Quick-hardening hydraulic composition, and mortar composition
A hydraulic composition with Portland cement, alumina cement, and gypsum addresses the balance between rapid hardening and pot life, enhancing construction efficiency.
Patent Information
- Application Number
- JP2023055301
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Existing hydraulic compositions face challenges in achieving a balance between rapid hardening and maintaining sufficient pot life, with amorphous calcium aluminate leading to shortened pot life and high calcium silicate mineral content hindering early strength development.
A hydraulic composition comprising Portland cement, alumina cement, and gypsum, with specific content ratios and vitrification rates, to maintain fluidity during construction and quick hardening post-completion.
The composition achieves an excellent balance between fast-setting properties and pot life, allowing for shortened construction periods.
Smart Images

Figure 2024142905000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a fast-setting hydraulic composition and a mortar composition. [Background technology]
[0002] From the perspective of shortening construction time, it is desirable for hydraulic compositions used in various civil engineering and architectural works to have the properties of maintaining a fluidity and consistency suitable for work during construction, and then hardening quickly after work is completed.
[0003] Patent Document 1 discloses a rapid-setting cement composition containing a rapid-setting admixture and cement. The rapid-setting admixture contains calcium aluminate, anhydrous gypsum, an inorganic carbonate, an oxycarboxylic acid, and alum. The calcium aluminate contains Al 2 O 3 It is described that the molar ratio of CaO to calcium carbonate is within the range of 1.5 to 2.0, and the vitrification rate is 80% or more. Patent Document 2 discloses a hydraulic composition containing cement containing calcium silicate mineral as the main component, calcium aluminates, metakaolin, sulfates, and lithium carbonate. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2021-160994 A [Patent Document 2] JP 2014-122129 A Summary of the Invention [Problem to be solved by the invention]
[0005] When amorphous calcium aluminate with a vitrification rate of 80% or more is used, rapid hardening is obtained, but the pot life is shortened. Also, if the content of cement mainly composed of calcium silicate mineral contained in the hydraulic composition is high, early strength development may not be sufficient, making it difficult to shorten the construction period.
[0006] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a rapid-setting hydraulic composition and a mortar composition which have an excellent balance between rapid hardening property and pot life and can shorten the construction period. [Means for solving the problem]
[0007] As a result of intensive research to solve the above problems, the present inventors have discovered that by setting the content of Portland cement and the vitrification rate of alumina cement in a fast-setting hydraulic composition containing hydraulic components including Portland cement, alumina cement and gypsum, and a setting regulator including alum, within specific ranges, a hydraulic composition can be obtained which maintains fluidity and softness suitable for work during construction, and then quickly hardens after the work is completed, allowing it to be quickly overcoated, thereby completing the present invention.
[0008] One aspect of the present invention relates to a rapid-setting hydraulic composition comprising hydraulic components including Portland cement, alumina cement, and gypsum, and a setting regulator including alum, the Portland cement content being less than 50 parts by mass per 100 parts by mass of the total amount of the hydraulic components, and the vitrification rate of the alumina cement being less than 80%.
[0009] Another aspect of the present invention relates to a mortar composition containing the above rapid-setting hydraulic composition and water. Effect of the Invention
[0010] According to the present invention, there can be provided a rapid-setting hydraulic composition and a mortar composition which have an excellent balance between rapid hardening property and pot life and can shorten the construction period. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, an embodiment of the present invention will be described, however, the present invention is not limited to the following embodiment.
[0012] [Fast-curing hydraulic composition] A rapid hardening hydraulic composition according to one embodiment contains hydraulic components including Portland cement, alumina cement, and gypsum, and a setting regulator including alum, the Portland cement content is less than 50 parts by mass relative to 100 parts by mass of the total amount of hydraulic components, and the vitrification rate of the alumina cement is less than 80%. The hydraulic composition has excellent flow maintenance (pot life of 30 minutes or more), and can reduce the time required for recoating. Each component contained in the hydraulic composition according to this embodiment will be described in detail below.
[0013] (hydraulic component) The hydraulic composition according to this embodiment contains portland cement, alumina cement, and gypsum as hydraulic components.
[0014] Examples of Portland cement include ordinary Portland cement, early-strength Portland cement, extra-early-strength Portland cement, moderate-heat Portland cement, low-heat Portland cement, and white Portland cement. Any commercially available product can be used. One or more of these can be used. It is preferable to use ordinary Portland cement or early-strength Portland cement, which is easy to obtain and has good workability.
[0015] The Blaine specific surface area of Portland cement is preferably 2500 to 6000 cm 2 / g, and more preferably 3000 to 5500 cm 2 / g, and more preferably 3300 to 5000 cm 2 / g. The Blaine specific surface area of Portland cement can be determined in accordance with JIS R 5201:2015. When the Blaine specific surface area of Portland cement is in the above-mentioned preferred range, the hydration reaction proceeds favorably, and appropriate workability and excellent strength development are obtained.
[0016] The content of Portland cement is more than 0 parts by mass and less than 50 parts by mass, relative to 100 parts by mass of the total amount of hydraulic components, from the viewpoint of adjusting the balance between rapid hardening property and pot life, and may be 1 to 49 parts by mass, 10 to 48 parts by mass, 20 to 47 parts by mass, 25 to 46 parts by mass, or 30 to 45 parts by mass.
[0017] From the viewpoint of the pot life of the mortar composition, the vitrification rate of the alumina cement is less than 80%, preferably 50% or less, more preferably 20% or less, and further preferably 10% or less.
[0018] The vitrification rate of alumina cement can be calculated by determining the scattering integrated intensity of the crystalline portion (A) and the scattering integrated intensity of the non-crystalline portion (B) from the X-ray diffraction of the alumina cement measured by X-ray diffraction method, and applying them to the following formula. Vitrification rate (%) = 100 × B / (A+B)
[0019] X-ray diffraction measurements can be performed using a powder X-ray diffractometer "D2 PHASER 2nd Gen" (manufactured by Bruker Japan Co., Ltd.) under conditions of a tube voltage of 30 kV, a tube current of 10 mA, a measurement range of 2θ = 5 to 70°, a step width of 0.02°, and a counting time of 0.5 seconds.
[0020] Several types of alumina cement with different mineral compositions are known and commercially available, but the main component in all cases is monocalcium aluminate (CA), and any commercially available product can be used regardless of its type. The main component of alumina cement is calcium aluminate. Examples of calcium aluminate include CA, C 12 A 7 , C 4 A.F., C.2 AS, etc. The alumina cement may contain only one type of these calcium aluminates, or may contain a plurality of types of calcium aluminates.
[0021] Alumina cement has a composition of CaO / Al from the viewpoint of rapid hardening. 2 O 3 The molar ratio is preferably more than 0.7, more preferably in the range of 0.8 to 2.8, and even more preferably in the range of 1.0 to 2.5.
[0022] The Blaine specific surface area of the alumina cement is preferably 2000 to 6000 cm 2 / g, and more preferably 2300 to 5000 cm 2 / g, and more preferably 2500 to 4000 cm 2 / g. The Blaine specific surface area of the alumina cement can be determined in accordance with JIS R 2521:1995. When the Blaine specific surface area of the alumina cement is in the above-mentioned preferred range, the hydration reaction proceeds favorably, and the rapid hardening property is further improved.
[0023] In order to adjust the balance between rapid hardening property and pot life, the content of alumina cement may be 10 parts by mass or more, 15 parts by mass or more, 20 parts by mass or more, or 25 parts by mass or more, and may be 50 parts by mass or less, 47 parts by mass or less, 45 parts by mass or less, or 42 parts by mass or less, relative to 100 parts by mass of the total amount of hydraulic components.
[0024] Examples of gypsum include anhydrous gypsum, hemihydrate gypsum, dihydrate gypsum, etc. The gypsum may be of any type, and one or more types may be used. Gypsum functions as a component that maintains the dimensional stability of the mortar composition after it has hardened.
[0025] The Blaine specific surface area of the gypsum is preferably 2000 to 8000 cm 2 / g, and more preferably 2500 to 7000 cm 2 / g, and more preferably 3000 to 6000 cm 2 / g. The Blaine specific surface area of the gypsum can be determined in accordance with JIS R 5201:2015. When the Blaine specific surface area of the gypsum is in the above-mentioned preferred range, the hydration reaction proceeds favorably, and appropriate workability and excellent dimensional stability are obtained.
[0026] In order to adjust the balance between rapid hardening property and pot life, the content of gypsum may be 1 part by mass or more, 5 parts by mass or more, 10 parts by mass or more, or 15 parts by mass or more, and may be 40 parts by mass or less, 35 parts by mass or less, or 30 parts by mass or less, relative to 100 parts by mass of the total amount of the hydraulic components.
[0027] (Set regulator) The hydraulic composition according to the present embodiment contains alum as a setting regulator, which can promote hardening of the mortar composition. Examples of alum include potassium aluminum sulfate and sodium aluminum sulfate.
[0028] The content of alum in the fast-setting hydraulic composition may be 0.01 to 3 parts by mass, 0.03 to 1 part by mass, 0.05 to 0.80 parts by mass, or 0.08 to 0.60 parts by mass per 100 parts by mass of the total amount of hydraulic components, from the viewpoint of further improving the fast-setting property.
[0029] (fine aggregate) The hydraulic composition according to the present embodiment may contain fine aggregate. Examples of fine aggregate include sands such as silica sand, river sand, land sand, sea sand, and crushed sand. The hydraulic composition may contain only one type of fine aggregate, or may contain two or more types of fine aggregate.
[0030] The content of the fine aggregate is preferably 30 to 300 parts by mass, more preferably 35 to 270 parts by mass, and even more preferably 40 to 250 parts by mass, relative to 100 parts by mass of the total amount of the hydraulic components. By setting the content of the fine aggregate within the above range, the strength of the hardened mortar body can be further improved without impairing the workability.
[0031] (Other Ingredients) The hydraulic composition according to this embodiment may contain one or more of blast furnace slag, limestone, slaked lime, fly ash, silica fume, expansive agent, fluidizing agent, water reducing agent, retarder, accelerator, shrinkage reducing agent, resin powder, thickener, defoamer, etc., within a range that does not substantially impair the object of the present invention.
[0032] The hydraulic composition according to the present embodiment is useful as a cross-section repair material for civil engineering and construction applications. The hydraulic composition according to the present embodiment can also be used as a joint filler, joint material, grout material, floor material, etc. for precast products.
[0033] (Mortar composition) The mortar composition of the present embodiment contains the above-mentioned rapid-setting hydraulic composition and water. The mortar composition can be prepared by kneading the rapid-setting hydraulic composition and water.
[0034] When preparing a mortar composition, the flow value and unit volume mass of the mortar composition can be adjusted by appropriately changing the amount of water. The flow value is a value measured in accordance with the test method described in JIS R 5201-2015 "Physical Test Methods for Cement."
[0035] The flow value of the mortar composition of the present embodiment at 5° C. is preferably 145 to 220 mm, more preferably 147 to 210 mm, and further preferably 150 to 200 mm. When the flow value of the mortar composition is in such a range, the mortar composition tends to have better workability.
[0036] The mortar composition of the present embodiment has suitable workability and recoating time when integrated with a concrete structure, and is suitable for shortening the construction period of various construction works in the fields of civil engineering and construction. EXAMPLES
[0037] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these examples.
[0038] To prepare the hydraulic composition and the mortar composition, the following materials were prepared. (1) Portland cement (high early strength Portland cement, manufactured by UBE Mitsubishi Cement Corporation, Blaine specific surface area 4500 cm) 2 / g) (2) Alumina cement (Imerys, Blaine specific surface area 3100 cm) 2 / g, CaO / Al 2 O 3 Molar ratio 1.8, vitrification rate 6%) (3) Amorphous alumina cement (Blaine specific surface area 4520 cm 2 / g, CaO / A l2 O3, molar ratio 1.78, vitrification rate 99%) (4) Gypsum (Blaine specific surface area 4140 cm 2 / g) (5) Setting agent Alum (potassium aluminum sulfate, AlK(SO 4 ) 2 12H 2 O, purity 96.5% or more) Potassium sulfate (K 2 SO 4 , purity 99% or more) Calcium formate (Ca(HCOO) 2 , purity 98% or more) (6) Fine aggregate (silica sand with a particle size of 2 mm or less)
[0039] [Preparation of hydraulic composition and mortar composition] A hydraulic composition was prepared by mixing the hydraulic components and the setting regulator in the ratio (parts by mass) shown in Table 1, and then 47 parts by mass of fine aggregate was added to 100 parts by mass of the total hydraulic components to prepare a powder. Water was then added to the powder at a water-powder ratio of 20% (300 g water / 1500 g powder) and kneaded to prepare a mortar composition.
[0040] (Recoating time) The mortar composition immediately after preparation was molded into a polypropylene container (inner dimensions 191×131×15 mm) with a plastering trowel to a thickness of 15 mm, and then cured in a test room at a temperature of 5±2°C and a relative humidity of 65±10%. The surface hardness of the hardened mortar was measured using a rubber hardness tester (manufactured by Kobunshi Keiki Co., Ltd., CS type), and the time from molding of the mortar composition until the hardness reached 70 (recoating time) was measured. The recoating time is preferably 120 minutes or less.
[0041] (Flow value) In accordance with the test method described in JIS R 5201:2015 "Physical Testing Methods for Cement," the flow value immediately after preparation (initial) of the mortar composition at 5°C and the flow value after 30 minutes were measured. The initial flow value is preferably 150 mm or more, and the flow value after 30 minutes is preferably 145 mm or more. The mortar composition of Comparative Example 4 had a short pot life, so the flow value after 30 minutes could not be measured.
[0042] [Table 1]
Claims
1. The concrete comprises hydraulic components including portland cement, alumina cement, and gypsum, and a setting modifier including alum; The content of the Portland cement is less than 50 parts by mass per 100 parts by mass of the total amount of the hydraulic components, The rapid-setting hydraulic composition has a vitrification rate of less than 80% of the alumina cement.
2. A mortar composition comprising the rapid-setting hydraulic composition according to claim 1 and water.
Citation Information
Patent Citations
Composition of rust-preventive, and rust-preventing method
JP2005220411A
Rapid-hardening cement for sea water resistant cement asphalt mortar and sea water resistant cement asphalt mortar using the same
JP2009167042A
Hydraulic composition
JP2014122129A
Ultrarapid hardening admixture and method for producing the same
JP2017186237A
Fast curing admixture
JP2020164413A