Austenitic stainless cast steel repair method
By adjusting laser beam intensity based on molten pool temperature during laser metal deposition, the method prevents excessive thermal energy accumulation, maintaining uniform properties and suppressing corrosion resistance deterioration in austenitic stainless steel cast steel repairs.
Patent Information
- Application Number
- JP2023055165
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-03-30
AI Technical Summary
Austenitic stainless steel cast steel experiences reduced corrosion resistance due to chromium carbide precipitation when exposed to high temperatures during laser metal deposition repairs, exacerbated by solidification segregation leading to localized chromium-deficient regions.
Adjust the intensity of the laser beam based on the detected temperature of the molten pool during laser metal deposition, moving the beam and metal powder injection along the repair site to maintain a consistent temperature and prevent excessive thermal energy accumulation.
Prevents austenitic stainless steel from being maintained at high temperatures, suppressing corrosion resistance deterioration and thermal deformation, ensuring uniform properties and high joint strength of the repair.
Smart Images

Figure 2024142821000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for repairing austenitic stainless cast steel. [Background technology]
[0002] It has been known that austenitic stainless steel materials, which have excellent corrosion resistance and work hardening characteristics, are used for turbine rotor blades (Patent Document 1). In addition, a method for repairing cracks that have occurred in turbine rotor blades is known in which the cracks are removed and the removed areas are overlaid with multiple layers by laser metal deposition (LMD method) (Patent Document 2). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2013-036451 A [Patent Document 2] JP 2011-106431 A Summary of the Invention [Problem to be solved by the invention]
[0004] When an austenitic stainless steel material is held at a high temperature of 600°C to 800°C for a certain period of time, chromium and carbon in the steel material are bonded to precipitate chromium carbide, and a chromium-deficient region is formed. When a chromium-deficient region is formed, the corrosion resistance is significantly reduced and corrosion is likely to progress. Furthermore, among austenitic stainless steel materials, cast steel formed by a casting method is prone to localized chromium-deficient regions because solidification segregation causes regions in the cast steel with a large amount of carbon and a small amount of chromium. Here, as described in Patent Document 2, when repairing a location where a crack has been removed by multi-layer build-up, heat accumulates in the cast steel around the repair location irradiated with a laser beam, resulting in a high temperature state. Therefore, when applying repair by laser metal deposition to austenitic stainless cast steel, it is necessary to consider the thermal effect on the cast steel around the repair location.
[0005] Therefore, the present invention has been made in consideration of the above circumstances, and has an object to suppress a decrease in the corrosion resistance of austenitic stainless cast steel when the austenitic stainless cast steel to be repaired is repaired by a laser metal deposition method. [Means for solving the problem]
[0006] In order to solve the above problems, there is provided a method for repairing austenitic stainless cast steel, comprising: a first step of irradiating a laser beam and spraying metal powder onto a repair area on the surface of austenitic stainless cast steel; a second step of detecting the temperature of a molten pool formed at the repair area by melting the metal powder with the laser beam; a third step of adjusting the intensity of the laser beam based on the detected temperature of the molten pool; and a fourth step of moving the irradiation point of the laser beam of the adjusted intensity and the injection point of the metal powder along the shape of the repair area. Effect of the Invention
[0007] According to the present invention, the intensity of the laser beam is adjusted based on the detected temperature of the molten pool, thereby preventing the austenitic stainless cast steel around the repair site from being maintained at a high temperature. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a schematic diagram of a laser metal deposition apparatus. [Diagram 2] 1 is a schematic diagram of a main part of a laser metal deposition apparatus. [Diagram 3] This is a process diagram showing the state of a cross section around a damaged portion of an object to be repaired in the order of steps. [Figure 4] 4 is a flowchart of the process of the control device. [Diagram 5] 4 is a flowchart of the process of the control device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. The embodiment described below is subject to various technically preferable limitations for implementing the present invention, but the scope of the present invention is not limited to the following embodiment and illustrated examples.
[0010] 1. Items to be repaired The repair object is an object on which the repair method according to the embodiment of the present invention is carried out. The repair object is an austenitic stainless cast steel. Cracks and the like occur in the repair object due to the collision of a foreign object, deterioration over time, and the like. The cracks and the surrounding areas are removed by cutting or blasting to form a groove in the repair object. The crack is an example of a damaged area. The groove corresponds to the repair area. It is to be noted that the repair method according to the embodiment may be applied to the damaged area as is, without forming a groove. In this case, the damaged area corresponds to the repair area.
[0011] For example, FIG. 1 shows an impeller 80 as an object to be repaired. The impeller 80 is a fluid machine used in, for example, a water intake pump installed in a power plant. The impeller 80 in the present invention is made of austenitic stainless steel cast steel. Austenitic stainless steel cast steel is known for its excellent corrosion resistance and work hardening characteristics.
[0012] 1, a blade 80a of an impeller 80 has a repair area 84. FIG 2 shows an enlarged view of the repair area 84. In this embodiment, the repair area 84 is a groove 83. The groove 83 as the repaired portion 84 is a depression formed on the surface of the impeller 80. The shape of the groove 83 is a truncated quadrangular pyramid shape narrowing toward the bottom 83a of the groove 83. The gradient α of the inclined surface 83b from the surface of the impeller 80 toward the bottom 83a of the groove 83 is, for example, 30° or 45° with respect to the bottom 83a.
[0013] 2. Laser Metal Deposition Equipment (LMD Equipment) The LMD device is a device that irradiates a repair area of a repair object with a laser beam and injects metal powder onto the repair area to melt the metal powder and form a weld bead on the repair area. Specifically, the device displaces the molten pool by moving the irradiated area of the laser beam and the irradiated area of the metal powder along the surface shape of the repair area, and forms a weld bead on the repair area that is the trajectory of the molten pool. The weld bead is the molten pool that solidifies after the laser beam passes through.
[0014] 1 and 2 are schematic diagrams of an LMD apparatus 10 according to this embodiment. The LMD apparatus 10 includes a holder 11 , a head 12 , a laser driver 15 , a non-contact temperature sensor 16 , a moving mechanism 17 , a powder supplier 18 , a shielding gas supplier 19 and a control device 20 .
[0015] The holder 11 is a member for holding the impeller 80. As shown in FIG. 1, the holder 11 is a stand, table, or tray having an upper surface on which the impeller 80 is placed. The impeller 80 is placed on the holder 11 and fixed with a fixing device (not shown). The holder for holding the object to be repaired is not limited to the holder 11 as shown in the example of FIG. 1, and various holders can be used in place of the holder 11 in the example of FIG. 1 as long as they can hold the object to be repaired, depending on the type or shape of the object to be repaired. For example, the holder may be a chuck for fixing the object to be repaired.
[0016] The head 12 is a member for irradiating a laser beam 91 from its tip 12a to a repair area 84. The head 12 is also a member for ejecting metal powder 92 from its tip 12a onto the area irradiated with the laser beam 91. The ejected metal powder 92 is heated and melted by being irradiated with the laser beam 91. As a result, a molten pool 85 is formed at the area irradiated with the laser beam 91. Furthermore, the head 12 ejects a shielding gas 93 from its tip 12a around the area irradiated with the laser beam 91.
[0017] The head 12 includes a head body 12e, a laser light source 12f, and an optical system 12g. The head body 12e is provided with a tapered tip. The tip of the head body 12e corresponds to the tip 12a of the head 12. A hollow 12b is formed inside the head body 12e. The hollow 12b opens at the tip of the head body 12e. The laser light source 12f is attached to the head body 12e in the hollow 12b and is directed toward the opening of the hollow 12b. The laser light source 12f is connected to a laser driver 15 consisting of a power circuit or the like via an optical fiber. The laser light source 12f is driven by the laser driver 15 to emit a laser beam 91 toward the opening of the hollow 12b. The optical system 12g is disposed between the laser light source 12f and the opening of the hollow 12b in the hollow 12b and is attached to the head body 12e. The optical system 12g has, for example, a collimating lens and a condensing lens. The optical system 12g collimates the laser beam 91 and then focuses the laser beam 91 on the repair portion 84. As a result, a focused spot of the laser beam 91 is formed on the repair portion 84. The location where the focused spot of the laser beam 91 is formed corresponds to the location irradiated with the laser beam 91.
[0018] A powder supply path 12c is formed inside the head body 12e. The powder supply path 12c opens at the tip of the head body 12e. At the tip of the head body 12e, the opening of the powder supply path 12c is arranged around the opening of the hollow 12b. The powder supply path 12c is connected to a powder feeder 18 via a pipe or the like. The powder feeder 18 supplies metal powder 92 to the powder supply path 12c. Then, the metal powder 92 passes through the powder supply path 12c and is ejected from the opening of the powder supply path 12c at the tip of the head body 12e. The ejection point where the metal powder 92 is ejected is a point where the focused spot of the laser beam 91 is formed. Therefore, the ejected metal powder 92 is heated and melted by the laser beam 91 at the focused spot of the laser beam 91. As a result, a molten pool 85 is formed at the repair site 84.
[0019] The metal powder 92 is made of steel, stainless steel, or other metal material. Among them, austenitic stainless steel material is preferable. The austenitic stainless steel material has excellent corrosion resistance and work hardening characteristics. Furthermore, among them, it is preferable that the austenitic stainless steel material has a lower carbon content than the austenitic stainless cast steel which is the repair part, and in particular, a low-carbon austenitic stainless steel material with a carbon content of 0.03% or less is preferable. By making the metal powder 92 a low-carbon austenitic stainless steel material, the amount of carbon that can react with chromium in the metal powder 92 or the impeller 80 which is the base material is reduced, so that the occurrence of a chromium-deficient region can be suppressed, and as a result, it is possible to suppress the deterioration of the corrosion resistance of the repair part of the impeller 80. Specific examples of the austenitic stainless steel material include SUS304, SUS316, and SUS316L, and examples of the low-carbon austenitic stainless steel material include SUS316L.
[0020] A gas supply passage 12d is formed inside the head body 12e. The gas supply passage 12d opens at the tip of the head body 12e. At the tip of the head body 12e, the opening of the gas supply passage 12d is arranged around the opening of the powder supply passage 12c. The gas supply passage 12d is connected to a shielding gas supplier 19 via piping or the like. The shielding gas supplier 19 supplies a shielding gas 93 to the gas supply passage 12d. Then, the shielding gas 93 passes through the gas supply passage 12d and is ejected from the opening of the gas supply passage 12d at the tip of the head body 12e. The ejected shielding gas 93 is blown onto the surface of the impeller 80 around the molten pool 85. The ejected shielding gas 93 shields the molten pool 85 from the surrounding air and suppresses reactions such as oxidation or nitridation of the molten metal in the molten pool 85. The shielding gas 93 is an inert gas such as argon gas.
[0021] The head 12 is attached to a moving mechanism 17 . The moving mechanism 17 is, for example, a manipulator or an XYZ scanning mechanism. The moving mechanism 17 moves the head 12 relatively to the impeller 80 so that the tip 12a of the head 12 follows the surface shape of the repair portion 84. When the moving mechanism 17 moves the head 12, the irradiation point of the laser beam 91 and the injection point of the metal powder 92 are displaced along the surface shape of the repair portion 84. As a result, the formation position of the molten pool 85 is displaced along the surface shape of the repair portion 84. After the laser beam 91 passes, the molten pool 85 solidifies and becomes a weld bead 86.
[0022] The non-contact temperature sensor 16 is a member for detecting the temperature of the molten pool 85. The non-contact temperature sensor 16 is attached to the moving mechanism 17 in a position away from the irradiation point of the laser beam 91 and the injection point of the metal powder 92, and is directed toward the irradiation point of the laser beam 91 and the injection point of the metal powder 92. The non-contact temperature sensor 16 is moved together with the head 12 relative to the impeller 80 by the moving mechanism 17. As a result, even if the formation position of the molten pool 85 is displaced, the non-contact temperature sensor 16 detects the temperature of the molten pool 85 from a position away from the molten pool 85. The non-contact temperature sensor 16 is connected to the control device 20 via wiring or the like. The non-contact temperature sensor 16 outputs a signal corresponding to the detected temperature to the control device 20.
[0023] The control device 20 has an interface circuit, a drive circuit, a computer, etc. The control device 20 is connected to the laser driver 15, the non-contact temperature sensor 16, the powder feeder 18, and the shielding gas feeder 19 via wiring or the like.
[0024] The control device 20 periodically acquires the temperature of the molten pool 85 detected by the non-contact temperature sensor 16 by inputting the signal output by the non-contact temperature sensor 16. The control device 20 adjusts the intensity of the laser beam 91 emitted by the laser source 12f so as to maintain the temperature of the molten pool 85 at a constant set temperature by feedback-controlling the output of the laser driver 15 based on the temperature detected by the non-contact temperature sensor 16.
[0025] The controller 20 controls the powder feeder 18 to activate and stop the powder feeder 18 and to adjust the amount of powder fed by the powder feeder 18 per unit time.
[0026] The control device 20 controls the shielding gas supply device 19 to operate the shielding gas supply device 19, stop the shielding gas supply device 19, and adjust the supply flow rate or supply pressure of the shielding gas 93 supplied by the shielding gas supply device 19.
[0027] The control device 20 controls the moving mechanism 17 according to a path program recorded in the computer's storage device, and causes the moving mechanism 17 to move the head 12 and the non-contact temperature sensor 16 so that the tip 12a of the head 12 follows the path set in the path program. Note that a controller may be connected to the control device 20, and an operator may operate the controller, causing the control device 20 to control the moving mechanism 17 according to an output signal from the controller, and cause the moving mechanism 17 to move the head 12 and the non-contact temperature sensor 16.
[0028] 2. Repair method A method for repairing impeller 80 will be described with reference to Fig. 3(a) to Fig. 3(e), Fig. 4 and Fig. 5. In this example, it is assumed that damaged portion 81 has occurred in impeller 80. Here, Fig. 3(a) to Fig. 3(e) are process diagrams showing the state of a cross section around damaged portion 81 of impeller 80 in the order of steps. Fig. 4 and Fig. 5 are flowcharts of the processing by control device 20.
[0029] (1) Beveling process An operator sets the impeller 80 in a cutting machine. The cutting machine removes a peripheral portion 82 (FIG. 3(a)) of a damaged portion 81 such as a dent or a crack that has occurred on the surface of the impeller 80, and forms a groove 83 as shown in FIG. 3(b). Here, the shape of the groove 83 is a quadrangular pyramid shape that narrows toward a bottom 83a of the groove 83. The gradient α of the slope 83b from the surface of the impeller 80 toward the bottom 83a of the groove 83 is, for example, 30° or 45° with respect to the bottom 83a.
[0030] (2) Laser metal deposition process After the groove preparation, the worker mounts the impeller 80 on the holder 11 of the LMD device 10. Then, the LMD device 10 starts. Then, the control device 20 causes the moving mechanism 17 to move the head 12 and the non-contact temperature sensor 16 to the vicinity of the groove 83 of the impeller 80, and to orient the tip 12a of the head 12 and the non-contact temperature sensor 16 toward the bottom 83a of the groove 83 (step S1).
[0031] Thereafter, the control device 20 controls the powder feeder 18 to supply a constant amount of metal powder 92 per unit time (step S2). The control device 20 also controls the shielding gas feeder 19 to supply shielding gas 93 (step S3). By simultaneously executing the processes of steps 2 and 3, the metal powder 92 and the shielding gas 93 are sprayed from the tip 12a of the head 12 toward the surface of the impeller 80 in the groove 83.
[0032] The control device 20 also causes the laser driver 15 to drive the laser light source 12f (step S4). Then, the laser light source 12f is turned on and emits a laser beam 91, which is irradiated from the tip 12a of the head 12 toward the surface of the impeller 80 in the groove 83. As a result, as shown in FIG. 2, the injected metal powder 92 is heated and melted by the laser beam 91, and a molten pool 85 in which the metal powder 92 is melted is formed on the surface of the impeller 80 in the groove 83.
[0033] During irradiation of the laser beam 91, the control device 20 feedback controls the output of the laser driver 15 based on the temperature of the molten pool 85 detected by the non-contact temperature sensor 16, and adjusts the intensity of the laser beam 91 so as to maintain the temperature of the molten pool 85 at a constant set temperature (step S5).
[0034] 5 is a chart showing a specific process flow of the feedback control. First, the control device 20 acquires the temperature of the molten pool 85 detected by the non-contact temperature sensor 16 (step S51). Next, the control device 20 compares the temperature detected by the non-contact temperature sensor 16 with a predetermined set temperature (step S52). If the controller 20 determines that the temperature detected by the non-contact temperature sensor 16 exceeds the set temperature, the controller 20 reduces the output power supplied to the laser light source 12f by the laser driver 15 (step S53). This reduces the intensity of the laser beam 91, and therefore the temperature of the molten pool 85. On the other hand, if the control device 20 determines that the temperature of the molten pool 85 detected by the non-contact temperature sensor 16 is lower than the set temperature, it increases the power supplied to the laser light source 12f by the laser driver 15 (step S54). This increases the intensity of the laser beam 91, and the temperature of the molten pool 85 also increases. If the control device 20 determines from the comparison that the temperature of the molten pool 85 detected by the non-contact temperature sensor 16 is equal to the set temperature, it maintains the output of the laser driver 15 unchanged (step S55).
[0035] Thereafter, the control device 20 periodically acquires the temperature detected by the non-contact temperature sensor 16 (step S51). Then, every time the control device 20 acquires the temperature of the molten pool 85 detected by the non-contact temperature sensor 16, it executes the comparison process of step S52 and the adjustment process of step S53, S54 or S55. Therefore, the intensity of the laser beam 91 is adjusted according to the change in the temperature of the molten pool 85, so that the temperature of the molten pool 85 is maintained at the set temperature.
[0036] The control device 20 controls the movement mechanism 17 in parallel with the feedback control (step S6). Specifically, the control device 20 causes the movement mechanism 17 to move the head 12 and the non-contact temperature sensor 16 so that the tip 12a of the head 12 follows the path set in the path program (step S6). As a result, the irradiation point of the intensity-adjusted laser beam 91 and the injection point of the metal powder 92 are displaced, and the molten pool 85 is displaced.
[0037] The movement of the tip 12a of the head 12 and the non-contact temperature sensor 16 in step S6 will be specifically described. First, the control device 20 causes the movement mechanism 17 to move the head 12 and the non-contact temperature sensor 16 so that the tip 12a of the head 12 and the non-contact temperature sensor 16 are aligned with the bottom 83a of the groove 83. As a result, a first weld bead layer 87a is formed at the bottom 83a of the groove 83 as shown in FIG. 3(c). Thereafter, the control device 20 causes the movement mechanism 17 to move the head 12 and the non-contact temperature sensor 16 so that the tip 12a of the head 12 and the non-contact temperature sensor 16 move away from the first weld bead layer 87a. The movement distance by which the tip 12a of the head 12 and the non-contact temperature sensor 16 move away from the first weld bead layer 87a corresponds to the thickness of one layer of the weld bead layer. Thereafter, controller 20 causes movement mechanism 17 to move head 12 and non-contact temperature sensor 16 such that tip 12a of head 12 and non-contact temperature sensor 16 are aligned along the surface of first weld bead layer 87a. As a result, second weld bead layer 87b is formed on first weld bead layer 87a, as shown in FIG. 3(d). By controller 20 controlling movement mechanism 17 in the above manner, multiple weld bead layers (three weld bead layers 87a-87c in the example shown in FIG. 3(e)) are deposited in order from bottom 83a of groove 83, and build-up 87 consisting of these weld bead layers is embedded in groove 83.
[0038] After the build-up 87 is formed, the LMD apparatus 10 stops. Then, the operator removes the impeller 80 from the holder 11 of the LMD apparatus 10.
[0039] (3) Surface treatment process After the laser metal deposition step, as shown in FIG. 3( f ), a grinder grinds away the portion of the build-up 87 that protrudes from the groove 83 , so that the surface of the build-up 87 is flush with the surface of the impeller 80 .
[0040] 3. Beneficial Effects (1) In the repair method according to this embodiment, the head 12 irradiates a laser beam 91 and sprays metal powder 92 onto a repair area 84 on the surface of an impeller 80 made of austenitic stainless cast steel, the non-contact temperature sensor 16 detects the temperature of a molten pool 85 of the metal powder 92 melted by the laser beam 91, the control device 20 adjusts the intensity of the laser beam 91 based on the temperature of the molten pool 85 detected by the non-contact temperature sensor 16, and the movement mechanism 17 moves the irradiated point of the laser beam 91 and the sprayed point of the metal powder 92 along the shape of the repair area 84. As the irradiated point of the laser beam 91 and the sprayed point of the metal powder 92 move, the molten pool 85 formed immediately before is cooled and solidified, and the next molten pool 85 is formed. In other words, the position of the molten pool 85 moves over time. The molten pool 85 formed by the irradiation of the laser beam 91 has a smaller spot size and a shallower melt depth than the molten pool formed by the weld build-up, and is therefore cooled relatively quickly. Therefore, by adjusting the intensity of the laser beam 91 based on the temperature of the molten pool 85 formed immediately before, it is possible to prevent excessive thermal energy from accumulating in the impeller 80 made of austenitic stainless cast steel around the repaired part. In this way, it is possible to adjust the impeller 80 made of austenitic stainless cast steel around the repaired part so that it is not maintained at a high temperature of 500°C or more, and therefore it is possible to prevent the corrosion resistance of the impeller 80 from decreasing. In addition, by preventing excessive thermal energy from being applied to the periphery of the repaired part, the thermal effect on the impeller 80 is not large, and therefore it is possible to prevent thermal deformation of the impeller 80. Furthermore, since the intensity of the laser beam 91 is adjusted based on the temperature of the molten pool 85, it is possible to prevent the temperature of the molten pool 85 from becoming too low, so that the metal powder 92 melts at an appropriate temperature regardless of the displacement speed of the irradiated portion of the laser beam 91, and the base material melts appropriately in the vicinity of the interface between the molten pool 85 and the base material. As a result, the build-up 87 is well formed. The molten pool 85 moves as the irradiation point of the laser beam 91 and the injection point of the metal powder 92 move, and the molten pool 85 can be adjusted to be kept at a constant temperature at any position. In this case, the build-up 87 formed is subject to uniform thermal effects at any part, and tends to have uniform properties and structure. For example, the build-up 87 is less likely to have localized precipitation or defects. The formed build-up 87 is made of austenitic stainless steel, and the impeller 80 is also made of austenitic stainless cast steel, so there is a high affinity between the build-up 87 and the impeller 80. Therefore, the bonding strength between the build-up 87 and the impeller 80 is high.
[0041] (2) In the repair method according to this embodiment, when the temperature of the molten pool 95 detected by the non-contact temperature sensor 16 is equal to the set temperature, the control device 20 adjusts the output of the laser driver 15 to maintain the intensity of the laser beam 91, thereby adjusting the intensity of the laser beam 91. When the temperature of the molten pool 95 detected by the non-contact temperature sensor 16 exceeds the set temperature, the control device 20 adjusts the output of the laser driver 15 to reduce the intensity of the laser beam 91, thereby adjusting the intensity of the laser beam 91. When the temperature of the molten pool 95 detected by the non-contact temperature sensor 16 is lower than the set temperature, the control device 20 adjusts the output of the laser driver 15 to increase the intensity of the laser beam 91, thereby adjusting the intensity of the laser beam 91. Therefore, even if the temperature of the molten pool 85 deviates from the set temperature, the temperature of the molten pool 85 can be returned to the set temperature by adjusting the intensity of the laser beam 91. In this way, the temperature of the molten pool 85 is maintained constant.
[0042] (3) In the repair method according to this embodiment, the area surrounding the damaged portion 81 on the surface of the impeller 80 is removed, and a truncated pyramid groove 83 is formed in the surface of the impeller 80 as a repair portion 84 . Since the peripheral portion 82 of the damaged portion 81 has been removed, it is easy to irradiate the laser beam 91 onto the surface within the groove 83. Therefore, repair can be easily performed by the laser metal deposition method. Since the groove 83 has a truncated pyramid shape, the bottom 83a of the groove 83 is flat. Therefore, the molten metal in the molten pool 85 easily wets the bottom 83a of the groove 83. Therefore, voids are unlikely to occur at the interface between the buildup 87 and the bottom 83a of the groove 83, and a good buildup 87 is formed. Since the groove 83 is a quadrangular pyramid, the angle between the bottom 83a and the slope 83b of the groove 83 is an obtuse angle. Therefore, the molten metal of the molten pool 85 easily enters the corner. As a result, voids are unlikely to occur at the corner, and a good build-up 87 is formed.
[0043] (4) In the repair method according to the present embodiment, as an example, the gradient α of the inclined surface 83b of the groove 83 is 20° to 70°. By making the gradient α 20° or more, the opening area of the groove 83 on the surface of the impeller 80 does not become too large, and the heating range becomes narrow. Therefore, the amount of heat input to the impeller 80 is small, and thermal deformation of the impeller 80 is suppressed. In addition, by making the gradient α 70° or less, preferably 45° or less, the molten metal of the molten base 85 easily enters the corner between the bottom 83a and the inclined surface 83b of the groove 83, and voids are less likely to occur, so that a good build-up 87 is formed.
[0044] (5) In the repair method according to the present embodiment, for example, the metal powder 92 is an austenitic stainless steel material. Therefore, the affinity between the build-up 87 and the impeller 80 is high, and the bonding strength between the build-up 87 and the impeller 80 is high.
[0045] (6) In the repair method according to the present embodiment, for example, the metal powder 92 is an austenitic stainless steel material having a lower carbon content than the austenitic stainless cast steel that is the repair portion. Because the carbon content in metal powder 92 is lower than the carbon content in the austenitic stainless cast steel which is the repair portion, even if the austenitic stainless cast steel around the repair portion becomes hot, the amount of carbon available to react with chromium in the austenitic stainless cast steel is small, so the generation of chromium depleted regions can be suppressed, and as a result, the corrosion resistance of impeller 80 can be suppressed from decreasing. (7) In the repair method according to the present embodiment, as an example, the metal powder 92 is an austenitic stainless steel material with a carbon content of 0.03% or less. By keeping the carbon content in metal powder 92 at 0.03% or less, even if the austenitic stainless cast steel around the repair area becomes hot, the amount of carbon available to react with chromium in the austenitic stainless cast steel is small, so that the generation of chromium-deficient regions can be suppressed, and as a result, the corrosion resistance of impeller 80 can be suppressed from decreasing.
[0046] 4. Modifications In the above embodiment, since the damaged portion 81 is small, the peripheral portion 82 of the damaged portion 81 is removed to form the groove 83 in the impeller 80. In contrast, if the concave damaged portion 81 is large and the surface of the impeller 80 within the damaged portion 81 is smooth, it is not necessary to form the groove 83. In this case, the damaged portion 81 corresponds to the repair portion 84. During irradiation of the laser beam 91, the control device 20 controls the moving mechanism 17 according to the path program, and causes the moving mechanism 17 to move the tip 12a of the head 12 and the non-contact temperature sensor 16 along the surface shape of the damaged portion 81.
[0047] In the above embodiment, the groove 83 is formed in a quadrangular pyramid shape. However, the groove 83 may be formed in another shape (for example, a hemisphere, a semi-ellipsoid, or a truncated cone). [Explanation of symbols]
[0048] 80...Impeller (austenitic stainless steel cast) 81…Damaged area 82…Periphery 83…bevel 83a…Bottom of groove 84...Repair area 85…Molten pool 87...Meat platter 91...Laser beam 92...Metal powder
Claims
1. A first step of irradiating a laser beam and spraying metal powder onto a repair area on a surface of austenitic stainless cast steel; a second step of detecting a temperature of a molten pool formed at the repair site by melting the metal powder with the laser beam; a third step of adjusting an intensity of the laser beam based on the detected temperature of the molten pool; a fourth step of moving the laser beam irradiated portion and the metal powder sprayed portion along the shape of the repair portion; A method for repairing austenitic stainless steel cast having the above structure.
2. In the third step, the temperature of the molten pool is maintained constant by adjusting the intensity of the laser beam.
2. A method for repairing austenitic stainless cast steel according to claim 1.
3. In the third step, when the detected temperature of the molten pool is equal to a predetermined set temperature, the intensity of the laser beam is maintained, when the detected temperature of the molten pool exceeds the set temperature, the intensity of the laser beam is reduced, and when the detected temperature of the molten pool is less than the set temperature, the intensity of the laser beam is increased.
2. A method for repairing austenitic stainless cast steel according to claim 1.
4. A forming step of forming a groove as the repair portion on the surface of the austenitic stainless cast steel by removing a periphery of a damaged portion generated on the surface of the austenitic stainless cast steel, 2. The method for repairing austenitic stainless cast steel according to claim 1, wherein the groove has a slope narrowing toward its bottom.
5. 5. The method for repairing austenitic stainless cast steel according to claim 4, wherein the gradient α of the inclined surface of the groove is 20° to 70°.
6. 2. The method for repairing austenitic stainless cast steel according to claim 1, wherein the metal powder is an austenitic stainless steel material.
7. 7. The method for repairing austenitic stainless cast steel according to claim 6, wherein the metal powder made of the austenitic stainless steel material has a carbon content lower than that of the austenitic stainless cast steel which is the repair portion.
8. 8. The method for repairing austenitic stainless cast steel according to claim 7, wherein the metal powder made of the austenitic stainless steel material has a carbon content of 0.03% or less.
Citation Information
Patent Citations
Superalloy cladding and fusion welding method
JP2016508070A
Laser build-up welding device, laser build-up welding method and weld repairing method
JP2018167320A
Multi-purpose computer numerically controlled processing machine and its processing method
JP2018512285A
Repair processes using laser metal powder deposition
JP7238122B2
Method of controlled remelting of or laser metal forming on the surface of an article
US20050040147A1