Manufacturing method of surface emission semiconductor laser element, and surface emission semiconductor laser element

The method of surface oxidation and oxide film removal in the manufacturing process addresses the challenges of resonance and threshold current issues in photonic crystal lasers by creating a thinner, flatter active layer, enhancing coupling efficiency and reducing defects, resulting in a high-performance surface-emitting semiconductor laser device.

JP2024143148APending Publication Date: 2024-10-11KYOTO UNIV +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023055673
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Conventional methods for manufacturing photonic crystal surface-emitting lasers face challenges in enhancing resonance effects and reducing threshold currents due to issues with pore layer thickness, surface roughness, and point defects, which hinder the close proximity of the hole layer and active layer, leading to reduced coupling efficiency.

Method used

A manufacturing method involving surface oxidation and oxide film removal followed by facet growth and annealing to form a buried layer, allowing for a thinner, flatter active layer with reduced Si concentration, enabling closer proximity of the hole and active layers.

Benefits of technology

This approach results in a surface-emitting semiconductor laser device with improved resonance effects, lower threshold values, and higher efficiency by ensuring a high-quality active layer with minimal surface roughness and point defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143148000001_ABST
    Figure 2024143148000001_ABST
Patent Text Reader

Abstract

To provide a manufacturing method of a surface emission semiconductor laser element having a high quality active layer, a lower threshold, and a higher efficiency, and is capable of enhancing a resonance effect by arranging a vacancy layer and an active layer close to each other, and to provide the surface emission semiconductor laser element.SOLUTION: A hole formation preparation layer is formed on a substrate (a), a hole formation layer is formed by forming, on the hole formation preparation layer, holes two-dimensionally arranged at each of lattice points (b), a surface of the hole formation layer is oxidized to form an oxide film and then the oxide film is removed (c), a first embedded layer is formed by performing facet growth for occluding the holes (d), a guide layer containing a vacancy layer having vacancies corresponding to the holes is formed by performing growth of a second embedded layer for flatly embedding the first embedded layer (e), and performs crystal growth of a semiconductor layer containing an active layer on the guide layer (f).SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a surface emitting semiconductor laser element having a photonic crystal, and to a surface emitting semiconductor laser element. [Background technology]

[0002] 2. Description of the Related Art In recent years, development of photonic-crystal surface-emitting lasers (PCSELs) using photonic crystals (PCs) has been progressing.

[0003] For example, Patent Document 1 proposes a method of embedding holes having a hexagonal columnar structure with side faces consisting of {10-10} in a group III nitride semiconductor layer using facet selective growth in order to enhance the diffraction effect in the hole layer in a photonic crystal laser and obtain a high resonance effect. It describes how this realizes a photonic crystal laser element equipped with a photonic crystal having a large filling factor and a large optical confinement coefficient.

[0004] Furthermore, Patent Document 2 proposes a method for embedding holes in a group III nitride semiconductor layer using mass transport in a photonic crystal laser, and describes how this method provides a photonic crystal laser with a large coupling coefficient for light waves propagating through the photonic crystal layer.

[0005] Furthermore, Patent Document 3 discloses that a photonic crystal layer (hole layer) is formed by performing a first burying growth for filling holes by facet growth and a second burying growth for flattening the surface. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Patent No. 7101370 [Patent Document 2] JP 2020-38892 A [Patent Document 3] WO2018 / 155710 A1 publication Summary of the Invention [Problem to be solved by the invention]

[0007] However, when the method described in Patent Document 1 is used, a hole layer with a sufficient hole filling rate can be formed, but the layer thickness for embedding the hole layer becomes thick, and the distance between the hole layer and the active layer cannot be reduced, and therefore the resonance effect in the hole layer cannot be enhanced.

[0008] The inventors of the present application have also found that when voids are filled using mass transport, a large amount of Si is deposited on the surface where the voids are formed, causing significant surface roughness. This surface roughness hinders the growth of a high-quality active layer with high flatness on the filling layer, and also makes it difficult to bring the void layer and the active layer close enough to each other, making it difficult to increase the coupling efficiency between the void layer and the active layer. Furthermore, when high concentration Si is introduced into the GaN film, point defects are likely to be introduced into the film, and from this viewpoint as well, it is preferable to remove the large amount of Si deposited on the surface.

[0009] For the reasons described above, in the conventional technology, it has been difficult to increase the resonance effect and lower the threshold current while maintaining a high output.

[0010] An object of the present invention is to provide a method for manufacturing a surface-emitting semiconductor laser element that is capable of increasing the resonance effect by bringing a hole layer and an active layer into close proximity, has a high-quality active layer, and has a low threshold and high efficiency, and also provides the surface-emitting semiconductor laser element. [Means for solving the problem]

[0011] A method for manufacturing a surface emitting semiconductor laser device according to one embodiment of the present invention includes the steps of: (a) forming a hole formation preparation layer on a substrate; (b) forming holes arranged two-dimensionally at each of the lattice points in the hole formation preparation layer to form a hole formation layer; (c) oxidizing the surface of the hole formation layer to form an oxide film, and then removing the oxide film; (d) forming a first burying layer by facet growth to close the hole; (e) growing a second burying layer that buries the first burying layer evenly to form a first guide layer including a hole layer having holes corresponding to the holes; (f) A manufacturing method comprising: growing crystals of a semiconductor layer including an active layer on the first guide layer.

[0012] A method for manufacturing a surface emitting semiconductor laser device according to another embodiment of the present invention includes the steps of: A method for manufacturing a surface emitting semiconductor laser device, comprising the steps of: (a) forming a hole formation preparation layer on a substrate; (b) forming holes arranged two-dimensionally at each of the lattice points in the hole formation preparation layer to form a hole formation layer; (c) oxidizing the surface of the hole formation layer to form an oxide film, and then removing the oxide film; (d) forming a first burying layer by facet growth to close the hole; (e) growing a second burying layer that buries the first burying layer evenly to form a first guide layer including a hole layer having holes corresponding to the holes; (f) flattening the surface of the first guide layer by etching the surface of the first guide layer by annealing in a hydrogen atmosphere; (g) A manufacturing method comprising: growing crystals of a semiconductor layer including an active layer on the flat etched first guide layer.

[0013] A surface emitting semiconductor laser device according to still another embodiment of the present invention comprises: An n-type semiconductor layer; a first guide layer including: a hole layer formed on the n-type semiconductor layer, the hole layer having holes arranged two-dimensionally at each lattice point; and a buried layer formed on the hole layer to close the holes; a semiconductor layer including an active layer formed on the buried layer; a second guide layer formed on the semiconductor layer including the active layer; The distance from the upper surface of the hole in the hole layer to the active layer is 4 to 200 nm. [Brief description of the drawings]

[0014] [Figure 1A] 1 is a cross-sectional view illustrating an example of the structure of a PCSEL element according to a first embodiment. [Figure 1B] 1B is an enlarged cross-sectional view showing a schematic diagram of holes arranged in the hole layer shown in FIG. 1A. [Figure 2A] FIG. 2 is a plan view showing a schematic top surface of a PCSEL element. [Figure 2B] 2 is a cross-sectional view that diagrammatically shows a cross section in a plane parallel to an n-side guide layer. FIG. [Figure 2C] FIG. 2 is a plan view showing a schematic view of the bottom surface of a PCSEL element. [Diagram 3] 1 is a flowchart showing a method for manufacturing the PCSEL device of the first embodiment. [Figure 4] 3A to 3C are cross-sectional views that diagrammatically show cross sections of an n-side guide layer in steps S0 to S3 of forming a buried layer. [Diagram 5] FIG. 2 is a plan view showing a schematic view of main openings and sub-openings in a resist, and main holes and sub-holes after etching. [Figure 6] 3 is a schematic diagram showing a cross section of the formed hole layer perpendicular to the central axis CX. FIG. [Figure 7] 1 shows a SIMS profile in the depth direction of a PCSEL device (EMB) manufactured by performing a surface oxidation / oxide film removal process (step S1). [Figure 8] 1 shows a SIMS profile in the depth direction of a PCSEL device (CMP) manufactured without performing the surface oxidation / oxide film removal process (step S1). [Figure 9A] FIG. 11 is a cross-sectional view illustrating an example of the structure of a PCSEL element according to a second embodiment. [Figure 9B] 9B is an enlarged cross-sectional view showing a schematic diagram of the hole layer of FIG. 9A and holes arranged in the hole layer. [Figure 10] 10 is a flowchart showing a method for manufacturing a PCSEL device according to a second embodiment. [Figure 11] FIG. 11 is a cross-sectional view that typically shows a cross section of the n-side guide layer at step S3A. [Figure 12] This is an SEM image showing a cross section of a substrate on which a buried layer was regrown after surface oxidation / oxide film removal processing, after which the surface was etched by H2 annealing. [Figure 13] FIG. 13 shows AFM images of the surfaces of samples (i) to (iv) shown in FIG. [Figure 14] 1 is a graph plotting surface roughness Ra in a 20 μm×20 μm area against thickness DE of the buried layer after etching. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] In the following, preferred embodiments of the present invention will be described, which may be modified and combined as appropriate. In the following description and accompanying drawings, substantially the same or equivalent parts are designated by the same reference numerals.

[0016] [First embodiment] 1. Structure of photonic crystal surface-emitting laser element A photonic crystal surface-emitting laser element (PCSEL element) is a surface-emitting semiconductor laser element that has a resonator layer in a direction parallel to the semiconductor light-emitting structure layers (n-side guide layer, light-emitting layer, p-side guide layer) that constitute the light-emitting element, and emits coherent light in a direction perpendicular to the resonator layer.

[0017] That is, in a PCSEL element, light waves propagating in a plane parallel to the air hole layer (photonic crystal layer) are diffracted by the diffraction effect of the photonic crystal to form a two-dimensional resonance mode, and are also diffracted in a direction perpendicular to the parallel plane. That is, in a PCSEL element, the light extraction direction is perpendicular to the resonance direction (in the plane parallel to the air hole layer).

[0018] Fig. 1A is a cross-sectional view showing an example of the structure of a photonic crystal surface-emitting laser device (PCSEL device) 10 according to an embodiment of the present invention, and Fig. 1B is an enlarged cross-sectional view showing an air hole layer 14P and air hole pairs 14K arranged in the air hole layer 14P in Fig. 1A.

[0019] Fig. 2A is a plan view diagrammatically illustrating the upper surface of the PCSEL device 10. Fig. 2B is a cross-sectional view diagrammatically illustrating the cross section of the hole layer 14P in a plane parallel to the n-side guide layer 14, and Fig. 2C is a plan view diagrammatically illustrating the lower surface of the PCSEL device 10.

[0020] 1A, a semiconductor structure layer 11 is formed on a light-transmitting element substrate 12. Note that semiconductor layers are stacked perpendicularly to a central axis CX of the semiconductor structure layer 11.

[0021] The semiconductor structure layer 11 is made of a hexagonal nitride semiconductor. In this embodiment, the semiconductor structure layer 11 is made of, for example, a GaN-based semiconductor.

[0022] More specifically, a semiconductor structure layer 11 consisting of a plurality of semiconductor layers is formed on an element substrate 12, in this order: an n-clad layer (first clad layer of a first conductivity type) 13, an n-side guide layer (first guide layer) 14 which is a guide layer provided on the n-side, a light distribution adjustment layer 23, an active layer (ACT) 15, a p-side guide layer (second guide layer) 16 which is a guide layer provided on the p-side, an electron barrier layer (EBL: Electron Blocking Layer) 17, a p-clad layer (second clad layer of a second conductivity type) 18, and a p-contact layer 19.

[0023] Although the case will be described where the first conductivity type is n-type and the second conductivity type opposite to the first conductivity type is p-type, the first conductivity type and the second conductivity type may be p-type and n-type, respectively.

[0024] The element substrate 12 is a hexagonal GaN single crystal substrate having a high transmittance for light emitted from the active layer 15. More specifically, the element substrate 12 is a hexagonal GaN single crystal substrate whose main surface (crystal growth surface) is a +c plane, which is a {0001} plane in which Ga atoms are arranged on the outermost surface. The back surface (light emission surface) is a -c plane, which is a (000-1) plane in which N atoms are arranged on the outermost surface. The -c plane is suitable as a light emission surface because it is resistant to oxidation and the like.

[0025] Although the element substrate 12 is not limited thereto, a so-called just substrate or, for example, a substrate whose main surface is offset by about 1° in the m-axis direction is preferable. For example, a substrate offset by about 0.3 to 0.7° in the m-axis direction can obtain mirror-finish growth under a wide range of growth conditions.

[0026] The back surface of the substrate opposite to the main surface is the light emitting surface, which is the "-c" surface, which is the (000-1) surface with N atoms arranged on the outermost surface. The -c surface is resistant to oxidation and is therefore suitable as a light extraction surface.

[0027] The composition, thickness, and other configurations of each semiconductor layer will be described below, but these are merely examples and can be modified as appropriate.

[0028] The n-clad layer 13 is, for example, n-Al 0.04 Ga 0.96 The N layer has a thickness of 2 μm. The aluminum (Al) composition ratio is set so that the refractive index is smaller than that of the layer adjacent to the active layer 15 side (that is, the n-side guide layer 14).

[0029] The n-side guide layer 14 is composed of a lower guide layer 14A, an air-hole layer 14P, which is a photonic crystal layer (PC layer), and a buried layer 14B. As shown in FIG. 1B, the photonic crystal layer 14P has a layer thickness dPC For example, the hole layer 14P has a thickness d PC is 40 to 180 nm.

[0030] In this specification, the air hole layer 14P refers to a layer portion from the upper end to the lower end of the air hole in the n-side guide layer 14 (see FIG. 1B). PC is equal to the height of the hole.

[0031] The lower guide layer 14A is, for example, n-GaN having a layer thickness of 100 to 400 nm. The void layer 14P is n-GaN having a layer thickness (or the height of the voids 14K) of 40 to 180 nm.

[0032] The buried layer 14B is made of n-GaN or n-InGaN, or undoped GaN or undoped InGaN. Alternatively, it may be a layer in which these semiconductor layers are stacked. The buried layer 14B has a layer thickness DE of, for example, 4 to 200 nm. The buried layer 14B is made of a first buried layer 14B1 and a second buried layer 14B2. In other words, the buried layer 14B is a stacked buried layer in which the second buried layer 14B2 is stacked on the first buried layer 14B1.

[0033] A light distribution adjustment layer 23 is provided on the second embedded layer 14B2, which is the surface layer of the embedded layer 14B. The light distribution adjustment layer 23 is a hetero semiconductor layer (a heterogeneous semiconductor layer) that has a different crystal composition from the second embedded layer 14B2 and forms a heterostructure with the second embedded layer 14B2.

[0034] The light distribution adjustment layer 23 may be a semiconductor layer of the same conductivity type as the second embedded layer 14B2, or at least one of them may be an i-layer (intrinsic semiconductor layer).

[0035] The light distribution-adjusting layer 23 is provided between the buried layer 14B and the active layer 15, and has a function of adjusting the coupling efficiency between the light propagating in the hole layer 14P and the hole layer 14P serving as a resonator. Alternatively, the light distribution-adjusting layer 23 may have a function as a SCH (Separate Confinement Heterostructure) layer used for the active layer of a bulk structure and a quantum well structure. In this embodiment, the light distribution adjustment layer 23 is made of undoped In. 0.03 Ga 0.97 N layers, and the layer thickness is, for example, 50 nm. The composition or refractive index and layer thickness of the light distribution adjustment layer 23 are selected according to the adjustment of the coupling efficiency.

[0036] The n-side semiconductor layer including the n-side guide layer 14 and the light distribution adjustment layer 23 is also referred to as a first semiconductor layer, but the light distribution adjustment layer 23 does not necessarily have to be provided.

[0037] The active layer 15, which is a light emitting layer, is, for example, a multiple quantum well (MQW) layer having two quantum well layers. The barrier layer and quantum well layer of the MQW are GaN (layer thickness 6.0 nm) and InGaN (layer thickness 4.0 nm), respectively. The central emission wavelength of the active layer 15 is 440 nm.

[0038] The active layer 15 is preferably disposed within 180 nm of the hole layer 14P (that is, within the period PK of the holes), in which case a high resonance effect is obtained by the hole layer 14P.

[0039] The p-side guide layer 16 is an undoped In 0.02 Ga 0.98 It is composed of a p-side guide layer (1) 16A which is an N layer (layer thickness 70 nm) and a p-side guide layer (2) 16B which is an undoped GaN layer (layer thickness 180 nm).

[0040] The p-side guide layer 16 is an undoped layer in consideration of light absorption by dopants (Mg: magnesium, etc.), but may be doped to obtain good electrical conductivity. In addition, the In composition and layer thickness of the p-side guide layer (1) 16A can be appropriately selected to adjust the electric field distribution in the oscillation operation mode.

[0041] The electron barrier layer (EBL) 17 is a magnesium (Mg) doped p-type Al 0.2 Ga 0.8 N layers, for example, having a layer thickness of 15 nm.

[0042] The p-cladding layer 18 is made of Mg-doped p-Al 0.06 Ga 0.94 The p-cladding layer 18 is an N layer having a thickness of, for example, 600 nm. The Al composition of the p-cladding layer 18 is preferably selected so that the refractive index is smaller than that of the p-side guide layer 16. The p-cladding layer 18 functions as a first p-cladding layer.

[0043] The p-contact layer 19 is a Mg-doped p-GaN layer having a thickness of, for example, 20 nm. The carrier density of the p-contact layer 19 is set to a concentration that allows ohmic junction with the transparent electrode 29, which is a transparent conductive layer provided on the surface of the p-contact layer 19. Instead of p-type GaN, p-type or undoped InGaN may be used. Alternatively, a layer in which a GaN layer and an InGaN layer are stacked may be used.

[0044] The layer consisting of the p-side guide layer 16, the electron barrier layer 17, the p-cladding layer 18 and the p-contact layer 19 is also referred to as a second semiconductor layer.

[0045] In this specification, "n-side" and "p-side" do not necessarily mean n-type and p-type. For example, the n-side guide layer means a guide layer provided on the n-side of the active layer, and may be an undoped layer (or an i-layer).

[0046] In addition, the n-cladding layer 13 may be composed of multiple layers instead of a single layer, and in that case, all layers do not need to be n layers (n-doped layers) and may include an undoped layer (i layer). The same applies to the guide layer 16 and the p-cladding layer 18.

[0047] Furthermore, it is not necessary to provide all of the semiconductor layers described above, and it is sufficient to have a configuration having a first semiconductor layer of a first conductivity type, a second semiconductor layer of a second conductivity type, and an active layer (light-emitting layer) sandwiched between these layers.

[0048] Furthermore, in this embodiment, the case where the void layer 14P (photonic crystal layer) is provided in the first semiconductor layer (n-type semiconductor layer) has been described, but the void layer may be provided in the second semiconductor layer (p-type semiconductor layer).

[0049] On the p-contact layer 19, a p-electrode 20B (second electrode) is formed as a translucent electrode / Ag / Au layer in which a translucent electrode 29 (not shown), a silver (Ag) layer, and a gold (Au) layer are laminated in this order. That is, the p-electrode 20B functions as a light reflecting layer, and the interface between the translucent electrode 29 and the Ag layer of the p-electrode 20B is a reflecting surface SR. The reflecting surface SR is provided parallel to the hole layer 14P.

[0050] The p-electrode 20B has a circular shape with a diameter RA centered on the central axis CX of the hole formation region 14R. Specifically, the transparent electrode 29 has a diameter of, for example, RA=300 μm in top view (i.e., when viewed from a direction perpendicular to the semiconductor structure layer 11). Note that Pd, Al, Al alloys, etc. may also be used as the p-electrode 20B. A pad electrode, etc. may also be provided on the p-electrode 20B.

[0051] The transparent electrode 29 is formed of a transparent conductor, for example, indium tin oxide (ITO). Note that the transparent electrode 29 is not limited to ITO, and other transparent conductors such as zinc tin oxide (ZTO), GZO (ZnO:Ga), and AZO (ZnO:Al) can be used.

[0052] The side and top surfaces of the semiconductor structure layer 11 and the side surfaces of the p-electrode 20B are made of SiO 2 The p-electrode 20B is covered with an insulating film 21 such as the insulating film 21. The insulating film 21 is formed so as to overlap the p-electrode 20B and cover the edge of the upper surface of the p-electrode 20B.

[0053] The insulating film 21 also functions as a protective film, protecting the aluminum (Al)-containing crystal layers that make up the PCSEL element 10 from corrosive gases and the like. It also prevents short circuits caused by adhesions or solder creeping up during mounting, contributing to improved reliability and yield. The material of the insulating film 21 is SiO 2 Not limited to ZrO 2 , HfO 2 , TiO 2 , Al 2 O 3 , SiNx, Si, etc. can be selected.

[0054] A circular cathode electrode 20A (first electrode) (see FIG. 2C) is formed on the back surface of the element substrate 12. In addition, an anti-reflection (AR) coating layer 27 is formed on the inner side of the cathode electrode 20A.

[0055] The cathode electrode 20A is made of Ti / Au and is in ohmic contact with the element substrate 12. In addition to Ti / Au, the electrode material may be selected from Ti / Al, Ti / Rh, Ti / Al / Pt / Au, Ti / Pt / Au, and the like.

[0056] The light emitted from the active layer 15 is diffracted by the air hole layer (PC layer) 14P. The light diffracted by the air hole layer 14P (diffraction surface WS) and directly emitted from the air hole layer 14P (direct diffracted light Ld: first diffracted light) and the light emitted by the diffraction of the air hole layer 14P and reflected by the reflecting surface SR (reflected diffracted light Lr: second diffracted light) are emitted to the outside from a light emission region 20L (FIG. 2C) of the rear surface (emission surface) 12R of the element substrate 12.

[0057] As shown in Fig. 2B, in the hole layer 14P, the holes 14K are periodically arranged in, for example, a rectangular hole-formation region 14R. As shown in Fig. 2C, the anode region RA is formed so as to be included in the hole-formation region 14R.

[0058] The cathode electrode 20A is provided as a ring-shaped electrode outside the p-electrode 20B so as not to overlap with the p-electrode 20B when viewed from a direction perpendicular to the hole layer 14P.

[0059] The region inside the cathode electrode 20A is the light emission region 20L. Also provided is a bonding pad 20C that is electrically connected to the cathode electrode 20 and for connecting a wire for power supply from the outside.

[0060] 2. Manufacturing method of the void layer and recrystallization growth The fabrication process and recrystallization growth of the hole layer are described below. Metalorganic Vapor Phase Epitaxy (MOVPE) is used as the crystal growth method. Note that the formation method is described below using the case where the hole layer 14P is a double lattice photonic crystal layer as an example, but a single lattice photonic crystal layer and a multiple lattice photonic crystal layer can also be formed in the same manner.

[0061] (a) Manufacturing flow Fig. 3 is a flowchart showing a method for manufacturing the PCSEL device 10. Below, with reference to Fig. 3, a detailed description will be given of the steps for manufacturing the PCSEL device 10 by forming air holes in the air hole layer by performing filling growth in the recesses (holes) and then growing the active layer and p-side guide layer.

[0062] 4 is a cross-sectional view that typically illustrates the cross section of the n-side guide layer 14 in steps S0 to S3 of forming the embedded layer 14B. For ease of explanation and understanding, FIG. 4 illustrates a case in which the hole layer 14P is a single lattice photonic crystal layer, but a multiple lattice photonic crystal layer can also be formed in the same manner.

[0063] The buried layer 14B (laminated buried layer) formed on the air-holes by recrystallization growth will be described in detail below with reference to FIGS. (Step S0) Formation of holes First, an n-type Al layer having an Al composition of 4% was formed on a substrate 12 as an n-clad layer 13. 0.04 Ga 0.96 An N layer was grown. Then, as shown in Fig. 4, a hole formation preparation layer 14E, which is an n-type GaN layer, was grown on the n-cladding layer 13. This hole formation preparation layer 14E is a preparation layer for forming the lower guide layer 14A and the air hole layer 14P containing air holes. The hole formation preparation layer 14E has a surface (upper surface) consisting of a flat (0001) plane.

[0064] After the hole formation preparation layer 14E was formed, the substrate was removed from the chamber of the MOVPE apparatus, and fine recesses (holes) were formed on the surface of the growth layer. After obtaining a clean surface by cleaning, a silicon nitride film (SiN x A resist for electron beam lithography was applied on top of this, and the device was placed in an electron beam lithography system to pattern a two-dimensional periodic structure.

[0065] Fig. 5 is a plan view showing the main opening K1 and sub-opening K2 of the resist, and the main hole 14H1 and sub-hole 14H2 after etching. As shown in Fig. 5, a pair of openings consisting of an oval main opening K1 and a sub-opening K2 smaller than the main opening K1 was two-dimensionally arranged in the plane of the resist in a square lattice shape with a period PK. For clarity of the drawing, the openings are shown with hatching.

[0066] More specifically, the main apertures K1 are arranged two-dimensionally with their centers of gravity CD1 in two mutually orthogonal directions (x-direction and y-direction) on the lattice points of a square lattice with a period PK, and the sub-apertures K2 are arranged two-dimensionally with their centers of gravity CD2 in the x-direction and y-direction on the lattice points of a square lattice with a period PK.

[0067] The major axes of the main aperture K1 and the sub aperture K2 are parallel to the <11-20> direction of the crystal orientation, and the minor axes of the main aperture K1 and the sub aperture K2 are parallel to the <1-100> direction.

[0068] The center of gravity CD2 of the sub-opening K2 is spaced apart from the center of gravity CD1 of the main opening K1 by Δx and Δy. Here, Δx=Δy. That is, the center of gravity CD2 of the sub-opening K2 is spaced apart from the center of gravity CD1 of the main opening K1 in the <1-100> direction.

[0069] The distance Δx, Δy between the centers of gravity of the main opening K1 and the sub-opening K2 was set to Δx=Δy=0.46PK. After developing the patterned resist, a SiN x The film was selectively dry etched. As a result, main openings K1 and sub-openings K2 arranged two-dimensionally on the lattice points of a square lattice with a period PK were formed in the SiN x formed to penetrate the membrane.

[0070] The period (hole spacing) PK was set to PK=177.5 nm in order to set the oscillation wavelength (λ) to 438 nm.

[0071] Next, the resist is removed and the patterned SiN x Using the film as a hard mask, recesses (holes) were formed on the GaN surface. A main hole 14H1 and a sub-hole 14H2, which are oblong cylindrical recesses dug vertically on the GaN surface, were formed by dry etching the GaN in the depth direction using a chlorine-based gas and argon gas in an ICP-RIE apparatus.

[0072] In addition, the recesses (holes) dug in the GaN surface portion by the above etching are simply called holes to distinguish them from air holes in the vacancy layer 14P. When there is no particular distinction between the main holes 14H1 and the sub-holes 14H2, they may be collectively called holes 14H.

[0073] The shape of the hole 14H is not limited to an elongated cylindrical shape, but may be a cylindrical shape, a polygonal shape, or the like.

[0074] As a result of the above, holes 14H were formed in the hole formation preparation layer 14E, and a hole formation layer 14J was formed (FIG. 4, S0).

[0075] (Step S1) Surface oxidation / oxide film removal The substrate with the hole 14H formed therein was degreased and then degreased with buffered hydrofluoric acid (BHF). x The membrane was removed.

[0076] SiN x After removing the membrane, the cells were incubated at room temperature for 24 h. 2 The gas is passed through the oven and irradiated with UV light. 2 The gas was activated, and the surface of the hole forming layer 14J was oxidized (10 min) by the generated ozone. 2 (glass) was formed on the upper surface of the hole forming layer 14J and on the surfaces inside the holes 14H.

[0077] After the ozone treatment, the substrate was immersed in buffered hydrofluoric acid (BHF) to remove the oxide film formed on the surface. Through the above steps, the Si bonded to Ga was removed.

[0078] Finally, the substrate was immersed in a semiconductor cleaning solution (Furuuchi Chemical: SemicoClean23) containing about 1% tetramethylammonium hydroxide (TMAH) for 10 minutes, and then rinsed with water.

[0079] (Step S2) Hole Closure - First Buried Growth Next, the substrate (FIG. 4) in which the hole 14H was formed (step S0) and the surface oxidation / oxide film removal process (step S1) was performed was degreased and cleaned, and then introduced again into the reactor of the MOVPE apparatus to perform recrystallization growth. 3 ) and trimethylgallium (TMG) were supplied to perform a first burying growth by facet growth, thereby closing the opening of hole 14H.

[0080] Specifically, the first burying growth was performed at a first temperature (920° C.) at which the shape of the hole 14H was transformed by mass transport into a shape composed of thermally stable surfaces.

[0081] More specifically, in this first temperature region, N atoms are attached to the top surface of the growth substrate, so that N-polarity faces are selectively grown. Therefore, as shown in FIG. 4, a crystal whose surface is a {1-101} facet is selectively grown. When the opposing {1-101} facets collide with each other, the hole 14H is blocked and filled (facet growth). This first filling growth by facet growth is performed, and a vacancy 14K is formed corresponding to the hole 14H.

[0082] In FIG. 4, the hole formation layer 14J (GaN layer) before the buried layer 14B is formed is indicated by a dashed line.

[0083] (Step S3) Planarization filling - second filling growth Subsequently, the hole 14H was closed by facet growth, and then a second burying layer 14B2 having a thickness of 50 nm was grown. The growth of the second burying layer 14B2 was performed by increasing the substrate temperature (growth temperature) to 1050° C. (second burying temperature) and then ionizing the SiO 2 layer with trimethylgallium (TMG) and NH 3 The second embedding temperature was higher than the first embedding temperature. However, if the growth surface of the second embedding layer 14B2 can be grown to be the (0001) plane, the temperature relationship between the second embedding temperature and the first embedding temperature may be reversed.

[0084] 4, a thermal effect causes mass transport to occur, and a second buried growth (flattened buried growth) is performed to form a second buried layer 14B2 having a (0001) surface. The first buried growth and the second buried growth form a buried layer 14B.

[0085] For ease of explanation, the layer from the upper surface of the hole layer 14P (the surface closer to the active layer 15) to the upper surface 14JS of the hole formation layer 14J (including a part of the hole formation layer 14J) is referred to as a first buried layer 14B1, and the layer from the upper surface 14JS of the hole formation layer 14J to the flat surface formed by the second buried growth is referred to as a second buried layer 14B2 (see FIG. 4, S3).

[0086] Moreover, the entire semiconductor layer from the upper surface of the hole layer 14P to the upper surface of the second buried layer 14B2 (including a part of the hole-formed layer 14J) is referred to as the buried layer 14B.

[0087] Here, the thickness of the first buried layer 14B1 is defined as D1, and the thickness of the second buried layer 14B2 is defined as D2. Therefore, the thickness of the buried layer 14B is given by D=D1+D2. In this specification, for each semiconductor layer of the n-side guide layer (first guide layer) 14, the “upper surface” refers to the surface on the side closer to the active layer 15.

[0088] In this embodiment, GaN is used for the second burying growth. The second burying layer 14B2 also functions as a light distribution adjusting layer for adjusting the coupling efficiency (light field) between light and the hole layer 14P.

[0089] That is, in this embodiment, undoped GaN is used for the first buried growth and the second buried growth. However, the first buried growth and the second buried growth are not limited to GaN, and n-GaN, n-InGaN, undoped GaN, undoped InGaN, or a combination of these semiconductors may be used.

[0090] (Step S4) Recrystallization growth Next, crystal growth of the layer above the light distribution adjustment layer 23 was carried out in a reactor on the substrate on which the etching of the buried layer 14B had been performed.

[0091] Specifically, the light distribution adjustment layer 23 is grown on the second buried layer 14B2. 0.03 Ga 0.97It is an N layer, which is a semiconductor layer (heterogeneous semiconductor layer) having a different crystal composition from the buried layer 14B (GaN layer).

[0092] Next, the active layer 15, the p-side guide layer (second guide layer) 16, the electron barrier layer (EBL) 17, the p-cladding layer 18, and the p-contact layer 19 were sequentially grown on the light distribution adjustment layer 23. In this manner, the PCSEL device 10 was fabricated.

[0093] (b) Vacancy layer The above-mentioned embedding process forms a hole layer 14P having a double lattice structure in which hole pairs 14K consisting of a main hole 14K1 and a subhole 14K2 are two-dimensionally arranged at each of the square lattice points. Here, the subhole 14K2 has a smaller hole diameter and height than the main hole 14K1. In the present invention, the upper surface of the hole in the hole layer 14P having a multi-lattice structure means the upper surface of the main hole 14K1 or the subhole 14K2 that is closer to the upper layer (active layer) (i.e., a hole having a shallower upper surface). Note that the hole pair 14K may be a single-photon structure in which holes of the same size are two-dimensionally arranged at each of the square lattice points, instead of the main hole 14K1 and the subhole 14K2 having different sizes.

[0094] 6 is a schematic diagram showing a cross section of the formed void layer 14P perpendicular to the central axis CX. When filling the holes 14H in the group III nitride, the shape of the holes 14H is deformed by mass transport into a shape composed of thermally stable surfaces, and voids 14K are formed.

[0095] That is, in the +c-plane substrate, the inner side surface of the hole 14H changes shape to a (1-100) plane (i.e., an m-plane), that is, changes shape from an oval cylindrical shape to an oval hexagonal prism-shaped hole 14K whose side surface is formed of an m-plane.

[0096] The formed primary void 14K1 had a long hexagonal prism shape with a long diameter of 72.5 nm, a short diameter of 43.5 nm, and a long diameter / short diameter ratio of 1.67. The secondary void 14K2 had a long diameter of 44.6 nm, a short diameter of 38.3 nm, and a long diameter / short diameter ratio of 1.16, and had a long hexagonal prism shape closer to a regular hexagonal prism than the primary void 14K1.

[0097] It was also confirmed that the distances Δx and Δy between the centers of gravity of the main hole 14K1 and the subhole 14K2 were 81.6 nm (Δx=Δy=0.46PK) and had not changed since before filling. It was also confirmed that the major axes of the main hole 14K1 and the subhole 14K2 were parallel to the <11-20> axis (i.e., the a-axis).

[0098] In addition, the void filling ratios (filling factors) FF1 and FF2 of the main voids 14K1 and the sub-voids 14K2 were calculated to be FF1 = 8.8% and FF2 = 4.2%. Here, the void filling ratio is the ratio of the area occupied by each void per unit area in a two-dimensional regular array. Specifically, when the areas of the main voids 14K1 and the sub-voids 14K2 in the void layer 14P are S1 and S2, respectively, the void filling ratios FF1 and FF2 of the main voids 14K1 and the sub-voids 14K2 are given by the following formulas.

[0099] FF1=S1 / PK 2 , FF2=S2 / PK 2 Through the above steps, the formation of the n-side guide layer 14 including the hole layer 14P is completed.

[0100] 3.Effects of surface oxidation / oxide film removal (a) Reduction of interface Si concentration 7 shows the results of SIMS (secondary ion mass spectrometry) measurement (SIMS profile) in the depth direction of a PCSEL device 10 (EMB) manufactured by performing a surface oxidation / oxide film removal process (step S1) on a substrate with holes 14H formed therein. For clarity of the figure, each semiconductor layer is indicated by its reference symbol. For example, "14B1" indicates the first buried layer 14B1, "14B2" indicates the second buried layer 14B2, and "23" indicates the light distribution adjustment layer 23.

[0101] FIG. 8 shows a SIMS profile in the depth direction of a PCSEL device (CMP) manufactured without carrying out the surface oxidation / oxide film removal process (step S1).

[0102] In the PCSEL element (CMP) in which surface oxidation / oxide film removal was not performed, the interface between the first buried layer 14B1 and the second buried layer 14B2 and the interface between the second buried layer 14B2 and the light distribution adjustment layer 23 had a 1×10 20 cm -3 A high concentration of Si was present.

[0103] On the other hand, as shown in Fig. 7, the Si concentration at the interface was reduced to 2 × 10 by oxidizing the surface Si through ozone treatment and removing the oxide film through BHF treatment. 19 cm -3 It is possible to reduce the amount of contamination to approximately 1 / 4 or less.

[0104] (b) Flatness of the regrowth layer On the semiconductor surface where the hole 14H was formed, a large amount of Si was deposited due to the adhesion of the SiNx film, which is a hard mask, and siloxane in the air. 3In an atmosphere where Si is dissociated at high temperatures), the surface Si reacts with N to form SiN. SiN forms an inversion domain on the GaN surface, which causes the polarity of GaN formed in the region contaminated by SiN on the top surface of the first buried layer by facet growth to be locally inverted, and an inversion domain is formed during shape change due to mass transport when forming the second buried layer 14B2, causing significant surface roughness. In addition, when doping with Si at a level that forms an inversion domain, point defects are likely to be introduced even if the buried layer can be grown while maintaining surface flatness.

[0105] That is, in the conventional technology, it is not possible to obtain a highly flat growth surface, and it is not possible to reduce the oscillation threshold current of the surface-emitting laser element. Also, since the hole layer 14P and the active layer 15 cannot be brought sufficiently close to each other, it is difficult to obtain a surface-emitting laser element having good characteristics and high coupling efficiency between the hole layer 14P and the active layer 15. Furthermore, a large number of point defects are introduced into the film, which deteriorates the crystallinity, making it difficult to obtain a surface-emitting laser element with good characteristics.

[0106] As described above, by performing the surface oxidation and oxide film removal treatment, the Si concentration at the interface can be significantly reduced and the formation of inversion domains can be suppressed, allowing the growth of a high-quality active layer with high flatness.

[0107] Therefore, a surface emitting semiconductor laser element with a low threshold and high efficiency can be provided.

[0108] [Second embodiment] Fig. 9A is a cross-sectional view showing an example of the structure of a photonic crystal surface-emitting laser device (PCSEL device) 30 according to a second embodiment, and Fig. 9B is an enlarged cross-sectional view showing an air hole layer 14P and air holes 14K arranged in the air hole layer 14P in Fig. 9A.

[0109] 10 is a flow chart showing a method for manufacturing the PCSEL device 30 of the second embodiment. Note that the same steps as those in the method for manufacturing the PCSEL device 10 of the first embodiment are denoted by the same reference numerals.

[0110] FIG. 11 is a cross-sectional view that diagrammatically shows a cross section of the n-side guide layer 14 in step S3A of the manufacturing method.

[0111] (a) Manufacturing method and structure of PCSEL element As shown in FIG. 10, in the PCSEL device 30, after performing a surface oxidation and oxide film removal process (step S1), the buried layer 14B is grown (steps S2 and S3). 2 The buried layer 14B was etched by annealing (Step S3A).

[0112] 11, the semiconductor layer on the void layer 14P was etched by TE from the surface of the buried layer 14B (thickness D). The thickness of the remaining buried layer 14B is DE (=D-TE). That is, the thickness from the top surface of the void 14K to the surface (top surface) of the remaining buried layer 14B is DE.

[0113] In other words, a buried layer 14BE (a thinned buried layer, hereinafter also referred to as a thinned buried layer) having a thickness DE is formed by the etching in step S3A.

[0114] That is, PCSEL device 30 differs from PCSEL device 10 of the first embodiment in that it has a thinned buried layer 14BE formed by etching, but is otherwise identical to PCSEL device 10 of the first embodiment.

[0115] (b) Thinning of buried layer -H 2 Annealing and Etching The buried layer 14B is immersed in H from the surface of the buried layer 14B. 2 The surface morphology of buried layer 14B (thinned buried layer 14BE) after etching by annealing was evaluated.

[0116] Specifically, samples (i) to (iv) were fabricated in which the thickness DE of the thinned buried layer 14BE (that is, the buried layer 14B after etching) was changed by changing the etching time.

[0117] As described above, the Si concentration at the interface is reduced to 2×10 19 cm -3 has been reduced to a certain extent.

[0118] FIG. 12 shows a state in which the surface of the semiconductor layer on which the buried layer 14B is regrown after the surface oxidation / oxide film removal process (step S1) is performed. 2 1 is an SEM image showing a cross section after etching by annealing.

[0119] As shown in FIG. 12, the thickness DE of the thinned buried layer 14BE was (i) DE=114 nm, (ii) DE=66 nm, (iii) DE=4 nm, and (iv) DE<1 nm.

[0120] H 2 In annealing in the atmosphere, the (0001) plane is a thermally stable plane, and the buried layer 14B can be etched and thinned while maintaining the flatness of the surface. Therefore, a high-quality active layer with high flatness can be grown on the buried layer 14B. The annealing atmosphere may contain Group III and Group V materials.

[0121] More specifically, in Group III nitride semiconductors, H 2 When high-temperature annealing is performed in an atmosphere, surface atoms are desorbed, and the surface is etched. At this time, the surface with the slowest etching rate remains, so the most thermally stable (0001) surface is formed on the surface. Therefore, when a +c-plane substrate is used, etching can be performed while maintaining the (0001) surface parallel to the substrate. This allows the buried layer 14B to be made thinner, and the interval (distance) between the vacancy layer 14P (vacancy layer) and the active layer 15 to be reduced.

[0122] The surface morphologies of samples (i) to (iv) were observed using an AFM (atomic force microscope). Fig. 13 shows AFM images of the surfaces of samples (i) to (iv).

[0123] When the thickness DE of the thinned buried layer 14BE was (i) DE=114 nm, (ii) DE=66 nm, (iii) DE=4 nm, and (iv) DE<1 nm, the surface roughness was Ra=0.633 nm, 0.508 nm, 0.532 nm, and 2.43 nm, respectively, in an area of ​​20 μm×20 μm.

[0124] It was found that a sufficiently flat surface could be obtained in the cases of (i) to (iii). It was also found that good flatness could be obtained even when the substrate was made extremely thin, at DE=4 nm (iii). In the case of (iv) DE<1 nm, significant surface roughness was observed.

[0125] FIG. 14 is a graph plotting the surface roughness Ra in a 20 μm×20 μm area versus the thickness DE of the thinned buried layer 14BE.

[0126] 14, it can be seen that a sufficiently flat surface can be obtained if DE≧4 nm. More specifically, it can be seen that if the thickness DE of the thinned embedding layer 14BE is 4 nm or more, the surface roughness Ra in a 20 μm×20 μm region can be Ra≦0.7 nm.

[0127] (c) Distance between the cavity layer and the active layer From the above results, it can be seen that if the distance between the air hole layer 14P and the active layer 15, i.e., the distance between the upper surface of the air holes 14K in the air hole layer 14P and the active layer 15, is 4 nm or more, a sufficiently flat active layer 15 can be obtained, and a surface-emitting laser element with high coupling efficiency between the air hole layer 14P and the active layer 15 and good characteristics can be obtained.

[0128] In order to obtain high coupling efficiency, the distance between the hole layer 14P and the active layer 15 is preferably 200 nm or less.

[0129] Furthermore, by setting the distance between the hole layer 14P and the active layer 15 to 4 to 150 nm, a surface-emitting semiconductor laser device having a higher resonance effect, a low threshold value, and high efficiency can be obtained.

[0130] In addition, when the active layer 15 is an active layer having a quantum well structure, the distance between the upper surface of the hole 14K and the active layer 15 refers to the distance between the upper surface of the hole 14K and the first quantum well layer (i.e., the quantum well layer closest to the hole layer 14P).

[0131] In addition, in the conventional multi-lattice structure hole layer, in order to obtain a high hole filling rate, a thicker buried layer may be required than in the single-lattice structure hole layer. According to the present invention, even in such a case, a thin buried layer can be used, and a high coupling efficiency (resonance effect) between the hole layer and the active layer can be obtained.

[0132] According to this embodiment, the hole layer 14P and the active layer 15 having high flatness can be provided close to each other. Specifically, as described above, if the thickness of the buried layer 14BE is 4 nm or more, the surface roughness Ra of the buried layer 14BE is Ra≦0.7 nm.

[0133] As shown in the SIMS measurement results of FIGS. 7 and 8, in the portion where the Si concentration in the first buried layer 14B1 is flat, the Si concentration is about 4.5×10 18 cm -3 This is approximately 6.0×10 compared to when the oxide film was not removed (Fig. 8). 18 cm -3 It can be seen that it is reduced compared to

[0134] Therefore, it can be understood that by oxidizing the surface of the hole formation layer 14J and removing the oxide film, the Si concentration in the buried layer 14B is reduced, and a semiconductor layer having high flatness can be regrown.

[0135] The first and second embodiments have been described above in detail. In the first and second embodiments, the case where the light distribution adjustment layer 23 is provided has been described, but the active layer 15 may be formed directly on the buried layer 14B or the buried layer 14BE without providing the light distribution adjustment layer 23. In this case, the hole layer 14P and the active layer 15 having high flatness may be provided adjacent to each other.

[0136] As described above in detail, according to the present invention, it is possible to provide a method for manufacturing a surface-emitting semiconductor laser element and a photonic crystal surface-emitting laser element that can enhance the resonance effect by bringing the hole layer and the active layer into close proximity to each other and have a high-quality active layer and have a low threshold and high efficiency.

[0137] Unless otherwise specified, the numerical values ​​and the like in the above-described embodiments are merely examples and may be modified as appropriate. In addition, although a double lattice structure PCSEL element has been illustrated, the present invention can be applied to a single lattice structure PCSEL element and generally to a multiple lattice structure PCSEL element.

[0138] Furthermore, although the present invention has been exemplified with respect to a photonic crystal layer in which the holes have a hexagonal columnar shape, the present invention can also be applied to photonic crystal layers in which the holes have an irregular columnar shape, such as a cylindrical, rectangular, polygonal, or teardrop shape. [Explanation of symbols]

[0139] 10: PCSEL element 12: Element substrate 13: First cladding layer 14: First guide layer 14A: Lower guide layer 14B: Buried layer 14BE: Buried layer 14B1: First buried layer 14B2: second buried layer 14B2: second buried layer 14E: Hole formation preparation layer 14J: Hole forming layer 14K: Hole / hole pair 14K1 / 14K2: Main / secondary hole 14P: Photonic crystal layer (hole layer) 15:Active layer 16: Second guide layer 17: Electron barrier layer 18: Second cladding layer 19: Contact layer 23: Light distribution adjustment layer

Claims

1. A method for manufacturing a surface emitting semiconductor laser device, comprising the steps of: (a) forming a hole formation preparation layer on a substrate; (b) forming holes arranged two-dimensionally at each of the lattice points in the hole formation preparation layer to form a hole formation layer; (c) oxidizing the surface of the hole formation layer to form an oxide film, and then removing the oxide film; (d) forming a first burying layer by facet growth to close the hole; (e) growing a second burying layer that buries the first burying layer flatly to form a first guide layer including a hole layer having holes corresponding to the holes; (f) growing crystals of a semiconductor layer including an active layer on the first guide layer.

2. A method for manufacturing a surface emitting semiconductor laser device, comprising the steps of: (a) forming a hole formation preparation layer on a substrate; (b) forming holes arranged two-dimensionally at each of the lattice points in the hole formation preparation layer to form a hole formation layer; (c) oxidizing the surface of the hole formation layer to form an oxide film, and then removing the oxide film; (d) forming a first burying layer by facet growth to close the hole; (e) growing a second burying layer that buries the first burying layer flatly to form a first guide layer including a hole layer having holes corresponding to the holes; (f) flattening the surface of the first guide layer by annealing in a hydrogen atmosphere; (g) growing a semiconductor layer including an active layer on the flat etched first guide layer.

3. 3. The method according to claim 1, wherein the step of forming the oxide film comprises oxidizing the surface of the hole formation layer with ozone.

4. the surface emitting semiconductor laser element is a GaN-based semiconductor laser element, The Si concentration at the interface between the guide layer and the semiconductor layer including the active layer is 2×10 19 cm -3 The method according to claim 1 or 2, wherein:

5. the surface emitting semiconductor laser element is a GaN-based semiconductor laser element, the crystal growth surface of the substrate is a {0001} surface; The facet plane of the facet growth is a {1-101} plane. The method according to claim 1 or 2.

6. 3. The method according to claim 1, wherein a distance from an upper surface of the hole in the hole layer to the active layer is 200 nm or less.

7. 3. The method according to claim 2, wherein the thickness of the second buried layer on the upper surface of the hole formation layer after the flattening etching is 4 nm or more.

8. An n-type semiconductor layer; a first guide layer including: a hole layer formed on the n-type semiconductor layer, the hole layer having holes arranged two-dimensionally at each lattice point; and a buried layer formed on the hole layer to close the holes; a semiconductor layer including an active layer formed on the buried layer; a second guide layer formed on the semiconductor layer including the active layer; a distance from an upper surface of the hole in the hole layer to the active layer is 4 to 200 nm; Surface-emitting semiconductor laser element.

9. 9. The surface emitting semiconductor laser device according to claim 8, wherein the surface roughness Ra of the buried layer is Ra≦0.7 nm.

10. the active layer has a quantum well structure, 9. The surface emitting semiconductor laser device according to claim 8, wherein the distance to the active layer is the distance between a quantum well closest to the hole layer and an upper surface of the hole.

11. 9. The surface emitting semiconductor laser element according to claim 8, wherein the semiconductor layer including the active layer is provided between the buried layer and the active layer, and includes a heterogeneous semiconductor layer having a crystal composition different from that of the buried layer.

Citation Information

Patent Citations

  • Surface-emitting laser element and manufacturing method of surface-emitting laser element

    JP2020038892A

  • Surface-emitting laser and method of manufacturing the surface-emitting laser

    JP7101370B2

  • Surface-emitting laser and method for manufacturing surface-emitting laser