Stator manufacturing method for rotary electric machines

The method of pre-applying and sequentially curing liquid resin on stator coils addresses wettability issues and uneven thickness in dip coating, ensuring uniform insulation with reduced steps and cycle time.

JP2024142694AInactive Publication Date: 2024-10-11AISIN CORP

Patent Information

Application Number
JP2023054945
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The dip coating method for applying liquid resin material to stator coils in rotating electric machines often results in locally thin coatings due to wettability issues, and repeated dipping processes can lead to voids and uneven thickness, necessitating multiple steps that increase cycle time.

Method used

A method involving a pre-applying step with ultraviolet curing followed by a single dipping step, where the liquid resin material is applied to critical areas before immersion, ensuring adequate thickness and uniform coverage through sequential curing and dipping processes.

Benefits of technology

This approach reduces the need for multiple dipping steps, ensures consistent insulation thickness, and minimizes voids and uneven thickness, thereby improving efficiency and reducing cycle time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142694000001_ABST
    Figure 2024142694000001_ABST
Patent Text Reader

Abstract

To secure a required thickness of an insulation coating at a position, which is easy to be thin locally, while reducing or eliminating the need to execute an immersion step a plurality of times.SOLUTION: A stator manufacturing method for rotary electric machines includes: a mounting step of forming a workpiece by mounting a plurality of coil pieces which form a stator coil in a stator core; a joining step of joining tip ends of one coil piece and another coil piece with each other at one end side of the workpiece in an axial direction after the mounting step; a depositing step of depositing a first liquid-state resin material onto a deposition target portion in the joined tip ends after the joining step; an immersion step of immersing, in a tub of a second liquid-state resin material, an immersion target portion including the deposition target portion in the workpiece after the deposition step or before the deposition step; and a curing step of curing the first liquid-state resin material and the second liquid-state resin material in the immersion target portion.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for manufacturing a stator for a rotating electric machine. [Background technology]

[0002] A method for manufacturing a stator for a rotating electric machine is known, which comprises preparing a workpiece for a rotating electric machine in which a plurality of coil pieces that form a stator coil are attached to a stator core, joining the tips of the plurality of coil pieces together at one axial end of the workpiece, applying a liquid resin material to a target portion including the joint (exposed conductor portion), and then hardening the liquid resin material to cover the joint with an insulating coating of the resin material. In this type of manufacturing method, a technique has been proposed in which the liquid resin material applied to the target portion is irradiated with ultraviolet light to harden the irradiated portion, and then the liquid resin material is heated to completely harden it. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2016-124878 A Summary of the Invention [Problem to be solved by the invention]

[0004] In the dip coating method, in which the target part is applied with a liquid resin material by immersing the target part in a tank of the liquid resin material, the liquid resin material can be applied efficiently to the entire target part, but there is a problem that the insulating coating of a part of the target part tends to become locally thin due to the influence of wettability, etc. In contrast, if the immersion process by the dip coating method is performed multiple times on one workpiece, this problem is solved, but a different new problem arises. That is, problems such as the occurrence of voids between the insulating coating part applied by the first dip coating and the insulating coating part applied by the second dip coating and the occurrence of locally thick parts of the insulating coating arise.

[0005] Therefore, in one aspect, the present disclosure aims to ensure the necessary thickness of the insulating coating in areas that tend to become locally thin while reducing or eliminating the need to perform the immersion process multiple times. [Means for solving the problem]

[0006] In one aspect, a mounting step of mounting a plurality of coil pieces forming a stator coil on a stator core to form a workpiece; a joining step of joining a tip end portion of one of the coil pieces and another of the coil pieces to each other at one axial end side of the workpiece after the mounting step; an attachment step of attaching a first liquid resin material to an attachment target site of the joined tip portion after the joining step; After the adhesion step or before the adhesion step, an immersion step of immersing an impregnation target portion including the adhesion target portion of the workpiece in a tank of a second liquid resin material; and a curing step of curing the first liquid resin material and the second liquid resin material in the impregnation target portion. Effect of the Invention

[0007] In one aspect, the present disclosure makes it possible to ensure the required thickness of the insulating coating in areas that tend to become locally thin, while reducing or eliminating the need to perform multiple dipping steps. [Brief description of the drawings]

[0008] [Figure 1] 4 is a schematic flowchart showing an example of a method for manufacturing a stator for a rotating electric machine. [Diagram 2] FIG. 2 is a diagram showing a schematic view of an entire workpiece for forming a stator for a rotating electric machine; [Diagram 3] 4 is a cross-sectional view taken along the axial direction of the workpiece in a state in which coil pieces are assembled to a stator core. FIG. [Figure 4] FIG. [Diagram 5]FIG. 2 is a schematic cross-sectional view of a coil piece. [Figure 6] FIG. 3 is an explanatory diagram of a joint, corresponding to an enlarged view of part Q1 in FIG. 2. [Figure 6A] 4 is an explanatory diagram of another type of joint, corresponding to an enlarged view of part Q1 in FIG. 2. [Figure 6B] 4 is an explanatory diagram of another type of joint, corresponding to an enlarged view of part Q1 in FIG. 2. [Figure 6C] 4 is an explanatory diagram of another type of joint, corresponding to an enlarged view of part Q1 in FIG. 2. [Figure 7] FIG. 1 is a perspective view showing a workpiece during a pre-attaching process from above, as an explanatory diagram of an overview of the pre-attaching process. [Figure 7A] FIG. 11 is an explanatory diagram of a dripping process in the pre-attaching process, and is a cross-sectional view showing a part of a workpiece during the dripping process. [Figure 8] FIG. 13 is a perspective view showing the workpiece during the pre-attaching process from above in an upright position. [Figure 8A] FIG. 11 is an explanatory diagram of a dripping process in the pre-attaching process, and is a cross-sectional view showing a part of a workpiece during the dripping process. [Figure 9] FIG. 11 is an explanatory diagram of a resin hardening step in the pre-attaching step, and is a cross-sectional view showing a part of the workpiece during the resin hardening step. [Figure 10] FIG. 13 is an explanatory diagram of a change in the circumferential range in the pre-attaching process, and is a diagram showing a schematic top view of the workpiece together with eight divided circumferential ranges. [Figure 11] 1 is a schematic side view of a workpiece before it is immersed in a tank of liquid resin material; FIG. [Figure 12] 1 is a schematic side view of a workpiece immersed in a tank of liquid resin material; FIG. [Figure 12A] FIG. 13 is an enlarged view of part Q8 in FIG. 12, which is a schematic enlarged view of a part of the workpiece to be impregnated (the joint and its surrounding area). [Figure 13] 13 is a schematic side view of the state of the workpiece being pulled further upward from the position during the liquid-draining rotation process. FIG. [Figure 14]13 is a schematic side view of a workpiece in a diagonally downward orientation undergoing a redeposition rotation process; FIG. [Figure 15] FIG. 2 is a schematic side view of a workpiece undergoing a resin hardening process; [Figure 16] FIG. 11 is a diagram showing a schematic side view of the state of the workpiece in a heating process. [Figure 17] 4A to 4C are explanatory diagrams of an insulating coating made of a liquid resin material produced by the production method according to the present embodiment. [Figure 18] 10A and 10B are explanatory diagrams of an insulating coating made of a liquid resin material produced by a comparative example production method. [Figure 19] FIG. 11 is an explanatory diagram of another example of a pre-attached target portion. [Figure 20] FIG. 2 is a cross-sectional photograph of an insulating coating formed by the manufacturing method according to this embodiment (a single dipping step). [Figure 21] FIG. 13 is a cross-sectional photograph of an insulating coating formed through two dipping steps in a comparative example (configuration not including a pre-attaching step). [Figure 22] FIG. 2 is a diagram showing an example of a cooling structure, and is a diagram showing a cross-sectional structure of a rotating electric machine. FIG. [Diagram 23] FIG. 13 is an explanatory diagram of a dripping step that may be performed following an upper surface resin curing step in the post-treatment step (step S220). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Each embodiment will be described in detail below with reference to the accompanying drawings. Note that the dimensional ratios in the drawings are merely examples and are not intended to be limiting, and shapes and the like in the drawings may be partially exaggerated for the sake of explanation.

[0010] The manufacturing method of a stator for a rotating electric machine described below can be applied to any stator for a rotating electric machine as long as the stator has a joint portion of the coil pieces at the coil end portion. In the following, as a suitable application example, a manufacturing method of a stator for a rotating electric machine that can function as a power source that generates a propulsive force for a vehicle will be described.

[0011] FIG. 1 is a schematic flow chart showing an example of a method for manufacturing a stator for a rotating electric machine. Note that FIG. 1 is a flow chart showing a schematic flow, and may include additional steps at any stage. FIGS. 2 to 6C are explanatory diagrams of a workpiece W. FIG. 2 is a diagram showing a schematic view of a workpiece W including a stator core 112 and a stator coil 114 for forming a stator 10 for a rotating electric machine. FIG. 3 is a cross-sectional view along the axial direction of the workpiece W in a state in which the coil pieces 52 are assembled to the stator core 112. FIG. 4 is a front view of one of the coil pieces 52 among the multiple coil pieces 52. FIG. 5 is a schematic cross-sectional view of the coil piece 52. FIG. 6 is an explanatory diagram of a joint 400, and FIGS. 6A to 6C are explanatory diagrams of the joint 400 and its variations, which are respectively explanatory diagrams of the Q1 part in FIG. 2. FIGS. 7 to 16 are explanatory diagrams of the present manufacturing method, and FIG. 7 is a perspective view showing the workpiece W during the pre-attaching step from above as an explanatory diagram of the outline of the pre-attaching step. FIG. 7A is an explanatory diagram of the dripping process in the pre-attaching process, and is a cross-sectional view showing a part of the work W during the dripping process. FIG. 8 is a perspective view showing the work W during the pre-attaching process in the case of an upright posture from above. FIG. 8A is an explanatory diagram of the dripping process in the pre-attaching process, and is a cross-sectional view showing a part of the work W during the dripping process. FIG. 9 is an explanatory diagram of the resin hardening process in the pre-attaching process, and is a cross-sectional view showing a part of the work W during the resin hardening process. Note that FIGS. 8A and 9 are cross-sectional views passing through the central axis I of the work W. Note that in FIGS. 8A and 9, for convenience of explanation, only the axial end of the coil end portion 114A of the stator coil 114 is illustrated without omission. FIG. 10 is an explanatory diagram of the change in the circumferential range in the pre-attaching process, and is a diagram showing the work W in a top view with the circumferential range divided into eight parts. FIG. 11 is a diagram showing the work W in a side view before being immersed in the tank 600 of the liquid resin material M0. FIG. 12 is a diagram showing a side view of the workpiece W immersed in a tank 600 of liquid resin material M0. FIG. 12A is an enlarged view of part Q8 in FIG. 12, and shows an enlarged schematic view of a part of the workpiece W to be impregnated (joint 400 and its surroundings). FIG. 13 is a diagram showing a side view of the workpiece W pulled up further upward from the position during the liquid-removal rotation process. FIG. 14 is a diagram showing a side view of the workpiece W in a diagonally downward orientation undergoing the reattachment rotation process. FIG. 15 is a diagram showing a side view of the workpiece W in a state in which a resin hardening process is being performed. FIG. 16 is a diagram showing a side view of the workpiece W in a heating process.

[0012] The Z direction is shown in Fig. 2 and other figures. The Z direction corresponds to the up-down direction, with the Z1 side and the Z2 side corresponding to the upper side and the lower side, respectively. The Y direction is shown in Fig. 3 and other figures. The Y direction corresponds to the radial direction, with the Y1 side corresponding to the radially outer side and the Y2 side corresponding to the radially inner side (the side closer to the central axis I of the stator core 112).

[0013] In the following description, unless otherwise specified, the axial direction refers to the direction in which the central axis I of stator core 112 (= the central axis of the workpiece W) extends, and the radial direction refers to the radial direction centered on the central axis I. Therefore, the radially outer side refers to the side away from the central axis I, and the radially inner side refers to the side closer to the central axis I. Additionally, the axially outer side refers to the side away from the axial center of stator core 112, and the axially inner side refers to the side closer to the axial center of stator core 112. Additionally, the circumferential direction corresponds to the direction of rotation around the central axis I.

[0014] This manufacturing method first includes a mounting step (step S200) of mounting a plurality of coil pieces 52 that form the stator coil 114 on the stator core 112 to form an assembly (hereinafter also referred to as a "workpiece W").

[0015] Here, the stator coil 114 includes a U-phase coil, a V-phase coil, and a W-phase coil (hereinafter, when U, V, and W are not distinguished, they are referred to as "phase coils"). The base end of each phase coil is connected to an input terminal (not shown), and the end of each phase coil is connected to the end of the other phase coil to form a neutral point. In other words, the stator coil 114 is star-connected. However, the connection mode of the stator coil 114 may be changed as appropriate depending on the required motor characteristics, etc. For example, the stator coil 114 may be delta-connected instead of star-connected.

[0016] Each phase coil of the stator coil 114 is formed by connecting a plurality of coil pieces 52. The coil pieces 52 are in the form of segment coils (segment conductors) obtained by dividing the phase coil into units that are easy to assemble (for example, units that can be inserted into two slots 23). As shown in FIG. 5, the coil pieces 52 are formed by covering a linear conductor (rectangular wire) 120 having a substantially rectangular cross section with an insulating film 130. Here, the linear conductor 120 is formed of copper, as an example. However, in a modified example, the linear conductor 120 may be formed of another conductive material such as iron. The cross-sectional shape of the linear conductor 120 may be other than rectangular.

[0017] In the example shown in Fig. 4, one coil piece 52 may be formed into a substantially U-shape having a pair of linear slot-accommodated portions 50 and a transition portion 54 connecting the pair of slot-accommodated portions 50. The transition portion 54 on the other axial side (upper side in Fig. 4) may be formed by forming in the circumferential direction from the state shown in Fig. 4. A joining tip portion 40 that is to be joined to a joining tip portion 40 of the transition portion 54 of another coil piece 52 is set at an end of the transition portion 54 on the other axial side (upper side in Fig. 4). The joining tip portion 40 is a portion from which the insulating film 130 has been removed (i.e., a portion from which the linear conductor 120 is exposed).

[0018] When the coil pieces 52 are assembled to the stator core 112, the pair of slot-receiving portions 50 are inserted into the slots 23 between the teeth 22 (see FIG. 3). In this case, the coil pieces 52 can be assembled, for example, in the axial direction.

[0019] 4 are inserted into each slot 23 in a radially aligned manner. Thus, a plurality of circumferentially extending transition portions 54 are aligned in the radial direction at both axial ends of the stator core 112. The transition portions 54 (and the joining tip portions 40 which are a part of the transition portions 54) form coil end portions 114A which are portions which protrude axially outward from the axial end faces of the stator core 112.

[0020] The coil pieces 52 may be wound around the stator core 112 in a lap winding manner. In the example shown in Fig. 4, the lower transition portion 54 may have an offset portion 521B that is offset from the other end by one layer in the radial direction. The upper transition portion 54 may also have a similar offset portion 521A (see Fig. 3).

[0021] 2 to 5 show the stator core 112 and the stator coil 114 having a specific structure, the structure of the stator core 112 and the stator coil 114 is arbitrary as long as the stator coil 114 has a joining tip portion 40. The winding method of the stator coil 114 is also arbitrary, and may be a winding method other than the lap winding type described above, such as a wave winding type.

[0022] Next, this manufacturing method includes a joining process (step S202) of joining the joining tips 40, which are the tips of one coil piece 52 and another coil piece 52, at one axial end side of the workpiece W. The joining tips 40 may be overlapped and the opposing sides may be joined. Any method may be used to join the joining tips 40, for example, welding. In this case, the welding may be achieved by any method such as laser welding or TIG welding. FIGS. 6A to 6C are schematic diagrams showing a joining portion 400 including a welded portion 401 (joint portion) formed on two joining tips 40 overlapped in the radial direction.

[0023] For example, when four or more coil pieces 52 are mounted in each slot 23 of the stator core 112 in a radially overlapping manner, the joining process may join multiple pairs in the radial direction, with two radially adjacent joining tip portions 40 (tip portions) being considered as one pair.

[0024] The joining range of the joining tip portions 40 and the posture of the joining tip portions 40 when joining (the posture when overlapping) are arbitrary. For example, as shown in FIG. 6, only the joining tip portions 40 may be overlapped in the radial direction in an oblique posture. In the example shown in FIG. 6, the joining tip portion 40 has an arc-shaped outer portion 402 that tapers toward the tip when viewed in the radial direction. In this case, the joining process may be realized by applying heat for welding (for example, heat by laser irradiation) to the radial abutment surfaces of the arc-shaped outer portions 402 of the joining tip portions 40 of the coil pieces 52. In this case, the axial size of the lead-side coil end portion 114A can be reduced. Alternatively, the joining tip parts 40 may be overlapped in the radial direction while standing upright in the up-down direction as shown in Fig. 6A, or overlapped in an X-shaped crossing manner as viewed in the radial direction as shown in Fig. 6B, or only the joining tip parts 40 among the parts extending in the circumferential direction may be overlapped in the radial direction as shown in Fig. 6C. Also, although not shown, the joining tip parts 40 may be overlapped in the axial direction while extending in the radial direction.

[0025] In the joining process, not only the coil pieces 52 are joined to each other, but also the coil pieces 52 may be joined to a bus bar or a terminal block (an output bus bar for connection to an inverter, not shown). For example, such a bus bar may include a bus bar forming the neutral point described above.

[0026] In this embodiment, as an example, the joint 400 is provided only on one axial side of the stator core 112. Hereinafter, for the sake of distinction, the side having the joint 400 among both axial sides of the stator core 112 (or both axial sides of the workpiece W) is also referred to as the lead side. Note that in a modified example, the joint 400 may be provided on both axial sides of the stator core 112. In the following description, a specific joint 400 among the several types of joints 400 described above may be illustrated and described with reference to Figures 6 to 6C and the like as appropriate, but the type of joint 400 to which this embodiment is applicable is arbitrary.

[0027] Next, in this manufacturing method, the workpiece W is set at the start position (workpiece carry-in position) for the pre-attaching process (step S204). At this time, the workpiece W may be set in a position in which the lead side is on the upper side (i.e., the joint portion 400 is on the upper side). Hereinafter, such a position in which the lead side is on the upper side is also referred to as the "upward position of the workpiece W". Also, the position in which the lead side is on the lower side is also referred to as the "downward position of the workpiece W".

[0028] Next, this manufacturing method includes a pre-application process (steps S206 to S216) in which liquid resin material M0 is applied to a pre-application target portion (an example of an application target portion), which is a specific portion of the workpiece W, and the liquid resin material M0 applied to the pre-application target portion is partially hardened.

[0029] In this embodiment, the liquid resin material M0 is preferably a resin material that has the property of being cured by heating and also by polymerization reaction when irradiated with ultraviolet light, so that the liquid resin material M0 can be cured by ultraviolet light irradiation in parallel with the dripping process described later.

[0030] The pre-attaching target portion of the workpiece W is set to a portion of the plurality of coil pieces 52 of the workpiece W. The pre-attaching target portion includes a portion where the thickness of the liquid resin material M0 is likely to become thin in a dipping process described later. The pre-attaching target portion also forms a part of a portion (impregnation target portion) that is immersed in a tank 600 of the liquid resin material M0 in a dipping process (step S218 described later) described later.

[0031] The pre-attaching process (steps S206 to S216) in this embodiment includes a dripping process (an example of an attachment process) in which the liquid resin material M0 is dripped and attached to the pre-attached portion of the workpiece W, and a resin hardening process (an example of an initial hardening process) in which the liquid resin material M0 in the pre-attached portion is hardened, and the time (period) in which the dripping process is performed on one workpiece W overlaps with the time (period) in which the resin hardening process is performed on the same workpiece W (step S210 described below). Note that overlap in this case includes both partial overlap and complete overlap.

[0032] Specifically, in the pre-attaching step, the present manufacturing method first includes a dripping step (step S206) of dripping the liquid resin material M0 onto a pre-attached portion of the workpiece W. The dripping step in step S206 is an initial step when starting to drip the liquid resin material M0 onto the workpiece W, and therefore does not have to be performed simultaneously with the resin curing step, unlike the step of step S210 described later. The dripping step may be realized in any manner.

[0033] In this embodiment, the pre-attachment target portion may be set in correspondence with the joint edge 122 of the joint tip portion 40. This is because the joint edge 122 has low wettability (wettability of the corner of the linear conductor 120), and therefore the thickness of the liquid resin material M0 applied in the immersion process (step S218) described later is likely to be thin.

[0034] The pre-attachment target area may be set to correspond to all of the joint edges 122 in the joining tip portion 40, but in this embodiment, it is set to correspond to a specific joint edge 122 among all of the joint edges 122 in the joining tip portion 40.

[0035] Specifically, in this embodiment, the specific joining tip portion 40 forms the joining portions 400 that are periodically arranged in the circumferential direction at the radially innermost or outermost positions. The pre-attachment target portion is set in correspondence with the joining portion edge 122 that faces the axially outer side and the radially inner side or the radially outer side of the specific joining tip portion 40.

[0036] More specifically, the specific joining tip portion 40 forming the joining portions 400 arranged periodically in the circumferential direction on the innermost side in the radial direction is also referred to as the "innermost specific joining tip portion 40". For the innermost specific joining tip portion 40, the pre-attachment target portion is set in correspondence with the joining edge 122 (hereinafter also referred to as the "innermost side joining edge 122") facing the axially outer side and the radially inner side of the innermost specific joining tip portion 40. In this case, the pre-attachment target portion may be a portion including the innermost side joining edge 122 or a side portion 440 in the vicinity thereof. The portion including the joining edge 122 includes a corner portion related to the joining edge 122, and the corner portion is composed of a portion facing the axially outer side and the side portion 440.

[0037] In addition, the specific joining tip portion 40 forming the joining portions 400 arranged periodically in the circumferential direction on the outermost side in the radial direction is also referred to as the "outermost specific joining tip portion 40". For the outermost specific joining tip portion 40, the pre-attachment target portion is set in correspondence with the joining edge 122 (hereinafter also referred to as the "outermost side joining edge 122") that faces the axially outer side and the radially outer side of the outermost specific joining tip portion 40. In this case, the pre-attachment target portion may be a portion including the outermost side joining edge 122 or a side portion 440 in the vicinity thereof. The portion including the joining edge 122 includes a corner portion related to the joining edge 122, and the corner portion is composed of a portion facing the axially outer side and the side portion 440.

[0038] In addition, among the joint edges 122 forming the joining tip portion 40, except for the innermost joint edge 122 and the outermost joint edge 122, the thickness of the liquid resin material M0 is likely to become relatively large in the immersion process described below due to the presence of other radially adjacent portions (portions of the coil pieces 52).

[0039] 7 shows a state in which the dripping process (step S206) is being performed on the workpiece W in an oblique posture. The manufacturing device for implementing the dripping process and the like may be, for example, an articulated robot having a hand for gripping the workpiece W, and a workpiece gripping unit 1000, which is a part of the manufacturing device, is shown in FIG. 7 and the like. In FIG. 7, an ultraviolet ray irradiation device 900 and a nozzle 920 are arranged for each of the pre-attachment target portion related to the joint edge 122 on the outermost diameter side and the pre-attachment target portion related to the joint edge 122 on the innermost diameter side. FIG. 7A is an enlarged view corresponding to part Q7 in FIG. 7.

[0040] In the example shown in FIG. 7A, the liquid resin material M0 is dripped from the nozzle 920 shown in FIG. 7 (see arrow R8). The nozzle 920 is connected to a supply source of the liquid resin material M0 (not shown). In the example shown in FIG. 7, two nozzles 920 are arranged above the respective pre-attached target portions in correspondence with each other. In this case, the upper nozzle 920 in FIG. 7 is associated with a portion including the outermost joint edge 122 as the pre-attached target portion (hereinafter, when distinguishing between them, it is also referred to as the "outer side pre-attached target portion"). The lower nozzle 920 in FIG. 7 is associated with the innermost joint edge 122 as the pre-attached target portion (hereinafter, when distinguishing between them, it is also referred to as the "inner side pre-attached target portion"). When the dripping process (step S206) is performed on the workpiece W in an oblique posture as shown in FIG. 7, it becomes easy to drip the liquid resin material M0 accurately onto the pre-attached target portion toward the joint edge 122.

[0041] However, the attitude of the workpiece W when performing the dripping process (step S206) may be other than the oblique attitude. For example, in the example shown in FIG. 8, the dripping process (step S206) is performed on the workpiece W in an upright attitude with the central axis I parallel to the vertical direction. Note that, although there is one nozzle 920 in the example shown in FIG. 8, multiple nozzles 920 may be arranged along the radial direction and / or the circumferential direction. This is also the case with the example shown in FIG. 7.

[0042] In this embodiment, the circumferential range in which the nozzle 920 is positioned with respect to the workpiece W is not the entire 360-degree circumferential range corresponding to the annular pre-attachment target portion of the workpiece W, but a part of the circumferential range. Hereinafter, the circumferential range of the annular pre-attachment target portion of the workpiece W that is impregnated with the liquid resin material M0 dripped from the nozzle 920 at a certain point in time is also referred to as the "dripping range" at that point in time. In addition, below, the dripping range (circumferential range) at a certain point in time is assumed to be an angle β (hereinafter also referred to as the "dripping range angle β"). The dripping range angle β is any angle significantly smaller than 360 degrees, and may be, for example, 45 degrees.

[0043] Next, this manufacturing method includes a rotation process (step S208) of rotating the workpiece W about the central axis I by a certain angle γ (hereinafter also referred to as "workpiece rotation angle γ").

[0044] In this embodiment, as an example, the rotating step rotates the workpiece W counterclockwise in top view as shown by the arrow R7 in Figs. 7 and 8. In a modified example, instead of rotating the workpiece W in one direction (counterclockwise or clockwise) by the workpiece rotation angle γ in top view, the nozzle 920 (and the ultraviolet ray irradiation device 900 described later) may be rotated by the workpiece rotation angle γ in the opposite direction in top view with respect to the workpiece W. The workpiece rotation angle γ may be the same as the dripping range angle β or may be slightly smaller than the dripping range angle β. The device on the equipment side that rotates the workpiece W is arbitrary, and for example, a multi-joint robot as shown in Fig. 7 may be used, or a rotary table 940 as shown in Fig. 8 may be used.

[0045] When the workpiece W is rotated in this manner, a portion of the annular pre-attachment target portion of the workpiece W that is different in circumferential range from the portion of the circumferential range onto which the liquid resin material M0 was dripped in step S206 is located below the nozzle 920. In other words, a portion of the annular pre-attachment target portion of the workpiece W that is shifted in circumferential range by the workpiece rotation angle γ is located below the nozzle 920.

[0046] Next, this manufacturing method includes a step (step S210) of simultaneously carrying out the dripping step and the resin curing step. Figures 7 and 8 show a schematic diagram of the state of the workpiece W when the dripping step and the resin curing step are carried out simultaneously (in parallel). In Figures 7 and 8, the liquid resin material M0 impregnated into the pre-attachment target portion of the workpiece W by the dripping step is shown by a hatched area M1. Also, in Figures 7 and 8, the rotation direction of the workpiece W is shown by an arrow R7.

[0047] In this embodiment, the resin curing step includes irradiating the pre-attached portion of the work W with ultraviolet light. In the example shown in FIG. 7 and FIG. 8, the ultraviolet light irradiation device 900 irradiates the liquid resin material M0 on the pre-attached portion of the work W with ultraviolet light. As a result, the surface side portion of the liquid resin material M0 dropped on the pre-attached portion of the work W is cured. In the example shown in FIG. 7 and FIG. 8, one ultraviolet light irradiation device 900 is provided for one pre-attached portion, but multiple ultraviolet light irradiation devices 900 may be provided for one pre-attached portion (for example, a pre-attached portion on the outer diameter side) along the radial direction and / or the circumferential direction. Note that FIG. 7 shows an ultraviolet light irradiation device 900A that irradiates the pre-attached portion on the inner diameter side of the work W and an ultraviolet light irradiation device 900B that irradiates the pre-attached portion on the outer diameter side of the work W. In addition, the ultraviolet light irradiation device 900 may be movable (movable) to positions such as the ultraviolet light irradiation devices 900A and 900B.

[0048] In this embodiment, the circumferential range in which the ultraviolet irradiation device 900 is positioned relative to the workpiece W is not the entire 360-degree circumferential range of the workpiece W, but a part of the circumferential range, similar to the circumferential range in which the nozzle 920 is positioned relative to the workpiece W. Hereinafter, the effective circumferential range in which the ultraviolet ray is irradiated from the ultraviolet irradiation device 900 at a certain point in time among the annular pre-attaching target portion of the workpiece W is also referred to as the "irradiation range" at that point in time. In addition, hereinafter, the irradiation range (circumferential range) at a certain point in time is assumed to be an angle η (hereinafter also referred to as the "irradiation range angle η"). The irradiation range angle η is any angle significantly smaller than 360 degrees. The irradiation range angle η is preferably approximately the same as the dripping range angle β described above.

[0049] The irradiation range at a certain time point is preferably adjacent to the dripping range at the same time point in the circumferential direction. In this case, as described later, the resin curing process (irradiation of ultraviolet rays) can be performed on the liquid resin material M0 dripped at a certain time point within a relatively short time from the time point. Since the boundary of the irradiation range may be unclear, for example, the irradiation range at a certain time point may be adjacent to the dripping range at the same time point in a manner that partially overlaps with it in the circumferential direction.

[0050] 10, when the dripping range at a certain time point is the circumferential range SC1, the irradiation range at the same time point may be the circumferential range SC8. However, the irradiation range at the same time point may include a circumferential end of the circumferential range SC1 (an end on the circumferential range SC8 side) slightly more than the circumferential range SC8.

[0051] Next, this manufacturing method again includes a rotation step (step S212) of rotating the workpiece W by the workpiece rotation angle γ around the central axis I. Note that the rotation direction in the rotation step in step S212 is the same as the rotation direction in the rotation step in step S208 described above.

[0052] Next, this manufacturing method includes a determination step (step S214) for determining whether the liquid resin material M0 has been dripped onto the entire 360-degree circumferential range of the pre-attachment target portion of the workpiece W. Here, for convenience of explanation, it is assumed that the workpiece rotation angle γ, dripping range angle β, and irradiation range angle η are all 45 degrees. In this case, as shown in FIG. 10, the dripping range angle β (and irradiation range angle η) can cover each of the 8 divided circumferential ranges. Therefore, in this case, this determination step may determine whether the rotation step with the workpiece rotation angle γ has been performed only seven times for one workpiece W. If the liquid resin material M0 has been dripped onto the entire 360-degree circumferential range of the pre-attachment target portion of the workpiece W, the process proceeds to the next step (step S216). On the other hand, if the liquid resin material M0 has not been dripped onto the entire 360-degree circumference of the pre-attachment target portion of the workpiece W, the process from step S210 is repeated until the liquid resin material M0 has been dripped onto the entire 360-degree circumference of the pre-attachment target portion of the workpiece W.

[0053] Next, this manufacturing method includes a resin hardening process (step S216) for the circumferential range (dripping range) onto which the liquid resin material M0 was last dripped, among the pre-applied portions of the workpiece W. The resin hardening process is the same as the resin hardening process (ultraviolet light irradiation) in step S210 described above. Note that the resin hardening process in step S216 is a process that is performed after the dripping process of the liquid resin material M0 onto the workpiece W is completed, and is therefore not performed simultaneously with the dripping process.

[0054] In this way, the liquid resin material M0 is dripped onto the entire circumference of the annular pre-attached portion of the workpiece W while the workpiece W rotates (see arrow R7 in Figures 7 and 8), and ultraviolet light is irradiated. That is, the dripping process and the resin hardening process are performed sequentially, one part at a time, along the circumferential direction of the pre-attached portion. At this time, the resin hardening process is performed sequentially, one part at a time, along the circumferential direction of the pre-attached portion, in the order in which the dripping processes were performed. Therefore, the resin hardening process for the portion of the circumferential range in which one dripping process has been performed is performed during the dripping process following that one dripping process. This allows the dripping process and the resin hardening process to be performed efficiently.

[0055] For example, in the example shown in FIG. 10, first, the initial dripping process (step S206) is performed on a portion of the circumferential range SC1 of the annular pre-attached portion of the workpiece W. Next, the workpiece W is rotated 45 degrees counterclockwise in the direction of FIG. 10 (step S208), and then the dripping process and the resin hardening process are simultaneously performed (step S210). At this time, the dripping process is performed on a portion of the circumferential range SC2 of the annular pre-attached portion of the workpiece W, and the resin hardening process is performed on a portion of the circumferential range SC1 of the annular pre-attached portion of the workpiece W. When the dripping process and the resin hardening process for each portion of the circumferential range are completed, the workpiece W is rotated 45 degrees counterclockwise in the direction of FIG. 10 (step S212), and then the dripping process and the resin hardening process are simultaneously performed again (step S210). At this time, the dripping process is performed on a portion of the circumferential range SC3 of the annular pre-attached portion of the work W, and the resin hardening process is performed on a portion of the circumferential range SC2 of the annular pre-attached portion of the work W. In this manner, each process of step S210 and step S212 is repeated. Then, in the final stage, the dripping process is performed on a portion of the circumferential range SC8 of the annular pre-attached portion of the work W, and the resin hardening process is performed on a portion of the circumferential range SC7 of the annular pre-attached portion of the work W. After that, the work W is rotated 45 degrees counterclockwise as viewed in the direction of FIG. 10 (step S212), and then the resin hardening process is performed on the portion of the circumferential range SC8 of the annular pre-attached portion of the work W (step S216), and the pre-attaching process for the work W is completed.

[0056] According to the resin hardening process of this embodiment, it is possible to significantly reduce CT (for example, by about half) compared to a case where a dripping process is performed on the entire circumference of the annular pre-fitting target portion of the workpiece W, and then a resin hardening process is performed on the entire circumference of the annular pre-fitting target portion of the workpiece W (hereinafter also referred to as a "non-simultaneous resin hardening process"). That is, according to the resin hardening process of this embodiment, the time (period) when the dripping process is performed on one workpiece W and the time (period) when the resin hardening process is performed on the same workpiece W overlap, so that it is possible to significantly reduce CT compared to a configuration where there is no overlap.

[0057] In this manufacturing method, as described above, the workpiece W is rotated intermittently for each workpiece rotation angle γ by the rotation processes in steps S208 and S212, but this is not limited to this. For example, the dripping process and the resin curing process may be performed simultaneously while the workpiece W is continuously rotated at a low speed.

[0058] Furthermore, in a non-simultaneous resin curing process, if the liquid resin material M0 drips under its own weight before the resin curing process is performed (see arrows R9 and R10 in FIG. 9), the necessary thickness of the insulating coating (e.g., the thickness necessary to ensure insulating performance) may not be ensured. In particular, the joint edge 122, which is the corner of the rectangular cross section of the coil piece 52, has low wettability (wettability of the corner of the linear conductor 120), so the insulating coating (cured product of the liquid resin material M0) on the joint edge 122 is likely to be significantly smaller than the thickness necessary to ensure insulating performance.

[0059] In this regard, if the resin curing step is performed immediately after the dripping step, the liquid resin material M0 is likely to be cured before it drips under its own weight. In other words, the liquid resin material M0 can be prevented from dripping as shown by the arrows R9 and R10 in Fig. 9. In this way, according to the resin curing step of this embodiment, as described above, the resin curing step is performed immediately after the dripping step, so that the necessary thickness of the insulating coating (cured product of the liquid resin material M0) can be ensured even for the joint edges 122 of the coil pieces 52, which have low wettability.

[0060] In addition, in the non-simultaneous resin curing process, if the liquid resin material M0 drips under its own weight after the dripping process is performed and before the resin curing process is performed (see arrows R9 and R10 in FIG. 9), the exposed area (area not covered by the resin member) on the side surface of the coil end portion 114A may be unnecessarily narrowed. If the exposed area on the side surface of the coil end portion 114A is insufficient, the cooling efficiency may decrease when a coolant (e.g., oil) is supplied to the side surface of the coil end portion 114A during operation of the rotating electric machine 1 (described later with reference to FIG. 22). In addition, if the liquid resin material M0 drips downward from the radial side surface of the pre-attachment target portion, it may adhere to the axial end surface (upper end surface) of the stator core 112. In this case, the liquid resin material M0 adhered to the stator core 112 needs to be removed separately with a scraper or the like.

[0061] In this regard, according to the resin curing process of this embodiment, as described above, the resin curing process is performed immediately after the dripping process, so that the possibility that the exposed area (area not covered with the resin material) on the side surface of the coil end portion 114A becomes unnecessarily narrow due to the liquid resin material M0 dripping under its own weight can be effectively reduced. Also, the possibility that the liquid resin material M0 adheres to the stator core 112 can be effectively reduced.

[0062] In a modified embodiment, a non-simultaneous resin curing step may be implemented, in which case the effects resulting from the pre-applying step described below can still be obtained.

[0063] Next, this manufacturing method includes an immersion step (step S218) of immersing the workpiece W in the tank 600 of liquid resin material M0. Fig. 11 is a schematic side view of the workpiece W before it is immersed in the tank 600 of liquid resin material M0, and Fig. 12 is a schematic side view of the workpiece W immersed in the tank 600 of liquid resin material M0.

[0064] The immersion step is performed so that the axial end (lower end in the downward orientation) of the workpiece W is immersed in the liquid resin material M0 (i.e., is located below the liquid surface 601 of the liquid resin material M0) while the workpiece W is maintained in a downward orientation. The impregnation target portion of the workpiece W is set to the portion of the multiple coil pieces 52 of the workpiece W. Specifically, the impregnation target portion of the workpiece W is the axial end (lead side end) of the multiple coil pieces 52, and includes the joint portion 400. More specifically, the impregnation target portion of the workpiece W includes a portion (including the joint portion 400) of each coil piece 52 of the workpiece W where the conductor (the conductor portion related to the linear conductor 120) is exposed. The impregnation target portion has an annular shape around the central axis I when viewed in the axial direction, and includes a part (a part on the axial end side) of the coil end portion 114A. In this embodiment, the impregnation target portion of the workpiece W includes the entire pre-attachment target portion of the workpiece W described above. The area of ​​the workpiece W to be impregnated may be a larger area than the area to be pre-applied, as long as it includes the area to be pre-applied of the workpiece W described above.

[0065] The impregnation target portion may be set to include neutral bus bar 59. In this case, neutral bus bar 59 is wrapped in liquid resin material M0, thereby ensuring electrical insulation of neutral bus bar 59. In other words, neutral bus bar 59 does not need to be in a form in which it is insulated by insert molding or the like with an insulating material such as a resin material in advance, but can be in the form of sheet metal (with the entire conductor material exposed). This makes it possible to efficiently ensure electrical insulation of neutral bus bar 59.

[0066] Fig. 12A is an enlarged view of part Q8 in Fig. 12, which is an enlarged schematic view of a portion of the impregnation target area of ​​the workpiece W (the joint 400 and its surrounding area). In the immersion process, unlike the above-mentioned dripping process, the inflow of the liquid resin material M0 into a relatively narrow flow path (see arrow R8 in Fig. 12A) on the upper surface 420 of the joint 400 is promoted. Therefore, in the immersion process, unlike the above-mentioned dripping process, it is possible to appropriately cover the upper surface 420 of the joint 400.

[0067] The immersion process may be performed in a state where the temperature of the liquid resin material M0 in the tank 600 is significantly higher than the ambient temperature so as to promote the flow of the liquid resin material M0 into a relatively narrow flow path onto the upper surface 420 of the joint 400. Since the immersion process can be started in a state where the viscosity of the liquid resin material M0 is relatively low, it becomes possible to efficiently spread the liquid resin material M0 over the upper surface 420 of the joint 400 and the like.

[0068] Next, the present manufacturing method includes a post-processing step (step S220) of lifting the workpiece W from the tank 600 and performing post-processing on the workpiece W lifted from the tank 600. Fig. 13 shows a schematic diagram of the state of the workpiece W when it is lifted.

[0069] In this manufacturing method, immediately after the workpiece W is lifted up, the liquid resin material M0 may drip due to its own weight. In FIG. 13, the liquid resin material M0 dripping due to its own weight is indicated by the symbol M22. Hereinafter, the liquid resin material M0 dripping due to its own weight out of the liquid resin material M0 impregnated in the impregnation target portion of the workpiece W is also referred to as the hanging portion M22. The hanging portion M22 has a so-called "icicle" shape, and due to the relatively high viscosity of the liquid resin material M0, it tends not to fall immediately (i.e., it tends to extend downward while remaining in the "icicle" shape).

[0070] The post-treatment is optional, but preferably includes a rotation step of rotating the workpiece W around the central axis I of the workpiece W. Hereinafter, the rotation step of the post-treatment is also referred to as a "re-attachment rotation step." In Fig. 14, the rotation by the re-attachment rotation step is shown diagrammatically by an arrow R15. In Fig. 14, the dashed dotted line H represents a horizontal line.

[0071] The re-adhesion rotation step includes rotating the workpiece W so that the drooping portion M22 is absorbed into the normal portion (the portion other than the drooping portion M22, i.e., the portion where the liquid resin material M0 is in a normal state). That is, the re-adhesion rotation step includes rotating the workpiece W so that the liquid resin material M0 (i.e., the drooping portion M22) dripping downward from one circumferential position in the impregnation target portion adheres to another circumferential position in the impregnation target portion.

[0072] The reattachment rotation process is preferably performed on the workpiece W in an obliquely downward orientation. The angle α (see FIG. 14) of the obliquely downward orientation is preferably relatively small. For example, the angle α (see FIG. 14) of the obliquely downward orientation may be preferably smaller than 45 degrees and larger than −20 degrees.

[0073] The post-processing may further include an inversion process for changing the orientation of the workpiece W to an upward orientation, and an upper surface resin curing process for performing a resin curing process of the liquid resin material M0 on the upper surface of the portion to be impregnated of the workpiece W in the upward orientation.

[0074] Fig. 15 shows a schematic diagram of a state in which a resin curing process is being performed. In the example shown in Fig. 15, the ultraviolet irradiation device 900 irradiates ultraviolet rays onto the upper surface of the impregnation target portion of the workpiece W (see arrow R13). This causes the upper portion (mainly the upper surface portion) of the liquid resin material M0 with which the impregnation target portion of the workpiece W is impregnated to be cured.

[0075] The ultraviolet irradiation device 900 preferably irradiates ultraviolet rays over the entire circumference of the upper surface of the portion to be impregnated of the workpiece W. This allows the liquid resin material M0 in the upper portion to be cured over the entire circumference of the portion to be impregnated. In this case, the workpiece W may be rotated about the central axis I, or the ultraviolet irradiation device 900 may be rotated. Alternatively, multiple ultraviolet irradiation devices 900 may be disposed circumferentially on the upper side of the workpiece W.

[0076] Preferably, a plurality of ultraviolet irradiation devices 900 are provided so as to enable irradiation from various directions, as shown in Fig. 15. In this case, the liquid resin material M0 in the upper portion of the portion to be impregnated of the workpiece W can be efficiently cured.

[0077] In this way, according to the present manufacturing method, the workpiece W is in an upward position, and the upper portion (axial end portion) of the liquid resin material M0 impregnated in the impregnation target portion is hardened. Therefore, it is possible to reduce the inconvenience that may occur when the resin hardening process is performed on the workpiece W pulled up from the tank 600 while it is in a downward position. Specifically, when the resin hardening process is performed on the lower surface of the impregnation target portion of the workpiece W pulled up from the tank 600 while it is in a downward position, the liquid resin material M0 impregnated in the impregnation target portion of the workpiece W may be hardened while dripping downward due to its own weight. In this case, the hardening liquid resin material M0 may return to the tank 600, which may affect the fluidity of the liquid resin material M0 in the tank 600. In contrast, according to the present manufacturing method, the resin hardening process is performed in an upward position as described above, so that such inconvenience can be reduced.

[0078] 15, the resin hardening process is performed by an ultraviolet ray irradiation device 900, which mainly irradiates the upper surface of the portion to be impregnated of the workpiece W, but instead of or in addition to this, the radially inner and / or radially outer side surfaces may be irradiated. This hardens the radially inner and / or radially outer portions (mainly the surface portions) of the liquid resin material M0 impregnated into the portion to be impregnated of the workpiece W, thereby more effectively reducing the possibility that the exposed range (the range not covered by the resin member) on the side surface of the coil end portion 114A will be unnecessarily narrow.

[0079] Next, this manufacturing method includes a heating step (step S222) of heating the workpiece W so that the liquid resin material M0 in the entire workpiece W is hardened. This heating step has a function of completely hardening the portion of the liquid resin material M0 that is not hardened in the above-mentioned resin hardening step (e.g., the portion inside the surface). The heating method in the heating step is arbitrary, and may be achieved, for example, by placing the workpiece W in a furnace. The liquid resin material M0 impregnated in the impregnation portion including the portion to be impregnated of the workpiece W is heated and completely hardened. As a result, an insulating coating of the liquid resin material M0 is formed on the stator coil 114.

[0080] The posture of the workpiece W in the heating process is arbitrary, but is preferably downward as shown in FIG. 16. FIG. 16 shows a schematic diagram of a plurality of workpieces W arranged side by side in a downward posture and undergoing a heating process. FIG. 16 shows a schematic diagram of a workpiece gripper 1000 of a part of a manufacturing device clamping a plurality of workpieces W, but the workpieces W may be supported on a table in such a manner that an end face of a stator core 112 abuts against an upper surface (not shown) of the table. FIG. 16 shows an example in which heat is radiated from below the workpiece W (see arrow R17), but the direction of heat radiation is arbitrary.

[0081] Next, the effects of this embodiment will be described with reference to FIGS.

[0082] FIG. 17 is an explanatory diagram of the insulating coating of the liquid resin material M0 manufactured by the manufacturing method according to this embodiment, and FIG. 18 is an explanatory diagram of the insulating coating of the liquid resin material M0 manufactured by the manufacturing method according to the comparative example, both of which are cross-sectional views passing through the central axis I of the workpiece W. For convenience of explanation, in FIG. 17 and FIG. 18, only the axial end of the coil end portion 114A of the stator coil 114 is illustrated in a schematic manner without omission. In FIG. 17, the liquid resin material M0 applied by the immersion process is shown by a hatched area M2 so that the liquid resin material M0 applied by the pre-applying process can be seen, and the hatched area M2 is shown in perspective so that the liquid resin material M0 applied by the pre-applying process (hatched area M1) can be seen.

[0083] The comparative example differs from the manufacturing method according to the present embodiment in that the pre-attaching step is omitted. In such a comparative example, as shown in FIG. 18, the thickness of the liquid resin material M0 applied by the dipping step is likely to be thin at the joint edges 122 on the outer diameter side and the inner diameter side. This is because, as described above, such areas have low wettability (wettability of the corners of the linear conductor 120) and do not have other areas (areas of the coil pieces 52) adjacent to them in the radial direction. For this reason, in the comparative example, for example, it becomes more necessary to repeat the dipping step two or more times. As a result, problems such as an increase in cycle time arise.

[0084] In contrast, according to this embodiment, as described above, in the pre-applying step, the liquid resin material M0 is applied to a portion (i.e., a portion to be pre-applied) where the thickness of the liquid resin material M0 applied in the dipping step is likely to become thin. When a thin film of the liquid resin material M0 is formed on the portion to be pre-applied by the pre-applying step, the wettability of the portion to be pre-applied with respect to the liquid resin material M0 can be increased. This makes it easier for the liquid resin material M0 to adhere to the portion to be pre-applied in the subsequent dipping step. As a result, the thickness of the insulating coating (cured product of the liquid resin material M0) on the joint edge 122 can be effectively increased even by the first dipping step. In other words, it becomes easy to ensure a relatively thick film thickness in one dipping step, and the number of dipping steps can be reduced (and the cycle time can be shortened accordingly). For example, it may be possible to reduce the number of dipping steps to only one.

[0085] In this way, according to this embodiment, it is possible to ensure the necessary thickness of the insulating coating in areas that tend to become locally thin, while reducing or eliminating the need to perform the dipping step multiple times.

[0086] In the above-mentioned manufacturing method, the pre-applied portion includes the joint edge 122, but is not limited thereto. For example, the pre-applied portion may be a side portion 440 in the vicinity of the joint edge 122, as shown by the liquid resin material M0 in FIG. 19. Specifically, the pre-applied portion may be a side portion 440 (side portion 440 facing radially outward) continuing to the joint edge 122 on the outermost diameter side. Also, the pre-applied portion may be a side portion 440 (side portion 440 facing radially inward) continuing to the joint edge 122 on the innermost diameter side. In this case, the pre-applied liquid resin material M0 functions as a dam, and can promote the adhesion of the liquid resin material M0 to the joint edge 122 in the vicinity. Therefore, in this case as well, the necessary thickness of the insulating coating of the liquid resin material M0 can be secured at the joint edge 122 on the outermost diameter side and the joint edge 122 on the innermost diameter side.

[0087] Here, further effects of this embodiment will be described with reference to FIG. 20 and FIG.

[0088] FIG. 20 is a cross-sectional photograph of an insulating coating 200 formed by the manufacturing method of this embodiment (one dipping process), and FIG. 21 is a cross-sectional photograph of an insulating coating 200' formed through two dipping processes by the above-mentioned comparative example (a configuration that does not have a pre-attaching process).

[0089] In the comparative example, problems occur such as the occurrence of voids 220 between the insulating coating portion applied by the first dipping step (dip coating) and the insulating coating portion applied by the second dip coating, and the occurrence of locally thick portions of the insulating coating 200' (see height H3 in FIG. 21). For example, in the example shown in FIG. 21, the height H3 of the central portion of the insulating coating 200' is significantly greater than the height H2 on both radial sides.

[0090] In contrast, according to this embodiment, it is possible to prevent the inconveniences that occur in the comparative example. That is, according to this embodiment, as described above, it is possible to reduce the number of dipping steps to only one, and in that case, it is possible to eliminate the inconveniences (problems of voids 220 and the height H3 of the central part becoming excessive) that occur due to performing the dipping steps two or more times. In addition, by reducing the number of dipping steps, it is also possible to reduce the amount of liquid resin material M0 required to form the insulating coating 200.

[0091] Next, with reference to FIG. 22, a cooling structure suitable for the rotating electric machine 1 incorporating the rotating electric machine stator 10 manufactured by the present manufacturing method will be described.

[0092] FIG. 22 is a diagram showing an example of a cooling structure, and is a diagram showing a part of the cross-sectional structure of the rotating electric machine 1. As shown in FIG.

[0093] In the example shown in FIG. 22, oil is supplied from the radially outer side and the radially inner side to the coil end portion 114A at both axial ends of the stator coil 114. Specifically, the oil supplied to the case inner oil passage 60 of the case 2 (see arrow R20A) is supplied to the radially outer side surface of the coil end portion 114A through the oil hole 62 penetrating toward the radially inner side (see arrow R20). The oil hole 62 may be disposed on the vertically upper side so as to promote the dripping of oil by gravity. In addition, the oil supplied to the axial center oil passage 64 of the rotor shaft 112A (see arrow R21A) is supplied to the radially inner side surface of the coil end portion 114A through the oil hole 66 penetrating toward the radially outer side (see arrow R21). This makes it possible to effectively improve the cooling performance of the coil end portion 114A by the oil from the oil hole 66 described above.

[0094] Although each embodiment has been described above in detail, the present invention is not limited to the specific embodiment, and various modifications and changes are possible within the scope of the claims. In addition, it is also possible to combine all or a plurality of the components of the above-described embodiments.

[0095] For example, in the above-described embodiment, the immersion process is performed after the dripping process, but the immersion process may be performed before the dripping process. In this case, the dripping process may be performed subsequent to the upper surface resin curing process related to the post-treatment process (step S220). FIG. 23 shows a schematic diagram of the dripping process performed subsequent to the upper surface resin curing process related to the post-treatment process (step S220). In this case, the liquid resin material can be applied to the pre-attachment target portion by positioning the nozzle 920 relative to the pre-attachment target portion. In this case, the pre-attachment target portion and the pre-attachment process may be read as the "post-attachment target portion" and the "post-attachment process". Such a post-attachment process may be performed in the same manner as the above-described pre-attachment process. In this case, the resin curing process (the resin curing process corresponding to the resin curing process in the pre-attachment process) may be simplified or omitted in consideration of the fact that the heating process follows.

[0096] In the above-described embodiment, the liquid resin material M0 (an example of a first liquid resin material) applied to the workpiece W in the pre-applying step and the liquid resin material M0 (an example of a second liquid resin material) applied to the workpiece W in the immersion step are the same material, but different materials may be used, or the materials may be substantially the same but have different properties (e.g., viscosity) due to differences in temperature, etc. For example, the liquid resin material M0 applied to the workpiece W in the pre-applying step may have a higher viscosity than the liquid resin material M0 applied to the workpiece W in the immersion step.

[0097] In the above-described embodiment, the workpiece W may be heated prior to the pre-attaching step. That is, the pre-heating step of heating the workpiece W may be performed prior to the pre-attaching step. Alternatively, the pre-heating step of heating the workpiece W may be performed prior to the immersion step (e.g., after the resin curing step in step S216).

[0098] In the above-described embodiment, instead of the dripping step in the pre-attaching step, a coating step or the like may be performed in the pre-attaching step. That is, the method of attaching the liquid resin material M0 to the pre-attaching target portion may be other methods such as coating, in addition to dripping. [Explanation of symbols]

[0099] 40... Joint portion (tip portion), 52... Coil piece, 112... Stator core, 114... Stator coil, W... Workpiece, M0... Liquid resin material

Claims

1. a mounting step of mounting a plurality of coil pieces forming a stator coil on a stator core to form a workpiece; a joining step of joining a tip end portion of one of the coil pieces and another of the coil pieces to each other at one axial end side of the workpiece after the mounting step; an attachment step of attaching a first liquid resin material to an attachment target site of the joined tip portion after the joining step; After the adhesion step or before the adhesion step, an immersion step of immersing an impregnation target portion including the adhesion target portion of the workpiece in a tank of a second liquid resin material; a curing step of curing the first liquid resin material and the second liquid resin material in the portion to be impregnated.

2. The immersion step is performed after the deposition step; 2. The method for manufacturing a stator for a rotating electric machine according to claim 1, further comprising an initial curing step of initially curing the first liquid resin material applied to the application target portion in the application step, prior to the immersion step.

3. the first liquid resin material has a property of being hardened by irradiation with ultraviolet light; 3. The method for manufacturing a stator for a rotating electric machine according to claim 2, wherein the initial curing process is performed in parallel with the adhering process by irradiating the first liquid resin material adhered to the adhesion target portion in the adhering process with ultraviolet light.

4. The coil pieces are rectangular wires having a rectangular cross section, 4. A method for manufacturing a stator for a rotating electric machine according to claim 1, wherein the attachment target portion includes at least a portion of a side portion of the coil piece that forms a corner together with a portion of the coil piece that faces axially outward, and the side portion faces in a direction intersecting the axial direction of the stator core.

Citation Information

Patent Citations

  • Thermosetting resin composition and rotary electric machine using the composition

    JP2016124878A

Cited By

  • Method of manufacturing stator

    EP4749893A1