 ° C and stirred for 10 hours to carry out a reaction, and the disappearance of methacrylic acid chloride was confirmed by gas chromatography measurement. Next, 70 parts by mass of diisopropyl ether was added as a solvent, and then 80 parts by mass of ion-exchanged water was mixed and stirred, and then the mixture was left to stand, and washing was repeated three times by a method of separating and removing the aqueous layer. Next, 0.02 parts by mass of p-methoxyphenol was added as a polymerization inhibitor, and 8 parts by mass of magnesium sulfate was added as a dehydrating agent. The mixture was allowed to stand for one day to completely dehydrate, and then the dehydrating agent was filtered off.

[0132] [ka]

[0133] (In the formula, X is a perfluoromethylene group or a perfluoroethylene group, and there are an average of 7 perfluoromethylene groups and an average of 8 perfluoroethylene groups per molecule.) Next, the solvent was distilled off under reduced pressure to obtain a compound having a poly(perfluoroalkylene ether) chain represented by the following formula (kb).

[0134] [ka]

[0135] (In the formula, X is a perfluoromethylene group or a perfluoroethylene group. There are an average of 7 perfluoromethylene groups and an average of 8 perfluoroethylene groups per molecule.) Next, 100 parts by mass of methyl isobutyl ketone was charged as a solvent in a glass flask equipped with a stirring device, a thermometer, a cooling tube, and a dropping device, and the temperature was raised to 105 ° C. while stirring under a nitrogen stream. Next, three types of dropping liquids, namely, 20 parts by mass of a compound (kb) having a poly(perfluoroalkylene ether) chain, a monomer solution in which 50.1 parts by mass of 3-hydroxy-1-adamantyl methacrylate (a compound represented by the following formula (k-c)) was dissolved in 120 parts by mass of methyl isobutyl ketone, and a polymerization initiator solution in which 10.5 parts by mass of t-butylperoxy-2-ethylhexanoate was dissolved in 80 parts by mass of methyl isobutyl ketone as a polymerization initiator, were set in separate dropping devices, and the flask was kept at 105 ° C. and dropped simultaneously over 2 hours. After the dropping was completed, the mixture was stirred at 105 ° C. for 5 hours, and then 262.1 parts by mass of the solvent was distilled off under reduced pressure to obtain a polymer (kd) solution.

[0136] [ka]

[0137] Next, 0.1 parts by mass of p-methoxyphenol as a polymerization inhibitor and 0.03 parts by mass of tin octylate as a urethane catalyst were added to the polymer (kd) solution obtained above, and stirring was started under an air stream. While maintaining the temperature at 60°C, 31.7 parts by mass of 2-methacryloyloxyethyl isocyanate was added dropwise over 1 hour. After the dropwise addition, the mixture was stirred at 60°C for 2 hours, then heated to 80°C and stirred for 10 hours, and the disappearance of the isocyanate group was confirmed by IR spectrum measurement. 70 parts by mass of methyl isobutyl ketone was added to obtain a methyl isobutyl ketone solution containing 50% of a fluorine-based resin (k-1) that does not fall under the category of fluorine-containing resin. The molecular weight of the obtained fluorine-based resin (k-1) that does not fall under the category of fluorine-containing resin was measured by GPC (polystyrene equivalent molecular weight), and the number average molecular weight was 1,500 and the weight average molecular weight was 4,100. The fluorine content of the fluorine-containing polymerizable resin (1) was 11 mass %, and the polymerizable unsaturated group equivalent was 500 g / eq.

[0138] (Synthesis Example 5: Synthesis of fluororesin (k-2) not corresponding to fluororesin α) In the same manner as in Synthesis Example 4, a compound (kb) having a poly(perfluoroalkylene ether) chain was obtained.

[0139] A glass flask equipped with a stirring device, a thermometer, a cooling tube, and a dropping device was charged with 101.6 parts by mass of methyl isobutyl ketone as a solvent, and the temperature was raised to 95 ° C. while stirring under a nitrogen stream. Next, three types of dropping liquids, namely 37.9 parts by mass of a compound (kb) having a poly(perfluoroalkylene ether) chain (liquid 1), 37.7 parts by mass of a solution in which 36.1 parts by mass of 2-methacryloyloxyethyl isocyanate was dissolved in 1.6 parts by mass of methyl isobutyl ketone (liquid 2), and 45.4 parts by mass of a solution in which 11.1 parts by mass of azobisdiisobutyronitrile, a radical polymerization initiator, was dissolved in 34.3 parts by mass of methyl isobutyl ketone (liquid 3), were set in separate dropping devices, and dropping was started simultaneously while maintaining the inside of the flask at 95 ° C., and liquids 1 and 2 were dropped for 2 hours, and liquid 3 was dropped for 2 hours and 20 minutes. After the dropwise addition was completed, the mixture was stirred at 95° C. for 10 hours, and then the solvent was distilled off to obtain a polymer (ke).

[0140] Next, 151.2 parts by mass of methyl ethyl ketone as a solvent, 0.066 parts by mass of p-methoxyphenol as a polymerization inhibitor, 0.496 parts by mass of dibutylhydroxytoluene, and 0.05 parts by mass of tin octylate as a urethanization catalyst were charged, and stirring was started under an air stream. While maintaining the temperature at 60°C, 97.8 parts by mass (57.7 parts by mass as PE3A) of a mixture of pentaerythritol triacrylate (hereinafter referred to as "PE3A") and pentaerythritol tetraacrylate (hereinafter referred to as "PE4A") ("Aronix M-305" manufactured by Toagosei Co., Ltd.; PE3A ratio 59% by mass, PE4A ratio 41% by mass) was added dropwise over 1 hour. After the dropwise addition, the mixture was stirred at 60°C for 2 hours, then heated to 80°C and stirred for 4 hours. Further, 0.113 parts by mass of tin octylate and 19.6 parts by mass of a mixture of PE3A and PE4A ("Aronix M-305" manufactured by Toagosei Co., Ltd.; PE3A ratio 59% by mass, PE4A ratio 41% by mass) (11.6 parts by mass as PE3A) were added, and the mixture was stirred at 80°C for 5 hours, after which the disappearance of the absorption peak of the isocyanate group was confirmed by IR spectrum measurement of the reaction solution. After cooling the reaction solution to room temperature, 103.9 parts by mass of methyl ethyl ketone was added, and the insoluble matter in the solution was filtered off to obtain a methyl ethyl ketone solution containing 42.6% of a fluororesin (k-2) that does not fall under the category of fluororesin. The molecular weight of this fluororesin (k-2), which does not fall under the category of fluorine-containing resin, was measured by GPC (polystyrene equivalent molecular weight) to find that the number average molecular weight was 1,000, the weight average molecular weight was 98,000, the maximum molecular weight was 3,000,000, the fluorine content was 15.3% by weight, and the radical polymerizable unsaturated group equivalent was 207 g / eq.

[0141] (Synthesis Example 6: Synthesis of radically polymerizable compound (M-1)) The compound described in Example 1 of Japanese Patent No. 5782281 was synthesized by the method described in the same example, and used as a radical polymerizable compound (M-1) having a fluorene skeleton.

[0142] (Synthesis Example 7: Synthesis of alkali-soluble resin (P-2)) In a 500 mL three-neck flask, 33 g of methyl methacrylate (0.33 mol), 33 g of styrene (0.32 mol), 34 g of methacrylic acid (0.39 mol), 3 g of 2,2'-azobis(2-methylbutyronitrile) (0.02 mol) and 150 g of PGMEA were charged and stirred at 90 ° C for 2 hours, then the internal temperature was raised to 100 ° C and reacted for another hour. 33 g of glycidyl methacrylate, 1.2 g of dimethylbenzylamine and 0.2 g of p-methoxyphenol were added to the resulting reaction solution and stirred at 90 ° C for 4 hours, and 50 g of PGMEA was added at the end of the reaction to obtain a PGMEA solution (solid concentration 40%) of an alkali-soluble resin (P-2). The alkali-soluble resin (P-2) had an acid value of 80.0 mgKOH / g and a weight average molecular weight of 22,000 as measured by GPC.

[0143] (Production Example 1: Production of Colorant Dispersion (DB-1)) 96 g of carbon black “#1000” (manufactured by Mitsubishi Chemical Corporation) having an average primary particle size of 18 nm, a dibutyl phthalate absorption of 56 cm3 / 100 g, and a pH value of 3.5 as a black pigment, 98 g of a 35 mass % PGMEA solution of the alkali-soluble resin (P-1) obtained in Synthesis Example 1, 17 g of an amine-based polymer dispersant DISPER BYK (registered trademark) 21116 (a PGMEA solution having a solid content of 40%, manufactured by BYK-Chemie KK; hereinafter, “BYK-21116”) as a dispersant, 235 g of PGMEA, and 103 g of 3-methoxybutyl acetate (hereinafter, MBA) were charged into a tank and stirred for 20 minutes with a homomixer to obtain a preliminary dispersion. The preliminary dispersion obtained was fed to a Kotobuki Industries Co., Ltd. disperser, Ultra Apex Mill UAM015, equipped with a centrifugal separator filled with 75% by volume of zirconia beads with a bead diameter of 0.10 mm, and dispersion was carried out for 139 minutes at a rotation speed of 9 m / s to obtain a colorant dispersion (DB-1) with a solids concentration of 25% and a colorant / (resin + dispersant) (mass ratio) of 70 / 30. The secondary particle diameter of the black pigment contained in (DB-1) was 61 nm. The secondary particle diameter was measured at 25°C using a dynamic light scattering particle size distribution measuring device (SZ-100; Horiba, Ltd.) by diluting (DB-1) with PGMEA and measuring the secondary particle diameter (D 50) was calculated as the average secondary particle size.

[0144] (Production Example 2: Production of Colorant Dispersion (DB-2)) A colorant dispersion (DB-2) with a solid content of 25% and a colorant / (resin+dispersant) (mass ratio) of 70 / 30 was obtained in the same manner as in Production Example 1, except that "MA100" (manufactured by Mitsubishi Chemical Corporation) was used as the black pigment. The secondary particle diameter of the black pigment contained in (DB-2) was 110 nm.

[0145] (Production Example 3: Production of colorant dispersion (r-1)) 50 g of PR254 (Irgaphor (registered trademark) Red BK-CF; manufactured by BASF Japan Co., Ltd.), 21 g of PR177 (Chromofine (registered trademark) Red 6125EC; manufactured by Dainichiseika Color & Chemicals Co., Ltd.), 70 g of BYK-21116 (polymer dispersant), 116 g parts by mass of a 40% by mass solution of the alkali-soluble resin (P-2) obtained in Synthesis Example 7 in PGMEA, and 291 g of PGMEA were mixed and dispersed using a mill-type disperser filled with zirconia beads to obtain a colorant dispersion (r-1).

[0146] Example 1 To 32.0 g of the colorant dispersion (DB-1), 11.0 g of a 35 mass% PGMEA solution of (P-1) as an alkali-soluble resin, 5.8 g of DPHA (a mixture of dipentaerythritol hexaacrylate and dipentaerythritol pentaacrylate, manufactured by Nippon Kayaku Co., Ltd.) as a radical polymerizable compound, 1.3 g of an acetophenone-based initiator IC379 (manufactured by BASF Japan Co., Ltd.) as a photopolymerization initiator, 3.3 g of a 30 mass% PGMEA solution of fluorine-containing resin (f-1), and 46.6 g of PGMEA were added, and a photosensitive colored resin composition (PB-1) with a solid concentration of 20% and a pigment / resin (mass ratio) of 30 / 70 was obtained.

[0147] Example 2 The amount of DPHA added was changed to 4.4 g, and 1.4 g of a radical polymerizable compound (M-1) having a fluorene skeleton was added. The same procedure as in Example 1 was repeated to obtain a photosensitive colored resin composition (PB-2) with a solid content of 20% and a pigment / resin (mass ratio) of 30 / 70.

[0148] Example 3 A photosensitive colored resin composition (PB-3) having a solid content of 20% and a pigment / resin (mass ratio) of 30 / 70 was obtained in the same manner as in Example 2, except that the same amount of NCI-831E was added instead of IC379.

[0149] Example 4 The same procedure as in Example 3 was repeated except that the amount of PGMEA added was changed to 26.5 g and an additional 20.0 g of BDG-AC was added, to obtain a photosensitive colored resin composition (PB-4) with a solid content of 20% and a pigment / resin (mass ratio) of 30 / 70.

[0150] Example 5 A photosensitive colored resin composition (PB-5) with a solid content of 20% and a pigment / resin (mass ratio) of 30 / 70 was obtained in the same manner as in Example 4, except that the same amount of DPMA was added instead of BDG-AC.

[0151] Example 6 To 45.5 g of colorant dispersion (DB-1), 5.3 g of 35 mass% PGMEA solution of (P-1), 3.5 g of DPHA, 1.2 g of (M-1), 1.1 g of NCI-831E, 3.3 g of 30 mass% PGMEA solution of fluorine-containing resin (f-1), and 40.2 g of PGMEA were added to obtain a photosensitive colored resin composition (PB-6) with a solid concentration of 20% and a pigment / resin (mass ratio) of 42 / 58.

[0152] Example 7 To 54.6 g of the colorant dispersion (DB-1), 1.5 g of a 35 mass% PGMEA solution of (P-1), 3.0 g of DPHA, 1.0 g of (M-1), 0.9 g of NCI-831E, 3.3 g of a 30 mass% PGMEA solution of fluorine-containing resin (f-1), and 35.8 g of PGMEA were added to obtain a photosensitive colored resin composition (PB-7) with a solid concentration of 20% and a pigment / resin (mass ratio) of 50 / 50.

[0153] Example 8 A photosensitive colored resin composition (PB-8) having a solid content of 20% and a pigment / resin (mass ratio) of 30 / 70 was obtained in the same manner as in Example 3, except that (DB-2) was used instead of (DB-1).

[0154] Example 9 A photosensitive colored resin composition (PB-9) was obtained in the same manner as in Example 1, except that a 30% by mass PGMEA solution of fluororesin (f-2) was used instead of a 30% PGMEA solution of fluororesin (f-1).

[0155] Example 10 To 31.9 g of the colorant dispersion (r-1), 1.9 g of a 35% solids concentration PGMEA solution of (P-1) as an alkali-soluble resin, 3.3 g of DPHA, 1.1 g of (M-1), 0.4 g of NCI-831E, 3.3 g of a 30% by mass PGMEA solution of fluorine-containing resin (f-1), and 58.0 g of PGMEA were added to obtain a photosensitive colored resin composition (DR-1) with a solids concentration of 20% and a pigment / resin (mass ratio) of 30 / 70.

[0156] Comparative Example 1 Instead of adding 3.3 g of 30 mass % PGMEA solution of fluorine-containing resin (f-1), 0.1 g of polyether-modified polydimethylsiloxane BYK-333 (manufactured by BYK-Chemie Co., Ltd.) was added, and the amount of PGMEA added was changed to 49.8 g. In the same manner as in Example 1, a photosensitive colored resin composition (PB-10) with a solid concentration of 20% and a pigment / resin (mass ratio) of 30 / 70 was obtained.

[0157] Comparative Example 2 Instead of adding BYK-333, 1.0 g of Megafac (registered trademark) F-477 (manufactured by DIC Corporation), a fluorine-based compound that does not have a double bond between carbon atoms, was added, and the amount of PGMEA added was changed to 48.9 g. In the same manner as in Comparative Example 1, a photosensitive colored resin composition (PB-11) with a solid concentration of 20% and a pigment / resin (mass ratio) of 30 / 70 was obtained.

[0158] Comparative Example 3 To 32.0 g of the colorant dispersion (DB-1), 11.0 g of a 35 mass% PGMEA solution of (P-1) as an alkali-soluble resin, 5.8 g of DPHA as a radical polymerizable compound, 1.3 g of an acetophenone-based initiator IC379 (manufactured by BASF Japan Ltd.) as a photopolymerization initiator, 2.0 g of a 50 mass% methyl isobutyl ketone solution of (k-1) as a fluorine-based resin that does not fall under the category of fluorine-containing resin, and 47.9 g of PGMEA were added to obtain a photosensitive colored resin composition (PB-12) with a solid concentration of 20% and a pigment / resin (mass ratio) of 30 / 70.

[0159] Comparative Example 4 A photosensitive colored resin composition (PB-13) with a solid content of 20% and a pigment / resin (mass ratio) of 30 / 70 was obtained in the same manner as in Comparative Example 3, except that 2.0 g of a 50 mass% methyl isobutyl ketone solution of (k-1) was added as a fluorine-based resin not corresponding to a fluorine-containing resin, and 2.4 g of a 42.6 mass% methyl ethyl ketone solution of (k-2) was added instead, and the amount of PGMEA added was changed to 47.5 g.

[0160] Comparative Example 5 To 31.9 g of the colorant dispersion (r-1), 4.8 g of 35 mass% PGMEA solution of (P-1) as an alkali-soluble resin, 4.4 g of DPHA, 0.4 g of NCI-831E, and 58.5 g of PGMEA were added to obtain a photosensitive colored resin composition (DR-2).

[0161] The results are shown in Tables 1 and 2.

[0162] [Table 1]

[0163] [Table 2]

[0164] The colored resin compositions of the examples have excellent jet blackness because of low values ​​of total reflection and diffuse reflection chromaticity of the film surface. In addition, the contact angle of PGMEA is low, and the recoatability is excellent.

[0165] On the other hand, the colored resin composition of the comparative example is inferior in jet blackness because the total reflection and diffuse reflection chromaticity values ​​of the film surface are high when it does not satisfy the requirement of the fluorine-containing resin described in claim 1. In addition, when it contains a fluorine-based compound that does not correspond to the fluorine-containing resin α, it is found that the contact angle value of PGMEA is high and the recoatability is poor, causing problems in forming a coating film in a later process.

[0166] Example 11 For (PB-5), the evaluation of [total reflection / diffuse reflection] was carried out in the same manner as in Example 5, except that the development processing time was changed to 30 seconds in the evaluation method of [total reflection / diffuse reflection].

[0167] Example 12 For (PB-5), the evaluation of [total reflection / diffuse reflection] was carried out in the same manner as in Example 5, except that the development processing time in the evaluation method of [total reflection / diffuse reflection] was changed to 90 seconds.

[0168] Example 13 For (PB-5), the evaluation of [total reflection / diffuse reflection] was carried out in the same manner as in Example 5, except that the development processing time in the evaluation method of [total reflection / diffuse reflection] was changed to 120 seconds.

[0169] The evaluation results for each example are shown in Table 3.

[0170] [Table 3]

[0171] As shown in the examples, even if the development time is changed, the total reflection and diffuse reflection chromaticity values ​​of the film surface are low, and therefore the color clarity and jet blackness are excellent. [Industrial Applicability]

[0172] The photosensitive colored resin composition and cured film of the present invention can be suitably used for light-shielding images such as black matrices of color filters in liquid crystal display devices and the like, colored partitions inside organic EL displays, mini LED displays, and light-shielding images such as black matrices inside micro LED displays.

Claims

1. A photosensitive colored resin composition comprising a colorant, an alkali-soluble resin, a photopolymerization initiator, a fluorine-containing resin containing a repeating unit derived from a fluorine-containing monomer represented by the following general formula (1) and a repeating unit derived from a polyalkylene oxide group-containing monomer represented by the following general formula (4), and a radical polymerizable compound: 【Chemistry 1】 [In the formula, R 1 represents a hydrogen atom or a methyl group. 1 R represents a divalent linking group. f is a structure represented by the following formula (2-1) or (2-2). 【Chemistry 2】 [In the formula, * indicates the point of attachment to the oxygen atom.] 【Chemistry 3】 [In the formula, R 2 represents a monovalent group having a carbon-carbon double bond. 2 R represents an alkylene group having 2 to 4 carbon atoms. 3 represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. 3 represents an integer of 2 or more.

2. 2. The photosensitive colored resin composition according to claim 1, wherein the fluorine-containing resin further contains a structural unit derived from an isocyanate group-containing compound represented by the following general formula (6): 【Chemistry 4】 [In the formula, R 6 represents a monovalent group having a carbon-carbon double bond. 4 is a divalent saturated aliphatic hydrocarbon group having 2 to 10 carbon atoms, and the saturated aliphatic hydrocarbon group may have an ether bond.

3. 3. The photosensitive colored resin composition according to claim 1, wherein all or a part of the radical polymerizable compound is a compound containing a fluorene skeleton or a polyfunctional acrylate compound having three or more functional groups.

4. 3. The photosensitive colored resin composition according to claim 1, wherein all or a part of the photopolymerization initiator is an oxime ester-based photopolymerization initiator.

5. The photosensitive colored resin composition according to claim 1 or 2, further comprising a solvent, the solvent having a vapor pressure of 0.01 Pa or more and 100 Pa or less at 20° C. being contained in an amount of 10 mass % or more relative to 100 mass % of the total solvent.

6. 3. The photosensitive colored resin composition according to claim 1, comprising a black pigment as a coloring material in an amount of 10% by mass or more and 60% by mass or less based on the solid content concentration.

7. 3. The photosensitive colored resin composition according to claim 1, wherein the secondary particle diameter of the colorant is 30 nm or more and 100 nm or less.

8. 3. The photosensitive colored resin composition according to claim 1, wherein when the photosensitive colored resin composition is cured, the contact angle of propylene glycol monomethyl ether acetate on the cured film is 10 degrees or less.

9. A cured film, which is produced by coating the photosensitive colored resin composition according to claim 1 or 2 on a substrate, followed by drying, exposing, developing and curing.

Citation Information

Patent Citations

  • Cured coloring film for image display devices, photo-sensitive coloring composition for image display devices, and image display device

    JP2018141849A

  • Photosensitive resin composition for black resist, cured film, method for producing cured film, and color filter and partition having cured film

    JP2022173086A