Resin composition, molded product, wire coating material, laminated glass interlayer, solar cell sealant, laminated sheet for solar cells, foam and footwear
A resin composition using biomass-derived ethylene-unsaturated ester copolymers and ethylene polymers addresses the environmental concerns of fossil fuel-based resins by maintaining performance while reducing carbon footprint.
Patent Information
- Application Number
- JP2023055619
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional ethylene-unsaturated ester copolymers are derived from fossil fuels, contributing to carbon dioxide emissions and resource depletion, and there is a need for a more environmentally friendly resin composition with equivalent performance to existing fossil fuel-based resins.
Developing a resin composition using ethylene-unsaturated ester copolymers and ethylene polymers, at least partially sourced from biomass, to achieve improved environmental friendliness without compromising on performance balance, melt physical properties, and resin compound properties.
The resin composition achieves the same performance balance as conventional fossil fuel-derived resins while significantly reducing environmental impact by utilizing biomass-derived materials, enhancing mechanical strength and flexibility.
Smart Images

Figure 2024143113000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition, a molded article, an electric wire covering material, an interlayer film for laminated glass, a solar cell encapsulant, a laminated sheet for solar cells, a foamed article, and footwear. [Background technology]
[0002] Ethylene-unsaturated ester copolymers such as ethylene-vinyl acetate copolymer and ethylene-ethyl acrylate copolymer are used in various applications because of their excellent transparency, flexibility, weather resistance, impact resistance, low-temperature properties, filler loading properties, etc. Examples of documents relating to resins containing such ethylene-unsaturated ester copolymers include Patent Documents 1 to 3.
[0003] Patent Document 1 describes an adhesive resin composition comprising: (A) 39 to 84.9% by weight of an ethylene-vinyl acetate copolymer consisting of 93 to 97% by weight of ethylene residue units and 3 to 7% by weight of vinyl acetate residue units and having a melt mass flow rate of 8 to 30 g / 10 min as measured by JIS K6924-1; (B) 5 to 20% by weight of an ethylene-vinyl acetate copolymer consisting of 80 to 90% by weight of ethylene residue units and 10 to 20% by weight of vinyl acetate residue units; (C) 5 to 20% by weight of low-density polyethylene; (D) 5 to 20% by weight of a tackifier resin; and (E) 0.1 to 1% by weight of an antistatic agent (E). The adhesive resin composition has excellent short-time heat sealability, heat seal strength stability, and heat seal time dependency, and furthermore, it is described that an easily peelable film obtained by forming an adhesive layer made of this adhesive resin composition on a support has excellent properties, for example, when adhered to a paper container, not causing fuzzing on the paper container upon peeling, and also maintains the initial peelability even when stored in a high-temperature environment after adhesion.
[0004] Patent Document 2 describes a cover tape for electronic component carriers, which has an adhesive layer that is heat-sealed to a plastic carrier tape having pockets for storing electronic components, and is characterized in that the adhesive layer is formed from a composition mainly composed of an ethylene-α-olefin copolymer or at least one of the α-olefin copolymers and an ethylene-vinyl acetate copolymer. The cover tape for electronic component carriers can be heat-sealed to the plastic carrier tape with sufficient adhesive strength and can be peeled off smoothly, regardless of whether the plastic carrier tape has been subjected to a release treatment or not, and regardless of whether an antistatic agent or conductive particles have been added to the adhesive, so that electronic components can be safely transported, and the safely transported electronic components can be picked up without jumping travel in the mounting process.
[0005] Patent Document 3 describes a heat-meltable composition comprising an ethylene-vinyl acetate copolymer (A), an olefin-based polymer (B), a wax (C) and a tackifier resin (D), the heat-meltable composition comprising 2 to 25 mass% of an ethylene-vinyl acetate copolymer (A) having an MFR of 100 to 2700 (g / 10 min) measured at a load of 21.18 N and 190°C, 10 to 40 mass% of an olefin-based polymer (B) having an MFR of 0.5 to 60 (g / 10 min) measured at a load of 21.18 N and 190°C, 35 to 65 mass% of a wax (C) having a melting point of 40 to 65°C, and 3 to 25 mass% of a tackifier resin (D) having a softening point of 100 to 160°C. It is described that the present invention provides a heat-meltable composition that has suitable sealing performance and opening strength for sealing a food container filled with contents, can be easily peeled off when the container is opened, does not allow the contents to adhere to the container when the container is opened, does not leave any heat-meltable composition on the flange of the container when the container is opened, and has impact resistance that prevents the contents from scattering even when the container is transported or dropped. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2014-25047 A [Patent Document 2] Japanese Patent Application Publication No. 10-17015 [Patent Document 3] JP 2018-150444 A Summary of the Invention [Problem to be solved by the invention]
[0007] On the other hand, resins containing such ethylene-unsaturated ester copolymers are generally derived from fossil fuels, but there are concerns that petroleum, a fossil fuel, will run out and that it emits a large amount of carbon dioxide during the manufacturing process and disposal process after the product is made, which raises concerns about its impact on global warming.
[0008] The present invention has been made in consideration of the above circumstances, and provides a resin composition which has improved environmental friendliness while having a performance balance of basic physical properties, melt properties and resin compound properties equivalent to those of resin compositions produced using only resins obtained from conventional fossil fuels. [Means for solving the problem]
[0009] The present inventors have found that, in a resin composition containing an ethylene-unsaturated ester copolymer (A) and an ethylene-based polymer (B) (excluding those corresponding to the above-mentioned ethylene-unsaturated ester copolymer (A)), by using components produced using raw materials derived from biomass for at least a part of each component, it is possible to obtain a resin composition having improved environmental friendliness while maintaining a performance balance of basic physical properties, melt properties and resin compound properties equivalent to those of a resin composition produced using only conventional raw materials derived from fossil fuels.
[0010] The present invention provides the following resin composition, molded article, electric wire covering material, laminated glass interlayer film, solar cell encapsulant, laminated sheet for solar cells, foam, and footwear.
[0011] [1] An ethylene-unsaturated ester copolymer (A), An ethylene-based polymer (B) (excluding those corresponding to the ethylene-unsaturated ester copolymer (A)), A resin composition comprising: The resin composition has a biomass content of more than 0 mass % and not more than 100 mass % as measured in accordance with ASTM D6866 for the entire resin composition. [2] When the total resin component of the resin composition is 100 mass%, The resin composition according to [1], wherein the content of the ethylene-unsaturated ester copolymer (A) is 1% by mass or more and 99% by mass or less. [3] When the total resin component of the resin composition is 100 mass%, The resin composition according to [1] or [2], wherein the content of the ethylene polymer (B) is from 1% by mass to 99% by mass. [4] The resin composition according to any one of [1] to [3], wherein a content of structural units derived from an unsaturated ester in the ethylene-unsaturated ester copolymer (A) is 1 mass% or more and 99 mass% or less, when the entire ethylene-unsaturated ester copolymer (A) is taken as 100 mass%. [5] The resin composition according to any one of [1] to [4], wherein the ethylene-based polymer (B) contains a low-density polyethylene. [6] The resin composition according to any one of [1] to [5], wherein the ethylene-based polymer (B) comprises a biomass ethylene-based polymer obtained by polymerizing a monomer containing ethylene derived from biomass. [7] The resin composition according to any one of [1] to [6], wherein a total content of the ethylene-unsaturated ester copolymer (A) and the ethylene-based polymer (B) is 2 mass% or more and 100 mass% or less, when the entire resin composition is taken as 100 mass%. [8] The resin composition according to any one of [1] to [7], wherein the ethylene-unsaturated ester copolymer (A) contains a biomass ethylene-unsaturated ester copolymer obtained by polymerizing a monomer containing ethylene derived from biomass. [9] The resin composition according to any one of [1] to [8], wherein the ethylene-unsaturated ester copolymer (A) contains an ethylene-vinyl acetate copolymer.
[10] The resin composition according to any one of [1] to [9], having a melt mass flow rate (MFR) of 0.1 g / 10 min or more and 300 g / 10 min or less, measured in accordance with JIS K 7210:1999 at 190°C under a load of 2160 g.
[11] A molded article obtained by molding the resin composition according to any one of [1] to
[10] .
[12] A wire covering material comprising the resin composition according to any one of [1] to
[10] .
[13] A laminated glass interlayer comprising the resin composition according to any one of [1] to
[10] .
[14] A solar cell encapsulant comprising the resin composition according to any one of [1] to
[10] .
[15] A laminate sheet for solar cells, comprising the resin composition according to any one of [1] to
[10] .
[16] A foam obtained by heating and foaming the resin composition according to any one of [1] to
[10] .
[17] Footwear comprising the foam according to
[16] . Effect of the Invention
[0012] According to the present invention, it is possible to provide a resin composition that has improved environmental friendliness while having a performance balance of basic physical properties, melt properties, and resin compound properties equivalent to those of conventional resin compositions produced using only fossil fuel-derived resins. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, embodiments of the present invention will be described with reference to the drawings. In this specification, "A to B" indicating a range of values means A or more and B or less unless otherwise specified.
[0014] 1.Resin composition The resin composition according to this embodiment contains an ethylene-unsaturated ester copolymer (A) and an ethylene-based polymer (B) (excluding those corresponding to the above-mentioned ethylene-unsaturated ester copolymer (A)), and the biomass content of the entire resin composition, as measured in accordance with ASTM D6866, is more than 0 mass% and 100 mass% or less.
[0015] According to the resin composition of this embodiment, it is possible to provide a resin composition which contains an ethylene-unsaturated ester copolymer (A) and an ethylene-based polymer (B), and at least a part of each component is produced using a biomass-derived raw material, thereby providing a resin composition which has an improved environmental friendliness while having a performance balance of basic physical properties, melt properties and resin compound properties equivalent to those of conventional resin compositions produced using only raw materials derived from fossil fuels.
[0016] In the resin composition according to this embodiment, when the entire resin components of the resin composition are taken as 100% by mass, the content of the ethylene-unsaturated ester copolymer (A) is preferably 1% by mass or more, more preferably 10% by mass or more, even more preferably 20% by mass or more, and even more preferably 30% by mass or more, from the viewpoint of further improving the performance balance of flexibility, melt properties, and resin compound properties, and is preferably 99% by mass or less, more preferably 90% by mass or less, even more preferably 80% by mass or less, and even more preferably 70% by mass or less, from the viewpoint of improving heat resistance.
[0017] In the resin composition according to this embodiment, when the entire resin components of the resin composition are taken as 100% by mass, the content of the ethylene-based polymer (B) is, from the viewpoint of further improving the performance balance of mechanical strength and heat resistance, preferably 1% by mass or more, more preferably 5% by mass or more, even more preferably 10% by mass or more, even more preferably 15% by mass or more, and even more preferably 20% by mass or more, and from the viewpoint of further improving the performance balance of flexibility and processability, is preferably 99% by mass or less, more preferably 90% by mass or less, even more preferably 80% by mass or less, and even more preferably 70% by mass or less.
[0018] In the resin composition according to the present embodiment, when the entire resin components of the resin composition are taken as 100% by mass, the total content of the ethylene-unsaturated ester copolymer (A) and the ethylene-based polymer (B) is preferably 2% by mass or more, more preferably 10% by mass or more, even more preferably 30% by mass or more, even more preferably 50% by mass or more, even more preferably 60% by mass or more, even more preferably 65% by mass or more, and even more preferably 70% by mass or more, from the viewpoint of improving the performance balance of basic physical properties, melt physical properties, and resin compound physical properties. There is no upper limit on the total content of the ethylene-unsaturated ester copolymer (A) and the ethylene-based polymer (B), but it is, for example, 100% by mass or less.
[0019] <Ethylene-unsaturated ester copolymer (A)> The ethylene-unsaturated ester copolymer (A) is a copolymer of ethylene and at least one unsaturated ester. The ethylene-unsaturated ester copolymer (A) may be in the form of a block copolymer, a random copolymer or a graft copolymer. In consideration of productivity, however, it is preferable to use a binary random copolymer, a ternary random copolymer, a graft copolymer of a binary random copolymer or a graft copolymer of a ternary random copolymer, and more preferably a binary random copolymer or a ternary random copolymer. Moreover, the ethylene-unsaturated ester copolymer (A) preferably contains one or two selected from an ethylene-vinyl ester copolymer and an ethylene-unsaturated carboxylic acid ester copolymer, and more preferably contains an ethylene-vinyl ester copolymer. The ethylene-unsaturated ester copolymer (A) may contain a polymerizable monomer other than ethylene and an unsaturated ester, for example, an α-olefin such as propylene, butene, or hexene.
[0020] The ethylene-vinyl ester copolymer includes, for example, one or more selected from ethylene-vinyl acetate copolymer, ethylene-vinyl propionate copolymer, ethylene-vinyl butyrate copolymer, and ethylene-vinyl stearate copolymer, and from the viewpoint of further improving basic physical properties, preferably includes ethylene-vinyl acetate copolymer.
[0021] Ethylene-unsaturated carboxylic acid ester copolymers are copolymers of ethylene and at least one unsaturated carboxylic acid ester. Specifically, it can be a copolymer made of ethylene and an unsaturated carboxylic acid alkyl ester.
[0022] As the unsaturated carboxylic acid in the unsaturated carboxylic acid ester, for example, at least one selected from the group consisting of acrylic acid, methacrylic acid, 2-ethylacrylic acid, crotonic acid, maleic acid, fumaric acid, itaconic acid, maleic anhydride, fumaric anhydride, itaconic anhydride, monomethyl maleate, monoethyl maleate, and monoethyl maleate can be used. Among these, from the viewpoint of further improving the productivity and sanitation of the ethylene-unsaturated ester copolymer (A), it is preferable that the unsaturated carboxylic acid includes at least one selected from the group consisting of acrylic acid and methacrylic acid. These unsaturated carboxylic acids may be used alone or in combination of two or more.
[0023] The alkyl moiety in the unsaturated carboxylic acid alkyl ester may have 1 to 12 carbon atoms, and more specifically, may be exemplified by alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, secondary butyl, 2-ethylhexyl, and isooctyl. The alkyl moiety in the alkyl ester preferably has 1 to 8 carbon atoms. Among these, the alkyl moiety preferably contains at least one selected from the group consisting of methyl and ethyl, and more preferably contains methyl.
[0024] As the unsaturated carboxylic ester, for example, it is preferable to use one or more selected from (meth)acrylic acid alkyl esters such as methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-propyl (meth)acrylate, isobutyl (meth)acrylate, n-butyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, dimethyl maleate, and diethyl maleate. Among these, it is more preferable to use one or more selected from methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-propyl (meth)acrylate, isobutyl (meth)acrylate, and n-butyl (meth)acrylate, it is even more preferable to use one or two selected from methyl (meth)acrylate and ethyl (meth)acrylate, and it is even more preferable to use methyl (meth)acrylate.
[0025] The content of structural units derived from ethylene in the ethylene-unsaturated ester copolymer (A), when the entire ethylene-unsaturated ester copolymer (A) is taken as 100 mass%, is preferably 50 mass% or more, more preferably 60 mass% or more, even more preferably 65 mass% or more, and even more preferably 70 mass% or more from the viewpoint of further improving the balance of performance such as mechanical strength, processability, and productivity, and is preferably 99 mass% or less, more preferably 90 mass% or less, and even more preferably 80 mass% or less from the viewpoint of further improving the melt properties, when the entire ethylene-unsaturated ester copolymer (A) is taken as 100 mass%,
[0026] The content of structural units derived from unsaturated ester in the ethylene-unsaturated ester copolymer (A), when the entire ethylene-unsaturated ester copolymer (A) is taken as 100 mass%, from the viewpoint of further improving flexibility and processability, is preferably 1 mass% or more, more preferably 4 mass% or more, even more preferably 10 mass% or more, even more preferably 15 mass% or more, even more preferably 20 mass% or more, and even more preferably 25 mass% or more, and from the viewpoint of further improving the performance balance of processability and mechanical strength, is preferably 99 mass% or less, more preferably 80 mass% or less, even more preferably 60 mass% or less, even more preferably 50 mass% or less, and even more preferably 40 mass% or less.
[0027] When the ethylene-unsaturated ester copolymer (A) is an ethylene-vinyl acetate copolymer, the content of constituent units derived from vinyl acetate can be determined in accordance with JIS K7192:1999 by heating the ethylene-vinyl acetate copolymer to 500°C or higher in an electric furnace to decompose it, and then subjecting the resulting acetic acid derived from vinyl acetate to neutralization titration.
[0028] The content of structural units derived from unsaturated ester in the ethylene-unsaturated ester copolymer (A) relative to the entire resin composition is preferably 1 mass% or more, more preferably 3 mass% or more, even more preferably 5 mass% or more, and even more preferably 8 mass% or more, from the viewpoint of further improving the performance balance of processability and mechanical strength, and is preferably 40 mass% or less, more preferably 30 mass% or less, and even more preferably 25 mass% or less, from the viewpoint of further improving the performance balance of processability and mechanical strength.
[0029] The content of structural units derived from unsaturated ester in the resin composition is calculated by the product of the content (mass%) of structural units derived from unsaturated ester in the ethylene-unsaturated ester copolymer (A) and the content of the ethylene-unsaturated ester copolymer (A) in the total amount of the resin composition.
[0030] The melt mass flow rate (MFR) of the ethylene-unsaturated ester copolymer (A), measured in accordance with JIS K 7210:1999 under conditions of 190°C and a load of 2160 g, is, from the viewpoint of further improving the physical properties of the resin compound, preferably 0.01 g / 10 min or more, more preferably 0.1 g / 10 min or more, even more preferably 1.0 g / 10 min or more, even more preferably 3.0 g / 10 min or more, and is preferably 300 g / 10 min or less, more preferably 250 g / 10 min or less, even more preferably 200 g / 10 min or less, even more preferably 150 g / 10 min or less, even more preferably 100 g / 10 min or less, even more preferably 50 g / 10 min or less, even more preferably 10 g / 10 min or less.
[0031] The ethylene-unsaturated ester copolymer (A) preferably contains an ethylene-unsaturated ester copolymer obtained by polymerizing a monomer containing ethylene derived from biomass. When the ethylene-unsaturated ester copolymer (A) contains an α-olefin other than ethylene, it may contain an ethylene-unsaturated ester copolymer obtained by polymerizing a monomer containing an α-olefin other than ethylene derived from biomass. From the viewpoint of further improving environmental friendliness, the biomass degree of the ethylene-unsaturated ester copolymer (A) is preferably more than 0 mass%, more preferably 0.01 mass% or more, even more preferably 0.1 mass% or more, even more preferably 10 mass% or more, even more preferably 20 mass% or more, even more preferably 30 mass% or more, even more preferably 40 mass% or more, even more preferably 50 mass% or more, even more preferably 60 mass% or more, even more preferably 70 mass% or more, even more preferably 80 mass% or more, even more preferably 90 mass% or more, even more preferably 95 mass% or more, and there is no particular upper limit to the biomass degree of the ethylene-unsaturated ester copolymer (A), but it is preferably 100 mass% or less. The method for producing ethylene derived from biomass and the biomass content will be described later.
[0032] The method for producing the ethylene-unsaturated ester copolymer (A) according to the present embodiment is not particularly limited, and it can be produced by a known method. For example, it can be obtained by radical copolymerization of each polymerization component under high temperature and high pressure. In addition, the ethylene-unsaturated ester copolymer (A) may be a commercially available product.
[0033] <Ethylene-based polymer (B)> The ethylene polymer (B) is polyethylene or a copolymer of ethylene and a polar monomer. However, the ethylene polymer (B) does not include those corresponding to the above-mentioned ethylene-unsaturated ester copolymer (A). From the viewpoint of further improving the mechanical strength, the ethylene polymer (B) preferably contains polyethylene.
[0034] From the viewpoint of further improving the mechanical strength of the resulting molded article, the ethylene-based polymer (B) preferably contains polyethylene, more preferably contains at least one selected from the group consisting of low-density polyethylene (LDPE), medium-density polyethylene (MDPE), and high-density polyethylene (HDPE), and even more preferably contains low-density polyethylene (LDPE). The ethylene polymer (B) is produced by a high pressure process, a medium pressure process or a low pressure process, preferably by a high pressure process. The ethylene polymer (B) may be a single polymer or a mixture of two or more kinds of ethylene polymers.
[0035] The ethylene polymer (B) preferably includes a biomass ethylene polymer obtained by polymerizing a monomer containing ethylene derived from biomass. From the viewpoint of further improving environmental friendliness, the biomass degree of the ethylene-based polymer (B) is preferably more than 0 mass%, more preferably 10 mass% or more, even more preferably 20 mass% or more, even more preferably 30 mass% or more, even more preferably 40 mass% or more, even more preferably 50 mass% or more, even more preferably 60 mass% or more, even more preferably 70 mass% or more, even more preferably 80 mass% or more, even more preferably 90 mass% or more, and even more preferably 93 mass% or more. There is no upper limit for the biomass degree of the ethylene-based polymer (B), but it is preferably 100 mass% or less. The method for producing ethylene derived from biomass and the biomass content will be described later.
[0036] The density of the ethylene polymer (B), as measured in accordance with JIS K 7112:1999, is preferably 900 kg / m from the viewpoint of further improving the mechanical strength. 3 More preferably, 905 kg / m 3 More preferably, 910 kg / m 3 More preferably, 915 kg / m 3 More preferably, 920 kg / m 3 From the viewpoint of further improving the balance of mechanical strength and flexibility, it is preferably 940 kg / m 3 Less than or equal to 930 kg / m 3 More preferably, 925 kg / m 3 or less, i.e., in the range of low density polyethylene.
[0037] The melt mass flow rate (MFR) of the ethylene polymer (B), measured according to JIS K 7210:1999 under conditions of 190°C and a load of 2160 g, is not limited as long as it can be mixed with the ethylene-unsaturated ester copolymer (A) and molded, but is preferably 0.01 g / 10 min or more, more preferably 0.1 g / 10 min or more, even more preferably 1 g / 10 min or more, even more preferably 2 g / 10 min or more, and is preferably 100 g / 10 min or less, more preferably 70 g / 10 min or less, even more preferably 50 g / 10 min or less, even more preferably 30 g / 10 min or less, and even more preferably 10 g / 10 min or less.
[0038] <Biomass-derived ethylene> The method for producing biomass-derived ethylene according to the present embodiment is not limited, and a known method can be used. Examples of the method for producing biomass-derived ethylene are given below.
[0039] "Biomass" refers to organic resources that are primarily derived from plants and animals, excluding fossil fuels. Methods for producing biomass-derived ethylene include, for example, a method in which plant raw materials are fermented by microorganisms to produce biomass-derived ethanol (bioethanol) and then dehydrated, and a method in which ethylene is extracted from biomass naphtha, which is produced using vegetable oil waste and residual oil as raw materials. The former raw materials include non-edible raw materials and edible raw materials. Examples of non-edible raw materials include cellulosic crops such as pulp, kenaf, and rice straw, waste paper, papermaking residues, wood, charcoal, compost, natural rubber, cotton, factory flue gas, waste gas, etc. Examples of edible raw materials include carbohydrate crops such as sugarcane, soybean pulp, corn, potatoes, wheat, and rice, buckwheat, and soybeans. As the former raw materials, one or more types selected from the group consisting of these can be used. As the latter raw material, various waste materials, unused resources, resource crops, etc. can be used. Specifically, oils and fats such as rapeseed oil and soybean oil, essential oils such as eucalyptus oil, vegetable oil cakes, etc. can be used. From the viewpoint of reducing the amount of carbon dioxide generated in the life cycle from the raw material to the disposal of the plastic product, it is preferable to use ethylene extracted from biomass naphtha.
[0040] Ethylene can be extracted from biomass naphtha by known methods such as heating, cracking, distillation, and purification, in the same manner as extraction from naphtha derived from fossil fuels.
[0041] The method for producing bioethanol is not limited, and for example, ethanol can be produced by contacting edible biomass raw materials such as sugarcane and corn with ethanol-producing microorganisms, such as yeast, or products derived from their crushed products to ferment sugar, and then purifying the ethanol. Ethanol can be purified by conventional methods such as distillation, membrane separation, and extraction. As a production method using non-edible raw materials as biomass raw materials, for example, ethanol can be obtained by using synthetic gas (gas mainly composed of carbon monoxide and hydrogen) generated by burning non-edible raw materials that are waste resources such as used paper and papermaking residues, and flue gas and waste gas emitted from factories, etc. as carbon sources and fermenting them with microorganisms.
[0042] The ethanol obtained as described above can be dehydrated to obtain biomass-derived ethylene. The dehydration reaction requires certain conditions, such as the type of catalyst, heating temperature, and pressure, but any of the conventional methods can be used.
[0043] In the process of producing the biomass ethylene obtained in this way, higher alcohol and higher alkene impurities may be produced during the ethanol fermentation and dehydration steps, and therefore these by-products can be removed before or after the dehydration of the ethanol.
[0044] <Biomass ratio> In the resin composition according to this embodiment, the biomass degree of the entire resin composition, measured in accordance with ASTM D6866, exceeds 0% by mass, from the viewpoint of improving environmental friendliness, and is preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 15% by mass or more, even more preferably 20% by mass or more, and even more preferably 25% by mass or more. There is no upper limit for the biomass degree of the entire resin composition, but it may be 100% by mass or less, or may be 90% by mass or less, 80% by mass or less, or may be 70% by mass or less. In ASTM D6866, radiocarbon from biomass ( 14 The biomass ratio is calculated by measuring the carbon concentration of fossil fuels. 14 C) shows a constant value, making it possible to distinguish it from biomass-derived carbon. For example, when polyethylene has a biomass content of more than 0 mass% but less than 100 mass%, it can be said to contain both biomass-derived ethylene and fossil fuel-derived ethylene.
[0045] In the present embodiment, the polymerization method for the ethylene-unsaturated ester copolymer (A) containing biomass-derived ethylene and the ethylene-based polymer (B) containing biomass-derived ethylene is not limited, and a conventionally known method similar to that in the case where fossil fuel-derived ethylene is used as the raw material can be used.
[0046] <Other ingredients> The resin composition according to the present embodiment may contain various additives within the scope of the present invention. Examples of such additives include one or more additives selected from the group consisting of inorganic fillers such as silica and talc, antioxidants, weathering stabilizers, wavelength conversion agents, antistatic agents, antifogging agents, antiblocking agents, slip agents, pigments, etc. Furthermore, the resin composition according to this embodiment may contain resins other than the ethylene-unsaturated ester copolymer (A) and the ethylene polymer (B) within the scope of the invention.
[0047] The resin composition according to the present embodiment can be prepared, for example, by simultaneously or continuously mixing the ethylene-unsaturated ester copolymer (A), the ethylene-based polymer (B) and any additives, and the mixing order is not limited. As a preparation method, it is preferable to melt mix them using a single screw extruder, a twin screw extruder, a Banbury mixer, a roll, various kneaders, etc. If necessary, the mixture can be made into pellets.
[0048] Hereinafter, the physical properties of the resin composition according to this embodiment will be described.
[0049] In the resin composition according to the present embodiment, the melt mass flow rate (MFR), measured in accordance with JIS K 7210:1999 under conditions of 190°C and a load of 2160 g, is, from the viewpoint of further improving the melt properties, moldability, and processability, preferably 0.1 g / 10 min or more, more preferably 1.0 g / 10 min or more, even more preferably 2.0 g / 10 min or more, and is preferably 300 g / 10 min or less, more preferably 200 g / 10 min or less, even more preferably 100 g / 10 min or less, even more preferably 50 g / 10 min or less, even more preferably 30 g / 10 min or less, and even more preferably 10 g / 10 min or less.
[0050] In the resin composition according to the present embodiment, the density measured in accordance with JIS K 7112:1999 is preferably 910 kg / m from the viewpoint of further improving the mechanical strength. 3 More preferably, 915 kg / m 3 More preferably, 920 kg / m 3 More preferably, 925 kg / m 3 From the viewpoint of further improving the balance of mechanical strength and processability, it is preferably 950 kg / m 3 Less than or equal to 945 kg / m 3 The following is the result.
[0051] In the resin composition according to the present embodiment, the melting point is preferably 80° C. or higher, more preferably 90° C. or higher, even more preferably 100° C. or higher, and even more preferably 105° C. or higher from the viewpoint of improving the balance of flexibility and resin compound physical properties, and is preferably 140° C. or lower, more preferably 130° C. or lower, even more preferably 120° C. or lower, and even more preferably 115° C. or lower from the viewpoint of further improving the performance balance of flexibility and resin compound physical properties. The melting point is measured, for example, by a differential scanning calorimeter (DSC) or the like.
[0052] In the resin composition according to this embodiment, the stress at break measured in accordance with JIS K 7161-1:2014 is preferably 5 MPa or more, more preferably 8 MPa or more, and even more preferably 10 MPa or more, from the viewpoint of further improving mechanical strength such as toughness. In the resin composition according to this embodiment, the upper limit of the stress at break measured in accordance with JIS K 7161-1:2014 is not limited, but may be, for example, 30 MPa or less, or 20 MPa or less.
[0053] In the resin composition according to this embodiment, the elongation at break measured in accordance with JIS K 7161-2:2014 is, from the viewpoint of further improving flexibility, preferably 450% or more, more preferably 480% or more, even more preferably 500% or more, and even more preferably 520% or more, and from the viewpoint of further improving the performance balance of mechanical strength and heat resistance, is preferably 900% or less, more preferably 850% or less, even more preferably 830% or less, and even more preferably 800% or less.
[0054] The stress at break (based on JIS K 7161-1:2014) and the elongation at break (based on JIS K 7161-2:2014) of the resin composition according to the present embodiment are measured using a tensile tester. The measurement can be performed by cutting a press sheet of the resin composition according to the present embodiment into a dumbbell shape according to the above JIS standard to prepare a test piece, and pulling it under the conditions of a chuck distance of 90 mm, a pulling speed of 50 mm / min, 23°C, and a relative humidity of 50% RH. The elongation at break represents the elongation of the test piece just before break between the designated gauge points in the tensile test. The stress at break is the value obtained by dividing the tensile force at the break point by the initial cross-sectional area of the test piece when the test piece breaks in the tensile test.
[0055] In the resin composition according to this embodiment, the flexural modulus at 23° C., measured in accordance with JIS K 7106:1995, is preferably 15 MPa or more, more preferably 20 MPa or more, even more preferably 25 MPa or more, and even more preferably 30 MPa or more, from the viewpoint of further improving the performance balance of heat resistance and mechanical strength, and is preferably 150 MPa or less, more preferably 140 MPa or less, even more preferably 130 MPa or less, and even more preferably 120 MPa or less, from the viewpoint of further improving the performance balance of flexibility, conformability, processability, and handleability.
[0056] In the resin composition according to this embodiment, the Shore A hardness, measured in accordance with JIS K 7215:1986, is preferably 70 or more, more preferably 75 or more, and even more preferably 80 or more, from the viewpoint of further improving the performance balance of moldability and flexibility, and is preferably 120 or less, more preferably 110 or less, and even more preferably 100 or less, from the viewpoint of further improving the performance balance of moldability and flexibility.
[0057] In the resin composition according to this embodiment, the Shore D hardness, measured in accordance with JIS K 7215:1986, is preferably 25 or more, more preferably 30 or more, and even more preferably 35 or more from the viewpoint of further improving heat resistance, and is preferably 70 or less, more preferably 65 or less, even more preferably 60 or less, and even more preferably 55 or less, from the viewpoint of further improving flexibility and processability.
[0058] The Shore A hardness and the Shore D hardness are measured in accordance with JIS K 7215:1986 using a type D durometer at 23°C.
[0059] In the resin composition according to this embodiment, the Vicat softening point measured under a load of 10 N in accordance with JIS K 7206:2016 is preferably 30°C or higher, more preferably 35°C or higher, and even more preferably 40°C or higher, from the viewpoint of further improving the performance balance of heat resistance, flexibility, processability, and handleability, and is preferably 100°C or lower, more preferably 90°C or lower, and even more preferably 80°C or lower.
[0060] The Vicat softening point is determined as follows. Using the resin composition according to this embodiment, a thermal deformation tester is used in accordance with JIS K 7206:2016, a needle indenter tool is placed at the top center of a test piece obtained from a press sheet of the resin composition so that the test piece is in contact with the test piece, and a load of 10 N is applied while the temperature of the heat transfer medium, silicone oil, is increased from 20°C at a heating rate of 50°C / h, and the temperature of the heat transfer medium is measured when the needle indenter penetrates 1 mm from the surface of the test piece.
[0061] The press sheet of the resin composition according to this embodiment used for the above physical properties is produced as follows. The resin composition of this embodiment is heated at 160°C for 4 minutes, during which degassing is performed 5 times, and then subjected to a compressive test at 160°C for 4 minutes under 9.8 MPa (100 kg / cm 2 ) conditions, then press molded at 20°C, 3 minutes, 14.7 MPa (150 kg / cm 2) and produce a 3 mm thick press sheet.
[0062] From the viewpoint of further improving processability, the melt tension at 160°C of the resin composition according to this embodiment is preferably 50 mN or more, more preferably 55 mN or more, and even more preferably 60 mN or more, and is preferably 100 mN or less, preferably 95 mN or less, and preferably 90 mN or less. From the viewpoint of further improving processability, the maximum take-up speed of the resin composition according to this embodiment at 160°C is preferably 10 m / min or more, more preferably 13 m / min or more, even more preferably 15 m / min or more, and is preferably 35 m / min or less, preferably 30 m / min or less, and preferably 25 m / min or less.
[0063] From the viewpoint of further improving processability, the melt tension at 180°C of the resin composition according to this embodiment is preferably 25 mN or more, more preferably 30 mN or more, and even more preferably 33 mN or more, and is preferably 80 mN or less, preferably 70 mN or less, and preferably 60 mN or less. From the viewpoint of further improving processability, the maximum take-up speed of the resin composition according to this embodiment at 180°C is preferably 10 m / min or more, more preferably 15 m / min or more, and even more preferably 20 m / min or more, and is preferably 50 m / min or less, preferably 45 m / min or less, and preferably 40 m / min or less.
[0064] From the viewpoint of further improving processability, the melt tension at 200°C of the resin composition according to this embodiment is preferably 10 mN or more, more preferably 15 mN or more, and even more preferably 18 mN or more, and is preferably 60 mN or less, preferably 50 mN or less, and preferably 40 mN or less. From the viewpoint of further improving processability, the maximum take-up speed of the resin composition according to this embodiment at 200°C is preferably 15 m / min or more, more preferably 20 m / min or more, even more preferably 25 m / min or more, and is preferably 60 m / min or less, preferably 55 m / min or less, preferably 50 m / min or less.
[0065] The method for measuring the melt tension and maximum take-off speed of the resin composition according to this embodiment will be described using the case at 160° C. as an example. Using a melt tension tester, the resin composition is filled into a barrel with a diameter of 9.55 mm heated to 160 ° C. The resin composition is extruded into a string-like shape from a capillary die with a diameter of 2.095 mm at a piston descending speed of 5 mm / min. The obtained string-like resin composition is passed through a pulley with a load cell installed at a position 300 mm below the capillary die, and the string-like resin composition is wound up with a winding roll. At this time, the winding speed of the string-like resin composition is linearly increased from an initial speed of 5.0 m / min to 200 m / min after 1 minute, and the load applied to the pulley with the load cell when the string-like resin composition breaks is defined as the melt tension [mN]. In addition, the value of the winding speed when the string-like resin composition breaks is defined as the maximum take-up speed [m / min]. The melt tension and maximum take-off speed at 180°C and 200°C were measured in the same manner as above, except that the barrel heating temperature was changed to 180°C or 200°C.
[0066] 2. Molded body The molded article of the present embodiment is obtained by molding the resin composition of the present embodiment. The molding method is not limited, and known molding methods such as extrusion molding, injection molding, compression molding, and blow molding can be used, and the molded article can be obtained by molding into various shapes such as a sheet shape, a film shape, a plate shape, and other three-dimensional shapes. The molded article of the present embodiment may be made only of the resin composition of the present embodiment, or may be made of the resin composition of the present embodiment and other components. The molded article of the present embodiment may be a part or the whole of a member.
[0067] Furthermore, the surface of the molded article of the present embodiment may be subjected to a frame treatment, a corona treatment, a plasma treatment, a hard coat treatment with an inorganic or organic compound, an antistatic treatment, an antireflection treatment, an electromagnetic shielding treatment, etc., within the scope of not impairing the effects of the present invention. These treatments can be performed on the surface of the molded article by deposition, sputtering, dipping, thermal transfer, etc.
[0068] The molded article of the present embodiment can be used in a wide range of fields, including, but not limited to, optical materials, electronic components, various machine components, foams, sheets, films, pipes, tubes, toys, and daily necessities.
[0069] 3.Wire sheathing material The wire covering material of the present embodiment includes the resin composition of the present embodiment or the molded article of the present embodiment. The wire covering material of the present embodiment is a material for protecting the surface of an electric wire, which is a conductor. A power cable generally has a layer structure of conductor / inner semi-conductive layer / insulating layer / outer semi-conductive layer / shielding layer / sheath from the inside, and the wire coating material refers to the part of the conductor that is the inner semi-conductive layer / insulating layer / outer semi-conductive layer / shielding layer / sheath. The resin composition of the present embodiment may be used for any of these layers, but is preferably used for one or two layers selected from the group consisting of the insulating layer and the semi-conductive layer because of its excellent melting properties.
[0070] The wire covering material may contain a filler, a flame retardant, and the like from the viewpoint of further improving the balance of performance among insulation properties, flame retardancy, and heat dissipation properties. The wire covering material of the present embodiment may contain components contained in conventionally known wire covering materials. In addition, the wire coating material may be directly applied to the outer circumference of the conductor, or other intermediate members, such as a shield conductor or other insulators, may be interposed between the conductor and the wire coating material.
[0071] The material and diameter of the conductor are not particularly limited and can be appropriately determined depending on the application. The thickness of the wire coating is also not particularly limited and can be appropriately determined taking into account the conductor diameter, etc.
[0072] The wire covering material can be produced by, for example, extrusion coating the outer periphery of a conductor using a conventionally known extrusion molding machine after melt-kneading the resin composition according to the present embodiment using a conventionally known kneading machine such as a Banbury mixer, a pressure kneader, or a roll.
[0073] 4. Interlayer film for laminated glass and solar cell encapsulant The laminated glass interlayer film of the present embodiment contains the resin composition of the present embodiment or the molded article of the present embodiment. A laminated glass interlayer is a material for producing laminated glass by providing transparent plate-like members such as glass on both sides of the laminated glass interlayer. By imparting various functions to the laminated glass interlayer, it is possible to impart design to the laminated glass by coloring it or sandwiching paper, cloth, etc., to impart crime prevention properties, and to impart effects such as weather resistance and strength.
[0074] The thickness of the laminated glass interlayer according to this embodiment is preferably 0.1 mm or more, more preferably 0.2 mm or more, and even more preferably 0.3 mm or more, and is preferably 10 mm or less, more preferably 5 mm or less, and even more preferably 2 mm or less. When the thickness of the laminated glass interlayer is equal to or greater than the lower limit, the mechanical strength of the laminated glass interlayer can be improved, whereas when the thickness of the laminated glass interlayer is equal to or less than the upper limit, the optical properties and interlayer adhesion of the resulting laminated glass can be improved.
[0075] The method for producing the laminated glass interlayer film according to this embodiment is not particularly limited, and any conventionally known production method can be used. The laminated glass interlayer film according to this embodiment can be produced by, for example, press molding, extrusion molding, T-die molding, injection molding, compression molding, cast molding, calendar molding, inflation molding, or the like.
[0076] The solar cell encapsulant of the present embodiment includes the resin composition of the present embodiment or the molded article of the present embodiment. The solar cell encapsulant according to this embodiment preferably has a thickness similar to that of the interlayer film of laminated glass, and can be manufactured by a similar manufacturing method.
[0077] 5.Laminated sheets for solar cells The laminate sheet for a solar cell of this embodiment contains the resin composition of this embodiment. The solar cell laminate sheet is a solar cell in which an encapsulant and a back sheet for protecting a solar cell element from the outside air are integrated. The resin composition of the present embodiment has an excellent balance of basic physical properties, melt physical properties, and resin compound physical properties, and therefore can be used as an adhesive layer between the encapsulant and the back sheet in the solar cell laminate sheet of the present embodiment. The thickness of the laminated sheet for a solar cell is not limited as long as the encapsulant can exhibit its performance as an encapsulant.
[0078] As the solar cell element, various types of solar cell elements can be used, for example, silicon-based elements such as single crystal silicon, polycrystalline silicon, and amorphous silicon, and III-V and II-VI compound semiconductor elements such as gallium-arsenide, copper-indium-selenium, and cadmium-tellurium.
[0079] 6. Foam The foam of the present embodiment is produced by heating and foaming the resin composition of the present embodiment. When the resin composition of the present embodiment is used for a foam, the resin composition may contain a chemical foaming agent, a foaming assistant, and the like, as necessary. The foam of the present embodiment uses the resin composition of the present embodiment, and therefore has an excellent balance of basic physical properties, melt properties, and resin compound properties, and is widely used in applications such as heat insulation materials, sound absorbing materials, shoe soles, buoys, automobile parts, and miscellaneous goods.
[0080] When the resin composition of the present embodiment is used for a foam, the resin composition can be melt-kneaded, and then, if necessary, pelletized, and molded into a shape suitable for the intended object, for example, into a sheet, using a T-die or roll, etc. The molding temperature for the resin composition varies depending on the composition of the resin composition and the molding method, but it is generally preferable to select a temperature suitable for the molding method within the temperature range of 100 to 200°C.
[0081] To form a foam from the molded article thus obtained, foaming may be performed using a press, a furnace, a foaming bath, or the like. When electron beam crosslinking is performed, the molded article may be irradiated with an electron beam before foaming to perform crosslinking. The foaming conditions vary depending on the types of chemical foaming agent, foaming assistant, etc., but generally, a temperature suitable for the foaming method should be selected from the temperature range of 150 to 250°C. The expansion ratio when foaming from the molded body is, for example, 2.1 times or more, and from the viewpoint of further improving cushioning properties, preferably 3.1 times or more, and from the viewpoint of further improving lightness, preferably 10 times or less, more preferably 8 times or less.
[0082] 7. Footwear The footwear of this embodiment is made of the foam of this embodiment. The foam of the present embodiment is used as a counter member constituting the heel portion of the footwear of the present embodiment. Examples of footwear include sports shoes, leather shoes, chemical shoes, sandals, etc.
[0083] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can also be adopted. Furthermore, the present invention is not limited to the above-described embodiment, and modifications and improvements within the scope of the present invention that can achieve the object of the present invention are included in the present invention. EXAMPLES
[0084] Hereinafter, the present embodiment will be described in detail with reference to examples, etc. However, the present embodiment is not limited to the description of these examples.
[0085] [material] The following components were used. The melt flow rate (MFR) was measured at 190°C and a load of 2160 g in accordance with JIS K 7210:1999. The density was measured in accordance with JIS K 7112:1999. The biomass ratio was measured in accordance with ASTM D6866.
[0086] <Ethylene-unsaturated ester copolymer (A)> Ethylene-vinyl acetate copolymer 1: Content of ethylene-derived structural units: 72% by mass, Content of vinyl acetate-derived structural units: 28% by mass, MFR (190°C, 2160g load): 4g / 10min, Biomass ratio: 0% by mass Ethylene-vinyl acetate copolymer 2: Content of ethylene-derived structural units: 72% by mass, Content of vinyl acetate-derived structural units: 28% by mass, MFR (190°C, 2160g load): 6g / 10min, Biomass ratio: 0% by mass
[0087] <Ethylene-based polymer (B)> Low-density polyethylene 1: Low-density polyethylene: Braskem, SEB853, MFR (190°C, 2160g load): 2.7g / 10min, density: 923kg / m 3 Biomass content: 95% by mass Low-density polyethylene 2: Low-density polyethylene, manufactured by Dow Mitsui Polychemicals, MFR (190°C, 2160g load): 3.7g / 10min, density: 923kg / m 3 , Biomass content: 0% by mass
[0088] [Examples 1 to 6 and Comparative Examples 1 to 3] <Preparation of resin composition (P)> The materials were mixed in advance in the proportions shown in Table 1, fed into a twin-screw extruder with a screw diameter of 30 mmφ, melt-kneaded under the following extrusion conditions or melt-kneading conditions, and granulated to prepare pellets of resin composition (P).
[0089] The extrusion conditions and melt-kneading conditions in the twin-screw extruder are as follows. Screw effective length L / D: 35 ·Extruder setting temperature (℃): C1 (110), C2 (160), C3 (180), C4 (180), C5 (180), H (180), D (180) Screw speed: 200 rpm Screen mesh: 60 / 120 / 60 Output: 15kg / h
[0090] [Biomass content of resin composition (P)] The biomass degree (mass%) of the resin composition (P) obtained in each example was calculated from the biomass degree of the low-density polyethylene 1 used as the raw material and the content of the low-density polyethylene 1 when the entire resin composition (P) was taken as 100 mass%.
[0091] [Content of structural units derived from vinyl acetate in resin composition (P)] The content (mass%) of constituent units derived from vinyl acetate in the resin composition (P) obtained in each example was calculated from the content of constituent units derived from vinyl acetate in the ethylene-unsaturated ester copolymer (A) used as the raw material and the content of the ethylene-unsaturated ester copolymer (A) when the entire resin composition (P) was taken as 100 mass%.
[0092] [MFR of resin composition (P)] The MFR (g / 10 min) of the resin composition (P) obtained in each example was measured under conditions of 190° C. and a load of 2160 g in accordance with JIS K 7210:1999.
[0093] [Density of resin composition (P)] The density (kg / cm) of the resin composition (P) obtained in each example 3 ) was measured in accordance with JIS K 7112:1999.
[0094] [Melting point of resin composition (P)] The melting point (° C.) of the resin composition (P) obtained in each example was measured using a differential scanning calorimeter (DSC).
[0095] <Press sheet production> The resin composition (P) obtained in each example was heated at 160°C for 4 minutes, during which time it was degassed 5 times, and then it was heated at 160°C for 4 minutes and compressed under 9.8 MPa (100 kg / cm 2 ) conditions, then press molded at 20°C, 3 minutes, 14.7 MPa (150 kg / cm 2 ) and press molded into a 3 mm thick press sheet.
[0096] The obtained press sheets were evaluated for breaking stress, breaking elongation, bending stiffness, Shore A hardness, Shore D hardness and Vicat softening point according to the following methods.
[0097] [Stress at break and elongation at break] The stress at break (based on JIS K 7161-1:2014) and elongation at break (based on JIS K 7161-2:2014) of the press sheets obtained in each example were measured using a tensile tester. The press sheets were cut into dumbbell shapes based on the above JIS standard to prepare test pieces, which were then pulled under the following conditions: chuck distance: 90 mm, tensile speed: 50 mm / min, 23°C, and relative humidity of 50% RH. The elongation at break represents the elongation of the test piece just before break between the designated gauge points in the tensile test. The stress at break is the value obtained by dividing the tensile force at the break point by the initial cross-sectional area of the test piece when the test piece breaks in the tensile test.
[0098] [Flexural rigidity] The flexural modulus (MPa) of the press sheet obtained in each example was measured in accordance with JIS K 7106: 1995. The press sheet was cut into a test piece having a length of 100 mm, a width of 20 mm, and a thickness of 3 mm, and the test piece was measured at 23°C using an automatic reading type "Olsen type stiffness tester" manufactured by Toyo Seiki Seisakusho.
[0099] [Shore A hardness and Shore D hardness] The Shore A hardness and Shore D hardness of the pressed sheet obtained in each example were measured in accordance with JIS K 7215: 1986. The pressed sheet was cut into a test piece having a length of 100 mm, a width of 20 mm, and a thickness of 3 mm, and the hardness was measured at 23°C using a type D durometer.
[0100] [Vicat softening point] The Vicat softening point (°C) of the press sheet obtained in each example was measured in accordance with JIS K 7206: 2016. Using a thermal deformation tester, a needle indenter was placed at the center of the top of the press sheet so that it was in contact with the press sheet, and while applying a load of 10 N, the temperature of the heat transfer medium, silicon oil, was increased from 20°C at a heating rate of 50°C / h, and the temperature of the heat transfer medium was measured when the needle indenter penetrated 1 mm from the surface of the test piece.
[0101] <Melt tension and maximum take-off speed> The melt tension and maximum take-up speed of the resulting resin composition (P) were measured by the following methods. Using a melt tension tester (manufactured by Toyo Seiki Seisakusho Co., Ltd.), the resin composition (P) was filled into a barrel with a diameter of 9.55 mm heated to 160 ° C. The resin composition (P) was extruded into a string shape from a capillary die with a diameter of 2.095 mm at a piston descending speed of 5 mm / min. The obtained string-like resin composition (P) was passed through a pulley with a load cell installed at a position 300 mm below the capillary die, and the string-like resin composition (P) was taken up by a take-up roll. At this time, the take-up speed of the string-like resin composition (P) was linearly increased from an initial speed of 5.0 m / min to 200 m / min after 1 minute, and the load applied to the pulley with the load cell when the string-like resin composition (P) broke was obtained as the melt tension [mN]. In addition, the value of the take-up speed when the string-like resin composition (P) broke was obtained as the maximum take-up speed [m / min]. Using the same method as above, the barrel heating temperature was changed to 180°C and 200°C, and the same measurements were carried out. The melt tension and maximum take-off speed results at 160°C, 180°C and 200°C are shown in Table 1.
[0102] [Table 1]
[0103] As is clear from Table 1, although the resin compositions (P) of Examples 1 and 2 contained raw materials derived from biomass, the MFR, density, melting point, stress at break, elongation at break, flexural modulus, Shore A hardness, Shore D hardness, and Vicat softening point all had the same content of structural units derived from vinyl acetate, and were equivalent to the resin composition (P) (Comparative Example 1) that used only raw materials derived from fossil fuels. Furthermore, the resin compositions (P) of Examples 1 and 2 had melt tensions at 160°C, 180°C, and 200°C equivalent to that of the resin composition (P) using only raw materials derived from fossil fuels (Comparative Example 1). The same was true in the comparison between Examples 3 and 4 and Comparative Example 2, and in the comparison between Examples 5 and 6 and Comparative Example 3.
Claims
1. An ethylene-unsaturated ester copolymer (A); An ethylene-based polymer (B) (excluding those corresponding to the ethylene-unsaturated ester copolymer (A)), A resin composition comprising: The resin composition has a biomass content of more than 0 mass% and not more than 100 mass%, as measured in accordance with ASTM D6866 for the entire resin composition.
2. When the total resin component of the resin composition is 100 mass%, The resin composition according to claim 1, wherein the content of the ethylene-unsaturated ester copolymer (A) is from 1% by mass to 99% by mass.
3. When the total resin component of the resin composition is 100 mass%, The resin composition according to claim 1 or 2, wherein the content of the ethylene polymer (B) is from 1% by mass to 99% by mass.
4. The resin composition according to any one of claims 1 to 3, wherein the content of structural units derived from unsaturated ester in the ethylene-unsaturated ester copolymer (A) is 1 mass% or more and 99 mass% or less, when the entire ethylene-unsaturated ester copolymer (A) is 100 mass%.
5. The resin composition according to any one of claims 1 to 4, wherein the ethylene-based polymer (B) contains a low-density polyethylene.
6. The resin composition according to any one of claims 1 to 5, wherein the ethylene-based polymer (B) comprises a biomass ethylene-based polymer obtained by polymerizing a monomer containing ethylene derived from biomass.
7. The resin composition according to any one of claims 1 to 6, wherein a total content of the ethylene-unsaturated ester copolymer (A) and the ethylene-based polymer (B) is 2 mass% or more and 100 mass% or less, when the entire resin composition is taken as 100 mass%.
8. The ethylene-unsaturated ester copolymer (A) comprises a biomass ethylene-unsaturated ester copolymer obtained by polymerizing a monomer containing ethylene derived from biomass. The resin composition according to any one of claims 1 to 7.
9. The resin composition according to any one of claims 1 to 8, wherein the ethylene-unsaturated ester copolymer (A) comprises an ethylene-vinyl acetate copolymer.
10. The resin composition according to any one of claims 1 to 9, wherein the melt mass flow rate (MFR) measured in accordance with JIS K 7210:1999 under conditions of 190 ° C. and a load of 2160 g is 0.1 g / 10 min or more and 300 g / 10 min or less.
11. A molded article obtained by molding the resin composition according to any one of claims 1 to 10.
12. A wire covering material comprising the resin composition according to any one of claims 1 to 10.
13. A laminated glass interlayer comprising the resin composition according to any one of claims 1 to 10.
14. A solar cell encapsulant comprising the resin composition according to any one of claims 1 to 10.
15. A laminated sheet for solar cells comprising the resin composition according to any one of claims 1 to 10.
16. A foam obtained by heating and foaming the resin composition according to any one of claims 1 to 10.
17. Footwear comprising the foam of claim 16.
Citation Information
Patent Citations
Cover tape for carrier of electronic part
JP1998017015A
Adhesive resin composition and easily peelable film
JP2014025047A
Heat-melting composition and use of the same
JP2018150444A