Silicon member and production method thereof
By bonding single-crystal silicon members with shifted cleavage directions, the silicon member addresses cracking issues in plasma processing apparatuses, ensuring stability and durability under thermal stress.
Patent Information
- Application Number
- JP2023055468
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-03-30
AI Technical Summary
Plasma processing apparatuses face issues with silicon members cracking due to increased high-frequency power, thermal expansion, warping, and thermal shock, particularly in large silicon members with through holes, which are prone to cracking during processing.
A silicon member is constructed by bonding multiple single-crystal silicon members with their cleavage directions shifted by 5° or more, ensuring that the cleavage directions at the bonding surfaces are different, thereby reinforcing the structure to prevent cracking.
The silicon member effectively suppresses cracking and ensures stable operation by distributing bending stress evenly, enhancing the silicon member's durability and resistance to thermal stress.
Smart Images

Figure 2024143017000002 
Figure 2024143017000003 
Figure 2024143017000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a silicon member used in a plasma processing apparatus and a method for manufacturing the silicon member. [Background technology]
[0002] Conventionally, in plasma processing apparatuses such as plasma etching apparatuses and plasma CVD apparatuses used in semiconductor device manufacturing processes, an electrode plate connected to a high-frequency power source and a stand are arranged, for example, one above the other in a chamber of the apparatus, and a silicon wafer is placed on the stand. A high-frequency voltage is applied while gas is caused to flow toward the silicon wafer from through holes (ventilation holes) formed in the electrode plate to generate plasma, and processing such as etching is performed on the silicon wafer.
[0003] In the above-mentioned plasma processing apparatus and the like, silicon members are widely used to suppress metal contamination in the chamber. For example, as an electrode plate used in a plasma processing apparatus, a silicon member having a structure in which a plurality of ventilation holes are formed in a silicon plate material is used.
[0004] Here, in order to suppress the generation of contamination and particles, the silicon members disposed in the chamber of a plasma processing apparatus or the like are made of single crystal silicon, which is the same material as the wafer to be processed, as shown in Patent Document 1, for example. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 3744726 Summary of the Invention [Problem to be solved by the invention]
[0006] In recent years, in the above-mentioned plasma processing apparatus, the output of high frequency waves applied has increased dramatically in order to improve the processing speed and processing accuracy of wafers. Accordingly, the heat input from the plasma to the silicon member has increased. As a result, the silicon member is not sufficiently cooled, and there is a risk that the silicon member may crack due to warping caused by thermal expansion or heat distribution of the silicon member or instantaneous thermal shock.
[0007] In particular, since single crystal silicon has a tendency to crack along the cleavage plane, when bending stress, such as that caused by applying a load along the cleavage direction, acts on the silicon member, cracks are likely to occur. Furthermore, silicon members disposed in the chamber of a plasma processing apparatus or the like are relatively large and require processing to form through holes and the like, and there is a risk that cracks may easily occur during this processing.
[0008] The present invention has been made in consideration of the above-mentioned circumstances, and has an object to provide a silicon member that can suppress the occurrence of cracks and can be used stably, and a method for manufacturing the silicon member. [Means for solving the problem]
[0009] In order to solve the above problems, the silicon member of aspect 1 of the present invention is a silicon member used in a plasma processing apparatus, and has a structure in which a plurality of single crystal silicon members are bonded together, and a pair of the single crystal silicon members stacked via a bonding surface are arranged such that the cleavage directions at the bonding surfaces are shifted by 5° or more.
[0010] According to the silicon member of aspect 1 of the present invention, a plurality of single crystal silicon members are bonded together, and a set of the single crystal silicon members are stacked via their bonding surfaces, and are arranged such that the cleavage directions at the bonding surfaces of the single crystal silicon members are offset from each other. Since the cleavage directions of the stacked single crystal silicon members are different from each other, the single crystal silicon members reinforce each other, and it is possible to suppress the occurrence of cracks in the silicon member even when bending stress is applied.
[0011] The silicon member of aspect 2 of the present invention is characterized in that in the silicon member of aspect 1, a pair of the single crystal silicon members stacked via a bonding surface have bonding surfaces each having the same crystal plane orientation. According to the silicon member of aspect 2 of the present invention, the bonding surfaces of a pair of the single crystal silicon members stacked via the bonding surfaces have the same crystal plane orientation. Therefore, by rotating the pair of the single crystal silicon members in an in-plane direction, the pair of the single crystal silicon members can be stacked so that the cleavage directions at the bonding surfaces are shifted.
[0012] The silicon member of aspect 3 of the present invention is characterized in that in the silicon member of aspect 1, a pair of the single crystal silicon members stacked via a bonding surface have bonding surfaces having different crystal plane orientations. According to the silicon member of aspect 3 of the present invention, the bonding surfaces of a pair of the single crystal silicon members stacked via the bonding surfaces have different crystal plane orientations, and therefore the cleavage directions at the bonding surfaces are different from each other. Therefore, the pair of the single crystal silicon members can be stacked so that the cleavage directions at the bonding surfaces are shifted.
[0013] The manufacturing method of a silicon member according to aspect 4 of the present invention is a manufacturing method of a silicon member according to any one of aspects 1 to 3, and is characterized by having a crystal orientation confirmation step of confirming the crystal orientation of the bonding surfaces of the single crystal silicon members, a single crystal silicon member stacking step of stacking a pair of the single crystal silicon members in such a manner that the cleavage directions at the bonding surfaces are shifted from each other, and a bonding step of bonding the stacked pair of the single crystal silicon members.
[0014] According to the manufacturing method of a silicon member of aspect 4 of the present invention, it is possible to stably manufacture a silicon member having a structure in which a plurality of single crystal silicon members are bonded together, and a set of the single crystal silicon members are stacked via their bonding surfaces, and the cleavage directions of the bonding surfaces of the single crystal silicon members are arranged so as to be misaligned. Effect of the Invention
[0015] According to the present invention, it is possible to provide a silicon member capable of suppressing the occurrence of cracks and being stably usable, and a method for manufacturing the silicon member. [Brief description of the drawings]
[0016] [Figure 1] 1A and 1B are explanatory views showing an example of a silicon member according to an embodiment of the present invention, in which (a) is a perspective view and (b) is an enlarged explanatory view of a bonding portion. [Diagram 2] FIG. 2 is an explanatory diagram of a single crystal silicon member constituting the silicon member according to one embodiment of the present invention. [Diagram 3] FIG. 1 is a flow diagram showing a method for manufacturing a silicon member according to an embodiment of the present invention. [Figure 4] 4 is an explanatory diagram of a lamination step in the method for producing the silicon member shown in Fig. 3. (a) shows alignment using a notch, and (b) shows alignment using a pin. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] A silicon member according to an embodiment of the present invention and a method for manufacturing the silicon member will be described below. The silicon member of this embodiment is, for example, a silicon member arranged in a chamber of a plasma processing apparatus such as a plasma etching apparatus or a plasma CVD apparatus used in a semiconductor device manufacturing process, and in this embodiment, is a silicon electrode plate having a structure in which a plurality of air holes are formed in the silicon plate material.
[0018] The silicon member 10 of this embodiment includes a plurality of vent holes 10A penetrating in the thickness direction, a first single crystal silicon member 11, and a second single crystal silicon member 12, as shown in FIG. As shown in FIGS. 1(a) and 1(b), the silicon member 10 of this embodiment has a structure in which a first single crystal silicon member 11 and a second single crystal silicon member 12 are bonded in the thickness direction, and the first single crystal silicon member 11 and the second single crystal silicon member 12 are stacked with a bonding layer 15 interposed therebetween.
[0019] In this embodiment, the bonding layer 15 is made of silicon oxide, and the first single crystal silicon member 11 and the second single crystal silicon member 12 are bonded to each other via the silicon oxide constituting the bonding layer 15. In this embodiment, the silicon oxide constituting the bonding layer 15 is SiO2.
[0020] In this embodiment, the bonding surface of the first single crystal silicon member 11 and the bonding surface of the second single crystal silicon member 12 have the same crystal plane orientation, and in this embodiment, the bonding surface of the first single crystal silicon member 11 and the bonding surface of the second single crystal silicon member 12 are each a (100) plane. Here, in the (100) plane of single crystal silicon, as shown in FIG. 2, the cleavage directions are two directions (X direction and Y direction) that are perpendicular to each other.
[0021] In this embodiment, the first single crystal silicon member 11 is arranged such that the cleavage direction (X1 direction, Y1 direction) at the bonding surface of the first single crystal silicon member 11 and the cleavage direction (X2 direction, Y2 direction) at the bonding surface of the second single crystal silicon member 12 are misaligned (i.e., the cleavage direction (X1 direction, Y1 direction) and the cleavage direction (X2 direction, Y2 direction) do not coincide with each other). The "cleavage direction at the bonding surface" is the direction in which the cleavage direction of the single crystal silicon member is projected onto the bonding surface.
[0022] Here, in this embodiment, as shown in FIG. 2(b), when the silicon member 10 is viewed in the thickness direction (stacking direction), it is preferable that the first single crystal silicon member 11 and the second single crystal silicon member 12 are stacked such that the angle (minimum angle) θ between the cleavage direction (X1 direction, Y1 direction) at the bonding surface of the first single crystal silicon member 11 and the cleavage direction (X2 direction, Y2 direction) at the bonding surface of the second single crystal silicon member 12 is 5° or more. In this embodiment, as described above, the bonding surfaces of the first single crystal silicon member 11 and the second single crystal silicon member 12 are (100) planes, and the cleavage directions at the bonding surfaces are two directions (X direction and Y direction) that are perpendicular to each other, so that the cleavage directions coincide with each other by rotating by 90°, and therefore the angle (minimum angle) θ between the cleavage direction (X1 direction, Y1 direction) at the bonding surface of the first single crystal silicon member 11 and the cleavage direction (X2 direction, Y2 direction) at the bonding surface of the second single crystal silicon member 12 is set to a range of 5° to 45°. Note that the angle (minimum angle) θ between the cleavage direction (X1 direction, Y1 direction) at the bonding surface of the first single crystal silicon member 11 and the cleavage direction (X2 direction, Y2 direction) at the bonding surface of the second single crystal silicon member 12 may be set to a range of 10° to 45°.
[0023] Next, a method for manufacturing the silicon member 10 according to the present embodiment will be described with reference to FIGS.
[0024] As shown in FIG. 3 , the manufacturing method of the silicon member 10 according to the present embodiment includes a crystal plane orientation confirmation step S01 for confirming the crystal plane orientations of the bonding surface of the first single crystal silicon member 11 and the bonding surface of the second single crystal silicon member 12, a single crystal silicon member stacking step S02 for stacking the first single crystal silicon member 11 and the second single crystal silicon member 12 in such a manner that the cleavage directions of the bonding surfaces of the first single crystal silicon member 11 and the second single crystal silicon member 12 are shifted from each other, a bonding step S03 for bonding the stacked first single crystal silicon member 11 and the second single crystal silicon member 12, and a processing step S04 for processing the bonded body of the first single crystal silicon member 11 and the second single crystal silicon member 12.
[0025] Each step of the method for producing the silicon member 10 according to this embodiment will be described in detail below.
[0026] (Crystal plane orientation confirmation process S01) Check the crystal plane orientation of the bonding surface of the first single crystal silicon member 11 and the bonding surface of the second single crystal silicon member 12. The crystal plane orientation can be measured by X-ray crystal orientation measurement.
[0027] (Single crystal silicon component stacking process S02) Next, the first single crystal silicon member 11 and the second single crystal silicon member 12 are stacked by rotating them relatively in the planar direction so that the cleavage direction (X1 direction, Y1 direction) at the bonding surface of the first single crystal silicon member 11 and the cleavage direction (X2 direction, Y2 direction) at the bonding surface of the second single crystal silicon member 12 are misaligned (i.e., the cleavage direction (X1 direction, Y1 direction) and the cleavage direction (X2 direction, Y2 direction) do not coincide with each other).
[0028] In this embodiment, as shown in FIG. 4(a), a notch 16 may be provided in the first single crystal silicon member 11 and the second single crystal silicon member 12, and the first single crystal silicon member 11 and the second single crystal silicon member 12 may be laminated in such a manner that the cleavage direction (X1 direction, Y1 direction) at the bonding surface of the first single crystal silicon member 11 and the cleavage direction (X2 direction, Y2 direction) at the bonding surface of the second single crystal silicon member 12 are misaligned. Alternatively, as shown in FIG. 4(b), pin holes 17 may be provided in the first single crystal silicon member 11 and the second single crystal silicon member 12, and lamination may be performed by aligning the members with the pin holes 17 and pins.
[0029] In this embodiment, a silicon-containing composition containing an organic silicon compound and a solvent is applied to the bonding surface of at least one of the first single crystal silicon member 11 and the second single crystal silicon member 12, and the first single crystal silicon member 11 and the second single crystal silicon member 12 are laminated via the silicon-containing composition.
[0030] Here, the organosilicon compound contained in the silicon-containing composition is preferably one or more selected from silicates, siloxanes, silazanes, silanols, and carboxylic acid silyl esters. In particular, it is preferable to use tetraethoxysilane (TEOS) as the organosilicon compound. The solvent contained in the silicon-containing composition is preferably one or more selected from the group consisting of water, alcohols, ethers, and esters.
[0031] Furthermore, the silicon-containing composition preferably contains an acid catalyst to promote the reaction. The acid catalyst is preferably one or more selected from the group consisting of hydrochloric acid, nitric acid, and hydrogen peroxide. In addition, the silicon-containing composition preferably contains a stabilizer to stabilize the state of the organosilicon compound contained in the silicon-containing composition. The stabilizer is preferably one or two selected from bidentate ligands, acetylacetone and dimethyl succinate.
[0032] Here, in the present embodiment, the silicon-containing composition is a liquid composition, and the composition preferably contains an organosilicon compound in the range of 1 mass% or more and 30 mass% or less, an acid catalyst in the range of 0.01 mass% or more and 0.5 mass% or less, a stabilizer in the range of 1 mass% or more and 40 mass% or less, and the remainder is a solvent and inevitable impurities.
[0033] The method of applying the silicon-containing composition is not particularly limited, and various existing methods such as spin coating, dip coating, spray coating, etc. can be appropriately selected. The thickness of the applied silicon-containing composition is not particularly limited, but in this embodiment, the thickness of the applied silicon-containing composition is within the range of 0.02 μm to 50 μm. Furthermore, it is preferable to provide a drying process after applying the silicon-containing composition. The drying process is preferably performed at a drying temperature of 60° C. to 200° C. and for a drying time of 1 minute to 60 minutes.
[0034] (Joining process S03) Next, the first single crystal silicon member 11 and the second single crystal silicon member 12 stacked as described above are heated while being pressurized in the stacking direction, and the first single crystal silicon member 11 and the second single crystal silicon member 12 are bonded together via the bonding layer 15. By heating, the applied silicon-containing composition is baked, and the silicon-containing composition becomes silicon oxide, and the first single crystal silicon member 11 and the second single crystal silicon member 12 are bonded together via a bonding layer 15 made of silicon oxide.
[0035] Here, the heating temperature in the bonding step S03 is preferably within a range of 200° C. or more and 800° C. or less. Moreover, the holding time at the heating temperature in the bonding step S03 is preferably within a range of 0.1 hours to 2 hours. Furthermore, the pressure load in the joining step S03 is set to 0 MPa or more and 100 MPa or less, and preferably 5 MPa or less.
[0036] After the bonding step S03, it is preferable to etch the bonded first single crystal silicon member 11 and second single crystal silicon member 12 using an etching solution containing hydrofluoric acid to remove silicon oxide protruding from the bonding surfaces. Here, examples of the etching solution containing hydrofluoric acid that can be used include diluted hydrofluoric acid, a mixture of hydrofluoric acid and nitric acid, and a mixture of hydrofluoric acid, nitric acid, and acetic acid.
[0037] (Processing process S04) Next, the bonded body of the first single crystal silicon member 11 and the second single crystal silicon member 12 is processed to have a predetermined shape. In this embodiment, the bonded body is drilled to form the vent holes (through holes) 10A. In addition, the surface of the bonded body is polished.
[0038] Through the various steps described above, the silicon member 10 of this embodiment is manufactured.
[0039] According to the silicon member 10 of the present embodiment configured as described above, the first single crystal silicon member 11 and the second single crystal silicon member 12 are laminated and bonded in the thickness direction, and the cleavage direction (X1 direction, Y1 direction) at the bonding surface of the first single crystal silicon member 11 and the cleavage direction (X2 direction, Y2 direction) at the bonding surface of the second single crystal silicon member 12 are arranged to be misaligned, so that when a load is applied to the cleavage direction of either the first single crystal silicon member 11 or the second single crystal silicon member 12, the other is in a state where the cleavage direction is misaligned, making it difficult to crack. As described above, even when a bending stress acts on the silicon member 10, it is possible to suppress the occurrence of cracks in the silicon member 10.
[0040] In the silicon member 10 of this embodiment, the bonding surface of the first single crystal silicon member 11 and the bonding surface of the second single crystal silicon member 12 have the same crystal plane orientation, specifically, the (100) plane. Therefore, by stacking the first single crystal silicon member 11 and the second single crystal silicon member 12 while rotating them relatively in the in-plane direction, the first single crystal silicon member 11 and the second single crystal silicon member 12 can be stacked so that the cleavage directions at the bonding surfaces are shifted.
[0041] Furthermore, in the silicon member 10 of this embodiment, the first single crystal silicon member 11 and the second single crystal silicon member 12 are reliably bonded to each other via the bonding layer 15 made of silicon oxide. Here, since Si,O of the silicon oxide constituting the bonding layer 15 does not become a contamination source in the semiconductor process, even if this silicon member 10 is disposed in a chamber of a plasma processing apparatus or the like, plasma processing can be stably performed.
[0042] Furthermore, the manufacturing method of the silicon member 10 of this embodiment includes a crystal plane orientation confirmation process S01 for confirming the crystal plane orientation of the bonding surface of the first single crystal silicon member 11 and the bonding surface of the second single crystal silicon member 12, a single crystal silicon member stacking process S02 for stacking the first single crystal silicon member 11 and the second single crystal silicon member 12 such that the cleavage direction (X1 direction, Y1 direction) of the bonding surface of the first single crystal silicon member 11 and the cleavage direction (X2 direction, Y2 direction) of the bonding surface of the second single crystal silicon member 12 are misaligned, and a bonding process S03 for bonding the stacked first single crystal silicon member 11 and second single crystal silicon member 12. This makes it possible to stably manufacture the silicon member 10 of this embodiment.
[0043] Although the embodiment of the present invention has been described above, the present invention is not limited to this, and can be modified as appropriate without departing from the technical concept of the invention. In this embodiment, the bonding surface of the first single crystal silicon member 11 and the bonding surface of the second single crystal silicon member 12 have the same crystal plane orientation, and the bonding surfaces of the first single crystal silicon member 11 and the second single crystal silicon member 12 are stacked by rotating them relatively in-plane, but the present invention is not limited to this.
[0044] For example, the bonding surface of the first single crystal silicon member 11 and the bonding surface of the second single crystal silicon member 12 may have different crystal plane orientations, and the first single crystal silicon member 11 and the second single crystal silicon member 12 may be stacked and arranged so that the cleavage directions at the bonding surfaces are offset from each other.
[0045] The crystal plane orientation of the bonding surface of the silicon member 12 may be the (100) plane, and the first single crystal silicon member 11 and the second single crystal silicon member 12 may be stacked and disposed so that the cleavage directions at the bonding surfaces are offset from each other.
[0046] The crystal plane orientation of the bonding surface of the first single crystal silicon member 11 may be the (111) plane, and the crystal plane orientation of the bonding surface of the second single crystal silicon member 12 may be the (110) plane, and the first single crystal silicon member 11 and the second single crystal silicon member 12 may be stacked and arranged so that the cleavage directions at the bonding surfaces are offset from each other.
[0047] The crystal plane orientation of the bonding surface of the first single crystal silicon member 11 may be a (100) plane, and the crystal plane orientation of the bonding surface of the second single crystal silicon member 12 may be a (111) plane. The first single crystal silicon member 11 and the second single crystal silicon member 12 may be stacked and arranged so that the cleavage directions at their bonding surfaces are offset from each other.
[0048] The crystal plane orientation of the bonding surface of the first single crystal silicon member 11 may be a (100) plane, and the crystal plane orientation of the bonding surface of the second single crystal silicon member 12 may be a (110) plane. The first single crystal silicon member 11 and the second single crystal silicon member 12 may be stacked and arranged so that the cleavage directions at their bonding surfaces are offset from each other.
[0049] The crystal plane orientation of the bonding surface of the first single crystal silicon member 11 may be a (110) plane, and the crystal plane orientation of the bonding surface of the second single crystal silicon member 12 may be a (100) plane, and the first single crystal silicon member 11 and the second single crystal silicon member 12 may be stacked and arranged so that the cleavage directions at their bonding surfaces are offset from each other.
[0050] The crystal plane orientation of the bonding surface of the first single crystal silicon member 11 may be a (110) plane, and the crystal plane orientation of the bonding surface of the second single crystal silicon member 12 may be a (111) plane. The first single crystal silicon member 11 and the second single crystal silicon member 12 may be stacked and arranged so that the cleavage directions at their bonding surfaces are offset from each other.
[0051] In addition, in this embodiment, the silicon-containing composition is heated to form a bonding layer 15 made of silicon oxide, and the first single crystal silicon member 11 and the second single crystal silicon member 12 are bonded to each other via the bonding layer 15 made of silicon oxide. However, the bonding method is not particularly limited.
[0052] For example, an Al-Si alloy with a Si content in the range of 0.5 mass% or more and 12.6 mass% or less may be disposed between the first single crystal silicon member 11 and the second single crystal silicon member 12 as a bonding material to form a bonding layer, and the first single crystal silicon member 11 and the second single crystal silicon member 12 stacked via this bonding material may be heated while being pressurized in the stacking direction to bond the first single crystal silicon member 11 and the second single crystal silicon member 12 together. At this time, an Al layer may be formed on the bonding surface of the first single crystal silicon member 11 and the bonding surface of the second single crystal silicon member 12, or a bonding material may be disposed between the facing Al layers. In this embodiment, the first single crystal silicon member 11 and the second single crystal silicon member 12 may be directly bonded to each other. EXAMPLES
[0053] The results of confirmatory experiments conducted to confirm the effectiveness of the present invention will be described below.
[0054] As examples of the present invention and comparative examples, two single crystal silicon plates (diameter 200 mm × thickness 6.5 mm) were prepared, the crystal plane orientations of their bonding surfaces were confirmed, and the first and second single crystal silicon plates were aligned so that the cross angle θ of the cleavage directions at each bonding surface was the value shown in Table 1. The first and second single crystal silicon plates were then laminated together. Then, by the method shown in Table 1, the first single crystal silicon plate and the second single crystal silicon plate were bonded together.
[0055] Here, in the "Al bonding" in Table 1, an Al film (thickness 1 μm) was sputter-formed on the bonding surfaces of the first single crystal silicon plate and the second single crystal silicon plate using an Al sputtering target. The first single crystal silicon plate and the second single crystal silicon plate were stacked so that the Al films faced each other, and pressure (3 MPa) was applied in the stacking direction, and a pressurized heat treatment was performed at a temperature of 600°C for 2 hours to bond the first single crystal silicon plate and the second single crystal silicon plate.
[0056] In the "direct bonding" method in Table 1, the bonding surfaces of the first and second single crystal silicon plates were mirror-finished and then irradiated with oxygen plasma to make them hydrophilic. The first and second single crystal silicon plates were stacked together so that the hydrophilic bonding surfaces faced each other, and pressure was applied in the stacking direction (6 MPa), and a pressurized heat treatment was performed at a temperature of 1000°C for 5 hours to bond the first and second single crystal silicon plates.
[0057] As a conventional example, a single silicon plate made of single crystal silicon was prepared. Five bending test pieces (width 4 mm, thickness 3 mm, length 40 mm) were taken from each of the silicon members of the above-mentioned invention example, comparative example, and conventional example, and a three-point bending test was carried out at room temperature using a Shimadzu Autograph AG-X, and the average value of the five pieces was calculated. The bending strength of the conventional example was set at 100, and the bending strengths of the examples of the present invention and the comparative examples were evaluated relative to this. The evaluation results are shown in Table 1.
[0058] [Table 1]
[0059] In Comparative Examples 1 and 2, the crystal plane orientation of the bonding surface of the first single crystal silicon plate and the bonding surface of the second single crystal silicon plate were the same as the (100) plane, and the cleavage directions were arranged to match, so that there was almost no improvement in bending strength compared to the conventional example. As shown in Table 1, the bending strength was improved by 2% compared to the conventional example in Comparative Example 1, and no change was observed in bending strength compared to the conventional example in Comparative Example 2. Thus, in Comparative Examples 1 and 2, the bending strength was improved by less than 5% compared to the conventional example.
[0060] In contrast, in Examples 1 to 4 of the present invention, the crystal plane orientation of the bonding surface of the first single crystal silicon plate and the bonding surface of the second single crystal silicon plate are the same as the (100) plane, but the cleavage directions are arranged to be offset, and therefore the bending strength was significantly improved compared to the conventional examples. As shown in Table 1, in Example 1 of the present invention, the angular difference in the cleavage directions was 5°, and the bending strength was improved by 6% compared to the conventional example, and in Example 2 of the present invention, the angular difference in the cleavage directions was 10°, and the bending strength was improved by 8% compared to the conventional example. Furthermore, in Example 3 of the present invention, the angular difference in the cleavage directions was 45°, and the bending strength was improved by 13% compared to the conventional example, and in Example 4 of the present invention, the angular difference in the cleavage directions was 45°, and the bending strength was improved by 9% compared to the conventional example.
[0061] In Example 5 of the present invention, the crystal plane orientation of the bonding surface of the first single crystal silicon plate is the (110) plane, and the crystal plane orientation of the bonding surface of the second single crystal silicon plate is the (100) plane, so that the cleavage directions are arranged to be offset, and the bending strength was significantly improved compared to the conventional example. Since the cleavage directions of the (110) plane and the (100) plane are different, the numerical value that minimizes the angle difference of the cleavage directions at the bonding surface is shown in Table 1 as the angle difference of the cleavage directions. As shown in Table 1, in Example 5 of the present invention, the angle difference of the cleavage directions is 5°, and the bending strength was improved by 6% compared to the conventional example. Thus, in Examples 1 to 5 of the present invention, the bending strength was improved by 5% or more compared to the conventional example.
[0062] As a result of the above, it was confirmed that the present invention can provide a silicon member capable of suppressing the occurrence of cracks and being stably usable, and a method for manufacturing the silicon member. [Explanation of symbols]
[0063] 10 Silicone parts 11 First single crystal silicon member 12 Second single crystal silicon member
Claims
1. A silicon member used in a plasma processing apparatus, A silicon member having a structure in which a plurality of single crystal silicon members are bonded together, wherein a set of the single crystal silicon members stacked via their bonding surfaces are arranged such that the cleavage directions at the bonding surfaces are offset from each other.
2. 2. The silicon member according to claim 1, wherein the pair of single crystal silicon members laminated via bonding surfaces have bonding surfaces each having the same crystal plane orientation.
3. 2. The silicon member according to claim 1, wherein the pair of single crystal silicon members laminated via bonding surfaces have bonding surfaces with different crystal plane orientations.
4. A method for producing a silicon member according to any one of claims 1 to 3, comprising the steps of: a crystal plane orientation confirmation step of confirming the crystal plane orientation of the bonding surface of the single crystal silicon member; a single crystal silicon member stacking step of stacking a pair of the single crystal silicon members such that the cleavage directions at the bonding surfaces of the single crystal silicon members are shifted by 5° or more; a bonding step of bonding a set of the stacked single crystal silicon members; A method for producing a silicon member, comprising:
Citation Information
Patent Citations
Bonded wafer
JP1995335511A
Semiconductor substrate and manufacture thereof
JP1997320912A
Semiconductor wafer device
JP2009040639A
Showerhead electrodes and showerhead electrode assemblies having low-particle performance for semiconductor material processing apparatuses
JP2015029132A
Electrode plate for plasma processing apparatus and manufacturing method therefor
JP2015191970A