Fabric

A high-density fabric with irregularly shaped monofilaments and a resin coating layer addresses abrasion and tear strength issues, ensuring durability and waterproofness in sports clothing and outdoor materials.

JP2024142987APending Publication Date: 2024-10-11TOYOBO TEXTILE CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023055421
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing fabrics used in sports clothing and outdoor materials face issues with abrasion resistance, tear strength, and moisture permeability, particularly when subjected to friction and rubbing against rough surfaces, leading to deterioration and loss of waterproofness.

Method used

A fabric design featuring high-density multifilaments with irregularly shaped monofilaments and a resin coating layer, optimized for lightweight, thin, and moisture-permeable properties, with a cover factor of 1,600 to 1,800 and a resin coating layer thickness of 1 μm to 10 μm, enhancing abrasion resistance and tear strength.

Benefits of technology

The fabric achieves unprecedented abrasion resistance, maintaining durability and waterproofness even under rough conditions, suitable for sports clothing and outdoor gear.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142987000001_ABST
    Figure 2024142987000001_ABST
Patent Text Reader

Abstract

To provide a fabric that is preferably used for clothing and materials, and has strong tearing force and excellent abrasion resistance despite light-weight and thin cloth.SOLUTION: A fabric has a textile that uses a multifilament for warp and weft, where at least one of the warp and the weft has an approximately square fiber cross section, has a single fiber fineness of 1dtex or more and 3.5dtex or less, the total fineness of 5dtex or more and 23dtex or less, and resin coating layer is laminated on one face of the textile.SELECTED DRAWING: Figure 6
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a fabric for use in sportswear such as downwear, down jackets, windbreakers, futons, sleeping bags, rainwear, and other such clothing, and in materials such as tents, etc. More specifically, the present invention provides a fabric whose surface is less likely to fluff due to rubbing when worn in the case of clothing such as outdoor wear, and due to rubbing against branches and leaves in the case of materials such as tents and backpacks, and whose waterproofness is less likely to decrease from the rubbed areas. [Background technology]

[0002] Clothing, particularly outerwear such as windbreakers, down jackets, downwear, and rainwear, can become frayed or easily torn due to friction at the sides and shoulders when worn or when carrying a backpack. In particular, downwear has become increasingly light in recent years, and although the side fabric is thin and light, when used during mountain climbing, it rubs against plants, rocks, backpacks, etc., causing surface tears and fraying, etc., causing deterioration, resulting in the down and feathers coming out of the surface of the side fabric. Similarly, rainwear has a problem in that the fabric is torn when rubbed against a backpack during mountain climbing, etc., and raindrops soak in through the outer fabric. In addition, materials such as backpacks and tents used for mountain climbing and camping are required to be made of fabrics that are resistant to abrasion by other objects. Thus, for clothing and materials used outdoors, fabrics that are thin and lightweight yet have excellent abrasion resistance are required.

[0003] For example, in Patent Document 1, a composite moisture-permeable waterproof membrane and a sheet using the same are proposed, which have continuous pores and a porous membrane made of a polymer material soluble in polar solvents and have continuous pores, and are laminated on at least a portion of at least one side of a hydrophobic membrane having a wettability index of 45 dyne / cm or less according to JIS K6768, in order to provide a composite moisture-permeable waterproof membrane and a sheet using the same that are resistant to condensation while maintaining high water vapor permeability, have excellent dimensional stability against water, and can provide functions such as deodorization, antibacterial properties, antifungal properties, antistatic properties, dry touch properties, and abrasion resistance. However, this moisture-permeable waterproof membrane is laminated on a woven fabric such as nylon, but the woven fabric is not specifically mentioned, and the friction durability of this moisture-permeable waterproof membrane is considered to be at most low and does not exceed the performance of a general moisture-permeable waterproof fabric.

[0004] In addition, Patent Document 2 discloses a moisture-permeable, waterproof fabric that is lightweight yet has excellent tear strength, and a textile product using the moisture-permeable, waterproof fabric, which is fabricated by laminating a moisture-permeable, waterproof layer on one side of a woven fabric A containing multifilaments, and further laminating a woven fabric B containing multifilaments with a total fineness of 25 dtex or less and having a ripstop structure, thereby forming a moisture-permeable, waterproof fabric having a basis weight of 110 g / m 2 The following moisture-permeable waterproof fabric has been proposed. However, this fabric has a limit to how light it can be made because the fabric is laminated on both sides of the moisture-permeable waterproof layer.

[0005] Furthermore, as a result of intensive research by the present applicant, a thin fabric with excellent abrasion resistance was proposed, which includes a synthetic multifilament containing an irregular monofilament having a substantially rectangular fiber cross section with a total fineness of 5 dtex to 60 dtex and a single yarn fineness of 1.0 dtex to 7.5 dtex, and in a cross section perpendicular to the synthetic multifilament, the average contact length between adjacent irregular monofilaments is 8 μm to 40 μm, and has been well received by consumers (Patent Document 3). However, this fabric alone has limitations in moisture permeability and waterproofing. In addition, even higher abrasion resistance was also required. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2005-74855 A [Patent Document 2] JP 2013-226750 A [Patent Document 3] International Publication No. 2016 / 113833 Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention has been made against the background of the problems in the conventional technology, and has an object to provide a fabric which is suitable for use in sports clothing and materials such as downwear, down jackets, windbreakers, futons, sleeping bags, rainwear, tents, bags, and backpacks, and which has high tear strength and good abrasion resistance while being lightweight and thin. [Means for solving the problem]

[0008] In order to prevent the fibers constituting the woven fabric from being broken due to friction during use as described above, which leads to deterioration in waterproofness and strength, the inventors have considered using a synthetic multifilament having a higher monofilament size and a smaller number of filaments than conventional fabrics. However, simply using a synthetic multifilament having a higher monofilament size and a smaller number of filaments causes problems such as the fabric becoming stiff and the fabric being difficult to coat. Therefore, the inventors have invented a material having moisture permeability and waterproofness, characterized in that the material is a woven fabric made of monofilaments having a total monofilament size of 5 dtex to 23 dtex and a substantially rectangular cross section and a monofilament size of 1 dtex to 3.5 dtex, and a resin coating layer is laminated on either the front or back surface of the woven fabric.

[0009] That is, the fabric according to the present invention has the following features. [1] A fabric having a woven material using multifilament warp and weft yarns, At least one of the warp yarns and the weft yarns has a substantially rectangular fiber cross section, a single yarn fineness of 1 dtex or more and 3.5 dtex or less, and a total fineness of 5 dtex or more and 23 dtex or less, The fabric has a resin coating layer laminated on one surface of the woven fabric. [2] The fabric according to [1], wherein the resin coating layer has a thickness of at least 1 μm to 10 μm. [3] The fabric according to [1] or [2], wherein the resin coating layer is a perforated film. [4] The fabric according to any one of [1] to [3], wherein the cover factor of the woven fabric is 1,600 or more and 1,800 or less. [5] The fabric has a basis weight of 60 g / m 2 The fabric according to any one of the following [1] to [4]. [6] The fabric according to any one of [1] to [5], which has an abrasion resistance of 50 or more times in an A-1 universal type abrasion resistance test in accordance with JIS L1096. [7] The fabric according to any one of [1] to [6], having a warp tear strength of 9.8 N or more and a weft tear strength of 9.8 N or more in a D-method tear strength test in accordance with JIS L1096. Effect of the Invention

[0010] The fabric of the present invention is a lightweight, thin, moisture-permeable, and waterproof fabric, and yet has excellent abrasion resistance, a property not found in the past. Rainwear, downwear, outdoor products, etc. using this fabric can be prevented from being damaged by rubbing or scratching against other fabrics, rocks, plants, etc., and can be provided with high durability while suppressing performance degradation. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is an explanatory diagram of a cross section of a fiber of a modified shaped monofilament used in the present invention. [Diagram 2] FIG. 2 is an SEM photograph showing a cross section of a woven fabric according to the present invention. [Diagram 3] FIG. 3 is an explanatory diagram that illustrates a typical example of the weave structure of the ripstop taffeta 1. As shown in FIG. [Figure 4] FIG. 4 is an explanatory diagram that illustrates a typical example of the weave structure of the ripstop taffeta 2. As shown in FIG. [Diagram 5] FIG. 5 is a schematic cross-sectional view of a spinneret outlet hole used for spinning diamond-shaped yarn. [Figure 6] FIG. 6 is a SEM photograph of a cross section of the fabric of Example 1. [Figure 7] FIG. 7 is an enlarged photograph of the effective film coating portion in FIG. [Figure 8] FIG. 8 is a SEM photograph of a cross section of the fabric of Comparative Example 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The fabric of the present invention is a lightweight, thin, high-density woven fabric that is moisture permeable and waterproof, yet has excellent abrasion resistance, a property not found in conventional fabrics. Downwear, rainwear, outdoor goods, etc. using this fabric can be prevented from being damaged by rubbing or scratching against other fabrics, rocks, plants, etc., and can be imparted with high durability while suppressing deterioration of performance.

[0013] First, the lightweight and thin woven fabric of the fabric according to the present invention will be specifically described. The fabric according to the present invention has a woven fabric using multifilaments as warp and weft threads. The woven fabric of the fabric is made thin by weaving thin fibers at a high density to extremely reduce the thickness, making it a lightweight, thin woven fabric. When a high level of thinness is pursued in a woven fabric, it is desirable that the multifilaments constituting the fabric are present in the fabric in a state where monofilaments constituting one multifilament are arranged in a row (see, for example, FIG. 2). It is preferable that the multifilaments constituting the fabric are synthetic multifilaments.

[0014] The woven fabric uses a multifilament including a deformed monofilament having a substantially rectangular fiber cross section. That is, at least one of the warp yarns and weft yarns constituting the woven fabric has a substantially rectangular fiber cross section. The term "substantially rectangular" refers to a polygon having four sides. As shown in FIG. 1, an approximately rectangular shape (including a parallelogram, a rhombus, and a rectangle, which will be described later) ideally has four clear vertices and four straight sides. However, in the process of producing the deformed monofilament, due to unevenness in the extrusion speed, discharge amount, and cooling speed of the resin, the approximately rectangular fiber cross section may not necessarily have clear vertices or may have curved sides. The approximately rectangular shape of the present invention also includes an approximately rectangular shape that includes such manufacturing problems (i.e., an approximately rectangular shape with unclear vertices and an approximately rectangular shape with curved sides).

[0015] The approximately quadrangle is preferably, for example, a parallelogram in which two pairs of opposite sides are parallel. If the two pairs of opposite sides are parallel, adjacent irregular monofilaments are more likely to come into contact with each other, and the irregular monofilaments used in the warp and the irregular monofilaments used in the weft are more likely to overlap in the thickness direction of the fabric, making it possible to suppress the deviation of the irregular monofilaments at a high level. The parallelogram has characteristics such as two pairs of diagonals having equal sizes and two pairs of opposite sides having equal lengths, and the parallelogram in the present invention also includes a rhombus with all four sides having the same length, a rectangle with all four interior angles having the same length, and a square with all four sides and all four interior angles having the same length.

[0016] In the present invention, the parallelogram, which is the shape of the fiber cross section of the irregular monofilament, is more preferably a rhombus with all four sides being equal in length. For example, in the case of a parallelogram or rectangle in which the lengths of two pairs of sides are significantly different (too flat), the arrangement of the monofilaments is likely to be disturbed when the irregular monofilaments come into contact with each other at sides of different lengths, and there are likely to be parts where the irregular monofilaments are not neatly aligned in a row, but by unifying the lengths of the four sides, they are more likely to be aligned in a row.

[0017] The irregular monofilament is preferably relatively thick so that the irregular monofilament does not break due to rubbing, scratching, etc. during use of the product using the fabric, resulting in a decrease in breathability and strength of the woven fabric. From this viewpoint, the single yarn fineness of the irregular monofilament is 1.0 dtex or more, preferably 1.5 dtex or more, more preferably 1.7 dtex or more, and even more preferably 2 dtex or more. On the other hand, if the irregular monofilament is too thick, the woven fabric becomes hard and it becomes difficult to make a high-density fabric, so the single yarn fineness of the irregular monofilament is 3.5 dtex or less, preferably 3.3 dtex or less, more preferably 3.2 dtex or less, and even more preferably 3 dtex or less.

[0018] The multifilament including the irregular monofilament has a total fineness of 5 dtex or more, preferably 7 dtex or more, more preferably 10 dtex or more, even more preferably 13 dtex or more, and 23 dtex or less, preferably 22 dtex or less, more preferably 21 dtex or less, and even more preferably 20 dtex or less. By adjusting the total fineness of the multifilament within the above range, a lightweight and thin woven fabric having the required strength can be obtained. On the other hand, if the fineness of the multifilament is below the lower limit, the required strength may not be obtained, and if it exceeds the upper limit, the woven fabric becomes bulky, making it difficult to obtain a lightweight and thin woven fabric.

[0019] The number of monofilaments contained in one multifilament is preferably 2 or more, more preferably 3 or more, and even more preferably 5 or more, and is preferably 30 or less, more preferably 20 or less, and even more preferably 15 or less. If the number of monofilaments is large, it is necessary to reduce the single yarn fineness of the monofilament, which is undesirable because the yarn becomes more likely to break.

[0020] The fibers constituting the multifilament are preferably synthetic fibers made of resin. The resin is not particularly limited, but examples thereof include polyesters such as polyethylene terephthalate and polybutylene terephthalate; polyamides such as nylon 6, nylon 66, nylon 46, nylon 12, nylon 610, nylon 612 or copolymers thereof; and synthetic polymers such as polyacrylonitrile, polyvinyl chloride, and polyvinyl alcohol. Among polyesters, polyethylene terephthalate is preferably used, and among polyamides, nylon 6 and nylon 66 are preferably used. Among them, polyamides are particularly preferred because they can soften the texture of the woven fabric and increase the tear strength of the woven fabric even when used for a deformed monofilament having a substantially rectangular cross section.

[0021] The relative viscosity of the resin constituting the synthetic multifilament is preferably 2.0 or more, more preferably 2.5 or more, and even more preferably 3.0 or more, for example, in the case of nylon, and the upper limit is not particularly limited, but can usually be 4.5 or less. If the relative viscosity of the resin is 2.0 or more, it is preferable because the obtained irregular monofilament has an appropriate breaking strength. Also, if the relative viscosity of the resin is 2.5 or more, the obtained irregular monofilament can have an appropriate breaking strength and breaking elongation. Furthermore, if the relative viscosity of the resin is 3.0 or more, when the fiber cross section of the irregular monofilament is made approximately rectangular, it is possible to clearly form four angles. On the other hand, if the relative viscosity of the resin is less than 2.0, the irregular cross section may have a weaker breaking strength than the round cross section, and problems such as a decrease in the tear strength of the product due to insufficient breaking strength, a decrease in breaking strength, and a deterioration in processing operability and a deterioration in product durability due to insufficient breaking elongation may occur.

[0022] When polyester is used as the resin constituting the synthetic multifilament, the intrinsic viscosity of the resin is preferably 0.5 or more, more preferably 0.55 or more, and even more preferably 0.58 or more. The upper limit is not particularly limited, but it can usually be 1.5 or less. If the intrinsic viscosity of the resin is 0.5 or more, it is preferable because the resulting irregularly shaped monofilament has an appropriate breaking strength. On the other hand, if the intrinsic viscosity of the resin is less than 0.5, the irregular cross section may have a weaker breaking strength than a round cross section, and problems such as a decrease in the tear strength and breaking strength of the product due to insufficient breaking strength, a deterioration in processing operability due to insufficient breaking elongation, and a deterioration in product durability may occur.

[0023] If necessary, the irregular monofilament may contain a hygroscopic substance, an antioxidant, a matting agent, an ultraviolet absorber, an antibacterial agent, etc. alone or in combination. In addition, the boiling water shrinkage rate, thermal stress, birefringence, thickness unevenness, etc. of the irregular monofilament are not particularly limited and may be set appropriately.

[0024] The breaking strength of the multifilament is not particularly limited, but is preferably 3.3 cN / dtex or more, more preferably 3.5 cN / dtex or more, and even more preferably 4.0 cN / dtex or more. If the strength of the multifilament is 3.3 cN / dtex or more, a woven fabric with appropriate tear strength can be obtained even with a multifilament having a high degree of deformation. The upper limit of the breaking strength of the multifilament is not particularly limited, but it can usually be 10 cN / dtex or less.

[0025] The breaking elongation of the multifilament is not particularly limited, but is preferably 30% or more, more preferably 35% or more, and even more preferably 40% or more, and is preferably 55% or less, more preferably 50% or less, and even more preferably 45% or less.

[0026] The multifilament used in the present invention will be specifically described. The multifilament of the present invention may be raw silk, may be subjected to crimping such as false twisting, or may be a mixture of two or more types of multifilaments, but it is preferable to use a synthetic multifilament of raw silk consisting of single fibers with the same cross section. Air entanglement and twisting are also possible, but it is preferable to avoid them as much as possible or to keep them to a minimum in order to improve productivity. If air entanglement is performed, it is preferable to set the degree of entanglement to about 1 to 35 in accordance with JIS L1013 8.15 (hook method).

[0027] In the multifilament used in the present invention, in order to make each irregular monofilament into an approximately quadrangular shape (particularly, a diamond shape), it is preferable to design the shape of the nozzle die outlet hole into a star shape as shown in FIG. 5. That is, a star-shaped die outlet hole capable of forming an approximately quadrangular irregular monofilament has four convex parts (for example, P to S in FIG. 5) and four concave parts (for example, T to W in FIG. 5), and it is preferable that the diagonal angles of two pairs of convex parts are equal and the diagonal lines of the convex parts are perpendicular to each other. When the raw resin is spun through such a star-shaped die outlet hole, the molten resin expands so as to spread within the four concave parts, and as a result, an irregular monofilament having a fiber cross section of an approximately quadrangular shape connecting the four convex parts is obtained. That is, the length of the side of the approximately quadrangle is approximately equal to the distance between the vertices of two adjacent convex parts (in FIG. 5, the lengths L1 and L2 of the side of the approximately quadrangle are approximately equal to the distance between the vertices RS and SP of the convex parts, respectively). Therefore, by adjusting the angle formed by connecting the three convex portions of the outlet hole, the interior angle of the approximate rectangle can be designed (i.e., the interior angle of Q in the approximate rectangle is approximately equal to the angle formed by connecting the three vertices P, Q, and R of the convex portions).

[0028] In addition, in this star-shaped nozzle, it is preferable that the tips of the four protrusions are rounded rather than sharp, as this makes it easier to form clear vertices without distorting the vertices of the approximate rectangle.

[0029] Furthermore, as a condition for changing the approximate rectangle into a parallelogram, it is preferable that the depth of the recesses (L3 in FIG. 5) is equal for all four recesses. The depth of the recesses is, for example, preferably 0.02 mm to 0.14 mm, and more preferably 0.04 mm to 0.12 mm. If the depth is less than 0.02 mm, the polymer may swell outward when the filament is spun, failing to form a perfect parallelogram, and if the depth is greater than 0.14 mm, even if the spun polymer swells, it may not swell enough, resulting in a star-shaped fiber cross section.

[0030] Furthermore, when cooling the spun polymer, it is preferable to set the position of the nozzle hole so that the cooling air hits each of the convex parts P, Q, R, and S in FIG. 5. Conversely, it is preferable to set the position of the nozzle hole so that the cooling air does not directly hit the concave parts T, U, V, and W in FIG. 5. By providing a portion where the cooling air is actively hit on such unevenness and a portion where the cooling air is not hit, it becomes easier to form an even parallelogram. In particular, the condition for turning a substantially square into a rhombus is that the lengths of the four sides must be equal while satisfying the above conditions, so that the viscosity of the polymer is preferably 0.5 or more in the case of polyester, and 2.5 or more in the case of polyamide. By adjusting the viscosity, it becomes easier to form a rhombus cross section with all four sides being equal.

[0031] The method for producing the multifilament having the above cross section is not particularly limited, but for example, polyamide-based synthetic multifilament and polyester-based synthetic multifilament can be produced in two steps using a continuous spinning and drawing device by the spin draw method, or a spinning device and a drawing device. In the case of the spin draw method, the speed of the spinning take-up godet roller is preferably set to 1500 m / min to 4000 m / min, and more preferably 2000 m / min to 3000 m / min.

[0032] The woven fabric of the present invention will be specifically described below. In order to obtain a thin woven fabric that is resistant to rubbing and scratching, the woven fabric preferably contains 45% by mass or more of multifilaments including irregular monofilaments, more preferably 55% by mass or more, and even more preferably 75% by mass or more, based on 100% by mass of the woven fabric. The upper limit is not particularly limited, but is preferably 100% by mass and may be 95% by mass or less. By making the content ratio of multifilaments including irregular monofilaments 45% by mass or more, a thin woven fabric with low breathability can be obtained.

[0033] When a high level of thinness is pursued in a woven fabric, it is desirable that the multifilaments constituting the woven fabric are present in the woven fabric in a state where the irregular monofilaments constituting one multifilament are arranged in a row as much as possible (see, for example, FIG. 2). When the irregular monofilaments are arranged in a row in this way, the fabric becomes extremely thin. In the cross section of the woven fabric in the direction perpendicular to the multifilaments, it is preferable that the irregular monofilaments are present in a single layer arrangement and / or a double layer arrangement in one synthetic multifilament. This is a characteristic unique to the thin woven fabric of the present invention, which contains a small number of monofilaments and uses thin multifilaments.

[0034] The cover factor (CF) of the woven fabric is, for example, preferably 1300 or more, more preferably 1450 or more, even more preferably 1500 or more, and particularly preferably 1600 or more. The upper limit is not particularly limited, but for example, it is preferably 2000 or less, more preferably 1900 or less, and even more preferably 1800 or less. By adjusting the cover factor of the woven fabric to the above range, a lightweight and thin woven fabric can be obtained. On the other hand, if the cover factor of the woven fabric is below the lower limit of the above range, a thin and light woven fabric can be obtained, but it is difficult to obtain high tear strength. In addition, if the cover factor of the woven fabric exceeds the upper limit of the above range, the woven fabric becomes heavy, which is not preferable. Here, the cover factor (CF) of the woven fabric is calculated by the following formula. CF = (T × (DT)) 1 / 2 +(W×(DW))1 / 2 [In the formula, T and W represent the warp and weft densities (counts / 2.54 cm) of the fabric, and DT and DW represent the thickness (dtex) of the warp and weft yarns constituting the fabric.]

[0035] The weave of the woven fabric is not particularly limited, and any weave such as plain weave, twill weave, satin weave, etc. can be used, and among them, plain weave is preferably used to reduce the breathability. Furthermore, in order to increase the tear strength of the woven fabric, for example, ripstop taffeta weaves as shown in Figures 3 and 4 are particularly preferably used.

[0036] The loom used for manufacturing the woven fabric is not particularly limited, and may be a water jet loom, an air jet loom, a rapier loom, etc. In particular, a water jet loom or an air jet loom is preferably used.

[0037] In the manufacture of woven fabrics, a low tension sizing machine is preferably used. Also, the healds used in the loom are preferably made of ceramic material to reduce friction with the yarn. Rectangular, parallelogram, and rhombus shapes, which have a contact area larger than a circular cross section, tend to induce fluffing, and by using ceramic material, weaving can be performed with low friction as described above, and fluffing tends to be suppressed.

[0038] The warp density of the woven fabric is, for example, preferably 50 / 2.54 cm or more, more preferably 80 / 2.54 cm or more, even more preferably 100 / 2.54 cm or more, and preferably 400 / 2.54 cm or less, more preferably 350 / 2.54 cm or less, and even more preferably 250 / 2.54 cm or less. By adjusting the warp density within the above range, the irregular monofilaments are likely to be arranged in a single row and / or double row, which is preferable. The weft density of the woven fabric is, for example, preferably 50 / 2.54 cm or more, more preferably 80 / 2.54 cm or more, and even more preferably 100 / 2.54 cm or more, and preferably 400 / 2.54 cm or less, more preferably 350 / 2.54 cm or less, and even more preferably 250 / 2.54 cm or less. The greige density and the finished density of the woven fabric may be the same or different.

[0039] The woven fabric is preferably refined, relaxed, preset dyed, finished, etc., using a general processing machine for thin fabrics. The woven fabric can also be subjected to softening, resin processing, silicone processing, etc., in order to adjust the texture and strength of the fabric. In the softening process, for example, amino-modified silicone, polyethylene-based, polyester-based, paraffin-based softeners, etc. can be used as the softening agent. In the resin processing, for example, various resins such as melamine resin, glyoxal resin, urethane-based, acrylic-based, polyester-based, etc. can be used as the resin processing agent.

[0040] In the present invention, a resin coating layer is laminated on one side of the woven fabric. One side of the woven fabric refers to the front or back side of the woven fabric. When coating the woven fabric with a resin that will become a moisture-permeable waterproof membrane, it is preferable to treat the woven fabric with a water repellent agent before laminating the resin coating layer. This is one way of preventing the resin solution from penetrating into the interior of the fabric during the manufacture of a moisture-permeable waterproof fabric. In this case, the water repellent agent may be a known agent such as a paraffin-based water repellent agent, a polysiloxane-based water repellent agent, or a fluorine-based water repellent agent, and the treatment may be a known method such as a commonly used padding method or spray method. When particularly good water repellency is required, a fluorine-based water repellent agent may be used, for example, by attaching Asahi Guard E061 (manufactured by AGC Corporation, a fluorine-based water repellent emulsion) at a concentration of 1 to 3% based on the fiber weight by a padding method, and then performing a heat treatment at 160°C for 1 minute.

[0041] In the present invention, by laminating an extremely thin resin coating layer on one side of the woven fabric (the side facing the skin when used as clothing), it is possible to significantly improve the abrasion resistance of the surface of the fabric, not only waterproofing, but also without compromising the original texture, thickness, and lightness of the lightweight, thin fabric. Although the reason why the abrasion resistance of the surface of the fabric is greatly improved by adhering an extremely thin layer of resin to one side of the fabric is not clear, it is thought that this is due to the anchor effect, in which the fibers on the back and front sides of the fabric are bonded together by the resin, making it difficult for the fibers to move within the fabric even if they are pulled by surface friction.

[0042] In the present invention, a fabric such as a woven fabric or knitted fabric is counted as one layer, and a resin coating film is counted as one layer. Specifically, 2 layers refers to a fabric coated with resin. A pattern layer with resin printed on it may be applied to the outer layer of the resin coating layer. In the present invention, this pattern layer is counted as 0.5 layers, and a layer configuration of woven fabric / resin coating layer / pattern layer is called 2.5 layers in the present invention. In addition, 3 layers refers to a fabric such as warp knit or circular knit attached to the lower surface of the film of the above 2 layers.

[0043] 6 and 7 show SEM cross-sectional photographs of an example of the fabric of the present invention.

[0044] The purpose of adding the 0.5 layer in the present invention is to provide design by laminating a pattern layer on the resin coating layer, to hide defects in processing such as coating streaks, to improve tack and comfort by improving the slipperiness, and to improve the abrasion resistance of the urethane resin layer. This pattern layer is mainly made of synthetic resin and is formed by applying it uniformly to the non-entire surface by gravure coating, rotary printing, flat screen printing, etc. As such synthetic resin, polyurethane resin, polyester resin, polyamide resin, acrylic resin, silicone resin, vinyl chloride resin, polyolefin resin, ethylene-vinyl acetate resin, etc. can be used, and these may be used alone or in mixture. In addition, when giving a slipperiness to the pattern layer, it is preferable to contain a lubricant. The lubricant is not particularly limited, and examples of organic lubricants include silicone compounds such as polydimethylsiloxane, and various heat-resistant organic filler fine powders. Examples of inorganic lubricants include silicon dioxide fine powder obtained by a wet method (precipitation method, gel method), various inorganic filler fine powders, etc. Furthermore, the pattern layer may contain cosmetic agents such as dyes, pigments, fillers, and pearl pigments, and functional agents such as heat storage agents, antibacterial agents, and deodorants, if necessary. In the present invention, another woven or knitted fabric may be laminated on the outside of the resin part of the two-layer moisture-permeable and waterproof fabric (three-layer fabric sandwich).

[0045] The resin coating layer is preferably a porous film (hereinafter, sometimes referred to as a "porous film"). When the resin coating layer is a porous film through which water vapor can pass through the holes, moisture permeability can be imparted to the fabric having the resin coating layer. There are a wet method and a dry method for forming the porous film. In the present invention, either the wet method or the dry method may be used, but the dry method is preferably used since it is advantageous for producing a lightweight and thin fabric.

[0046] The fabric is a polyurethane resin film with a mass of 15 g / m on a water-repellent treated fabric.2 Less than 1 g / m 2 More than 10g / m 2 The following porous membrane is preferably formed. The porous membrane is formed by dissolving the polyurethane formulation solution in a solution such that the mass of the dried resin membrane is 1 to 10 g / m 2 It is preferable to coat the resin film so that the mass of the dry resin film is 10 g / m 2 If the thickness exceeds this range, the amount of resin increases and the thickness of the resin coating layer increases, so that the fabric tends to become heavy and hard.

[0047] The thickness of the porous film forming the resin coating layer can be about 1 μm to 30 μm. In particular, the thickness of the porous film is preferably 1 μm or more, more preferably 1.5 μm or more, and even more preferably 2 μm or more, and is preferably 30 μm or less, more preferably 20 μm or less, and even more preferably 10 μm or less. If the thickness of the porous film is less than 1 μm, the waterproofness of the fabric is reduced. If the thickness of the porous film exceeds 30 μm, the fabric obtained becomes heavy and the feel becomes hard. As a method for forming the resin coating layer of the porous film, either a wet method or a dry method may be used, but in order to keep the thickness of the resin coating layer low, a dry method is more advantageous than a wet method.

[0048] Next, a method for forming a porous urethane film using a wet method will be exemplified. In the method for forming a porous urethane film using a wet method, a synthetic polymer solution mainly composed of a polyurethane resin is dissolved in water so that the mass of the dried resin film is 1 to 10 g / m 2 After coating so that the resin solidifies in water at 5 to 30°C, the resin is washed with hot water at 30 to 80°C, and then dried to form a porous film. 2 It is difficult to achieve a water pressure resistance of 500 mm or more with a thickness of less than 10 g / m 2If the thickness exceeds 0.1 g / m, the thickness of the resulting fabric will be large and the weight of the fabric will tend to be heavy. When applying the resin solution, a knife coater, a comma coater, a reverse coater, or the like may be used for coating, but a direct coating method such as a floating knife method, a knife-on-roll method, or a knife-on-bed method is preferred from the viewpoint of productivity because it is fast and low cost. Among the direct coating methods, the floating knife method in particular can be used to achieve a coating thickness of 0.1 g / m 2 More than 10g / m 2 Coating is relatively easy with the following application weight:

[0049] The synthetic polymer mainly composed of polyurethane resin used to form the resin coating layer may be a copolymer obtained by reacting polyisocyanate with polyol, but as the solvent for the polymer, a resin solution mainly composed of a polar organic solvent suitable for wet film formation such as N,N-dimethylformamide or N-methylpyrrolidone, and the like, and the viscosity of the resin solution is preferably close to Newtonian viscosity in terms of the fluidity of the resin liquid, the quality of the coating obtained, and the moisture permeability and waterproofing performance.

[0050] As a resin liquid for forming a resin coating layer using a wet method, for example, a solution formed by dissolving the polyurethane resin in a polar organic solvent can be used. Examples of the polar organic solvent that can be used include N,N-dimethylformamide, dimethylacetamide, dimethylsulfoxide, N-methylpyrrolidone, and hexamethylenephosphonamide.

[0051] The synthetic polymer mainly composed of polyurethane resin as referred to here means one consisting only of polyurethane resin or one containing 50% or more of a polyurethane component. Examples of synthetic polymers containing synthetic polymers other than polyurethane resin include polyacrylic acid, polyvinyl chloride, polystyrene, polybutadiene, polyamino acids, and copolymers thereof. Of course, compounds modified with fluorine, silicone, etc. can also be used.

[0052] A typical example of a method for making a porous film using a dry method is described below. One method is to apply a polyurethane emulsion of W / O type emulsion to a woven fabric, and then heat-treat the woven fabric to volatilize organic solvents with a boiling point lower than that of water, such as toluene and methyl ethyl ketone, contained in the W / O type emulsion, and solidify the polyurethane with the remaining water, and then evaporate the water to form a porous resin coating layer on the coating film. Another method is a foaming method. Examples of the foaming method include a method in which thermally expandable microcapsules are added to a polyurethane solution, the polyurethane solution is applied to a woven fabric, laminated, and then heat-treated to expand (foam) the microcapsules to form a porous resin coating layer, and a method (chemical foaming method) in which carbon dioxide gas is generated by the reaction of water with isocyanate using water or steam as a foaming agent to form a porous resin coating layer on the woven fabric. In the present invention, any of the above methods can be used, but the method using a polyurethane emulsion of W / O type emulsion is particularly preferred. By forming a porous membrane using a W / O type polyurethane emulsion, the thickness of the porous membrane can be made thinner, and moisture permeability can be improved.

[0053] In the case of a method of using a polyurethane emulsion of W / O type emulsion in the formation of a porous membrane using a dry method, the volatile solvent may be a ketone solvent or an aromatic hydrocarbon solvent, etc., and examples of the ketone solvent include acetone, methyl ethyl ketone (MEK), methyl isobutyl ketone, etc., and examples of the aromatic hydrocarbon solvent include toluene, xylene, etc. The particle size of the polyurethane fine particles in the polyurethane emulsion is preferably about 0.05 μm or more and 5 μm or less.

[0054] The heat treatment temperature for forming a porous resin coating layer varies depending on the type of polyurethane and the foaming method, but for example, heat treatment may be performed at about 60°C to 200°C for about 1 second to 1 hour. In particular, when using a polyurethane emulsion of W / O type emulsion, it is also preferable to perform heat treatment in two stages. For example, in order to volatilize the low-boiling organic solvent first, heat treatment may be performed in advance at 40°C to 110°C, more preferably 50°C to 90°C, for about 10 seconds to 10 minutes, and then heat treatment may be performed at 100°C to 200°C for about 15 seconds to 10 minutes to form a porous resin coating layer (film formation).

[0055] In order to improve the strength of the porous membrane formed by the dry method, it is also preferable to include an isocyanate-based crosslinking agent in the solid content of the resin solution forming the porous membrane in an amount of 1% by mass to 12% by mass. More preferably, it is preferable to include an isocyanate-based crosslinking agent in an amount of 2% by mass to 10% by mass. If the content of the isocyanate-based crosslinking agent in the resin solution forming the porous membrane is less than 1% by mass, the strength of the porous membrane and the adhesive strength with the fabric body may not be improved. On the other hand, if the content of the isocyanate-based crosslinking agent in the resin solution forming the porous membrane exceeds 12% by mass, the texture of the porous membrane may become hard.

[0056] Examples of isocyanate crosslinking agents include tolylene 2,4-diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate, and hexamethylene diisocyanate. In addition, triisocyanates obtained by addition reaction of these diisocyanates with compounds containing active hydrogen are also used. Examples of compounds containing active hydrogen include trimethylolpropane and glycerin.

[0057] The thickness of the resin coating layer is preferably at least 1 μm to 10 μm. In other words, the resin coating layer preferably includes a portion having a thickness of 1 μm to 10 μm. By making the thickness of the resin coating layer at least 1 μm to 10 μm, the fabric can be made lightweight while exhibiting sufficient waterproofness and abrasion resistance.

[0058] In order to make the thickness of the resin coating layer at least 1 μm or more and 10 μm or less, it is preferable to form the resin coating layer by a dry method. Conventionally, when forming a resin coating layer on a fabric, it has been common to use the above-mentioned wet method in which the resin forming the resin coating layer is applied to the fabric and the fabric is immersed in a coagulating liquid that coagulates the resin to form a film. In the film formation by the wet method, the film thickness of the resin coating layer can be increased and the water pressure resistance of the fabric can be improved, but the weight of the fabric becomes heavy. On the other hand, in forming a resin coating layer on a fabric, by using a dry method in which the resin forming the resin coating layer is applied to the fabric and dried to form a film, a resin coating layer with a smaller thickness than that of the wet method can be formed, and it is possible to make a lightweight fabric while preventing water permeation.

[0059] In the present invention, when the amount of resin applied to the woven fabric is reduced and the coating process is performed, it is necessary to reduce the viscosity of the resin. In this case, if the woven fabric has a low density, the resin may partially impregnate the woven fabric and may strike through during processing. Therefore, the woven fabric of the present invention uses a high-density woven fabric. Before the resin coating process, the fabric is subjected to a calendar process to reduce the unevenness of the woven fabric, which makes it easier to apply the resin uniformly with a thin film thickness. Therefore, it is preferable to apply the coating process to the surface of the woven fabric that has been subjected to the calendar process. In other words, it is preferable that the resin coating layer is laminated on the surface of the woven fabric that has been subjected to the calendar process.

[0060] As described above, in forming the resin coating layer, the fabric is resin-coated using a knife or the like, so pressure is applied to the fabric during resin coating. Therefore, the resin constituting the resin coating layer may penetrate between or into the fibers constituting the fabric. In other words, the fabric may have a portion where the resin constituting the resin coating layer penetrates into the interior of the fabric that the fabric has.

[0061] In the present invention, it is also preferable to further apply a water-repellent treatment after forming a moisture-permeable waterproof layer on the woven fabric in order to further improve waterproofing. The water-repellent agent used may be a known agent such as a paraffin-based water-repellent agent, a polysiloxane-based water-repellent agent, or a fluorine-based water-repellent agent, as in the pretreatment described above, and the water-repellent treatment may be performed by a padding method, a spraying method, a coating method, or the like as appropriate. Note that this treatment is not included in the number of layers described above.

[0062] The thickness of the fabric according to the present invention is preferably 40 μm or more and 85 μm or less. More preferably, it is desirable that it is 70 μm or less. On the other hand, if the thickness of the fabric is less than 40 μm, sufficient abrasion resistance and sufficient tear strength are not obtained. Also, if the thickness of the fabric is more than 85 μm, the texture is hard and the product using the present invention tends to be bulky when folded and carried.

[0063] The fabric weight is 70g / m 2 It is preferable that the thickness is less than 60 g / m 2 More preferably, it is 50 g / m or less. 2 More preferably, it is 20 g / m or less. 2 It is preferable that the thickness is 25 g / m or more. 2 More preferably, it is 30 g / m or more. 2 It is more preferable that the weight of the fabric is 20 g / m or more. 2 If it is less than this, the fabric will have a light weight, but will not have sufficient tear strength or water pressure resistance.

[0064] <Moisture permeability> The fabric is preferably a moisture-permeable waterproof fabric having moisture permeability, and has a moisture permeability of 4000 g / m according to JIS L 1099:2012 3.7.1.1 A-1 method (calcium chloride method). 2 It is preferable that the moisture permeability of the fabric is 4000g / m 2 If the moisture permeability is 24 hours or more, stuffiness can be suppressed when the fabric is used as clothing. The moisture permeability of the fabric is more preferably 7000 g / m 2 More than 24 hours.

[0065] <Waterproof> The water pressure resistance of the fabric, which is an index of waterproofness, is preferably 5 kPa or more according to JIS L1092:2009 7.1.2 B method (high water pressure method). The upper limit of the water pressure resistance of the fabric varies depending on the type of fiber constituting the fabric, the composition of the resin layer, etc., but is roughly 10 kPa.

[0066] <Tear strength> The tear strength of the fabric according to JIS L1096:2010 8.15.5 D method (pendulum method) is not particularly limited, but is preferably 9.8N or more in both the warp and weft directions, more preferably 12N or more, even more preferably 20N or more, preferably 50N or less, more preferably 40N or less, and even more preferably 30N or less. By setting the tear strength of the fabric within the above range, a fabric that is light and thin and has the necessary tear strength can be obtained. On the other hand, if the tear strength is less than 9.8N, the tear strength of the fabric may be insufficient depending on the application. Also, if the tear strength exceeds 50N, the fineness of the woven fabric constituting the fabric needs to be increased, which is undesirable because the fabric tends to become thick and hard.

[0067] <Wear resistance> The fabric preferably can withstand 50 or more cycles before breaking in an abrasion test according to JIS L1096:2010 8.19 A-1 method (flat method). In a more preferred embodiment, the fabric can withstand 60 or more cycles before breaking in an abrasion test, in an even more preferred embodiment, 100 or more cycles, and in a particularly preferred embodiment, 120 or more cycles.

[0068] <Application> The fabric according to the present invention thus obtained is a lightweight, thin, moisture-permeable, waterproof, high-density woven fabric, and has excellent abrasion resistance not previously available, and therefore the fabric according to the present invention can be preferably used for the lining of downwear, down jackets, windbreakers, futons, sleeping bags, rainwear, tents, bags, backpacks, etc. EXAMPLES

[0069] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples, and can be modified as long as it meets the gist of the invention, and all of these modifications are included in the technical scope of the present invention. The performances of the examples and comparative examples of the present invention were evaluated by the following methods.

[0070] <Relative viscosity> A sample solution was prepared by dissolving the sample in 96.3±0.1% by mass of reagent-grade concentrated sulfuric acid to a polymer concentration of 10 mg / ml. Using an Ostwald viscometer with a water drop time of 6 to 7 seconds at a temperature of 20°C±0.05°C, the drop time T1 (seconds) of 20 ml of the prepared sample solution and the drop time T0 (seconds) of 20 ml of 96.3±0.1% by mass of reagent-grade concentrated sulfuric acid used to dissolve the sample were measured at a temperature of 20°C±0.05°C. The relative viscosity (RV) of the resin used was calculated using the following formula. RV=T1 / T0

[0071] <Measurement of single fiber cross section> (1) Measuring the length of a side Using a VH-Z450 microscope and a VH-6300 measuring instrument (Keyence Corporation), the length of each side of the cross section of the irregular monofilament was measured at a magnification of 1500 times, and the average value of the three measured values ​​was taken as the side length.

[0072] (2) Measurement of interior angles Using a VH-Z450 microscope and a VH-6300 measuring instrument (manufactured by Keyence Corporation), the cross section of the irregular monofilament was photographed at a magnification of 1500 times, and the acute and obtuse angles were measured using a commercially available protractor (manufactured by Kokuyo Co., Ltd.). The average value of the measurements for each of the three pieces was taken as the angle.

[0073] <Single yarn size (monofilament size)> The single filament fineness was calculated by subtracting the number of filaments from the total fineness of the multifilament. Single yarn size = total size / number of filaments

[0074] <Total fineness (multifilament fineness)> Three 100 m long skeins of multifilament were prepared, and the mass (g) of each was measured, the average value was calculated, and multiplied by 100 to obtain the total fineness.

[0075] <Cover factor> The cover factor (CF) of the fabric was calculated according to the following formula. CF = (T × (DT)) 1 / 2 +(W×(DW)) 1 / 2 [In the formula, T and W represent the warp and weft densities (counts / 2.54 cm) of the fabric, and DT and DW represent the thickness (dtex) of the warp and weft threads constituting the fabric.]

[0076] <Water repellency> The water repellency of the fabric was measured based on JIS L1092:2009 7.2 Water repellency test (spray test). The water repellency after 0 washes is measured using a fabric sample before washing, and the water repellency after 20 washes is measured using a fabric sample after washing 20 times by the washing method described below.

[0077] <Washing Instructions> The washing of the fabric was carried out in accordance with the C4N method described in JIS L1930:2014 Appendix F. "After 20 washes" refers to the measurement result after washing, spin-drying and drying were repeated 20 times. The drying was carried out by hanging to dry. The water repellency after 20 washes was measured by the above-mentioned method.

[0078] <Wear test> The abrasion test was performed in accordance with JIS L1096:2010 8.19 A-1 method (plane method). The test piece was placed face up on the rubber membrane of a universal testing machine and fixed with a clamp. The mass of the sample (g / m2) was removed from the abrasive paper specified in JIS R6253. 2) was selected and fixed to the crank of the testing machine, and a pressure load was applied to rub the test piece in multiple directions. The end point was when the test piece was worn down to form a hole of 8 mm ± 1 mm, and the number of frictions at that point was calculated, and the average value of five abrasion tests was calculated. In the present invention, the high-density woven surface of the fabric was used as the measurement surface to measure the friction durability of the fabric surface.

[0079] <Tear strength> The tear strength of the fabric was measured in both warp and weft directions in accordance with JIS L1096:2010 8.15.5 Tear Strength Method D (Pendulum Method).

[0080] <Moisture permeability of fabric> The moisture permeability of the fabric was measured according to JIS L1099:2012 3.7.1.1 A-1 method (calcium chloride method). The temperature was 40°C and the humidity was 90% RH, and the average value was n=3. The moisture permeability of the fabric was also measured according to JIS L1099:2012 3.7.2.1 B-1 method (potassium acetate method).

[0081] <Water pressure resistance of fabric> The water pressure resistance of the fabric was measured in accordance with JIS L1092:2009 7.1.2 Method B (high water pressure method).

[0082] Example 1 A nylon 6 polymer chip having a relative viscosity of 3.5 was melt-spun from a spinneret having seven discharge holes (with a shape shown in FIG. 5, L1: 0.481 mm, L2: 0.481 mm, L3: 0.07 mm, angle a: 54°) at a spinning temperature of 282° C. Of the two godet rollers, the speed of the first godet roller was set to 2800 m / min, the speed of the second godet roller was set to 4000 m / min, and the temperature of the second godet roll was set to 160° C. to obtain a synthetic multifilament having a fineness of 17 dtex and consisting of seven monofilaments having a rhombic cross section with an angle a: 54°, sides A and A': 18.7 μm, and sides B and B': 18.7 μm in the approximately rectangular shape shown in FIG. 1. The synthetic multifilament was used for the warp and weft, and the warp density was set to 213 threads / 2.54 cm and the weft density was set to 181 threads / 2.54 cm, and the fabric was woven in a ripstop structure.

[0083] The fabric was scoured and dyed in the usual way (acid dye DiacidFast Red 3B: 2% owf, manufactured by Mitsubishi Chemical Corporation). It was then padded with a 5% by mass aqueous dispersion of Asahiguard E061 (fluorine-based water repellent emulsion, manufactured by AGC Corporation) (squeezing rate 35%), dried, and heat-treated at 160°C for 1 minute to obtain a fabric for coating. The obtained fabric had a warp density of 226 threads / 2.54 cm and a weft density of 197 threads / 2.54 cm.

[0084] Next, the laminate was calendered at a temperature of 160°C, a pressure of 30 kg / cm, and a speed of 20 m / min using a calendering machine with a mirror roll, and the resin solution shown in the following formulation 1 was applied at a coating amount of 8 g / m using a floating knife coater. 2 The solution was applied to the surface of the fabric that had been calendared using a drying method at 80°C for 2 minutes, and then dry-heat treated at 150°C for 1 minute to obtain a fabric with a porous film having an average thickness of 5 μm.

[0085] (Formulation 1) Heimullen X-3040 (manufactured by Dainichiseika Chemicals Mfg. Co., Ltd., ether-based polyurethane resin, solid content 30%, solvent: MEK:water = 94:6) 100 parts by weight Resamine X (isocyanate compound, manufactured by Dainichiseika Color & Chemicals Mfg. Co., Ltd.) 2 parts by weight Methyl ethyl ketone: 15 parts by mass Toluene: 15 parts by mass White pigment...5 parts by mass Water...40 parts by mass

[0086] The results of evaluation of the obtained fabric such as warp density, weft density, tear strength, abrasion evaluation, water resistance, water repellency, moisture permeability, etc., as well as the results of evaluation of products using the fabric are shown in Table 1.

[0087] Example 2 A fabric was produced in the same manner as in Example 1, except that the first layer of fabric was woven in a ripstop structure using 22 dtex, 7 filament diamond-shaped nylon 6 fiber with a warp density of 182 threads / 2.54 cm and a weft density of 177 threads / 2.54 cm, and was evaluated. The results are shown in Table 1.

[0088] Example 3 A fabric was produced in the same manner as in Example 1, except that the first layer of fabric was woven in a ripstop structure using 11 dtex, 5 filament diamond-shaped nylon 6 fiber, with a warp density of 256 threads / 2.54 cm and a weft density of 230 threads / 2.54 cm, and was evaluated. The results are shown in Table 1.

[0089] Example 4 A fabric was produced in the same manner as in Example 1, except that the first layer of fabric was woven in a ripstop structure using 17 dtex, 7 filament diamond-shaped polyester fiber with a warp density of 213 threads / 2.54 cm and a weft density of 181 threads / 2.54 cm, and was evaluated. The results are shown in Table 1.

[0090] Example 5 A fabric was produced in the same manner as in Example 1, except that the weft of the first layer of the fabric was made of 17 dtex, 7 filament, round cross section nylon fiber, the warp density was set to 213 threads / 2.54 cm, the weft density was set to 181 threads / 2.54 cm, and the fabric was woven in a ripstop structure, and evaluation was performed. The results are shown in Table 1.

[0091] Example 6 A fabric was produced in the same manner as in Example 1, except that the warp yarn of the first layer of the woven fabric was a 17 dtex, 7 filament, round cross section nylon fiber, the warp density was set to 213 threads / 2.54 cm, the weft density was set to 181 threads / 2.54 cm, and the fabric was woven in a ripstop structure, and evaluation was performed. The results are shown in Table 1.

[0092] Example 7 The polyurethane porous film forming resin solution (solid content 21%, viscosity 15000 mPa s / 25°C) of the following formulation 2 was applied at a rate of 60 g / m 2 The mixture was then solidified in water at 20°C for 1 minute, washed with overflowing hot water at 40°C for 5 minutes, dried at 120°C for 2 minutes, and cured at 170°C for 1 minute to obtain a fabric with a porous film having an average thickness of 30 μm.

[0093] (Formulation 2) Laxskin UJ8517 (Seiko Chemicals Corporation, polyurethane resin for wet film formation, solid content 27%) ··· 100 parts by weight Luxkin UJ8518M (Seiko Chemicals Corporation, polyurethane resin containing silica to improve moisture permeability, solid content 21%)...30 parts by weight Resamine X (isocyanate compound, manufactured by Dainichiseika Color & Chemicals Mfg. Co., Ltd.) 1 part by mass N,N-Dimethylformamide ··· 25 parts by mass

[0094] Comparative Example 1 A fabric was produced in the same manner as in Example 1, except that the first layer of fabric was woven in a ripstop structure using 44 dtex, 12 filament diamond-shaped nylon 6 fiber with a warp density of 145 threads / 2.54 cm and a weft density of 135 threads / 2.54 cm, and was evaluated. The results are shown in Table 1.

[0095] Comparative Example 2 A fabric was produced in the same manner as in Example 1, except that the first layer of the fabric was woven in a ripstop structure using 17 dtex, 12 filament, circular cross section nylon 6 fiber, with a warp density of 214 / 2.54 cm and a weft density of 170 threads / 2.54 cm. The results are shown in Table 1.

[0096] Comparative Example 3 A fabric was produced in the same manner as in Example 1, except that the first layer of fabric was woven in a ripstop structure using 22 dtex, 20 filament, round cross section nylon 6 fiber, with a warp density of 178 / 2.54 cm and a weft density of 161 threads / 2.54 cm, and was evaluated. The results are shown in Table 1.

[0097] Comparative Example 4 A woven fabric was woven in the same manner as in Example 1. It was dyed by a conventional method and dyed and finished by a known method. Then, it was calendered once. Then, the woven fabric was impregnated with a 5% solution of Asahiguard E061, squeezed with a mangle, dried, and then heat-treated at 160°C for 30 seconds. The resin shown in the following formulation 3 was applied to a release paper using a knife coater, and dried at 100°C using an air oven to obtain a resin non-porous film. A resin non-porous film was applied to the surface of the woven fabric that had been calendered using an adhesive resin by a lamination method, and evaluation was performed. The results obtained are shown in Table 1. Also, a cross-sectional SEM photograph of the obtained laminated fabric is shown in FIG. 8.

[0098] (Formulation 3) Water-swellable ester polyurethane resin: 75 parts Water-swellable ether-based polyurethane resin: 35 parts N,N'-Dimethylformamide 80 parts HU-720P (moisture absorbing / releasing fine particles: manufactured by Nippon Exlan Kogyo Co., Ltd.) ··· 10 parts Coronate HL ··· Division 3

[0099] Comparative Example 5 The first layer of fabric was prepared in the same manner as in Example 1, and then dyed, water-repellent, and calendered to prepare a woven fabric, which was then evaluated. The results are shown in Table 1.

[0100] [Table 1] [Industrial Applicability]

[0101] The present invention makes it possible to obtain a lightweight, thin, breathable and waterproof fabric, which can be made into a more abrasion-resistant fabric. Since the fabric is also extremely durable, it is possible to provide high-performance clothing, which is expected to make a significant contribution to the industrial sector. [Explanation of symbols]

[0102] A, A', B, B', L1, L2: Lengths of the sides of an approximate rectangle a, a', b, b': interior angles of an approximate rectangle P, Q, R, S: Convex T, U, V, W: Concave L3: Depth of recess

Claims

1. A fabric having a woven material using multifilament warp and weft, At least one of the warp yarns and the weft yarns has a substantially rectangular fiber cross section, a single yarn fineness of 1 dtex or more and 3.5 dtex or less, and a total fineness of 5 dtex or more and 23 dtex or less, The fabric has a resin coating layer laminated on one surface of the woven fabric.

2. The fabric according to claim 1 , wherein the resin coating layer has a thickness of at least 1 μm to 10 μm.

3. The fabric according to claim 1 or 2, wherein the resin coating layer is a perforated film.

4. The fabric according to claim 1 or 2, wherein the cover factor of the woven fabric is 1,600 or more and 1,800 or less.

5. The fabric has a basis weight of 60 g / m 2 3. The fabric according to claim 1 or 2, wherein:

6. 3. The fabric according to claim 1 or 2, which has abrasion resistance of 50 or more times in an A-1 universal type abrasion resistance test in accordance with JIS L1096.

7. 3. The fabric according to claim 1, wherein the tear strength in the warp direction is 9.8 N or more and the weft direction is 9.8 N or more in a tear strength test according to JIS L1096 D method.

Citation Information

Patent Citations

  • Moisture-permeable, water-proof composite film and moisture-permeable, water-proof composite sheet using the film

    JP2005074855A

  • Moisture-permeable waterproof fabric and fiber product

    JP2013226750A

  • Thin woven fabric

    WO2016113833A1