Method of producing article
The wrapping process with rollers and specific protective layers addresses cracking and adhesion issues in transfer layer application, ensuring robust and weather-resistant adherends.
Patent Information
- Application Number
- JP2023055083
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
The hydraulic transfer process used in existing methods for applying a transfer layer to adherends can result in cracking due to uniform water pressure, especially at corners, and the adhesion between protective layers is often insufficient, leading to issues like lifting and poor weather resistance.
A method involving a wrapping process using rollers to sequentially bond a transfer sheet's layers to multiple adherend surfaces, incorporating a first protective layer with a curable resin composition and a second protective layer with higher flexibility, and applying a design layer for improved adhesion and weather resistance.
This method effectively suppresses cracking and lifting of the transfer layer, enhances adhesion between protective layers, and provides high weather resistance, making it suitable for exterior products.
Smart Images

Figure 2024142771000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method of manufacturing an article. [Background technology]
[0002] It is known that a transfer layer (a layer transferred from a transfer sheet) of a transfer sheet is transferred to an adherend such as a metal member or a resin member to decorate the adherend. For example, Patent Document 1 discloses a rain gutter in which an oxide film layer is arranged on the outer surface of an aluminum base material, a decorative layer is arranged on the outer surface of the oxide film layer, and a pattern is applied to the surface of the decorative layer. Specifically, Patent Document 1 discloses forming a decorative layer by hydraulic transfer processing on the outer surface of an anodized aluminum base material. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-12283 A Summary of the Invention [Problem to be solved by the invention]
[0004] The water pressure transfer process described in Patent Document 1 is a technique for transferring a transfer layer of a transfer sheet to an adherend by applying water pressure uniformly to the adherend and the transfer sheet. Since the transfer layer is thinner than, for example, a decorative sheet, cracks may occur in the transfer layer if the transfer layer is suddenly bent at the corner of the adherend when water pressure is applied uniformly.
[0005] The present disclosure has been made in consideration of the above-mentioned circumstances, and provides a method for manufacturing an article that suppresses the occurrence of cracks in a transfer layer when the transfer layer is transferred to an adherend. [Means for solving the problem]
[0006] The present disclosure provides a method for manufacturing an article, comprising: a preparation step of preparing an adherend having multiple surfaces and a transfer sheet having a release film and a transfer layer; and a wrapping step of sequentially bonding the transfer layer of the transfer sheet to the multiple surfaces of the adherend using a roller. Effect of the Invention
[0007] The method for manufacturing an article according to the present disclosure has the effect of suppressing the occurrence of cracks in the transfer layer when the transfer layer is transferred to an adherend. [Brief description of the drawings]
[0008] [Figure 1] 1 is a schematic cross-sectional view illustrating a transfer sheet according to the present disclosure. [Diagram 2] 1A and 1B are schematic side views and schematic cross-sectional views illustrating an example of an adherend in the present disclosure. [Diagram 3] 1 is a schematic side view illustrating a lapping process in the present disclosure; [Figure 4] 4A to 4C are sectional views taken along lines AA, BB, CC, DD, and EE in FIG. [Diagram 5] FIG. 4 is an explanatory diagram illustrating the axial direction of each roller. [Figure 6] 1A to 1C are schematic cross-sectional views illustrating a lapping process step in the present disclosure. [Figure 7] 1A to 1C are schematic cross-sectional views illustrating a lapping process step in the present disclosure. [Figure 8] 1 is a schematic cross-sectional view illustrating an example of an adherend in the present disclosure. [Figure 9] 1 is a schematic cross-sectional view illustrating an example of an adherend in the present disclosure. [Figure 10] 1 is a schematic cross-sectional view illustrating an example of an adherend in the present disclosure. [Figure 11] FIG. 1 is a schematic cross-sectional view illustrating a portion of an article according to the present disclosure. [Figure 12] FIG. 2 is an explanatory diagram illustrating a production line for carrying out the method for producing an article according to the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The following describes the embodiments with reference to the drawings. However, the present disclosure can be implemented in many different forms and should not be limited to the description of the embodiments exemplified below. In addition, the drawings may show the width, thickness, and shape of each part in a schematic manner compared to the actual form in order to make the description clearer, but this is merely an example and should not be interpreted as being limiting.
[0010] In this specification, when describing a mode in which another component is disposed on a certain component, the term "above" or "below" includes both cases in which another component is disposed directly above or below the certain component so as to be in contact with the component, and cases in which another component is disposed above or below the certain component with another component interposed therebetween, unless otherwise specified. In addition, in this specification, when describing a mode in which another component is disposed on the surface of a certain component, the term "on the surface" includes both cases in which another component is disposed directly above or below the certain component so as to be in contact with the component, and cases in which another component is disposed above or below the certain component with another component interposed therebetween, unless otherwise specified.
[0011] The method for producing the article according to the present disclosure will now be described in detail.
[0012] The method for producing an article in the present disclosure includes a preparation step of preparing a transfer sheet and an adherend. FIG. 1(a) is a schematic cross-sectional view illustrating a transfer sheet in the present disclosure. As shown in FIG. 1(a), a transfer sheet 10 has a release film 1 and a transfer layer X arranged on one surface of the release film 1. The transfer layer X shown in FIG. 1(a) is formed by applying a first protective layer 2 and a second protective layer 3 from the release film 1 side in a thickness direction D. T In this order, the transfer sheet 10 may further include a design layer 4 on the surface of the second protective layer 3 opposite to the first protective layer 2, as shown in FIG.
[0013] Fig. 2(a) is a schematic side view illustrating an example of an adherend in the present disclosure, and Fig. 2(b) is a cross-sectional view taken along line AA in Fig. 2(a). As shown in Figs. 2(a) and (b), the adherend 20 is oriented in a longitudinal direction D L 3 is a schematic cross-sectional view illustrating a lapping process according to the present disclosure. In FIG. 3, the adherend 20 is wrapped around the adherend 20 in the longitudinal direction D. L While conveying the adherend 20 along the axis, the transfer layer X of the transfer sheet 10 is sequentially bonded to multiple surfaces of the adherend 20 using multiple rollers 60 (60a to 60e).
[0014] According to the present disclosure, by performing wrapping processing in which the transfer layer of the transfer sheet is sequentially laminated to the multiple surfaces of the adherend using a roller, it is possible to suppress the occurrence of cracks in the transfer layer when the transfer layer is transferred to the adherend. As described above, the water pressure transfer processing described in Patent Document 1 is a technology in which the transfer layer of the transfer sheet is transferred to the adherend by utilizing the fact that water pressure is uniformly applied to the adherend and the transfer sheet. Since the transfer layer is thinner than, for example, a decorative sheet, when water pressure is uniformly applied, if the transfer layer is suddenly bent at the corner portion of the adherend (the boundary portion between adjacent surfaces on the adherend), cracks may occur in the transfer layer. In contrast, in the present disclosure, a wrapping processing is performed in which the transfer layer of the transfer sheet is sequentially laminated to the multiple surfaces of the adherend using a roller. That is, the transfer layer is gradually bent at the corner portion of the adherend using a roller (especially a guide roller described later). This makes it possible to suppress the occurrence of cracks in the transfer layer.
[0015] In addition, after the transfer layer of the transfer sheet is attached to the adherend, the release film is usually peeled off from the transfer layer. Therefore, the peel strength of the release film and the transfer layer is weak. Therefore, when the transfer layer is bent suddenly at the corner of the adherend, there is a possibility that lifting occurs between the release film and the transfer layer. In contrast, in the present disclosure, the transfer layer is gradually bent at the corner of the adherend using a roller (particularly a guide roller described later). This can suppress the occurrence of lifting between the release film and the transfer layer. As described later, when the transfer layer has a first protective layer, the first protective layer may be prepared by curing a composition for forming the first protective layer. When the transfer layer is bent suddenly at the corner of the adherend, cracks may occur in the first protective layer. In contrast, in the present disclosure, the transfer layer is gradually bent at the corner of the adherend using a roller (particularly a guide roller described later). This can suppress the occurrence of cracks in the first protective layer.
[0016] In addition, as described later, the article in the present disclosure is preferably an exterior product (an article for outdoor use). Exterior products are exposed to harsh environments compared to interior products (articles for indoor use), and therefore high weather resistance is required. For example, when manufacturing an exterior product using a decorative sheet, a transparent resin layer may be provided on the decorative sheet for the purpose of improving strength. In this case, since the transparent resin layer is a relatively thick layer, for example, high weather resistance is imparted by adding a sufficient amount of weather resistance agent to the transparent resin layer. In contrast, it is technically difficult to impart high weather resistance to a transfer sheet that does not have a layer corresponding to the transparent resin layer. In the present disclosure, as described later, it is preferable that the transfer layer has a first protective layer and a second protective layer, and both the first protective layer and the second protective layer contain a weather resistance agent. This makes it possible to impart high weather resistance while maintaining the properties required for the first protective layer (for example, surface properties such as scratch resistance) and the properties required for the second protective layer (for example, adhesion).
[0017] In addition, in the case of a transfer sheet, the adhesion of the first protective layer and the second protective layer is likely to be insufficient. Here, in the case of a decorative sheet, a design layer is usually formed on a base layer, then a second protective layer is formed on the design layer, and then the first protective layer is formed on the second protective layer. The first protective layer is typically prepared by curing a composition for forming the first protective layer formed on the second protective layer, so that the adhesion of the first protective layer and the second protective layer is good. In contrast, in the case of a transfer sheet, the first protective layer is typically formed on a release film, then a second protective layer is formed on the first protective layer, and then a design layer is formed on the second protective layer. The first protective layer is typically prepared by curing a composition for forming the first protective layer on a release film. Since the second protective layer is formed on the cured first protective layer, the adhesion of the first protective layer and the second protective layer is likely to be insufficient. In the present disclosure, it is preferable that the second protective layer is a layer having higher flexibility than the first protective layer. This can increase the adhesion of the first protective layer and the second protective layer.
[0018] 1. Preparation process The preparation step in the present disclosure is a step of preparing an adherend having a plurality of surfaces, and a transfer sheet having a release film and a transfer layer.
[0019] (1) Transfer sheet The transfer sheet in the present disclosure has a release film and a transfer layer.
[0020] (i) Transfer layer The transfer layer in the present disclosure is a layer transferred from a transfer sheet. The transfer layer preferably has a protective layer that protects the surface of the adherend. In addition, the transfer layer preferably has a design layer on the side of the protective layer opposite to the release film.
[0021] (a) Protective layer The transfer layer in the present disclosure preferably has a protective layer. The protective layer is not particularly limited. The transfer layer may have only one protective layer, or may have two or more protective layers. For example, the transfer layer may be a single layer of the first protective layer described later, or a single layer of the second protective layer described later. In particular, the transfer layer preferably has the first protective layer and the second protective layer described later in this order in the thickness direction from the release film side. This is because it is particularly useful as a transfer sheet used for exterior products (items for outdoor use).
[0022] (a-1) First protective layer The transfer layer in the present disclosure preferably has a first protective layer. The first protective layer contributes to improving the surface properties (e.g., scratch resistance) of the article. The first protective layer and the release film may be arranged so as to be in direct contact with each other, or may be arranged via another layer.
[0023] The first protective layer preferably contains a cured product (crosslinked structure) of a curable resin composition as a resin component. The proportion of the cured product of the curable resin composition is, for example, 70% by mass or more, 90% by mass or more, 95% by mass or more, or 100% by mass, based on the total resin components constituting the first protective layer.
[0024] Examples of the curable resin composition used in the first protective layer include an ionizing radiation curable resin composition and a heat curable resin composition. Examples of the ionizing radiation curable resin composition include an electron beam curable resin composition and an ultraviolet ray curable resin composition. Among these, an electron beam curable resin composition is preferred because it does not require a polymerization initiator, has little odor, and is less likely to cause coloring.
[0025] The ionizing radiation curable resin composition is a composition containing a compound having an ionizing radiation curable functional group (hereinafter, also referred to as "ionizing radiation curable compound"). The ionizing radiation curable functional group is a group that crosslinks and cures when irradiated with ionizing radiation, and examples of such functional groups include functional groups having an ethylenic double bond, such as a (meth)acryloyl group, a vinyl group, and an allyl group. In the present disclosure, the (meth)acryloyl group refers to an acryloyl group or a methcroyl group.
[0026] Ionizing radiation refers to electromagnetic waves or charged particle beams that have an energy quantum capable of polymerizing or crosslinking molecules. Examples of ionizing radiation include electron beams (EB) and ultraviolet rays (UV). Other examples of ionizing radiation include electromagnetic waves such as X-rays and gamma rays, and charged particle beams such as alpha rays and ion beams.
[0027] The ionizing radiation curable resin composition preferably contains, as the ionizing radiation curable compound, one or more selected from, for example, urethane (meth)acrylate, epoxy (meth)acrylate, polyester (meth)acrylate, polyether (meth)acrylate, polycarbonate (meth)acrylate, and acrylic (meth)acrylate. Among them, the ionizing radiation curable resin composition preferably contains at least urethane (meth)acrylate as the ionizing radiation curable compound. In the present disclosure, urethane (meth)acrylate refers to urethane acrylate or urethane methacrylate. The urethane (meth)acrylate is preferably a caprolactane-based urethane (meth)acrylate.
[0028] When the ionizing radiation curable resin composition contains a caprolactane-based urethane (meth)acrylate, the caprolactane-based urethane (meth)acrylate preferably has 2 or more and 4 or less functional groups, more preferably 2 or more and 3 or less functional groups.
[0029] The ionizing radiation curable resin composition may contain a caprolactane-based urethane (meth)acrylate and a non-caprolactane-modified urethane (meth)acrylate. In this case, the content of the caprolactane-based urethane (meth)acrylate contained in the first protective layer is M CLUA The content of urethane (meth)acrylate not modified with caprolactone is M UA Let us assume that UA and M. CLUA M for the sum of CLUA Mass ratio (M CLUA / (M UA +M CLUA )) is, for example, 40% by mass or more and 90% by mass or less, alternatively 45% by mass or more and 80% by mass or less, or 50% by mass or more and 70% by mass or less.
[0030] Caprolactan-based urethane (meth)acrylate can usually be obtained by reacting caprolactan-based polyol, organic isocyanate, and hydroxy (meth)acrylate. For example, a method of synthesis includes reacting polycaprolactan-based polyol with organic polyisocyanate to generate a polyurethane prepolymer containing -NCO groups (isocyanate groups) at both ends, and then reacting it with hydroxy (meth)acrylate.
[0031] Caprolactane polyols may be commercially available, preferably having two hydroxyl groups and a number average molecular weight of 500 to 3000, more preferably 750 to 2000. In addition, polyols other than caprolactane polyols, such as ethylene glycol, diethylene glycol, 1,4-butanediol, 1,6-hexanediol, etc., may be used in combination in any ratio. As the organic polyisocyanate, a diisocyanate having two isocyanate groups is preferred, and from the viewpoint of suppressing yellowing, isophorone diisocyanate, hexamethylene diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, trimethylhexamethylene diisocyanate, etc. are preferred. As the hydroxy(meth)acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, caprolactane-modified 2-hydroxyethyl acrylate, etc. are preferred.
[0032] When the ionizing radiation curable resin composition contains a caprolactane polyol, the caprolactane urethane (meth)acrylate is preferably a caprolactane diol urethane (meth)acrylate. The caprolactane diol urethane (meth)acrylate refers to a urethane (meth)acrylate having a diethylene glycol terminal, among caprolactane urethane (meth)acrylates. By using the caprolactane diol urethane (meth)acrylate, it is possible to suppress the occurrence of cracks and whitening in the first protective layer.
[0033] The ionizing radiation curable resin composition may contain a hydroxyl group-containing (meth)acrylate as an ionizing radiation curable compound. Examples of the hydroxyl group-containing (meth)acrylate include hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, hydroxybutyl acrylate, hydroxybutyl methacrylate, 1,4-cyclohexane dimethanol monoacrylate, polyethylene glycol monoacrylate, polyethylene glycol monomethacrylate, trimethylolpropane diacrylate, trimethylolpropane dimethacrylate, pentaerythritol triacrylate, pentaerythritol trimethacrylate, dipentaerythritol hexaacrylate, dipentaerythritol hexamethacrylate, glycidyl acrylate, glycidyl methacrylate, isocyanuric acid monoacrylate, isocyanuric acid monomethacrylate, isocyanuric acid diacrylate, isocyanuric acid dimethacrylate, glycerin diacrylate, and glycerin dimethacrylate. The hydroxyl group-containing (meth)acrylate may be a hydroxyl group-containing (meth)acrylate modified with ethylene oxide (EO), propylene oxide (PO), caprolactone, etc. The proportion of the hydroxyl group-containing (meth)acrylate in the ionizing radiation curable resin composition is, for example, 10% by mass or more and 90% by mass or less.
[0034] The number average molecular weight of the ionizing radiation curable compound is, for example, from 200 to 10,000, may be from 1,000 to 10,000, or may be from 2,000 to 10,000. The number average molecular weight is an average molecular weight measured by GPC analysis and converted into standard polystyrene.
[0035] For example, when the ionizing radiation curable compound is an ultraviolet ray curable compound, the ionizing radiation curable compound preferably contains at least one of a photopolymerization initiator and a photopolymerization accelerator. Examples of the photopolymerization initiator include acetophenone, benzophenone, α-hydroxyalkylphenone, Michler's ketone, benzoin, benzyl dimethyl ketal, benzoyl benzoate, α-acyloxime ester, acylphosphine oxide, and thioxanthones. Examples of the photopolymerization accelerator include p-dimethylaminobenzoic acid isoamyl ester and p-dimethylaminobenzoic acid ethyl ester.
[0036] The first protective layer preferably contains a weathering agent. Examples of the weathering agent include an ultraviolet absorbing agent and a light stabilizer. The first protective layer preferably contains at least one of an ultraviolet absorbing agent and a light stabilizer. The first protective layer may contain one or more ultraviolet absorbing agents. Similarly, the first protective layer may contain one or more light stabilizers.
[0037] Examples of the ultraviolet absorbing agent contained in the first protective layer include organic ultraviolet absorbing agents such as triazine-based ultraviolet absorbing agents, benzotriazole-based ultraviolet absorbing agents, benzophenone-based ultraviolet absorbing agents, oxybenzophenone-based ultraviolet absorbing agents, salicylic acid ester-based ultraviolet absorbing agents, and cyano(meth)acrylate-based ultraviolet absorbing agents, and inorganic ultraviolet absorbing agents such as titanium dioxide, cerium oxide, and zinc oxide. Among these, triazine-based ultraviolet absorbing agents are more preferable.
[0038] Examples of triazine-based ultraviolet absorbers include hydroxyphenyl triazine-based ultraviolet absorbers. Examples of hydroxyphenyl triazine-based ultraviolet absorbers include 2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triazine, 2-[4-[(2-hydroxy-3-dodecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2,4-bis[2-hydroxy-4-butoxyphenyl]-6-(2,4-dibutoxyphenyl)-1,3,5-triazine, azine, 2-[4-[(2-hydroxy-3-tridecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-[4-[(2-hydroxy-3-(2'-ethyl)hexyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, and 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5[2-(2-ethylhexanoyloxy)ethoxy]phenol.
[0039] The content of the ultraviolet absorber in the first protective layer is, for example, 0.5 parts by mass to 10 parts by mass, alternatively 0.8 parts by mass to 8 parts by mass, or alternatively 1 part by mass to 5 parts by mass, relative to 100 parts by mass of the ionizing radiation curable compound. If the content of the ultraviolet absorber is high, bleeding out of the ultraviolet absorber may occur, whereas if the content of the ultraviolet absorber is low, sufficient ultraviolet absorbing performance may not be obtained.
[0040] The light stabilizer contained in the first protective layer may be, for example, a hindered amine light stabilizer. Examples of the hindered amine light stabilizer include 1,2,2,6,6-pentamethyl-4-piperidinyl methacrylate, bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate, bis(2,2,6,6-pentamethyl-4-piperidyl)sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidinyl)sebacate, methyl(1,2,2,6,6-pentamethyl-4-piperidinyl)sebacate, and 2,4-bis[N-butyl-N-(1-cyclohexyloxy-2,2,6,6-tetramethylpiperidin-4-yl)amino]-6-(2-hydroxyethylamine)-1,3,5-triazine).
[0041] The content of the light stabilizer in the first protective layer is, for example, 1 part by mass to 10 parts by mass, or may be 1.5 parts by mass to 8 parts by mass, or may be 2 parts by mass to 5 parts by mass, relative to 100 parts by mass of the ionizing radiation curable compound. If the content of the light stabilizer is high, bleeding out of the light stabilizer may occur, and if the content of the light stabilizer is low, sufficient light stability may not be obtained.
[0042] The first protective layer may contain additives such as silicone compounds, polymerization inhibitors, crosslinking agents, antistatic agents, adhesion improvers, antioxidants, leveling agents, thixotropy imparting agents, coupling agents, plasticizers, antifouling agents, defoamers, and fillers. The thickness of the first protective layer is, for example, 2 μm or more and 20 μm or less, 3 μm or more and 15 μm or less, or 4 μm or more and 10 μm or less. If the first protective layer is thin, sufficient weather resistance may not be obtained, and if the first protective layer is thick, cracks may easily occur in the first protective layer, and good adhesion may not be obtained.
[0043] (a-2) Second protective layer The transfer layer in the present disclosure preferably has a second protective layer on the side opposite to the release film of the first protective layer. The second protective layer is preferably a layer that is softer than the first protective layer. The second protective layer and the first protective layer may be disposed so as to be in direct contact with each other, or may be disposed via another layer.
[0044] The second protective layer preferably contains a cured product (crosslinked structure) of a curable resin composition as a resin component. The proportion of the cured product of the curable resin composition is, for example, 70% by mass or more, 90% by mass or more, 95% by mass or more, or 100% by mass, based on the total resin components constituting the second protective layer.
[0045] The curable resin composition used in the second protective layer may be, for example, a thermosetting resin composition. The thermosetting resin composition is a composition that contains at least a thermosetting resin, and is a composition that is cured by heating. Examples of the thermosetting resin include (meth)acrylic resins, phenolic resins, urea melamine resins, epoxy resins, unsaturated polyester resins, and silicone resins. The thermosetting resin composition preferably contains a urethane (meth)acrylic resin as the thermosetting resin. The thermosetting resin composition may further contain a curing agent such as an isocyanate curing agent or an epoxy curing agent.
[0046] In addition, when the curable resin composition contains a urethane (meth)acrylic resin, the urethane (meth)acrylic resin is preferably a urethane (meth)acrylic copolymer, more preferably a polycarbonate-based urethane (meth)acrylic copolymer. The polycarbonate-based urethane (meth)acrylic copolymer is a resin obtained by radically polymerizing a (meth)acrylic monomer with a polycarbonate-based polyurethane polymer obtained by reacting a polycarbonate diol with a (di)isocyanate.
[0047] Examples of the (di)isocyanate include aromatic isocyanates such as 4,4'-diphenylmethane diisocyanate, 2,4-tolylene diisocyanate, 1,5-naphthalene diisocyanate, n-isocyanate phenylsulfonyl isocyanate, o-isocyanate phenylsulfonyl isocyanate, and p-isocyanate phenylsulfonyl isocyanate; aliphatic isocyanates such as 1,6-hexamethylene diisocyanate; and alicyclic isocyanates such as isophorone diisocyanate, hydrogenated xylylene diisocyanate, and hydrogenated diphenylmethane diisocyanate.
[0048] Examples of the (meth)acrylic monomer include (meth)acrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, and isobutyl (meth)acrylate.
[0049] In the polycarbonate-based urethane (meth)acrylic copolymer, the mass ratio of the urethane component to the total of the (meth)acrylic component and the urethane component ([urethane component] / ([(meth)acrylic component]+[urethane component]) is, for example, 70 mass% or more and 95 mass% or less, alternatively 75 mass% or more and 95 mass% or less, or alternatively 80 mass% or more and 90 mass% or less.
[0050] The second protective layer preferably contains a weathering agent. Examples of weathering agents include ultraviolet absorbers and light stabilizers. The second protective layer preferably contains at least one of an ultraviolet absorber and a light stabilizer. The preferred types and modes of the weathering agent are the same as those described in "(a-1) First Protective Layer" above, and therefore will not be described here. In particular, the second protective layer preferably contains a triazine-based ultraviolet absorber. The second protective layer preferably contains a hindered amine-based light stabilizer.
[0051] The content of the ultraviolet absorber in the second protective layer is, for example, 0.1 parts by mass or more and 50 parts by mass or less, or may be 3 parts by mass or more and 40 parts by mass or less, or may be 10 parts by mass or more and 35 parts by mass or less, relative to 100 parts by mass of the resin component. The content of the ultraviolet absorber in the second protective layer (content relative to 100 parts by mass of the resin component) may be greater than the content of the ultraviolet absorber in the first protective layer (content relative to 100 parts by mass of the resin component).
[0052] The content of the light stabilizer in the second protective layer is, for example, 0.1 to 15 parts by mass, or 1 to 15 parts by mass, or 3 to 10 parts by mass, relative to 100 parts by mass of the resin component. The content of the light stabilizer in the second protective layer (content relative to 100 parts by mass of the resin component) may be greater than the content of the light stabilizer in the first protective layer (content relative to 100 parts by mass of the resin component).
[0053] The second protective layer may contain additives such as silicone compounds, polymerization inhibitors, crosslinking agents, antistatic agents, adhesion improvers, antioxidants, leveling agents, thixotropy imparting agents, coupling agents, plasticizers, antifouling agents, defoamers, and fillers. The thickness of the second protective layer is, for example, 2 μm to 10 μm, or 3 μm to 8 μm, or 3 μm to 5 μm. If the second protective layer is thin, the adhesion (particularly initial adhesion) with the relatively hard first protective layer may be reduced. On the other hand, if the second protective layer is thick, the movement of the second protective layer due to heat becomes large, and cracks are likely to occur in the first protective layer.
[0054] (b) Other layers The transfer layer in the present disclosure may or may not have a design layer on the side opposite to the release film of the protective layer. By providing a design layer, the design of the article is improved. The design layer and the protective layer may be arranged so as to be in direct contact with each other, or may be arranged via another layer.
[0055] Examples of the design layer include a solid layer (a layer coated with ink) and a pattern layer (a layer printed with ink). The transfer sheet may have a pattern layer and a solid layer in this order from the release film side as the design layer. Examples of the pattern in the pattern layer include wood grain, stone grain, sand grain, tiled pattern, brickwork pattern, cloth grain pattern, leather-squeezed pattern, geometric figures, letters, symbols, abstract patterns, and floral patterns.
[0056] The design layer usually contains a colorant and a binder resin. Examples of the colorant include inorganic pigments such as carbon black (ink), iron black, titanium white, antimony white, yellow lead, titanium yellow, red iron oxide, cadmium red, ultramarine blue, and cobalt blue, organic pigments (including dyes) such as quinacridone red, isoindolinone yellow, nickel azo complex, phthalocyanine blue, and azomethine azo black, metal pigments such as aluminum and brass, and pearl pigments such as titanium dioxide-coated mica and basic lead carbonate.
[0057] Examples of binder resins include urethane-based resins, acrylic polyol-based resins, (meth)acrylic resins, ester-based resins, amide-based resins, butyral-based resins, styrene-based resins, urethane-acrylic copolymers, vinyl chloride-vinyl acetate copolymers, vinyl chloride-vinyl acetate-acrylic copolymers, chlorinated propylene-based resins, nitrocellulose-based resins, and cellulose acetate-based resins.
[0058] The design layer may contain additives such as ultraviolet absorbers, light stabilizers, hardeners, plasticizers, catalysts, etc., as necessary. The thickness of the design layer is, for example, 0.5 μm or more and 20 μm or less, or may be 1 μm or more and 10 μm or less, or may be 2 μm or more and 5 μm or less.
[0059] The transfer layer in the present disclosure may or may not have an adhesive layer on the surface of the protective layer opposite to the release film. The adhesive layer and the protective layer may be arranged so as to be in direct contact with each other, or may be arranged via another layer (e.g., a design layer). The adhesive layer may contain a component having adhesive properties. Examples of the component having adhesive properties include (meth)acrylic resins, vinyl chloride-vinyl acetate copolymers, vinyl acetate resins, ester resins, epoxy resins, imide resins, and rubber resins.
[0060] The adhesive layer may be a so-called pressure-sensitive adhesive layer. The adhesive layer has pressure-sensitive adhesiveness at room temperature. Examples of the resin contained in the adhesive layer include (meth)acrylic resin, vinyl resin, ester resin, urethane resin, amide resin, epoxy resin, rubber resin, and ionomer resin. The adhesive layer may be a so-called heat seal layer. The heat seal layer exhibits pressure-sensitive adhesiveness by heat. Examples of the resin contained in the heat seal layer include (meth)acrylic resin, urethane resin, olefin resin, ester resin, epoxy resin, urea resin, melamine resin, phenol resin, and vinyl resin. The thickness of the adhesive layer is, for example, 1 μm or more and 30 μm or less.
[0061] (c) Transfer layer The thickness of the transfer layer is, for example, 8 μm or more, and may be 10 μm or more, 12 μm or more, or 14 μm or more, while the thickness of the transfer layer is, for example, 50 μm or less, and may be 40 μm or less, or 30 μm or less.
[0062] (ii) Release film The transfer sheet in the present disclosure has a release film facing the transfer layer.
[0063] The release film is preferably a resin film. Examples of the resin contained in the resin film include ester resins, olefin resins, styrene resins, vinyl resins, (meth)acrylic resins, amide resins, imide resins, and carbonate resins.
[0064] The release film preferably contains an ester-based resin or an olefin-based resin. Examples of ester-based resins include polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyethylene naphthalate (PEN), and polyethylene terephthalate-isophthalate copolymers. Among these, PET or PBT is preferred, and PET is more preferred, from the viewpoint of being less susceptible to thermal shrinkage during the production of the transfer sheet and shrinkage due to irradiation with ionizing radiation.
[0065] Examples of olefin resins include polyethylene, polypropylene, polybutene, ethylene-propylene copolymer, and ethylene-propylene-butene copolymer. Among these, polypropylene is preferred from the viewpoint of being less susceptible to thermal shrinkage during the production of the transfer sheet and to shrinkage due to irradiation with ionizing radiation. The release film may be, for example, a paper processed with polypropylene (PP).
[0066] The release film may be a stretched film or an unstretched film. The stretch ratio in the machine direction (MD) of the stretched film is, for example, 5 times or more and 30 times or less. The stretch ratio in the width direction (TD) of the stretched film is, for example, 5 times or more and 30 times or less. The thickness of the release film is, for example, 10 μm or more and 200 μm or less, may be 15 μm or more and 150 μm or less, or may be 20 μm or more and 100 μm or less.
[0067] The release film may contain a matting agent kneaded therein. A part of the kneaded matting agent is usually exposed from the release film. By adding a matting agent to the release film, the peel strength of the release film and the transfer layer can be adjusted. Examples of the matting agent include inorganic particles and organic particles. Examples of the inorganic particles include silica, alumina, calcium carbonate, magnesium carbonate, calcium sulfate, barium sulfate, and kaolin. Examples of the organic particles include acrylic beads, urethane beads, nylon beads, silicone beads, silicone rubber beads, polycarbonate beads, and polyolefin wax (e.g., polypropylene wax, polyethylene wax). The average particle size of the matting agent is, for example, 1.0 μm or more and 10 μm or less, and may be 2.0 μm or more and 8.0 μm or less. The average particle size of the matting agent is determined by the D 50 This refers to.
[0068] The release film may have a mat layer containing a mat agent on the surface on the transfer layer side. The mat agent used in the mat layer is the same as described above. The mat layer may also contain a cured product (crosslinked structure) of a curable resin composition as a resin component. Examples of the curable resin composition used in the mat layer include an ionizing radiation curable resin composition and a thermosetting resin composition. Details of the ionizing radiation curable resin composition and the thermosetting resin composition are the same as described above. The mat layer may also contain a thermoplastic resin as a resin component. The mat layer may contain additives such as a release agent, an ultraviolet absorber, an infrared absorber, a light stabilizer, a polymerization inhibitor, a crosslinking agent, an antistatic agent, an antioxidant, a leveling agent, a coupling agent, a plasticizer, a defoamer, a filler, a thermal radical generator, and an aluminum chelating agent, as necessary. The thickness of the mat layer is not particularly limited, but is, for example, 0.1 μm or more and 10 μm or less.
[0069] (iii) Transfer sheet The transfer sheet in the present disclosure has a release film (first release film) and a transfer layer. The transfer sheet may have a second release film on the side of the transfer layer opposite to the release film. For example, when the transfer sheet is wound into a roll, the occurrence of blocking can be suppressed. Details of the second release film are the same as those described above for the first release film, so the description here is omitted.
[0070] (iv) Method for preparing transfer sheet The method of producing the transfer sheet in the present disclosure is not particularly limited. For example, when producing the transfer sheet shown in FIG. 1(a), it is preferable to form a first protective layer 2 on one side of a release film 1, and then form a second protective layer 3 on the side of the first protective layer 2 opposite to the release film 1. Also, when producing the transfer sheet shown in FIG. 1(b), it is preferable to form a first protective layer 2 on one side of a release film 1, then form a second protective layer 3 on the side of the first protective layer 2 opposite to the release film 1, and then form a design layer 4 on the side of the second protective layer 3 opposite to the first protective layer 2.
[0071] The method for forming the first protective layer may be, for example, a method of applying a composition for forming the first protective layer to the surface of a release film and curing the composition. The method for applying the composition may be, for example, a gravure printing method, a bar coating method, a roll coating method, a reverse roll coating method, or a comma coating method. The curing method may be, for example, a method of irradiating ionizing radiation such as an electron beam or ultraviolet light.
[0072] The method for forming the second protective layer may, for example, be a method of applying a composition for forming the second protective layer to the surface of the first protective layer opposite to the release film, and curing it as necessary. The method for applying the composition may, for example, be a gravure printing method, a bar coating method, a roll coating method, a reverse roll coating method, or a comma coating method. The curing method may, for example, be heat. The method for forming the design layer may, for example, be a method of applying an ink containing a colorant, a binder resin, and a solvent to the surface of the second protective layer opposite to the first protective layer.
[0073] (2) Adherent An example of the adherend in the present disclosure is a metal member. The metal member and the resin contained in the transfer layer are different materials, so the adhesion between them is likely to be low. In this case, the adhesion between the adherend and the transfer layer can be improved by adhering the adherend and the transfer layer, for example, via an adhesive layer described later. In particular, exterior products (items for outdoor use) are exposed to harsh environments, so it is desirable for the adhesion between the adherend and the transfer layer to be high.
[0074] The metal member is a member containing a simple metal or a metal alloy. Examples of metals used for the metal member include aluminum, iron, steel, and copper. The metal member is preferably an aluminum member. This is because aluminum members are lightweight and have excellent corrosion resistance, and are useful as adherends for exterior products (items for outdoor use). The aluminum member is a member containing aluminum or an aluminum alloy. The aluminum member preferably has an aluminum oxide coating on the surface. This is because the corrosion resistance of the aluminum member is improved. Examples of methods for forming the aluminum oxide coating include anodizing.
[0075] Another example of the adherend is a resin member. Examples of the resin used in the resin member include polycarbonate resin, vinyl chloride resin, acrylic resin, ester resin, styrene resin, olefin resin, acrylonitrile-butadiene-styrene copolymer (ABS resin), phenol resin, cellulose resin, and rubber. Another example of the adherend is a wood member. Examples of the wood member include a wood veneer, wood plywood, particle board, and wood fiber board. Examples of wood used in the wood member include cedar, cypress, pine, and lauan. Another example of the adherend is a ceramic member. The material of the ceramic member may be glass, ceramics, or other ceramics, non-cement ceramic materials such as gypsum, or non-ceramic ceramic materials such as ALC (lightweight aerated concrete).
[0076] The shape of the adherend is not particularly limited, but examples thereof include a plate shape, a sheet shape, and a three-dimensional shape. A three-dimensional shape is a three-dimensional shape expressed by the coordinates of the X-axis, the Y-axis, and the Z-axis. The adherend has multiple surfaces. The above surfaces may be flat or curved. Details of the multiple surfaces of the adherend will be described later in "3. Wrapping process".
[0077] 2.Adhesive layer formation process The adhesive layer forming step in the present disclosure is a step of forming an adhesive layer on the surface of the transfer layer opposite to the release film or on the multiple surfaces of the adherend. The method for manufacturing an article in the present disclosure preferably includes an adhesive layer forming step after the preparation step and before the wrapping step described below.
[0078] The adhesive used in the adhesive layer is not particularly limited, and known adhesives can be used. Examples of adhesives include heat-sensitive adhesives and pressure-sensitive adhesives. Examples of resins used in the adhesive include acrylic resins, urethane resins, vinyl chloride resins, vinyl acetate resins, ester resins, amide resins, vinyl chloride-vinyl acetate copolymers, and styrene-acrylic copolymers. In addition, two-liquid curing polyurethane adhesives using an isocyanate compound as a curing agent and polyester adhesives may be used as the adhesive. In addition, the adhesive is preferably a solvent-based adhesive or a polyurethane reactive (PUR) adhesive.
[0079] In the adhesive layer forming step, the adhesive layer coating liquid may be applied to the surface of the transfer layer of the transfer sheet opposite to the release film to form an adhesive layer. In this case, there is an advantage that the adhesive layer coating liquid can be uniformly applied to the transfer sheet. On the other hand, in the adhesive layer forming step, the adhesive layer coating liquid may be applied to multiple surfaces of the adherend to form an adhesive layer. In this case, there is an advantage that the effect of thermal shrinkage of the adhesive is less likely to occur.
[0080] The viscosity of the adhesive layer coating liquid is, for example, 3,000 mPa·s or more and 30,000 mPa·s or less. Examples of the coating method of the adhesive layer coating liquid include a slot die method, a gravure direct method, a gravure reverse method, a microgravure method, and a knife coating method. When applying the adhesive layer coating liquid, the adhesive layer coating liquid may be heated. In particular, when the adhesive layer coating liquid contains a PUR adhesive, it is preferable to heat the adhesive layer coating liquid. The heating temperature of the adhesive layer coating liquid is, for example, 80°C or more and 160°C or less. After applying the adhesive layer coating liquid, the formed coating layer may be dried. The drying temperature is, for example, 50°C or more and 100°C or less.
[0081] The thickness of the adhesive layer is not particularly limited, but may be, for example, 2 μm to 100 μm, 2 μm to 50 μm, or 2 μm to 35 μm. For example, when the transfer sheet has the above-mentioned adhesive layer, the adhesive layer forming step may not be performed.
[0082] 3. Wrapping process The wrapping process in the present disclosure is a process of sequentially laminating the transfer layer of the transfer sheet to the multiple surfaces of the adherend using a roller. "Sequential lamination" refers to laminating a transfer sheet to one surface of the adherend, and then laminating a transfer sheet to a surface adjacent to the surface to which the transfer sheet was laminated. Usually, the operation of laminating a transfer sheet to a surface adjacent to the surface to which the transfer sheet was laminated is repeated. For example, a transfer sheet is laminated to a first surface of the adherend, then a transfer sheet is laminated to a second surface adjacent to the first surface, and then a transfer sheet is laminated to a third surface adjacent to the second surface.
[0083] The multiple surfaces of the adherend are preferably surfaces extending in the longitudinal direction of the adherend. In the lapping process, a single roller may be used to sequentially attach the transfer sheet to the multiple surfaces of the adherend, or multiple rollers may be used to sequentially attach the transfer sheet to the multiple surfaces of the adherend. In the lapping process, it is preferable to fix the position of the roller and transport the adherend and the transfer sheet.
[0084] As shown in FIG. 3, in the lapping process, the adherend 20 is wrapped in a wrapping paper in the longitudinal direction D L It is preferable to sequentially laminate the transfer layer X of the transfer sheet 10 to multiple surfaces of the adherend 20 using multiple rollers 60 (60a to 60e) while conveying the adherend 20 along the track. In the wrapping process, the transfer layer X of the transfer sheet 10 is laminated to one surface of the adherend 20 using the rollers 60, and then the transfer layer X of the transfer sheet 10 is laminated to the other surface of the adherend 20 using the rollers 60 successively.
[0085] As shown in Fig. 4(a), the first roller 60a is pressed against the first surface S1 of the adherend 20 via the transfer sheet 10. This causes the transfer sheet 10 (transfer layer X) to be attached to the first surface S1 of the adherend 20. Although not shown in particular, it is preferable that the above-mentioned adhesive layer is formed between the adherend and the transfer sheet (transfer layer). In Fig. 4(a), the axial direction A1 of the first roller 60a is horizontal.
[0086] Next, as shown in Fig. 4(b), the transfer sheet 10 is guided so as to be folded by the first guide rollers 60b, 60b', and then, as shown in Fig. 4(c), the second rollers 60c, 60c' are pressed against the second surfaces S2, S2' of the adherend 20 via the transfer sheet 10, respectively. This causes the transfer sheet 10 (transfer layer X) to be attached to the second surfaces S2, S2' of the adherend 20. In Fig. 4(c), the axial directions A2, A2' of the second rollers 60c, 60c' are vertical.
[0087] Next, as shown in Fig. 4(d), the transfer sheet 10 is guided to be folded by the second guide roller 60d, and then, as shown in Fig. 4(e), the third roller 60e is pressed against the third surface S3 of the adherend 20 via the transfer sheet 10. This causes the transfer sheet 10 (transfer layer X) to be attached to the third surface S3 of the adherend 20. In Fig. 4(e), the axial direction A3 of the third roller 60e is horizontal.
[0088] (1) First roller, first guide roller and second roller 4(a) to (c), the adherend 20 preferably has a first surface S1 extending in the longitudinal direction (depth direction of the paper) and a second surface S2 extending in the longitudinal direction and in contact with the first surface S1. The first roller 60a is a roller for pressing the transfer sheet 10 against the first surface S1 of the adherend 20. Similarly, the second roller 60c is a roller for pressing the transfer sheet 10 against the second surface S2 of the adherend 20. Meanwhile, the first guide roller 60b is a roller disposed between the first roller 60a and the second roller 60c.
[0089] That is, the transfer sheet 10 is pressed against the first surface S1 of the adherend 20 using the first roller 60a, then the transfer sheet 10 is guided to the second surface S2 of the adherend 20 using the first guide roller 60b, and then the transfer sheet 10 is pressed against the second surface S2 of the adherend 20 using the second roller 60c. Alternatively, as shown in Figs. 4(b) and (c), the transfer sheet 10 may be attached simultaneously to the second surface S2 and the second surface S2' that are in contact with the first surface S1. In this case, it is preferable to use the first guide roller 60b' and the second roller 60c'.
[0090] As shown in Figs. 4(a) to (c) and 5(a), the axial direction A1 of the first roller 60a and the axial direction A2 of the second roller 60c usually intersect. The axial direction A1 may be a horizontal direction, a vertical direction, or any direction between the horizontal direction and the vertical direction. The angle formed by the axial direction A1 and the axial direction A2 is not particularly limited, and may be, for example, 30° or more, 45° or more, or 60° or more. Meanwhile, the angle is usually less than 180°, and may be 150° or less, or 120° or less.
[0091] As shown in FIG. 5(a), the angle from the axial direction A1 of the first roller to the axial direction A2 of the second roller is defined as θ 12 The axial direction A1 of the first roller to the axial direction A of the first guide roller M The angle to 1MThe above angle (central angle) is an angle in the same circumferential direction. 12 and θ 1M θ 12 >θ 1M It is preferable that the above condition is satisfied. By gradually changing the axial direction of each roller along the longitudinal direction of the adherend 20, it is possible to further suppress the occurrence of cracks in the transfer layer when the transfer layer is transferred to the adherend.
[0092] As shown in FIG. 4(a), the number of first rollers 60a pressing the transfer sheet 10 against the first surface S1 of the adherend 20 may be one. On the other hand, as shown in FIGS. 6(a) and 6(b), the number of first rollers 60a pressing the transfer sheet 10 against the first surface S1 of the adherend 20 may be two or more. In FIG. 6(a), the first roller 60a1 presses the transfer sheet 10 against the first surface S1 at the center of the first surface S1 of the adherend 20. Then, in FIG. 6(b), the first rollers 60a2 and 60a2′ press the transfer sheet 10 against the first surface S1 at the end side of the center of the first surface S1 of the adherend 20. In this way, it is preferable that the region where the two or more first rollers 60a press the transfer sheet 10 changes from the center of the first surface S1 to the end of the first surface S1 from the upstream to the downstream in the longitudinal direction. By using two or more first rollers, the occurrence of wrinkles can be effectively suppressed.
[0093] As shown in Figs. 4(a) to (c), the number of first guide rollers 60b arranged between the first roller 60a and the second roller 60c in the longitudinal direction (depth direction of the paper) of the adherend 20 may be one. On the other hand, as shown in Figs. 6(c) and (d), the number of first guide rollers 60b arranged between the first roller 60a and the second roller 60c in the longitudinal direction (depth direction of the paper) of the adherend 20 may be multiple. In Fig. 6(c), the first guide roller 60b1 is used to guide the transfer sheet 10 to the second surface S2 side of the adherend 20, and then, in Fig. 6(d), the first guide roller 60b2 is used to further fold the transfer sheet 10 to the second surface S2 side of the adherend 20. By using two or more first guide rollers, the occurrence of wrinkles can be effectively suppressed.
[0094] When there are multiple first guide rollers, the axial direction A1 of the first roller is the axial direction A of two or more first guide rollers. M 6(a), (c), and (d), the axial direction of the first roller 60a is A1, the axial direction of the first guide roller 60b1 is A2, and the axial direction of the first guide roller 60b2 is A3. M1 The axial direction of the first guide roller 60b2 is A M2 As shown in FIG. 5B, the axial direction A1 of the first roller 60b1 is M1 The angle to 1M1 The axial direction A1 of the first roller 60b2 is M2 The angle to 1M2 In this disclosure, θ 1M1 and θ 1M2 θ 1M2 >θ 1M1 It is preferable that the above condition is satisfied. By gradually changing the axial direction of each guide roller along the longitudinal direction of the adherend, it is possible to further suppress the occurrence of cracks in the transfer layer when the transfer layer is transferred to the adherend.
[0095] As shown in FIG. 4(c), the number of second rollers 60c pressing the transfer sheet 10 against the second surface S2 of the adherend 20 may be one. On the other hand, as shown in FIGS. 6(e) to 6(g), the number of second rollers 60c pressing the transfer sheet 10 against the second surface S2 of the adherend 20 may be two or more. In FIG. 6(e), the second roller 60c1 presses the transfer sheet 10 against the second surface S2 at the end of the second surface S2 of the adherend 20 on the first surface S1 side. Then, in FIG. 6(f), the second roller 60c2 presses the transfer sheet 10 against the second surface S2 at the center of the second surface S2 of the adherend 20. Then, in FIG. 6(g), the second roller 60c3 presses the transfer sheet 10 against the second surface S2 at the end of the second surface S2 of the adherend 20 opposite to the first surface S1. In this way, it is preferable that the area where the two or more second rollers 60c press the transfer sheet 10 changes from the end of the second surface S2 on the first surface S1 side to the end of the second surface S2 on the opposite side to the first surface S1 from the upstream to downstream in the longitudinal direction. By using two or more second rollers, the occurrence of wrinkles can be effectively suppressed.
[0096] (2) Second roller, second guide roller, and third roller 4(c) to (e), it is preferable that the adherend 20 extends in the longitudinal direction (depth direction of the paper) and further has a third surface S3 in contact with the second surface S2. The third roller 60e is a roller for pressing the transfer sheet 10 against the third surface S3 of the adherend 20. Meanwhile, the second guide roller 60d is a roller disposed between the second roller 60c and the third roller 60e.
[0097] That is, the transfer sheet 10 is pressed against the second surface S2 of the adherend 20 using the second roller 60c, then the transfer sheet 10 is guided toward the third surface S3 of the adherend 20 using the second guide roller 60d, and then the transfer sheet 10 is pressed against the third surface S3 of the adherend 20 using the third roller 60e.
[0098] As shown in Figs. 4(c) to (e) and 5(a), the axial direction A2 of the second roller 60c and the axial direction A3 of the third roller 60e usually intersect. The axial direction A2 may be horizontal, vertical, or any direction between the horizontal and vertical directions. The angle between the axial direction A2 and the axial direction A3 is not particularly limited, but may be, for example, 30° or more, 45° or more, or 60° or more. Meanwhile, the angle is usually less than 180°, and may be 150° or less, or 120° or less.
[0099] As shown in FIG. 5(a), the angle from the axial direction A2 of the second roller to the axial direction A3 of the third roller is defined as θ 23 The axial direction A from the axial direction A2 of the second roller to the axial direction A of the second guide roller N The angle to 2N The above angle (central angle) is an angle in the same circumferential direction. 23 and θ 2N θ 23 >θ 2N It is preferable that the above condition is satisfied. By gradually changing the axial direction of each roller along the longitudinal direction of the adherend 20, it is possible to further suppress the occurrence of cracks in the transfer layer when the transfer layer is transferred to the adherend.
[0100] As shown in Fig. 4(c) to (e), the number of second guide rollers 60d arranged between the second roller 60c and the third roller 60e in the longitudinal direction (depth direction of the paper) of the adherend 20 may be one. On the other hand, as shown in Fig. 7(a) and (b), the number of second guide rollers 60d arranged between the second roller 60c and the third roller 60e in the longitudinal direction (depth direction of the paper) of the adherend 20 may be multiple. In Fig. 7(a), the second guide roller 60d1 is used to guide the transfer sheet 10 to the third surface S3 side of the adherend 20, and then, in Fig. 7(b), the second guide roller 60d2 is used to further fold the transfer sheet 10 to the third surface S3 side of the adherend 20. By using two or more second guide rollers, the occurrence of wrinkles can be effectively suppressed.
[0101] When there are multiple second guide rollers, the axial direction A2 of the second roller is the axial direction A of two or more second guide rollers. N As shown in Fig. 6(g), Fig. 7(a) and (b), the axial direction of the second roller 60c is A2, and the axial direction of the second guide roller 60d1 is A N1 The axial direction of the second guide roller 60d2 is A N2 As shown in FIG. 5B, the axial direction A2 of the second roller is aligned along the axial direction A of the second guide roller 60d1. N1 The angle to 2N1 The axial direction A2 of the second roller is set to the axial direction A N2 The angle to 2N2 In this disclosure, θ 2N1 and θ 2N2 θ 2N2 >θ 2N1 It is preferable that the above condition is satisfied. By gradually changing the axial direction of each guide roller along the longitudinal direction of the adherend, it is possible to further suppress the occurrence of cracks in the transfer layer when the transfer layer is transferred to the adherend.
[0102] As shown in FIG. 4(e), the number of third rollers 60e pressing the transfer sheet 10 against the third surface S3 of the adherend 20 may be one. On the other hand, as shown in FIGS. 7(c) to 7(e), the number of third rollers 60e pressing the transfer sheet 10 against the third surface S3 of the adherend 20 may be two or more. In FIG. 7(c), the third roller 60e1 presses the transfer sheet 10 against the third surface S3 at the end of the third surface S3 of the adherend 20 on the second surface S2 side. Then, in FIG. 7(d), the third roller 60e2 presses the transfer sheet 10 against the third surface S3 at the center of the third surface S3 of the adherend 20. Then, in FIG. 7(e), the third roller 60e3 presses the transfer sheet 10 against the third surface S3 at the end of the third surface S3 of the adherend 20 on the opposite side to the second surface S2. In this way, it is preferable that the area where the two or more third rollers 60e press the transfer sheet 10 changes from the end of the third surface S3 on the second surface S2 side to the end of the third surface S3 on the opposite side to the second surface S2 from the upstream to downstream in the longitudinal direction. By using two or more third rollers, the occurrence of wrinkles can be effectively suppressed.
[0103] Among the multiple surfaces of the adherend, the surface to which the transfer sheet is attached is defined as the Nth surface (N≧4). The Nth surface is a surface that extends in the longitudinal direction and is in contact with the (N-1)th surface. In this case, the multiple rollers preferably include a (N-1)th roller that presses the transfer sheet against the (N-1)th surface, an Nth roller that is disposed downstream of the (N-1) roller in the longitudinal direction and presses the transfer sheet against the Nth surface, and an (N-1)th guide roller that is disposed between the (N-1)th roller and the Nth roller. The (N-1)th roller, the (N-1)th guide roller, and the Nth roller are the same as those described above for each roller and each guide roller, so that the description here is omitted. In the wrapping process, the transfer sheet may be attached to a part of the multiple surfaces extending in the longitudinal direction, or the transfer sheet may be attached to all of the multiple surfaces extending in the longitudinal direction.
[0104] (3) Outer shape of the cross section of the adherend The outer edge shape of the cross section (cross section normal to the longitudinal direction) of the adherend in the present disclosure is not particularly limited, but examples thereof include polygonal shapes such as triangles and rectangles, and circular shapes such as circles and ellipses. Examples of quadrilateral shapes include squares, rectangles, trapezoids, and rhombuses. For example, the outer edge shape of the cross section of the adherend 20 shown in FIG. 2(b) is a square. On the other hand, the outer edge shape of the cross section of the adherend 20 shown in FIG. 8(a) is a trapezoid, and the outer edge shape of the cross section of the adherend 20 shown in FIG. 8(b) is a hexagon. In addition, the cross section of the adherend may be solid or hollow.
[0105] The first surface of the adherend is appropriately set according to the outer edge shape of the cross section of the adherend. For example, as shown in FIG. 9(a), the top surface of the adherend 20 may be set as the first surface S1. Alternatively, as shown in FIG. 9(b), the side surface of the adherend 20 may be set as the first surface S1. Although not shown, the bottom surface of the adherend may be set as the first surface. As shown in FIGS. 4(a) to 4(c), after the transfer sheet 10 is attached to the first surface S1 of the adherend 20, both of the two surfaces adjacent to the first surface S1 may be set as the second surfaces S2 and S2', and the transfer sheet 10 may be attached to those surfaces simultaneously. On the other hand, as shown in Figures 9(a) and (b), after a transfer sheet (not shown) is attached to the first surface S1 of the adherend 20, one of the two surfaces adjacent to the first surface S1 may be set as the second surface S2, and the other may be set as the surface to which the transfer sheet is finally attached (the fourth surface S4 in Figures 9(a) and (b)).
[0106] As shown in FIG. 2(b), the third surface S3 may be a surface facing the first surface S1. The "surface facing the first surface S1" refers to a surface having an area overlapping at least a part of the first surface S1 when viewed from the normal direction of the first surface S1. On the other hand, as shown in FIG. 10(a), the third surface S3 does not have to be a surface facing the first surface S1. In such a case, as shown in FIG. 10(b), it is not necessary to use a second guide roller between the second roller (a roller that presses the transfer sheet against the second surface S2) and the third roller (a roller that presses the transfer sheet against the third surface S3).
[0107] In the wrapping process, the transfer sheet may be supplied from a roll of the original sheet of the transfer sheet. The supply speed of the transfer sheet is, for example, 3 m / min or more and 50 m / min or less. Supplying the transfer sheet from the original roll enables continuous production and improves productivity. The tension when supplying the transfer sheet is not particularly limited. In addition, in the wrapping process, the adherend may be heated. The adherend may be heated before the transfer sheet is bonded. That is, the transfer sheet may be bonded to the heated adherend. In addition, the adherend and the transfer sheet may be heated at the same time as the transfer sheet is bonded to the adherend. Specifically, a heated roller may be used. The heating temperature of the roller is, for example, 200° C. or less, and may be 180° C. or less. If the heating temperature is high, the transfer sheet may be softened more than necessary. On the other hand, the heating temperature of the roller is, for example, 100° C. or more, may be 110° C. or more, or may be 120° C. or more.
[0108] Fig. 11(a) is a schematic cross-sectional view corresponding to region α in Fig. 4(e). As shown in Fig. 11(a), an article with a release film 50 having at least a transfer sheet 10 and an adherend 20 is obtained by a wrapping process. Moreover, as shown in Fig. 11(a), the article with a release film 50 preferably has an adhesive layer 30 between the transfer sheet 10 and the adherend 20. Moreover, the article with a release film 50 shown in Fig. 11(a) is obtained by wrapping the release film 1, the transfer layer X, the adhesive layer 30 and the adherend 20 in a thickness direction D. T In this order,
[0109] The method for manufacturing an article according to the present disclosure may include a peeling step of peeling the release film from the transfer layer after the wrapping step. As shown in FIG. 11(b), the peeling step provides an article 100 having at least the transfer layer X and the adherend 20. Also, as shown in FIG. 11(b), the article 100 preferably has an adhesive layer 30 between the transfer layer X and the adherend 20. Also, the article 100 shown in FIG. 11(b) has the transfer layer X, the adhesive layer 30, and the adherend 20 arranged in a thickness direction D. TIn this order,
[0110] 4. Manufacturing method of the article The manufacturing method of the article in the present disclosure includes the above-mentioned steps. FIG. 12 is an explanatory diagram for explaining a manufacturing line for carrying out the manufacturing method of the article in the present disclosure. In FIG. 12, the transfer sheet 10 is supplied from the original roll 11, and the transfer sheet 10 is transported using a plurality of guide rollers 80. During the transport of the transfer sheet 10, a coating liquid for forming an adhesive layer is applied from a coating device 72 to the transfer layer X of the transfer sheet 10 supported by a roll 71, and the adhesive layer (not shown) is formed by drying the transfer layer X by a drying device 73. Meanwhile, the adherend 20 is transported in the longitudinal direction using a transport device 74, and the transfer sheet 10 is sequentially bonded to a plurality of surfaces of the adherend 20 in a wrapping processing device 75 having a plurality of rollers 60.
[0111] The article in the present disclosure has an adherend having a plurality of surfaces and a transfer layer disposed so as to follow the plurality of surfaces. An adhesive layer may be disposed between the adherend and the transfer layer. The article in the present disclosure is used, for example, as a building material. The building material is used, for example, in buildings such as houses, offices, stores, hospitals, and clinics. The article may be an exterior product (an article for outdoor use) or an interior product (an article for indoor use). Specific examples of the article include exterior walls, roofs, eaves ceilings, louvers, door pockets, window frames, doors, door frames, handrails, fences, and drying racks.
[0112] The present disclosure is not limited to the above-described embodiments. The above-described embodiments are merely examples, and anything that has substantially the same configuration as the technical idea described in the claims of the present disclosure and exhibits similar effects is included in the technical scope of the present disclosure. EXAMPLES
[0113] (Preparation of transfer sheet) A mirror-finished polyester film (thickness: 38 μm) that had not been subjected to an easy-adhesion treatment was prepared as a release film. The composition for forming the first protective layer described below was applied to one side of the release film by gravure coating to form an uncured resin layer. Then, the composition was irradiated with 50 kGy of electron beams at an acceleration voltage of 165 kV to cure the composition, thereby forming a first protective layer having a thickness of 5 μm. Then, the surface of the first protective layer opposite to the release film was irradiated with corona radiation. <Composition for forming first protective layer> ·Ionizing radiation curable resin composition: 100 parts by mass Caprolactam-based urethane acrylate: 30 parts by weight Pentaerythritol triacrylate (hydroxyl group-containing acrylate): 70 parts by mass UV absorber: 2 parts by weight (product name: TINUVIN479, BASF) Light stabilizer with reactive functional groups: 2 parts by weight (product name: Sanol LS-3410, Nippon Nyukazai Co., Ltd.)
[0114] Next, the composition for forming the second protective layer described below was applied by gravure coating onto the corona-irradiated surface of the first protective layer, and dried to form a second protective layer having a thickness of 3.5 μm. <Composition for forming second protective layer> Polycarbonate-based urethane acrylic copolymer: 100 parts by weight UV absorber: 17 parts by weight (product name: TINUVIN400, BASF) UV absorber: 13 parts by weight (product name: TINUVIN479, BASF) Hindered amine light stabilizer: 8 parts by weight (product name: TINUVIN123, BASF) Anti-blocking agent: 9 parts by weight (silica particles, average particle size 3 μm) Hardener: 25 parts by weight (hexamethylene diisocyanate)
[0115] Next, the ink for forming the design layer described below was applied to the surface of the obtained second protective layer by gravure coating and dried to form the design layer. This resulted in a transfer sheet having a release film, a first protective layer, a second protective layer, and a design layer in this order in the thickness direction. The obtained transfer sheet was wound into a roll to form a raw roll. <Ink for forming design layer> ·Resin composition: 100 parts by mass Acrylic resin: 80 parts by weight Vinyl chloride-vinyl acetate copolymer: 20 parts by weight Pigments
[0116] (Production of goods) In the same manner as in Figs. 6, 7 and 12, the transfer layer X of the transfer sheet 10 described above was sequentially bonded to the multiple surfaces S (S1, S2, S2', S3 in Fig. 2(b)) of the adherend 20 using multiple rollers. Specifically, a square piece of aluminum material with a cross section of 4.0 cm x 4.0 cm and a length of 2.0 m was prepared as the adherend 20. Next, the transfer sheet 10 was supplied from the original roll, and an adhesive layer (not shown) was formed by applying an adhesive layer coating liquid to the surface of the transfer layer X opposite to the release film 1 and drying it, and the transfer layer X of the transfer sheet 10 and the adherend 20 were bonded to each other via the adhesive layer using multiple rollers. As the multiple rollers, multiple first rollers 60a, multiple first guide rollers 60b, multiple second rollers 60c, multiple second guide rollers 60d, and multiple third rollers 60e were used. After the transfer layer X of the transfer sheet 10 was attached to the multiple surfaces S (S1, S2, S2', S3) of the adherend 20, the release film 1 was peeled off from the transfer layer X to obtain an article. When the transfer layer X of the obtained article was visually inspected, it was confirmed that no cracks had occurred in the transfer layer.
[0117] Thus, in the present disclosure, for example, the following inventions are provided:
[0118] [1] A preparation step of preparing an adherend having a plurality of surfaces and a transfer sheet having a release film and a transfer layer; a lapping process step of sequentially laminating the transfer layer of the transfer sheet to the multiple surfaces of the adherend using a roller; The method for manufacturing an article comprising the steps of:
[0119] [2] A plurality of the rollers are arranged along the longitudinal direction of the adherend, The adherend has a first surface extending in the longitudinal direction and a second surface extending in the longitudinal direction and in contact with the first surface, the plurality of rollers include a first roller that presses the transfer sheet against the first surface, a second roller that is disposed downstream of the first roller in the longitudinal direction and presses the transfer sheet against the second surface, and a first guide roller that is disposed between the first roller and the second roller; When viewed from the longitudinal direction, an axial direction A1 of the first roller and an axial direction A2 of the second roller intersect with each other, When viewed from the longitudinal direction, the angle from the axial direction A1 of the first roller to the axial direction A2 of the second roller is defined as θ 12 and the axial direction A from the axial direction A1 of the first roller to the first guide roller M The angle to 1M In this case, the above θ 12 and the above θ 1M θ 12 >θ 1M A method for manufacturing the article described in [1], which satisfies the above.
[0120] [3] The adherend further has a third surface extending in the longitudinal direction and in contact with the second surface, the plurality of rollers include a third roller that is disposed downstream of the second roller in the longitudinal direction and presses the transfer sheet against the third surface, and a second guide roller that is disposed between the second roller and the third roller; When viewed from the longitudinal direction, an axial direction A2 of the second roller and an axial direction A3 of the third roller intersect with each other, When viewed from the longitudinal direction, the angle from the axial direction A2 of the second roller to the axial direction A3 of the third roller is defined as θ 23 and the axial direction A from the axial direction A2 of the second roller to the second guide roller N The angle to 2N In this case, the above θ 23 and the above θ 2N θ 23 >θ 2N A method for manufacturing an article according to [1] or [2], which satisfies the above.
[0121] [4] The axial direction A1 and the axial direction A3 are horizontal directions, The method for manufacturing an article described in [3], wherein the axial direction A2 is a vertical direction.
[0122] [5] The plurality of rollers includes two or more of the first guide rollers, When viewed from the longitudinal direction, the axial direction A1 of the first roller is offset from the axial direction A of the two or more first guide rollers. M The method for manufacturing an article described in any one of [2] to [4], wherein the angle between the upstream side and the downstream side increases from the upstream side to the downstream side in the longitudinal direction.
[0123] [6] the plurality of rollers includes two or more of the second guide rollers, When viewed from the longitudinal direction, the axial direction A2 of the second roller is offset from the axial direction A of the two or more second guide rollers. N The method for manufacturing an article described in [3] or [4], wherein the angle between the upstream side and the downstream side increases from the upstream side to the downstream side in the longitudinal direction.
[0124] [7] The method for manufacturing the article described above is a method for manufacturing an article described in any one of [1] to [6], which includes an adhesive layer formation step of forming an adhesive layer on the surface of the transfer layer opposite the release film or on the multiple surfaces of the adherend after the preparation step and before the wrapping processing step.
[0125] [8] The method for manufacturing an article described in any one of [1] to [7], wherein in the wrapping process, the transfer sheet is supplied from a roll of the transfer sheet.
[0126] [9] The method for manufacturing an article according to any one of [1] to [8], wherein the adherend is heated in the wrapping process.
[0127]
[10] The method for producing an article described in any one of [1] to [9], wherein the transfer layer has a first protective layer and a second protective layer, in that order from the release film side, in the thickness direction.
[0128]
[11] The method for producing an article according to
[10] , wherein the first protective layer comprises a cured product of an ionizing radiation curable resin composition.
[0129]
[12] The method for producing an article according to
[10] or
[11] , wherein the second protective layer comprises a cured product of a thermosetting resin composition.
[0130]
[13] The method for producing an article according to any one of
[10] to
[12] , wherein the first protective layer contains at least one of an ultraviolet absorber and a light stabilizer.
[0131]
[14] The method for producing an article according to any one of
[10] to
[13] , wherein the second protective layer contains at least one of an ultraviolet absorber and a light stabilizer.
[0132]
[15] The method for manufacturing an article described in any one of
[10] to
[14] , wherein the transfer layer has a design layer on the side of the second protective layer opposite to the first protective layer.
[0133]
[16] The method for manufacturing an article according to any one of [1] to
[15] , wherein the article is an exterior product. [Explanation of symbols]
[0134] 1 ... Release film 2 … 1st protective layer 3…Second protective layer 4 … Design layer 10 ... Transfer sheet 20 … Adherent 50 ... Items with release film 100 … Goods
Claims
1. A preparation step of preparing an adherend having a plurality of surfaces and a transfer sheet having a release film and a transfer layer; a lapping process step of sequentially laminating the transfer layer of the transfer sheet to the multiple surfaces of the adherend using a roller; The method for manufacturing an article comprising the steps of:
2. A plurality of the rollers are arranged along the longitudinal direction of the adherend, The adherend has a first surface extending in the longitudinal direction and a second surface extending in the longitudinal direction and in contact with the first surface, the plurality of rollers include a first roller that presses the transfer sheet against the first surface, a second roller that is disposed downstream of the first roller in the longitudinal direction and presses the transfer sheet against the second surface, and a first guide roller that is disposed between the first roller and the second roller; When viewed from the longitudinal direction, the axial direction A of the first roller 1 and the axial direction A of the second roller 2 and crossed, When viewed from the longitudinal direction, the axial direction A of the first roller 1 to the axial direction A of the second roller 2 The angle to 12 and the axial direction A of the first roller 1 axial direction A from the first guide roller M The angle to 1M In this case, the θ 12 and the θ 1M θ 12 >θ 1M The method for producing an article according to claim 1 , which satisfies the above.
3. The adherend further has a third surface extending in the longitudinal direction and in contact with the second surface, the plurality of rollers include a third roller that is disposed downstream of the second roller in the longitudinal direction and presses the transfer sheet against the third surface, and a second guide roller that is disposed between the second roller and the third roller; When viewed from the longitudinal direction, the axial direction A of the second roller 2 and the axial direction A of the third roller 3 and crossed, When viewed from the longitudinal direction, the axial direction A of the second roller 2 to the axial direction A of the third roller 3 The angle to 23 and the axial direction A of the second roller 2 axial direction A from the second guide roller N The angle to 2N In this case, the θ 23 and the θ 2N θ 23 >θ 2N The method for producing an article according to claim 2 , which satisfies the above.
4. The axial direction A 1 and the axial direction A 3 is the horizontal direction, The axial direction A 2 The method for manufacturing an article according to claim 3 , wherein the direction is vertical.
5. The plurality of rollers includes two or more of the first guide rollers, When viewed from the longitudinal direction, the axial direction A of the first roller 1 to the axial direction A of the two or more first guide rollers M The method for manufacturing an article according to claim 2 , wherein the angle between the upstream side and the downstream side increases in the longitudinal direction.
6. The plurality of rollers includes two or more second guide rollers, When viewed from the longitudinal direction, the axial direction A of the second roller 2 to the axial direction A of the two or more second guide rollers N The method for manufacturing an article according to claim 3 , wherein the angle between the upstream side and the downstream side increases from the upstream side to the downstream side in the longitudinal direction.
7. The method for manufacturing an article according to claim 1, further comprising, after the preparation step and before the wrapping step, an adhesive layer formation step of forming an adhesive layer on the surface of the transfer layer opposite the release film or on the multiple surfaces of the adherend.
8. The method for manufacturing an article according to claim 1 , wherein in the wrapping process, the transfer sheet is supplied from a raw sheet roll of the transfer sheet.
9. The method for manufacturing an article according to claim 1 , wherein the adherend is heated in the wrapping process.
10. The method for manufacturing an article according to claim 1 , wherein the transfer layer has a first protective layer and a second protective layer in this order in a thickness direction from the release film side.
11. The method for producing an article according to claim 10 , wherein the first protective layer comprises a cured product of an ionizing radiation curable resin composition.
12. The method for manufacturing an article according to claim 10 , wherein the second protective layer comprises a cured product of a thermosetting resin composition.
13. The method for manufacturing an article according to claim 10 , wherein the first protective layer contains at least one of an ultraviolet absorbing agent and a light stabilizer.
14. The method for manufacturing an article according to claim 10 , wherein the second protective layer contains at least one of an ultraviolet absorbing agent and a light stabilizer.
15. The method for manufacturing an article according to claim 10 , wherein the transfer layer has a design layer on a surface of the second protective layer opposite to the first protective layer.
16. The method of claim 1 , wherein the article is an exterior product.
Citation Information
Patent Citations
Rain gutter
JP2020012283A