Thermosetting resin composition, phenoxy resin, composite resin composition, resin sheet, metal base board, and electronic device
A thermosetting resin composition with a mesogenic skeleton and thermally conductive filler improves thermal conductivity, addressing the inadequacies of existing epoxy resin compositions for heat dissipation in electronic components.
Patent Information
- Application Number
- JP2023054890
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Existing thermosetting resin compositions, particularly those based on epoxy resins, do not achieve sufficient thermal conductivity for effective heat dissipation in high-power electronic components.
Incorporation of a dihydroxy compound and a bifunctional epoxy compound with a mesogenic skeleton into the thermosetting resin composition, along with a thermally conductive filler, to enhance thermal conductivity and heat resistance.
The resulting cured products exhibit high thermal conductivity, making them suitable for heat dissipation applications in electronic devices.
Smart Images

Figure 2024142652000053 
Figure 2024142652000054 
Figure 2024142652000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermosetting resin composition, a resin sheet made of the thermosetting resin composition, an electronic device comprising a cured product of the resin sheet as a thermally conductive sheet, a metal base substrate comprising the cured product of the resin sheet, and an electronic device comprising the metal base substrate, as well as a phenoxy resin and a composite resin composition containing the phenoxy resin. [Background technology]
[0002] With the high integration of semiconductors and the rapid improvement of the processing power of electronic devices, electronic components with high processing power generate a lot of heat. Therefore, heat countermeasures to effectively dissipate heat from electronic components to the outside have become a very important issue. As a countermeasure for such heat dissipation, thermally conductive members made of heat dissipating materials such as metals, ceramics, and polymer compositions are used for heat dissipation members such as printed wiring boards, semiconductor packages, housings, heat pipes, heat sinks, and heat diffusion plates.
[0003] Among these heat dissipation members, thermally conductive epoxy resin molded products molded from epoxy resin compositions are excellent in electrical insulation properties, mechanical properties, heat resistance, chemical resistance, adhesive properties, etc., and are therefore widely used mainly in the electrical and electronic fields as castings, laminates, sealing materials, thermally conductive sheets, adhesives, etc.
[0004] Epoxy resin compositions constituting thermally conductive epoxy resin molded bodies are known to contain a thermally conductive filler with high thermal conductivity blended into a polymer matrix material such as resin, rubber, etc. Examples of thermally conductive fillers that have been used include metal oxides such as aluminum oxide, magnesium oxide, zinc oxide, and quartz, metal nitrides such as boron nitride and aluminum nitride, metal carbides such as silicon carbide, metal hydroxides such as aluminum hydroxide, metals such as gold, silver, and copper, carbon fibers, and graphite.
[0005] When even higher thermal conductivity is required, thermally conductive epoxy resin compositions and thermally conductive epoxy resin molded bodies in which a special thermally conductive filler is blended with epoxy resin have been proposed (for example, Patent Document 1). It has also been proposed to improve the thermal conductivity and heat resistance of the epoxy resin itself (for example, Patent Document 2). In Patent Document 2, an insulating composition with improved thermal conductivity is obtained by polymerizing a liquid crystal epoxy resin having a mesogen group. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2015-193504 A [Patent Document 2] Patent Application No. 2004-331811 Summary of the Invention [Problem to be solved by the invention]
[0007] However, as a result of investigations by the present inventors, it was found that the resin composition described in Patent Document 2 has room for further improvement in terms of thermal conductivity. [Means for solving the problem]
[0008] The present invention has been made in consideration of the above problems, and has been completed based on the discovery that a compound having a specific mesogenic skeleton has high thermal conductivity.
[0009] According to the present invention, there are provided a thermosetting resin composition, a phenoxy resin, a composite resin composition, a resin sheet, a metal base substrate, and an electronic device, as shown below. [1] A dihydroxy compound (A) represented by formula (1-1), A bifunctional epoxy compound (B) having two epoxy groups, represented by the formula (d-EP), A thermosetting resin composition comprising: [ka] In formula (1-1), R 11 may be the same or different and each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms, R 12 may be the same or different and each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms, [ka] In formula (d-EP), X is a divalent group having a mesogenic skeleton. Thermosetting resin composition. [2] The thermosetting resin composition according to item [1], The dihydroxy compound (A) has a structure represented by formula (1-2): [ka] In formula (1-2), R 11 and R 12 has the same meaning as that in the above formula (1-1), [3] The thermosetting resin composition according to item [1] or [2], In the formula (d-EP), X contains a divalent group represented by formula (2). [ka] In formula (2), R 1 ~R 8 each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms, and * represents a linking position. [4] The thermosetting resin composition according to item [3], In the group represented by formula (2), R 1 , R 4 , R 5 , and R 8 is an alkyl group having 1 to 4 carbon atoms, and R 2 , R3 , R 6 , and R 7 is a hydrogen atom. [5] The thermosetting resin composition according to item [3], In the group represented by the formula (2), R 1 , R 4 , R 5 , and R 8 is a methyl group, and R 2 , R 3 , R 6 , and R 7 is a hydrogen atom. [6] The thermosetting resin composition according to item [3], In the group represented by the formula (2), R 1 ~R 8 are all hydrogen atoms. [7] The thermosetting resin composition according to any one of items [1] to [6], The thermosetting resin composition further comprises a curing accelerator. [8] The thermosetting resin composition according to any one of items [1] to [7], The thermosetting resin composition further comprises a thermally conductive filler. [9] A resin sheet comprising the thermosetting resin composition according to any one of items [1] to [8].
[10] A heat generating member; A heat dissipation member; a thermally conductive sheet provided between the heat generating component and the heat dissipating component, The thermally conductive sheet is made of a cured resin sheet according to item [9].
[11] A metal substrate; A thermally conductive sheet; A metal base substrate comprising, in this order, The thermally conductive sheet is a metal base substrate made of a cured resin sheet according to item [9].
[12] An electronic device comprising the metal base substrate according to item
[11] .
[13] A phenoxy resin having a structure represented by formula (3), [ka] In formula (3), n is a number representing a repeating unit and represents an integer of 2 to 50; X is a divalent group having a mesogenic skeleton, Y is a divalent group represented by formula (1-3), [ka] In formula (1-3), R 11 may be the same or different and each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms, R 12 may be the same or different and each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms, * indicates the linking position. Phenoxy resin.
[14] The phenoxy resin according to item
[13] , In the formula (3), Y is a divalent group represented by the formula (1-4), [ka] In formula (1-4), R 11 and R 12 is defined as the same as in the above formula (1-3), and * represents a linking position. A phenoxy resin.
[15] The phenoxy resin according to item
[13] or
[14] , In the formula (d-EP), X contains a divalent group represented by formula (2). [ka] In formula (2), R 1 ~R 8each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms, and * represents the linking position; phenoxy resin.
[16] The phenoxy resin according to item
[15] , In the group represented by the formula (2), R 1 , R 4 , R 5 , and R 8 is an alkyl group having 1 to 4 carbon atoms, and R 2 , R 3 , R 6 , and R 7 is a hydrogen atom.
[17] The phenoxy resin according to item
[15] , In the group represented by the formula (2), R 1 , R 4 , R 5 , and R 8 is a methyl group, and R 2 , R 3 , R 6 , and R 7 is a hydrogen atom, phenoxy resin.
[18] The phenoxy resin according to item
[15] , In the group represented by the formula (2), R 1 ~R 8 Phenoxy resin, in which all of the atoms are hydrogen.
[19] Epoxy resin; A thermosetting resin (excluding the epoxy resin), A phenoxy resin represented by formula (3), A composite resin composition comprising: [ka] In formula (3), n is a number representing a repeating unit and represents an integer of 2 to 50; X is a divalent group having a mesogenic skeleton, Y is a divalent group represented by formula (1-3), [ka] In formula (1-3), R 11 may be the same or different and each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms, R 12 may be the same or different and each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms, * indicates the linking position. Composite resin composition.
[20] The composite resin composition according to item
[19] , In the formula (3), Y is a divalent group represented by the formula (1-4), [ka] In formula (1-4), R 11 and R 12 is defined as the same as in the above formula (1-3), and * represents a linking position.
[21] The composite resin composition according to item
[19] or
[20] , In the formula (3), X contains a divalent group represented by the formula (2), [ka] In formula (2), R 1 ~R 8 each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms, and * represents a linking position.
[22] The composite resin composition according to item
[21] , In the group represented by formula (2), R 1 , R 4 , R 5 , and R 8 is an alkyl group having 1 to 4 carbon atoms, and R 2 , R 3 , R 6 , and R 7 is a hydrogen atom.
[23] The composite resin composition according to item
[21] , In the group represented by formula (2), R 1 , R 4 , R 5 , and R 8 is a methyl group, and R 2 , R 3 , R 6 , and R 7 is a hydrogen atom.
[24] The composite resin composition according to item
[21] , In the group represented by formula (2), R 1 ~R 8 and all of the above are hydrogen atoms.
[25] The composite resin composition according to any one of items
[19] to
[24] , The composite resin composition, wherein the phenoxy resin has a weight average molecular weight of 2,000 or more and 10,000 or less.
[26] The composite resin composition according to any one of items
[19] to
[25] , The composite resin composition includes at least one thermosetting resin selected from the group consisting of a cyanate resin, a maleimide resin, a phenolic resin, and a benzoxazine resin.
[27] The composite resin composition according to any one of items
[19] to
[26] , wherein the thermally conductive filler comprises boron nitride.
[28] The composite resin composition according to any one of items
[19] to
[27] , further comprising a curing accelerator.
[29] A resin sheet comprising the composite resin composition according to any one of items
[19] to
[28] .
[30] A heat generating member; A heat dissipation member; a thermally conductive sheet provided between the heat generating component and the heat dissipating component, The thermally conductive sheet is made of a cured resin sheet according to item
[29] .
[31] A metal substrate; A thermally conductive sheet; A metal base substrate comprising, in this order, The thermally conductive sheet is a metal base substrate made of a cured resin sheet according to item
[29] .
[32] An electronic device comprising the metal base substrate according to item
[31] . Effect of the Invention
[0010] According to the present invention, there is provided a thermosetting resin composition which provides a cured product having high thermal conductivity. [Brief description of the drawings]
[0011] [Figure 1] 1 is a schematic cross-sectional view showing a structure of a metal base substrate according to an embodiment of the present invention. [Diagram 2] 1 is a schematic cross-sectional view showing a configuration of an electronic device using a metal base substrate according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In all drawings, similar components are given similar reference symbols and their description will be omitted as appropriate. In addition, "~" indicates "above" to "below" unless otherwise specified.
[0013] [Thermosetting resin composition] The thermosetting resin composition according to the first embodiment of the present invention comprises: A dihydroxy compound (A) represented by formula (1-1), and a difunctional epoxy compound (B) having two epoxy groups, represented by the formula (d-EP).
[0014] [ka]
[0015] In formula (1-1), R 11 may be the same or different and each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms, R 12 may be the same or different and each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms.
[0016] [ka]
[0017] In formula (d-EP), X is a divalent group having a mesogenic skeleton.
[0018] The thermosetting resin composition of the present embodiment contains a dihydroxy compound represented by the above formula (1-1). The compound represented by formula (1-1) has high planarity and high rigidity. Therefore, the cured product of the thermosetting resin composition containing this has high thermal conductivity.
[0019] The thermosetting resin composition of the present embodiment contains a bifunctional epoxy compound having a mesogenic skeleton represented by formula (d-EP). By containing such an epoxy compound having a mesogenic skeleton, the thermosetting resin composition of the present embodiment has high thermal conductivity when it is cured.
[0020] Hereinafter, the components used in the thermosetting resin composition in the first embodiment will be described.
[0021] (Dihydroxy Compounds) The dihydroxy compound used in the thermosetting resin composition of this embodiment has a structure represented by formula (1-1).
[0022] [ka]
[0023] In formula (1-1), R 11may be the same or different, and each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms. R 11 is preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and more preferably a hydrogen atom or an alkyl group having 1 carbon atom (a methyl group). R 12 may be the same or different, and each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms. R 12 is preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and more preferably a hydrogen atom or an alkyl group having 1 carbon atom (a methyl group). Particularly preferably, R 11 and R 12 are all hydrogen atoms.
[0024] Among the dihydroxy compounds represented by the above formula (1-1), it is preferable to use the dihydroxy compound represented by the formula (1-2) since it has particularly high planarity.
[0025] [ka]
[0026] In formula (1-2), R 11 and R 12 has the same meaning as in the above formula (1-1), and the same applies to preferred embodiments.
[0027] The dihydroxy compound represented by formula (1-1) may be a commercially available product or may be synthesized by a method known in the art. For example, R 11 and R 12 The compound represented by formula (1-2), in which all of are hydrogen atoms, can be synthesized by subjecting 6-bromo-2-naphthol and 4-hydroxyphenylboronic acid to a coupling reaction in a solvent in the presence of a palladium catalyst and a base.
[0028] The amount of the dihydroxy compound represented by the formula (1-1) in the thermosetting resin composition of the present embodiment is, for example, 2% by mass to 50% by mass, preferably 5% by mass to 40% by mass, based on the total solid content of the thermosetting resin composition. By adding the dihydroxy compound within the above range, the fluidity of the resulting resin composition can be adjusted to a desired level, and the thermal conductivity of the cured product can be improved.
[0029] (Difunctional epoxy compound) The difunctional epoxy compound used in the thermosetting resin composition of the present embodiment is a compound represented by the formula (d-EP).
[0030] [ka]
[0031] In formula (d-EP), X is a divalent group having a mesogenic skeleton. Since the thermosetting resin composition of the present embodiment contains a bifunctional epoxy compound having a mesogenic skeleton, the resulting cured product has high thermal conductivity and high heat resistance.
[0032] Examples of the mesogenic skeleton of the X group in formula (d-EP) include a biphenyl skeleton, a naphthalene skeleton, a phenylbenzoate skeleton, an azobenzene skeleton, a stilbene skeleton, a cyclohexylbenzene skeleton, and derivatives thereof. When the X group has the above-mentioned mesogenic skeleton, the cured product of the obtained thermosetting resin composition can have high thermal conductivity.
[0033] In one embodiment, at least one of the X groups in formula (d-EP) is a group represented by formula (2). By using a bifunctional epoxy compound in which the X group in formula (d-EP) is a mesogenic skeleton represented by formula (2), the cured product of the thermosetting resin composition of this embodiment has high thermal conductivity and excellent heat resistance.
[0034] [ka]
[0035] In formula (2), R 1 ~R 8 each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms, and * represents the linking position.
[0036] In one embodiment, the bifunctional epoxy compound is a compound in which R1, R4, R5, and R8 in formula (2) are alkyl groups having 1 to 4 carbon atoms, and R2, R3, R6, and R7 are hydrogen atoms. Among them, the bifunctional epoxy compound is an epoxy compound in which R1, R4, R5, and R8 in formula (2) are alkyl groups having 1 carbon atom (methyl group), and R2, R3, R6, and R7 are hydrogen atoms (X group is a "tetramethylbiphenyl group"). By using such a bifunctional epoxy compound, the cured product of the obtained thermosetting resin composition can have a good balance between thermal conductivity and heat resistance.
[0037] In one embodiment, the bifunctional epoxy compound is an epoxy compound in which R1, R4, R5, and R8 in formula (2) are alkyl groups having one carbon atom, and R2, R3, R6, and R7 are hydrogen atoms (X group is a "biphenyl group"). By using such a bifunctional epoxy compound, the cured product of the obtained thermosetting resin composition has excellent thermal conductivity and heat resistance.
[0038] In one embodiment, the bifunctional epoxy compound represented by formula (d-EP) is preferably a compound containing a tetramethylbiphenyl group and a biphenyl group as the X group. By containing such a combination of bifunctional epoxy compounds, the cured product of the obtained thermosetting resin composition can have an excellent balance between thermal conductivity and heat resistance.
[0039] The bifunctional epoxy compounds may be used alone or in combination of two or more.
[0040] The amount of the bifunctional epoxy compound represented by the formula (d-EP) in the thermosetting resin composition of the present embodiment is, for example, 50% by mass or more and 98% by mass or less, and preferably 60% by mass or more and 95% by mass or less, based on the total solid content of the thermosetting resin composition. By blending the bifunctional epoxy compound within the above range, the curing properties of the resulting resin composition can be adjusted to an appropriate level.
[0041] (Cure accelerator) The thermosetting resin composition of the present embodiment may contain a curing accelerator. The type and amount of the curing accelerator are not particularly limited, and an appropriate one can be selected from the viewpoints of reaction speed, reaction temperature, storage property, etc.
[0042] Examples of the curing accelerator that can be used include imidazoles, organic phosphorus compounds, tertiary amines, phenolic compounds, organic acids, etc. These may be used alone or in combination of two or more. Among these, from the viewpoint of increasing the heat resistance of the resulting resin composition, it is preferable to use a nitrogen atom-containing compound such as imidazoles.
[0043] Examples of the imidazoles include 2-methylimidazole, 2-ethyl-4-methylimidazole, 2-phenyl-4-methylimidazole, 2,4-diethylimidazole, 2-phenyl-4-methyl-5-hydroxyimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, 1-cyanoethyl-2-phenylimidazole, and 1-cyanoethyl-2-phenylimidazolium trimellitate.
[0044] Examples of the organic phosphorus compound include triphenylphosphine, tri-p-tolylphosphine, tetraphenylphosphonium tetraphenylborate, triphenylphosphine triphenylborane, and 1,2-bis-(diphenylphosphino)ethane. Examples of the tertiary amines include triethylamine, tributylamine, 1,4-diazabicyclo[2.2.2]octane, and 1,8-diazabicyclo(5,4,0)undecene-7. Examples of the phenol compound include phenol resin, bisphenol A, nonylphenol, 2,2-bis(3-methyl-4-hydroxyphenyl)propane, and allylphenol. Examples of the organic acid include acetic acid, benzoic acid, salicylic acid, and p-toluenesulfonic acid.
[0045] The amount of the curing accelerator to be added is, for example, 0.01 to 10 mass%, preferably 0.02 to 5 mass%, and more preferably 0.05 to 1.5 mass%, based on the total solid content of the thermosetting resin composition.
[0046] (Thermal conductive filler) The thermosetting resin composition of the present embodiment may contain a thermally conductive filler. By blending the thermally conductive filler, the thermosetting resin composition of the present embodiment can be used as a material for producing a heat dissipation member. The thermally conductive filler may contain, for example, highly thermally conductive inorganic particles having a thermal conductivity of 20 W / m·K or more. Examples of highly thermally conductive inorganic particles include alumina, aluminum nitride, boron nitride, silicon nitride, silicon carbide, and magnesium oxide. These may be used alone or in combination of two or more.
[0047] When boron nitride is used as the thermally conductive filler, the boron nitride may contain monodisperse particles, agglomerated particles, or a mixture thereof, of scaly boron nitride. The scaly boron nitride may be granulated. By using agglomerated particles of scaly boron nitride, the thermal conductivity of the resulting thermosetting resin composition can be further increased. The agglomerated particles may be sintered particles or non-sintered particles.
[0048] When a thermally conductive filler is used, the amount of the filler is, for example, 40% by mass to 90% by mass, preferably 50% by mass to 80% by mass, based on the total solid content of the thermosetting resin composition. By using the thermally conductive filler in the amount within the above range, the thermal conductivity of the cured product can be improved while maintaining the handleability of the obtained resin composition. The thermally conductive filler may be surface-treated with a silane coupling agent.
[0049] (Silane coupling agent) The thermosetting resin composition of the present embodiment may contain a silane coupling agent. This can improve the compatibility of the thermally conductive filler in the thermosetting resin composition. The coupling agent may be added to the thermosetting resin composition, or may be used by treating the surface of the thermally conductive filler.
[0050] The amount of the silane coupling agent to be added is from 0.05% by mass to 3% by mass, and preferably from 0.1% by mass to 2% by mass, based on the mass of the thermally conductive filler.
[0051] (Other Ingredients) The thermosetting resin composition of the present embodiment may contain other components in addition to the above-mentioned components. Examples of the other components include an antioxidant and a leveling agent.
[0052] (Method for producing thermosetting resin composition) The thermosetting resin composition of the present embodiment can be prepared as a resin varnish (a varnish-like thermosetting resin composition) by dissolving, mixing, and stirring the above-mentioned components other than the thermally conductive filler in a solvent. This mixing can be performed using various mixers such as an ultrasonic dispersion type, a high-pressure collision dispersion type, a high-speed rotation dispersion type, a bead mill type, a high-speed shear dispersion type, and a rotation-revolution dispersion type.
[0053] The solvent is not particularly limited, but examples thereof include acetone, methyl isobutyl ketone, toluene, ethyl acetate, cyclohexane, heptane, cyclohexanone, tetrahydrofuran, dimethylformamide, dimethylacetamide, dimethylsulfoxide, ethylene glycol, cellosolve-based solvents, carbitol-based solvents, anisole, and N-methylpyrrolidone.
[0054] When the thermosetting resin composition contains a thermally conductive filler, the thermally conductive filler is added to the resin varnish and kneaded using a three-roll mill or the like to obtain a B-stage filler-containing thermosetting resin composition. By adding the filler during kneading, it is possible to disperse the inorganic filler more uniformly in the thermosetting resin, but this is not limited thereto. The thermally conductive filler may be added during kneading, or may be added during mixing of the resin varnish. After kneading, the mixture may be cooled and solidified, and the kneaded product may be processed into a granular, tablet, or sheet shape.
[0055] [Phenoxy resin] The phenoxy resin according to the second embodiment of the present invention has a structure represented by formula (3).
[0056] [ka]
[0057] In formula (3), n is a number representing a repeating unit and represents an integer of 2 to 50, preferably an integer of 5 to 40, more preferably an integer of 6 to 30, and further more preferably an integer of 8 to 20. X is a divalent group having a mesogenic skeleton. Y is a divalent group represented by formula (1-3).
[0058] [ka]
[0059] In formula (1-3), R 11 may be the same or different and each independently represent a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms, preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and more preferably a hydrogen atom or an alkyl group having 1 carbon atom (a methyl group). R 12 may be the same or different and each independently represent a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms, preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and more preferably a hydrogen atom or an alkyl group having 1 carbon atom (a methyl group). * indicates the linking position. Particularly preferably, R 11 and R 12 are all hydrogen atoms.
[0060] The divalent group represented by "Y" in formula (3) is particularly preferably a group represented by formula (1-4). The group represented by formula (1-4) has high planarity, and therefore the phenoxy resin represented by formula (3) containing this group has high rigidity and, as a result, high thermal conductivity.
[0061] [ka]
[0062] In formula (1-4), R 11 and R 12 has the same meaning as in the above formula (1-3), and * represents the linking position.
[0063] In the phenoxy resin represented by the above formula (3), X in the formula (3) is a divalent group having a mesogenic skeleton. The phenoxy resin used in the thermosetting resin composition of this embodiment contains the structural unit (X) having a mesogenic skeleton, and thus the cured product thereof has high thermal conductivity and high heat resistance.
[0064] Examples of the mesogenic skeleton of the X group in formula (3) include a biphenyl skeleton, a naphthalene skeleton, a phenylbenzoate skeleton, an azobenzene skeleton, a stilbene skeleton, a cyclohexylbenzene skeleton, and derivatives thereof. Since the X group has the above-mentioned mesogenic skeleton, the phenoxy resin can have high thermal conductivity.
[0065] In one embodiment, at least one of the X groups in formula (3) is a group represented by formula (2). By including a structure having a mesogenic skeleton represented by formula (2), the phenoxy resin has high thermal conductivity and excellent heat resistance, and therefore the thermosetting resin of this embodiment containing the phenoxy resin can have high thermal conductivity.
[0066] [ka]
[0067] In formula (2), R 1 ~R 8 each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms, and * represents the linking position.
[0068] In one embodiment, the group represented by formula (2) is preferably a group in which R1, R4, R5, and R8 are alkyl groups having 1 to 4 carbon atoms, and R2, R3, R6, and R7 are hydrogen atoms. Among them, a group in which R1, R4, R5, and R8 are alkyl groups having 1 carbon atom, and R2, R3, R6, and R7 are hydrogen atoms in formula (2) (referred to as a "tetramethylbiphenyl group") is preferred because the phenoxy resin containing it can achieve a good balance between thermal conductivity and heat resistance.
[0069] In one embodiment, the group represented by formula (2) may be a group in which R1, R4, R5, and R8 are alkyl groups having one carbon atom, and R2, R3, R6, and R7 are hydrogen atoms (referred to as a "biphenyl group"). By including such a group, the phenoxy resin has excellent thermal conductivity and heat resistance.
[0070] In one embodiment, the phenoxy resin represented by formula (3) preferably contains a tetramethylbiphenyl group and a biphenyl group as the X group. A phenoxy resin containing a combination of these groups can have a good balance between thermal conductivity and heat resistance.
[0071] The phenoxy resin represented by formula (3) contains a divalent group represented by the above formula (1-3) as the Y group. The group represented by formula (1-3) has high planarity and high rigidity. Therefore, the phenoxy resin containing such a group has high thermal conductivity, and as a result, the cured product obtained from the thermosetting resin composition containing it has high thermal conductivity.
[0072] The weight average molecular weight (Mw) of the phenoxy resin represented by formula (3) is, for example, 2,000 to 10,000, preferably 2,500 to 8,000, more preferably 3,000 to 7,000, and even more preferably 3,500 to 6,500. Mw is a value measured by gel permeation chromatography and converted using a standard polystyrene calibration curve. By setting Mw in the above range, the thermal conductivity of the phenoxy resin can be further improved.
[0073] In this embodiment, the weight average molecular weight (Mw) of the phenoxy resin represented by formula (3) can be measured by obtaining a molecular weight distribution curve using GPC (Gel Permeation Chromatography). The weight average molecular weight (Mw), number average molecular weight (Mn), and polydispersity (PDI: Mw / Mn) of the phenoxy resin are calculated using polystyrene-equivalent values obtained from a calibration curve of standard polystyrene (PS) obtained by GPC measurement.
[0074] The measurement conditions for GPC are, for example, as follows. Tosoh Corporation gel permeation chromatography device HLC-8320GPC Column: TSK-GEL GMH, G2000H, SuperHM-M manufactured by Tosoh Corporation Detector: UV detector for liquid chromatography Measurement temperature: 40℃ Solvent: THF Sample concentration: 2.0 mg / ml
[0075] The polydispersity (Mw / Mn) of the phenoxy resin represented by formula (3) is, for example, 1.00 to 7.00, preferably 2.00 to 6.00, and more preferably 3.50 to 5.50. By setting the polydispersity within the above range, the thermal conductivity and flowability of the phenoxy resin can be further improved.
[0076] The phenoxy resin represented by formula (3) may contain a low molecular weight phenoxy resin having a weight average molecular weight (Mw) of 1000 or less. When the phenoxy resin contains a low molecular weight phenoxy resin, the low molecular weight phenoxy resin is, for example, 5% or more and 60% or less, preferably 5% or more and 50% or less, as a ratio of the total area of components corresponding to a weight average molecular weight Mw of 1,000 or less to the total area 100% of the entire molecular weight distribution obtained by GPC measurement. The phenoxy resin containing the low molecular weight phenoxy resin in the above range has improved fluidity and excellent handleability. Therefore, for example, the processing stability is improved when the resin composition of the present embodiment is processed into the form of a sheet or film.
[0077] The epoxy equivalent of the phenoxy resin represented by formula (3) is, from the viewpoint of the effects of the present invention, for example, 300 to 6,000 g / eq, preferably 350 to 5,000 g / eq, and more preferably 400 to 4,500 g / eq.
[0078] The phenoxy resin represented by formula (3) has the above-mentioned structure, and thus the cured product has high thermal conductivity. The thermal conductivity of the cured product of the phenoxy resin is, for example, 0.30 W / (m·K) or more. Since the phenoxy resin itself has high thermal conductivity, the cured product of the resin composition containing the phenoxy resin also has high thermal conductivity, and therefore can be suitably used for applications such as heat dissipation members.
[0079] (Production of phenoxy resin) The phenoxy resin represented by formula (3) used in this embodiment can be synthesized by reacting a bifunctional epoxy compound represented by formula (d-EP) with a dihydroxy compound represented by formula (1-1). The bifunctional epoxy compound represented by formula (d-EP) is the same as the bifunctional epoxy compound represented by formula (d-EP) in the first embodiment. The dihydroxy compound represented by formula (1-1) is the same as the dihydroxy compound represented by formula (1-1) in the first embodiment.
[0080] [ka]
[0081] [ka]
[0082] The above reaction can be carried out in the absence of a solvent or in the presence of a reaction solvent using a reaction catalyst.
[0083] Suitable reaction solvents include aprotic organic solvents such as methyl ethyl ketone, dioxane, tetrahydrofuran, acetophenone, N-methylpyrrolidone, dimethyl sulfoxide, N,N-dimethylacetamide, sulfolane, propylene glycol monomethyl ether, cyclohexanone, etc. The use of a reaction solvent can reduce the initial viscosity and improve the reactivity of the raw material monomers.
[0084] As the reaction catalyst, a conventionally known polymerization catalyst can be used, and alkali metal hydroxides, tertiary amine compounds, quaternary ammonium compounds, tertiary phosphine compounds, quaternary phosphonium compounds, and imidazole compounds are preferably used.
[0085] Specifically, a bifunctional epoxy compound represented by formula (d-EP), a dihydroxy compound represented by formula (1-1), a reaction catalyst, and optionally a reaction solvent are added and melt-mixed under stirring. The heating temperature during melt-mixing is about 90 to 150°C, the mixing time is about 30 minutes to 2 hours, and the reaction pressure is normal pressure. After melt-mixing, the mixed solution is heated and a polymerization reaction is carried out at a predetermined reaction temperature under reduced pressure or normal pressure. The reaction temperature is about 140 to 180°C, the reaction time is about 2 hours to 10 hours, and the reaction pressure is about 1 to 760 Torr.
[0086] After the reaction is completed, the phenoxy resin can be obtained as a resin dissolved in a suitable solvent by performing solvent replacement, etc. In addition, the phenoxy resin obtained by the solvent reaction can be obtained as a solid resin that does not contain the solvent by performing a solvent removal treatment using an evaporator, etc.
[0087] In the above synthesis method, a phenoxy resin having a desired weight average molecular weight can be obtained by appropriately selecting reaction conditions such as the amounts of starting materials used, reaction temperature, reaction time, etc. to adjust the degree of polymerization.
[0088] [Composite resin composition] The composite resin composition according to the third embodiment of the present invention comprises: An epoxy resin (A); A thermosetting resin (excluding the epoxy resin) (B); A phenoxy resin (C) represented by formula (3), and a thermally conductive filler (D). Here, the phenoxy resin (C) represented by formula (3) is the phenoxy resin according to the second embodiment.
[0089] [ka]
[0090] In formula (3), n is a number representing a repeating unit and represents an integer of 2 to 50; X is a divalent group having a mesogenic skeleton, Y is a divalent group represented by formula (1-3).
[0091] [ka]
[0092] In formula (1-3), R 11 may be the same or different and each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms, R 12 may be the same or different and each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms, * indicates the linking position.
[0093] Since the composite resin composition of the present embodiment has the above composition, it has high thermal conductivity and can be suitably used, for example, as a thermally conductive sheet for electronic devices. The components used in the composite resin composition of the present embodiment will be described below.
[0094] (Epoxy resin (A)) The composite resin composition of the present embodiment includes an epoxy resin (A). Examples of the epoxy resin (A) include glycidyl ethers of bisphenol A type, F type, S type, AD type, etc., hydrogenated bisphenol A type glycidyl ether, phenol novolac type glycidyl ether, cresol novolac type glycidyl ether, bisphenol A type novolac type glycidyl ether, naphthalene type glycidyl ether, biphenol type glycidyl ether, dihydroxypentadiene type glycidyl ether, triphenylmethane type epoxy resin, phenol novolac type epoxy resin, cresol novolac type epoxy resin, and hydroquinone type glycidyl ether, and at least one of them can be used. From the viewpoint of the effects of the present invention, the epoxy resin (A) preferably contains at least one selected from naphthalene-type glycidyl ethers, biphenol-type glycidyl ethers, dihydroxypentadiene-type glycidyl ethers, and hydroquinone-type glycidyl ethers.
[0095] The epoxy resin (A) may preferably contain an epoxy resin containing a mesogenic skeleton, which can further enhance the thermal conductivity (heat dissipation) of the cured product of the resin composition. It is believed that when epoxy resins containing a mesogenic skeleton are cured, a higher-order structure (liquid crystal phase or crystalline phase) is formed by the mesogenic skeleton. It is believed that the thermal conductivity (heat dissipation) is further increased by the transfer of heat through the higher-order structure. The presence of the higher-order structure in the cured product can be confirmed by observation with a polarizing microscope.
[0096] The mesogenic skeleton may be any skeleton that facilitates liquid crystallinity or crystallinity through intermolecular interactions. The mesogenic skeleton preferably includes a conjugated structure. Specific examples of the mesogenic skeleton include a biphenyl skeleton, a phenylbenzoate skeleton, an azobenzene skeleton, a stilbene skeleton, a naphthalene skeleton, an anthracene skeleton, a chalcone skeleton, and a phenanthrene skeleton.
[0097] The epoxy resin (A) particularly preferably contains a condensed polycyclic aromatic hydrocarbon skeleton, and particularly preferably contains a naphthalene skeleton.
[0098] Here, for example, in the case of a biphenyl skeleton (-C6H4-C6H4-), the central carbon-carbon single bond of the structure may "rotate" due to thermal motion at high temperatures, resulting in a decrease in liquid crystallinity. Similarly, in the case of a phenylbenzoate skeleton (-C6H4-COO-C6H4-), the ester bond may rotate at high temperatures. However, in the case of a condensed polycyclic aromatic hydrocarbon skeleton such as a naphthalene skeleton, in principle, there is no decrease in liquid crystallinity due to such rotation. In other words, by including a condensed polycyclic aromatic hydrocarbon skeleton in an epoxy resin, the heat dissipation properties of the resulting resin cured product in a high-temperature environment can be further improved.
[0099] In addition, by adopting a naphthalene skeleton as the polycyclic aromatic hydrocarbon skeleton, the epoxy resin can be prevented from becoming too rigid while obtaining the above-mentioned merits. This is because the naphthalene skeleton is relatively small as a mesogen skeleton. The epoxy resin not becoming too rigid is preferable in terms of preventing cracks and the like caused by the stress during curing of the composite resin composition of the present embodiment being easily relaxed.
[0100] The epoxy resin (A) preferably contains a di- or higher-functional epoxy resin. In other words, it is preferable that one epoxy resin molecule contains two or more epoxy groups. The number of functional groups of the epoxy resin is preferably 2 to 6, and more preferably 2 to 4. From the viewpoint of the effects of the present invention, the epoxy resin (A) in this embodiment preferably contains at least one epoxy resin selected from the compounds represented by the following formula:
[0101] [ka]
[0102] The epoxy equivalent of the epoxy resin (A) is, for example, 100 to 200 g / eq, preferably 105 to 190 g / eq, and more preferably 110 to 180 g / eq. By using an epoxy resin having an appropriate epoxy equivalent, it is possible to control the curability and optimize the physical properties of the cured product.
[0103] In one embodiment, the epoxy resin (A) preferably further contains another epoxy resin that is liquid or semi-solid at room temperature (23° C.). Specifically, it is preferable that a part or all of the epoxy resin is liquid or semi-solid at 23° C. By using a liquid or semi-solid epoxy resin, it becomes easier to form a cured product in a desired shape.
[0104] In one embodiment, the epoxy resin (A) preferably contains a combination of an epoxy resin that is liquid at room temperature and an epoxy resin that is semi-solid or solid at room temperature, which improves the moldability of the resulting composite resin composition.
[0105] The epoxy resin (A) is, for example, 5% by mass to 40% by mass, preferably 7% by mass to 35% by mass, and more preferably 10% by mass to 30% by mass, based on the resin component (100% by mass) of the composite resin composition not including the thermally conductive particles (D). This ensures sufficient curability, and allows a cured resin product with excellent thermal conductivity and insulation to be obtained.
[0106] (Thermosetting resin (B)) The composite resin composition of the present embodiment contains a thermosetting resin (B). Here, the thermosetting resin (B) does not contain the above-mentioned epoxy resin (A). The thermosetting resin (B) may be a thermosetting compound containing a mesogenic structure (mesogenic skeleton) in the molecule, or a thermosetting compound not containing a mesogenic structure in the molecule.
[0107] Examples of the thermosetting resin (B) include cyanate resins, maleimide resins, phenol resins, benzoxazine resins, polyimide resins, unsaturated polyester resins, melamine resins, silicone resins, acrylic resins, and phenol derivatives and derivatives thereof, and at least one of these may be included.
[0108] In this embodiment, the thermosetting resin (B) preferably contains at least one selected from a cyanate resin, a maleimide resin, a phenol resin, and a benzoxazine resin, and more preferably contains a cyanate resin. As these thermosetting resins, any monomer, oligomer, or polymer having two or more reactive functional groups in one molecule can be used, and there are no particular limitations on the molecular weight or molecular structure.
[0109] <Cyanate resin> As the cyanate resin, known ones can be used within the scope of the effects of the present invention. The cyanate resin can include one or more selected from, for example, novolac type cyanate resin; bisphenol type cyanate resin such as bisphenol A type cyanate resin, bisphenol E type cyanate resin, tetramethyl bisphenol F type cyanate resin; naphthol aralkyl type cyanate resin obtained by reacting naphthol aralkyl type phenol resin with cyanogen halide; dicyclopentadiene type cyanate resin; and biphenylene skeleton-containing phenol aralkyl type cyanate resin. Among these, from the viewpoint of the effects of the present invention, it is more preferable to include at least one of novolac type cyanate resin and naphthol aralkyl type cyanate resin, and it is particularly preferable to include novolac type cyanate resin.
[0110] As the novolac type cyanate resin, for example, one represented by the following general formula (I) can be used.
[0111] [ka]
[0112] The average repeating unit n of the novolac cyanate resin represented by the general formula (I) is any integer. The average repeating unit n is not particularly limited, but is preferably 1 or more, more preferably 2 or more. When the average repeating unit n is equal to or more than the above lower limit, the heat resistance of the novolac cyanate resin is improved, and the elimination and volatilization of low molecular weight compounds during heating can be further suppressed. In addition, the average repeating unit n is not particularly limited, but is preferably 10 or less, more preferably 7 or less. When n is equal to or less than the above upper limit, the melt viscosity can be suppressed from increasing, and the moldability of the composite resin composition can be improved. Therefore, the production efficiency is improved when the composite resin composition is molded into a sheet-like product.
[0113] As the cyanate resin, naphthol aralkyl type cyanate resin represented by the following general formula (II) is also preferably used. The naphthol aralkyl type cyanate resin represented by the following general formula (II) is obtained by condensing a naphthol aralkyl type phenol resin obtained by reacting naphthols such as α-naphthol or β-naphthol with p-xylylene glycol, α,α'-dimethoxy-p-xylene, 1,4-di(2-hydroxy-2-propyl)benzene, etc., with a cyanogen halide. The repeating unit n in the general formula (II) is preferably an integer of 10 or less. When the repeating unit n is 10 or less, a more uniform resin sheet can be obtained. In addition, intramolecular polymerization is less likely to occur during synthesis, and separation during washing with water is improved, which tends to prevent a decrease in yield.
[0114] [ka]
[0115] In the above general formula (II), R each independently represents a hydrogen atom or a methyl group, and n represents an integer of 1 or more and 10 or less.
[0116] When a cyanate resin is used, the blending amount thereof is, for example, 10% by mass to 70% by mass, preferably 15% by mass to 60% by mass, and more preferably 20% by mass to 50% by mass, based on the resin component (100% by mass) of the composite resin composition not including the thermally conductive particles (D). This ensures sufficient curability, and allows a resin sheet with even higher thermal conductivity and insulation to be obtained.
[0117] <Maleimide resin> The maleimide resin is preferably, for example, a maleimide resin having at least two maleimide groups in the molecule.
[0118] Examples of maleimide resins having at least two maleimide groups in the molecule include resins having two maleimide groups in the molecule, such as 4,4'-diphenylmethane bismaleimide, m-phenylene bismaleimide, p-phenylene bismaleimide, 2,2-bis[4-(4-maleimidophenoxy)phenyl]propane, bis-(3-ethyl-5-methyl-4-maleimidophenyl)methane, 4-methyl-1,3-phenylene bismaleimide, N,N'-ethylene dimaleimide, N,N'-hexamethylene dimaleimide, bis(4-maleimidophenyl)ether, bis(4-maleimidophenyl)sulfone, 3,3-dimethyl-5,5-diethyl-4,4-diphenylmethane bismaleimide, and bisphenol A diphenyl ether bismaleimide; and resins having three or more maleimide groups in the molecule, such as biphenyl aralkyl maleimide and polyphenylmethane maleimide.
[0119] <Phenol resin> Examples of the phenolic resin include novolac-type phenolic resins such as phenol novolac resin, cresol novolac resin, and bisphenol A novolac resin, and resol-type phenolic resin. One of these may be used alone, or two or more may be used in combination. Among the phenolic resins, it is preferable to use phenol novolac resin.
[0120] <Benzoxazine resin> Specific examples of the benzoxazine resin include o-cresol aniline type benzoxazine resin, m-cresol aniline type benzoxazine resin, p-cresol aniline type benzoxazine resin, phenol-aniline type benzoxazine resin, phenol-methylamine type benzoxazine resin, phenol-cyclohexylamine type benzoxazine resin, phenol-m-toluidine type benzoxazine resin, phenol-3,5-dimethylaniline type benzoxazine resin, bisphenol A-aniline type benzoxazine resin, bisphenol A-amine type benzoxazine resin, bisphenol F-aniline ... Examples of the benzoxazine resin include aniline type benzoxazine resin, bisphenol S-aniline type benzoxazine resin, dihydroxydiphenylsulfone-aniline type benzoxazine resin, dihydroxydiphenylether-aniline type benzoxazine resin, benzophenone type benzoxazine resin, biphenyl type benzoxazine resin, bisphenol AF-aniline type benzoxazine resin, bisphenol A-methylaniline type benzoxazine resin, phenol-diaminodiphenylmethane type benzoxazine resin, triphenylmethane type benzoxazine resin, and phenolphthalein type benzoxazine resin.
[0121] From the viewpoint of the effects of the present invention, the content of the thermosetting resin (B) is, for example, 0.1 mass % to 70 mass %, preferably 0.5 mass % to 65 mass %, and more preferably 1 mass % to 60 mass %, relative to the resin component (100 mass %) of the composite resin composition not including the thermally conductive particles (D).
[0122] (Phenoxy resin (C)) The composite resin composition of the present embodiment contains a phenoxy resin (C). As the phenoxy resin (C), the phenoxy resin according to the second embodiment described above can be used.
[0123] The blending amount of the phenoxy resin (C) is, for example, 2% by mass to 50% by mass, preferably 5% by mass to 40% by mass, and more preferably 10% by mass to 30% by mass, based on the resin component (100% by mass) of the composite resin composition not including the thermally conductive particles (D). By using the phenoxy resin (C) in the amount within the above range, the composite resin composition has good handleability and good sheet formability.
[0124] (Thermal conductive filler (D)) The composite resin composition of the present embodiment contains a thermally conductive filler (D). The thermally conductive filler (D) may, for example, contain a highly thermally conductive inorganic filler having a thermal conductivity of 20 W / m·K or more. The highly thermally conductive inorganic filler may, for example, contain at least one selected from silica, alumina, aluminum nitride, boron nitride, silicon nitride, silicon carbide, and magnesium oxide. These may be used alone or in combination of two or more.
[0125] The boron nitride may include monodisperse particles, agglomerated particles, or a mixture thereof, of scaly boron nitride. The scaly boron nitride may be granulated. By using agglomerated particles of scaly boron nitride, the thermal conductivity can be further increased. The agglomerated particles may be sintered particles or non-sintered particles.
[0126] The thermally conductive filler (D) may contain 60% by mass or more, preferably 65% by mass or more, and more preferably 70% by mass or more of the boron nitride. The upper limit is not particularly limited, but may be 100% by mass or less, preferably 95% by mass or less, and more preferably 90% by mass or less.
[0127] The content of the thermally conductive filler (D) is 100% by mass to 400% by mass, preferably 150% by mass to 350% by mass, and more preferably 200% by mass to 330% by mass, based on the resin component (100% by mass) of the composite resin composition. By making it equal to or more than the lower limit, the thermal conductivity can be improved. By making it equal to or less than the upper limit, the deterioration of processability can be suppressed.
[0128] (Cure accelerator) The composite resin composition of the present embodiment may contain a curing accelerator as necessary. The type and amount of the curing accelerator are not particularly limited, but an appropriate one can be selected from the viewpoints of reaction rate, reaction temperature, storage properties, and the like.
[0129] Examples of the curing accelerator include imidazoles, organic phosphorus compounds, tertiary amines, phenolic compounds, organic acids, etc. These may be used alone or in combination of two or more. Among these, from the viewpoint of improving heat resistance, it is preferable to use a nitrogen atom-containing compound such as imidazoles. Specific examples of the curing accelerator are the same as those in the thermosetting resin composition according to the first embodiment described above.
[0130] The content of the curing accelerator is 0.01 to 10 mass%, preferably 0.02 to 5 mass%, and more preferably 0.05 to 1.5 mass%, relative to 100 mass% in total of the epoxy resin (A) and the thermosetting resin (B).
[0131] (Silane coupling agent) The composite resin composition of the present embodiment may contain a silane coupling agent. This can improve the compatibility of the thermally conductive filler (D) in the composite resin composition. The coupling agent may be added to the composite resin composition, or may be used by treating the surface of the thermally conductive filler.
[0132] (Other additives) The composite resin composition of the present embodiment may contain other components in addition to the above-mentioned components. Examples of the other components include an antioxidant and a leveling agent.
[0133] [Method of manufacturing composite resin composition] The composite resin composition of the present embodiment can be produced, for example, by dissolving, mixing, and stirring the above-mentioned components other than the thermally conductive filler (D) in a solvent to prepare a resin varnish (a thermosetting resin composition in a varnish form), and then mixing the thermally conductive filler (D) into the resin varnish. The resin components can be mixed using various mixers such as those using an ultrasonic dispersion method, a high-pressure collision dispersion method, a high-speed rotation dispersion method, a bead mill method, a high-speed shear dispersion method, and a rotation-revolution dispersion method.
[0134] The solvent is not particularly limited, but examples thereof include acetone, methyl isobutyl ketone, toluene, ethyl acetate, cyclohexane, heptane, cyclohexanone, tetrahydrofuran, dimethylformamide, dimethylacetamide, dimethylsulfoxide, ethylene glycol, cellosolve-based solvents, carbitol-based solvents, anisole, and N-methylpyrrolidone.
[0135] The step of kneading the thermally conductive filler (D) into the resin varnish can be carried out using a three-roll mill or the like. By adding a thermally conductive filler to the resin varnish, it is possible to disperse the inorganic filler more uniformly in the resin, but this is not limited thereto. The thermally conductive filler may be added during kneading, or may be added when mixing the resin varnish. After kneading, the mixture may be cooled and solidified, and the kneaded product may be processed into a granular, tablet, or sheet shape. The composite resin composition is preferably provided in a B-stage state.
[0136] [Resin sheet] The resin sheet of the present embodiment is a sheet formed by molding the above-mentioned thermosetting resin composition or composite resin composition. The specific form of the resin sheet includes a carrier substrate and a resin layer formed on the carrier substrate and made of the thermosetting resin composition or composite resin composition of the present embodiment.
[0137] The resin sheet can be obtained by, for example, applying a varnish-like thermosetting resin composition or composite resin composition onto a carrier substrate to obtain a coating film (resin layer) and then subjecting the coating film to a solvent removal treatment. The solvent content in the resin sheet can be 10 mass% or less based on the entire thermosetting resin composition or composite resin composition. For example, the solvent removal treatment can be performed under conditions of 80°C to 200°C and 1 minute to 30 minutes.
[0138] The resin sheet (resin layer) of this embodiment is preferably provided in a B-stage state.
[0139] In this embodiment, the carrier substrate may be, for example, a polymer film or a metal foil. Examples of the polymer film include, but are not limited to, polyolefins such as polyethylene and polypropylene, polyesters such as polyethylene terephthalate and polybutylene terephthalate, polycarbonates, release papers such as silicone sheets, and thermoplastic resin sheets having heat resistance such as fluorine-based resins and polyimide resins. Examples of the metal foil include, but are not limited to, copper and / or copper-based alloys, aluminum and / or aluminum-based alloys, iron and / or iron-based alloys, silver and / or silver-based alloys, gold and gold-based alloys, zinc and zinc-based alloys, nickel and nickel-based alloys, and tin and tin-based alloys.
[0140] The resin substrate of the present embodiment has an insulating layer made of the cured product of the thermosetting resin composition or the composite resin composition. This resin substrate can be used as a material for a printed circuit board on which electronic components such as LEDs and power modules are mounted.
[0141] [Electronic equipment] The cured resin sheet is used as a thermally conductive sheet interposed between a heat generating body and a heat dissipating body.
[0142] Examples of the heating element include a semiconductor element, an LED element, a substrate on which a semiconductor element or an LED element is mounted, a Central Processing Unit (CPU), a power semiconductor, a lithium ion battery, and a fuel cell. Examples of the heat dissipator include a heat sink, a heat spreader, and a heat dissipation (cooling) fin. The heat dissipation insulating member may be partially composed of the thermosetting resin composition or composite resin composition of the present embodiment, and specific examples thereof include a heat dissipation sheet obtained by curing the above-mentioned thermosetting resin composition or composite resin composition, and a laminate in which the heat dissipation sheet and a substrate are laminated (for example, the metal base substrate 100 in FIG. 1). The substrate is not particularly limited as long as it is a heat dissipating metal substrate, and may be, for example, a copper substrate, a copper alloy substrate, an aluminum substrate, or an aluminum alloy substrate, with a copper substrate or an aluminum substrate being preferred, and a copper substrate being more preferred. By using a copper substrate or an aluminum substrate, the heat dissipation properties of the heat dissipation insulating member can be improved. The heat dissipating and insulating member is composed partly of the thermosetting resin composition or composite resin composition of this embodiment, and has a thermal conductivity of preferably 12 W / m·K or more, and more preferably 15 W / m·K or more. The heat dissipating insulation member and the heat sink may be formed on one side or both sides of the heating element. In addition, various base materials or layers may be provided between the heating element and the heat dissipating insulation member, or between the heat dissipating insulation member and the heat sink, as long as they do not affect the heat dissipation properties.
[0143] In this embodiment, the heat generating body, the heat dissipation and insulation member, and the heat dissipation body can be appropriately combined from those described above to obtain a laminated structure. The laminated structure can be used for various applications requiring heat dissipation and insulation, such as semiconductor devices, smartphones, LED bulbs and lights, power modules, lithium ion batteries, fuel cells, wireless base stations, and uninterruptible power supplies.
[0144] [Metal base board] A metal base substrate (heat dissipating resin member) 100 of this embodiment will be described with reference to FIG. FIG. 1 is a schematic cross-sectional view showing an example of the configuration of a metal base substrate 100. As shown in FIG.
[0145] As shown in Fig. 1, the metal base substrate 100 may include a metal substrate 101, an insulating layer 102 provided on the metal substrate 101, and a metal layer 103 provided on the insulating layer 102. The insulating layer 102 may be made of one material selected from the group consisting of a resin layer made of the above-mentioned thermosetting resin composition or composite resin composition, a cured product of the thermosetting resin composition or composite resin composition, and a laminate. Each of these resin layers and laminates may be made of a thermosetting resin composition (resin sheet) in a B-stage state before the circuit processing of the metal layer 103, and may be a cured product obtained by curing the resin composition after the circuit processing.
[0146] The metal layer 103 is provided on the insulating layer 102 and is subjected to circuit processing. Examples of metals constituting the metal layer 103 include one or more selected from copper, copper alloys, aluminum, aluminum alloys, nickel, iron, tin, and the like. Among these, the metal layer 103 is preferably a copper layer or an aluminum layer, and is particularly preferably a copper layer. By using copper or aluminum, the circuit processing property of the metal layer 103 can be improved. The metal layer 103 may be a metal foil available in a plate shape, or a metal foil available in a roll shape.
[0147] The lower limit of the thickness of the metal layer 103 is, for example, 0.01 mm or more, and preferably 0.035 mm or more, so long as it is applicable to applications requiring a high current. The upper limit of the thickness of the metal layer 103 is, for example, 10.0 mm or less, and preferably 5 mm or less. If the thickness is less than this value, the circuit processability can be improved, and the substrate as a whole can be made thinner.
[0148] The metal substrate 101 has a role of dissipating heat accumulated in the metal base substrate 100. The metal substrate 101 is not particularly limited as long as it is a heat dissipating metal substrate, but may be, for example, a copper substrate, a copper alloy substrate, an aluminum substrate, or an aluminum alloy substrate, with a copper substrate or an aluminum substrate being preferred, and a copper substrate being more preferred. By using a copper substrate or an aluminum substrate, the heat dissipation properties of the metal substrate 101 can be improved. The thickness of the metal substrate 101 can be appropriately set as long as it does not impair the object of the present invention.
[0149] The upper limit of the thickness of the metal substrate 101 is, for example, 20.0 mm or less, and preferably 5.0 mm or less. If the thickness is less than this value, the workability of the metal base substrate 100 in the contour processing, cutting processing, and the like can be improved.
[0150] The lower limit of the thickness of the metal substrate 101 is, for example, 0.01 mm or more, and preferably 0.6 mm or more. By using a metal substrate 101 having a thickness of this value or more, the heat dissipation properties of the metal base substrate 100 as a whole can be improved.
[0151] In this embodiment, the metal base substrate 100 can be used for various substrate applications, but because of its excellent thermal conductivity and heat resistance, it can be used as a printed circuit board that uses an LED or a power module.
[0152] The metal base substrate 100 may have a metal layer 103 that is circuitized by etching or the like into a pattern. In this metal base substrate 100, a solder resist (not shown) may be formed on the outermost layer, and connection electrodes may be exposed so that electronic components can be mounted thereon by exposure and development.
[0153] [Semiconductor Devices] The metal base substrate (heat dissipation and insulation member) 100 of the embodiment can be used in various applications requiring heat dissipation and insulation properties, for example, in electronic devices such as semiconductor devices. FIG. 2 is a schematic cross-sectional view showing an example of a semiconductor device using the metal base substrate 100. As shown in FIG. A semiconductor element 201 is mounted on a metal layer 103 of a metal base substrate 100 via an adhesive layer 202 (die attach material). The semiconductor element 201 is connected to a connection electrode portion formed on the metal base substrate 100 via a bonding wire 203, and is mounted on the metal base substrate 100. The semiconductor element 201 is then encapsulated on the metal base substrate 100 by an encapsulation resin layer 205 .
[0154] A heat sink 207 is provided on the metal substrate 101 side of the metal base substrate 100 via a thermally conductive layer 206 (thermal interface material (TIM)). The heat sink 207 is made of a material with excellent thermal conductivity, such as aluminum, iron, or copper.
[0155] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can also be adopted. EXAMPLES
[0156] EXAMPLES Hereinafter, the present invention will be described with reference to examples and comparative examples, but the present invention is not limited to these.
[0157] <Example A1, Comparative Example A1> (Preparation of Thermosetting Resin Composition Containing Dihydroxy Compound) A resin composition was obtained by mixing the components according to the composition shown in Table 1. Details of each component in Table 1 are as follows. The amount of each component in Table 1 is expressed in parts by mass.
[0158] (Dihydroxy Compounds) Dihydroxy compound 1: a compound represented by the following formula (1-5): [ka]
[0159] Multifunctional phenolic resin 1: Novolac type phenolic resin (Sumitomo Bakelite Co., Ltd., PR-55617)
[0160] (Difunctional epoxy compound) Bifunctional epoxy compound 1: a tetramethylbiphenyl type epoxy compound represented by the following formula (4) (manufactured by Mitsubishi Chemical Corporation, YX-4000H, solid at room temperature) [ka]
[0161] (Cure accelerator) Curing accelerator 1: 2-methyl-imidazole
[0162] (Measurement of physical properties of thermosetting resin composition) (Measurement of thermal conductivity) The resin composition of Example A1 or Comparative Example A1 was set in a mold coated with a release agent, and compression molding was performed at 180°C for 30 minutes to obtain a resin molded product of 10 mm square x 1 mm thick. Then, curing was performed in an oven at 180°C for 180 minutes to obtain a resin molded product 1 (a sample for measuring thermal conductivity). From the obtained resin molded body 1, a test piece of 10 mm square × 1 mm thickness was processed for thickness direction measurement. Next, the thermal diffusivity (α) [m 2The thermal diffusivity was measured at 25°C in an air atmosphere. The results are shown in Table 1. A higher thermal diffusivity value indicates higher thermal conductivity.
[0163] [Table 1]
[0164] <Example B1> (Preparation of phenoxy resin) The following method was used to prepare Phenoxy Resin 1. The raw material monomers used in the preparation of the phenoxy resin are shown below. Epoxy monomer 1: a tetramethylbiphenyl type epoxy compound represented by the following formula (4) (manufactured by Mitsubishi Chemical Corporation, YX-4000H, solid at room temperature) [ka]
[0165] Dihydroxy compound 1: a dihydroxy compound represented by the following formula (1-5): [ka]
[0166] (Preparation of phenoxy resin 1) Epoxy monomer 1 (75.8 parts by weight), dihydroxy compound 1 (24.2 parts by weight), triphenylphosphine (TPP) (0.04 parts by weight), and solvent (cyclohexanone) (2 parts by weight) were dropped into a reactor and melt-mixed at 110°C to 120°C for 1 hour. The equivalent ratio (Ep / Ph) of epoxy monomer 1 to phenol monomer 1 was 2.00. The obtained mixed liquid was heated to 170°C, and reacted while removing the solvent under reduced pressure at that temperature. It was confirmed by GPC that the molecular weight was the target, and the reaction was stopped to obtain phenoxy resin 1. The reaction was carried out for 5 hours. After the reaction, it was cooled to room temperature, and the obtained solid was pulverized and collected as a brown powdery solid. 95 parts by weight of phenoxy resin 1 represented by the following formula (3) was obtained. (In formula (3), the average value of the number of repeating units n is 3.4, X is a structural unit derived from epoxy monomer 1, Y is a structural unit derived from dihydroxy compound 1, the weight average molecular weight Mw measured by GPC is 2000, and the polydispersity (Mw / Mn) is 3.84.) [ka]
[0167] (Measurement of thermal conductivity of phenoxy resin) The phenoxy resin 1 (99 parts by mass) obtained above was mixed with 2-methyl-imidazole (1 part by mass) as a curing accelerator to obtain a resin composition. This resin composition was set in a mold coated with a release agent, and compression molded at 180°C for 30 minutes to obtain a resin molded product of 10 mm square and 1 mm thick. It was then cured in an oven at 180°C for 180 minutes to obtain a resin molded product 2 (a sample for measuring thermal conductivity). From the obtained resin molded body 2, a test piece was cut into a size of 10 mm square and 1 mm thick for measurement in the thickness direction. Next, the thermal diffusivity (α) [m 2 The thermal conductivity of the cured material of phenoxy resin 1 was 0.35 W / m K.
[0168] <Examples C1 to C2, Comparative Example C1> (Preparation of Composite Resin Composition) A resin composition was obtained by mixing the components according to the composition shown in Table 2. Details of each component in Table 2 are as follows. The amount of each component in Table 2 is expressed in parts by mass.
[0169] (Epoxy resin) Epoxy resin 1: Epoxy resin with the following structure (DIC, HP-4032D, liquid at room temperature) [ka]
[0170] Epoxy resin 2: Dicyclopentadiene type epoxy resin (DIC, EPICLON HP-7200L, solid at room temperature) Epoxy resin 3: Biphenyl type epoxy resin (Mitsubishi Chemical Corporation, YX-4000K, solid at room temperature)
[0171] (cyanate resin) Cyanate resin 1: Primaset "PT-30S" manufactured by Lonza
[0172] (Phenol Resin) Phenolic resin 1: Allyl group-containing phenolic novolac resin (manufactured by Meiwa Kasei Co., Ltd., product name "MEH-8000H")
[0173] (Phenoxy resin) Phenoxy resin 1: Phenoxy resin 1 obtained in Example B1 above Phenoxy resin 2: bisphenol A type phenoxy resin represented by the following formula (7) (no mesogen structure, manufactured by Mitsubishi Chemical Corporation, YP-55)
[0174] [ka]
[0175] (Thermal conductive filler) Thermally conductive filler 1: Agglomerated boron nitride (HP40, manufactured by Mizushima Ferroalloy Co., Ltd.)
[0176] (Measurement of physical properties of cured composite resin composition) The cured product of the composite resin composition obtained above was measured for the following physical properties.
[0177] (Thermal Conductivity) -Making resin molded products The obtained composite resin composition containing the thermally conductive filler was sandwiched between 0.018 mm copper foil and compression molded at 10 MPa, 180°C, and 90 minutes to obtain a resin molded product 3 (thermal conductivity measurement sample 3). A 10 mm square sample for thermal diffusivity measurement was cut out from the obtained molded product 3 and used for thermal diffusivity measurement.
[0178] Density (specific gravity) of resin molded body The density (specific gravity) measurement was performed in accordance with JIS K 6911 (general testing method for thermosetting plastics). Test pieces were cut out from the resin molded body 3 to a size of 2 cm in length and 2 cm in width. The unit of density (specific gravity) (ρ) is g / cm. 3 Let us assume that.
[0179] -Specific heat of resin molded body The specific heat (Cp) of the resin molded body 3 thus obtained was measured by a DSC method.
[0180] -Measurement of thermal conductivity of resin molded products From the obtained resin molded body 3, a test piece of 10 mm square was cut out for measurement in the thickness direction. Next, the thermal diffusion coefficient (α) in the thickness direction of the plate-shaped test piece was measured by a non-steady method using a Xe flash analyzer LFA467 HyperFlash manufactured by NETZSCH. The measurement was performed under the condition of air atmosphere and 25°C. The thermal conductivity of the resin molded body was calculated from the measured values of thermal diffusion coefficient (α), specific heat (Cp), and density (ρ) according to the following formula. The results are shown in Table 2. Thermal conductivity [W / m K]=α[m 2 / s]×Cp[J / kg K]×ρ[g / cm 3 ]
[0181] (moisture absorption rate) A test piece for measuring moisture absorption rate was prepared by cutting out a 5 cm square piece from the obtained resin molded body 3 and removing the copper foil by etching. The moisture absorption rate (%) was calculated from the change in weight before and after the treatment when the piece was left for 48 hours under the conditions of 30°C / 90% RH.
[0182] (solder heat resistance) The obtained resin molded body 3 was cut into 50 mm x 50 mm with a grinder saw, and then etched to prepare a sample with only half of the copper foil remaining, which was evaluated in accordance with JIS C 6481. The evaluation was performed by immersing the sample in a solder bath at 300°C for 5 minutes and then checking for the presence or absence of abnormalities in appearance. The evaluation criteria were as follows. <Evaluation criteria> A: No abnormalities B: Abnormal (bulges all over the area)
[0183] (Moisture absorption and solder heat resistance) The obtained resin molded body 3 was cut to 50 mm x 50 mm with a grinder saw, and then half of the surface was etched according to JIS C 6481 to prepare a sample. After leaving it for 2 days in an environment with a temperature of 40°C and a humidity of 90%, it was floated with the copper foil side down in a solder bath at 297°C, and the presence or absence of appearance abnormalities was checked after 1 minute. The evaluation criteria were as follows. The results are shown in Table 1. <Evaluation criteria> A: No abnormalities B: Blistering (bulging areas all over)
[0184] [Table 2] [Explanation of symbols]
[0185] 100 Metal base board 101 Metal Substrate 102 Insulating layer 103 Metal layer 200 Semiconductor device 201 Semiconductor elements 202 Adhesive layer 203 Bonding Wire 205 Sealing resin layer 206 Thermal Conduction Layer 207 Heatsink
Claims
1. A dihydroxy compound (A) represented by formula (1-1), A bifunctional epoxy compound (B) having two epoxy groups, represented by the formula (d-EP), A thermosetting resin composition comprising: 【Chemistry 1】 In formula (1-1), R 11 may be the same or different and each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms; R 12 may be the same or different and each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms; 【Chemistry 2】 In formula (d-EP), X represents a divalent group having a mesogenic skeleton. Thermosetting resin composition.
2. The thermosetting resin composition according to claim 1, The dihydroxy compound (A) has a structure represented by formula (1-2): 【Chemistry 3】 In formula (1-2), R 11 and R 12 is the same as that in the above formula (1-1), a thermosetting resin composition.
3. The thermosetting resin composition according to claim 1, In the formula (d-EP), X contains a divalent group represented by formula (2). 【Chemistry 4】 In formula (2), R 1 ~R 8 each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms, and * represents a linking position.
4. The thermosetting resin composition according to claim 3, In the group represented by formula (2), R 1 , R 4 , R 5 , and R 8 is an alkyl group having 1 to 4 carbon atoms, R 2 , R 3 , R 6 , and R 7 is a hydrogen atom.
5. The thermosetting resin composition according to claim 3, In the group represented by formula (2), R 1 , R 4 , R 5 , and R 8 is a methyl group, R 2 , R 3 , R 6 , and R 7 is a hydrogen atom.
6. The thermosetting resin composition according to claim 3, In the group represented by formula (2), R 1 ~R 8 are all hydrogen atoms.
7. The thermosetting resin composition according to claim 1, The thermosetting resin composition further comprises a curing accelerator.
8. The thermosetting resin composition according to claim 1, The thermosetting resin composition further comprises a thermally conductive filler.
9. A resin sheet comprising the thermosetting resin composition according to claim 1.
10. A heat generating member; A heat dissipation member; a thermally conductive sheet provided between the heat generating component and the heat dissipating component, An electronic device, wherein the thermally conductive sheet is made of a cured product of the resin sheet according to claim 9.
11. A metal substrate; A thermally conductive sheet; A metal base substrate comprising, in this order, The thermally conductive sheet is a metal base substrate comprising a cured product of the resin sheet according to claim 9.
12. An electronic device comprising the metal base substrate according to claim 11.
13. A phenoxy resin having a structure represented by formula (3): 【Chemistry 5】 In formula (3), n is a number representing a repeating unit and is an integer of 2 to 50; X is a divalent group having a mesogenic skeleton, Y is a divalent group represented by formula (1-3), 【Chemistry 6】 In formula (1-3), R 11 may be the same or different and each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms; R 12 may be the same or different and each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms; * indicates the linking position. Phenoxy resin.
14. The phenoxy resin according to claim 13, In the formula (3), Y is a divalent group represented by the formula (1-4), 【Chemistry 7】 In formula (1-4), R 11 and R 12 is defined as the same as in the above formula (1-3), and * represents a linking position. A phenoxy resin.
15. The phenoxy resin according to claim 13, In the formula (d-EP), X contains a divalent group represented by formula (2). 【Chemistry 8】 In formula (2), R 1 ~R 8 each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms, and * represents a linking position; phenoxy resin.
16. 16. The phenoxy resin according to claim 15, In the group represented by formula (2), R 1 , R 4 , R 5 , and R 8 is an alkyl group having 1 to 4 carbon atoms, R 2 , R 3 , R 6 , and R 7 is a hydrogen atom.
17. 16. The phenoxy resin according to claim 15, In the group represented by formula (2), R 1 , R 4 , R 5 , and R 8 is a methyl group, R 2 , R 3 , R 6 , and R 7 is a hydrogen atom, phenoxy resin.
18. 16. The phenoxy resin according to claim 15, In the group represented by formula (2), R 1 ~R 8 Phenoxy resin, in which all of the atoms are hydrogen.
19. Epoxy resin, A thermosetting resin (excluding the epoxy resin), A phenoxy resin represented by formula (3), A composite resin composition comprising: 【Chemistry 9】 In formula (3), n is a number representing a repeating unit and is an integer of 2 to 50; X is a divalent group having a mesogenic skeleton, Y is a divalent group represented by formula (1-3), 【Chemistry 10】 In formula (1-3), R 11 may be the same or different and each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms; R 12 may be the same or different and each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms; * indicates the linking position. Composite resin composition.
20. The composite resin composition according to claim 19, In the formula (3), Y is a divalent group represented by the formula (1-4), 【Chemistry 11】 In formula (1-4), R 11 and R 12 is defined as the same as in the above formula (1-3), and * represents a linking position.
21. The composite resin composition according to claim 19, In the formula (3), X contains a divalent group represented by the formula (2), 【Chemistry 12】 In formula (2), R 1 ~R 8 each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms, and * represents a linking position.
22. The composite resin composition according to claim 21, In the group represented by formula (2), R 1 , R 4 , R 5 , and R 8 is an alkyl group having 1 to 4 carbon atoms, R 2 , R 3 , R 6 , and R 7 is a hydrogen atom.
23. The composite resin composition according to claim 21, In the group represented by formula (2), R 1 , R 4 , R 5 , and R 8 is a methyl group, R 2 , R 3 , R 6 , and R 7 is a hydrogen atom.
24. The composite resin composition according to claim 21, In the group represented by formula (2), R 1 ~R 8 and all of the above are hydrogen atoms.
25. The composite resin composition according to claim 19, The phenoxy resin has a weight average molecular weight of 2,000 or more and 10,000 or less.
26. The composite resin composition according to claim 19, The composite resin composition, wherein the thermosetting resin includes at least one selected from a cyanate resin, a maleimide resin, a phenolic resin, and a benzoxazine resin.
27. 20. The composite resin composition of claim 19, wherein the thermally conductive filler comprises boron nitride.
28. 20. The composite resin composition of claim 19, further comprising a curing accelerator.
29. A resin sheet comprising the composite resin composition according to any one of claims 19 to 28.
30. A heat generating member; A heat dissipation member; a thermally conductive sheet provided between the heat generating component and the heat dissipating component, 30. An electronic device, wherein the thermally conductive sheet is made of a cured product of the resin sheet according to claim 29.
31. A metal substrate; A thermally conductive sheet; A metal base substrate comprising, in this order, 30. A metal base substrate, wherein the thermally conductive sheet is made of a cured product of the resin sheet according to claim 29.
32. 32. An electronic device comprising the metal base substrate of claim 31.
Citation Information
Patent Citations
Low-viscosity waterborne epoxy resin and preparation method thereof
CN112646123A
High-stability water-borne epoxy resin and preparation method thereof
CN112759741A
Toughened type water-borne epoxy resin and preparation method thereof
CN112759742A
Toughened flame-retardant water-borne epoxy resin and preparation method thereof
CN112794989A
Polymerizable naphthalene compound
JP2012240945A