Tantalum carbide coating material and compound semiconductor growth device

A tantalum carbide coating with controlled crack intersections and adhesion strength addresses the peeling issue in high-temperature environments, improving durability and reducing costs for compound semiconductor manufacturing.

JP2024143156APending Publication Date: 2024-10-11SHIN ETSU CHEMICAL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023055682
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The high manufacturing costs of compound semiconductors like SiC are due to the need for highly heat-resistant members with superior corrosion resistance, and tantalum carbide coatings tend to peel off in harsh high-temperature environments.

Method used

A tantalum carbide coating material with controlled crack intersections, surface roughness, and adhesion strength is developed to prevent peeling, using a chemical vapor deposition method.

Benefits of technology

The coating material effectively suppresses peeling in high-temperature corrosive environments, enhancing durability and reducing manufacturing costs by extending the lifespan of components in compound semiconductor growth devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143156000001_ABST
    Figure 2024143156000001_ABST
Patent Text Reader

Abstract

To provide a tantalum carbide coating material capable of suppressing the peeling of a tantalum carbide coating film in hot corrosive environments, and a compound semiconductor growth device that uses the tantalum carbide coating material.SOLUTION: The present invention relates to a tantalum carbide coating material 1 including a base material 12 and a tantalum carbide coating film 11 that coats at least a part of the base material 12, wherein the number of intersections of cracks present on the surface of the tantalum carbide coating film 11 per unit area is 25 / cm2 or less. A compound semiconductor growth device according to the present invention uses the tantalum carbide coating material according to the present invention.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a tantalum carbide coating material having a substrate surface coated with a tantalum carbide coating film, and a compound semiconductor growth apparatus using the tantalum carbide coating material. [Background technology]

[0002] Carbides such as tantalum carbide, niobium carbide, zirconium carbide, hafnium carbide, and tungsten carbide have a high melting point and are excellent in chemical stability, strength, toughness, and corrosion resistance. Therefore, by coating a carbon substrate with a carbide, the properties of the carbon substrate, such as heat resistance, chemical stability, strength, toughness, and corrosion resistance, can be improved. Carbide-coated carbon materials, in which a carbide film is coated on the surface of a carbon substrate, particularly tantalum carbide-coated carbon materials, are used as components of compound semiconductor growth devices for compound semiconductors such as SiC (silicon carbide), GaN (gallium nitride), and AlN (aluminum nitride). For example, in a manufacturing device for SiC single crystals, Patent Document 1 discloses the use of a crucible in which the inner surface of a graphite substrate is coated with tantalum carbide in order to obtain higher quality crystals. Patent Document 2 also discloses the use of a guide member in a manufacturing device for SiC single crystals, the inner wall of which is coated with tantalum carbide. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2019-99453 A [Patent Document 2] JP 2019-108611 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, compound semiconductors have a problem in that their manufacturing costs are higher than those of conventional Si semiconductors. To further reduce this manufacturing cost, highly heat-resistant components with improved corrosion resistance are required. For example, the manufacturing environment for SiC single crystals is a harsh environment with temperatures exceeding 2000°C. Tantalum carbide coating materials are required to have high durability and not to cause peeling of the tantalum carbide coating film even in such a high-temperature corrosive environment.

[0005] Therefore, an object of the present invention is to suppress peeling of a tantalum carbide coating film in a high-temperature corrosive environment. [Means for solving the problem]

[0006] As a result of intensive research, the inventors have found that the fewer the number of intersections of cracks present on the surface of the tantalum carbide coating film, the less likely the tantalum carbide coating film is to peel off after use in the production of SiC single crystals, and have completed the present invention. [1] A tantalum carbide coating material comprising a substrate and a tantalum carbide coating film covering at least a portion of the substrate, the tantalum carbide coating film having a surface with a crack intersection number per unit area of ​​25 / cm 2 Tantalum carbide coated material, which is: [2] The tantalum carbide coating material according to the above [1] or [2], wherein the average length Rsm of the roughness curve element on the surface of the tantalum carbide coating film is 10 μm or less. [3] The tantalum carbide coating material according to the above [1] or [2], wherein the average length Rsm of the roughness curve elements at the interface between the substrate and the tantalum carbide coating film is 0.1 mm or more and 5.0 mm or less. [4] The tantalum carbide coated material according to any one of the above [1] to [3], wherein the substrate is a carbon substrate containing carbon as a main component. [5] The tantalum carbide coated material according to any one of the above [1] to [4], wherein the adhesive strength between the tantalum carbide coating film and the substrate is 5 MPa or more. [6] The linear thermal expansion coefficient of the substrate is 3.5 × 10 -6 / ℃ or more 7.5×10 -6 The tantalum carbide coated material according to any one of the above [1] to [5], wherein the thermal expansion coefficient is 0.05 to 0.5 / °C or less. [7] A compound semiconductor growth apparatus using the tantalum carbide coating material according to any one of [1] to [6] above. Effect of the Invention

[0007] According to the present invention, it is possible to provide a tantalum carbide coating material capable of suppressing peeling of a tantalum carbide coating film in a high-temperature corrosive environment, and a compound semiconductor growth apparatus using the tantalum carbide coating material. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a schematic cross-sectional view illustrating a tantalum carbide coated material according to this embodiment. [Diagram 2] FIG. 2 is a schematic diagram of an externally heated low-pressure CVD apparatus. [Diagram 3] Figure 3(a) is an image of a film surface when there are two cracks per unit area that intersect, and Figure 3(b) is an image of the a-a' cross section of Figure 3(a). [Figure 4] Figure 4(a) is an image of a film surface when there are two cracks per unit area that do not intersect, and Figure 4(b) is an image of the b-b' cross section of Figure 4(a). [Diagram 5] FIG. 5 is a scanning electron microscope (SEM) photograph of the surface of a tantalum carbide coated carbon material after use in the production of SiC single crystals. [Figure 6] FIG. 6 is a diagram for explaining a method for measuring the adhesive strength between a tantalum carbide coating film and a substrate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Referring to FIG. 1, a tantalum carbide coating material according to one embodiment of the present invention will be described.

[0010] [Tantalum carbide coating material] A tantalum carbide coating material 1 according to one embodiment of the present invention includes a substrate 12 and a tantalum carbide coating film 11 that coats at least a portion of the substrate 12. The number of intersections of cracks present on the surface of the tantalum carbide coating film 11 per unit area is 25 / cm. 2 The following is the result.

[0011] (base material) The substrate 12 in the tantalum carbide coating material 1 in one embodiment of the present invention is not limited to a particular type as long as it is suitable for the intended use. Examples of the substrate 12 include carbon substrates mainly made of carbon materials such as isotropic graphite, extruded graphite, pyrolytic graphite, and carbon fiber reinforced carbon composite materials (C / C composites), and high melting point metal substrates made of high melting point metal materials such as tantalum. Among these, the substrate 12 in the tantalum carbide coating material 1 in one embodiment of the present invention is preferably a carbon substrate mainly made of carbon. The shape and characteristics of the substrate are not particularly limited, and a substrate processed into any shape depending on the intended use can be used.

[0012] <Linear thermal expansion coefficient> The linear thermal expansion coefficient of the substrate 12 is preferably 3.5×10 -6 / ℃ or more 7.5×10 -6 / °C or less. The linear thermal expansion coefficient of the carbon substrate 12 is 3.5×10 -6 / ℃ or more 7.5×10 -6 / °C or less, the occurrence of cracks on the surface of the tantalum carbide coating material 1 can be further suppressed. From this viewpoint, the linear thermal expansion coefficient of the carbon substrate 12 is more preferably 3.5×10 -6 / ℃ or more 7.5×10 -6 / °C or less, and more preferably 5.6 × 10 -6 / ℃ or more 7.5×10 -6 / °C or less. The linear thermal expansion coefficient of the tantalum carbide coating film 11 is approximately 6.3×10 -6 / °C. The linear thermal expansion coefficient of the substrate can be measured in accordance with JIS R 1618.

[0013] (Tantalum carbide coating) The tantalum carbide coating film 11 contains tantalum carbide as a main component and coats the substrate 12. The tantalum carbide coating film 11 may coat a portion of the substrate 12, or may coat the entire substrate 12.

[0014] <Number of crack intersections> The number of intersections of cracks on the surface of the tantalum carbide coating film 11 per unit area is 25 / cm 2 The number of intersections of cracks on the surface of the tantalum carbide coating film 11 per unit area is 25 / cm 2 If the number is greater than 1, damage to the substrate 12 occurring through cracks present on the surface of the tantalum carbide coating film 11 will become greater in a high-temperature corrosive environment, and the tantalum carbide coating film 11 may peel off. From this perspective, the number of intersections of cracks present on the surface of the tantalum carbide coating film 11 per unit area is preferably 24.9 pcs / cm. 2 More preferably, 23 particles / cm 2 or less, and more preferably 21.3 particles / cm 2 and even more preferably 13.4 cells / cm 2 or less, and particularly preferably 6.8 particles / cm 2 The lower limit of the range of the number of intersections of cracks present on the surface of the tantalum carbide coating film 11 per unit area is 0 pieces / cm 2 The number of intersections of cracks present on the surface of the tantalum carbide coating film 11 per unit area can be adjusted by the average length Rsm of the roughness curve elements on the surface of the substrate 12 and the linear thermal expansion coefficient of the substrate 12.

[0015] The reason why a small number of intersections of cracks per unit area on the surface of the tantalum carbide coating film 11 can suppress peeling of the tantalum carbide coating film 11 will be explained below. Note that this explanation does not limit the tantalum carbide coating material of the present invention. It is known that when a tantalum carbide coating material 1 having a crack on the surface of the tantalum carbide coating film 11 is exposed to a high-temperature corrosion environment of 2000°C or higher, the substrate 12 is damaged around the crack (see, for example, JP 2022-87846 A). When the damaged portion of the substrate 12 becomes large, the substrate 12 is no longer able to support the tantalum carbide coating film 11, and as a result, the tantalum carbide coating film 11 peels off. In the vicinity of the intersection of the cracks, the damage to the substrate 12 becomes large due to the two cracks, so the damage to the substrate 12 becomes large rapidly. As a result, the peeling of the tantalum carbide coating film 11 becomes even more likely to occur. Note that when the peeling of the tantalum carbide coating film 11 occurs, damage progresses in the portion of the substrate 12 from which the tantalum carbide coating film 11 peeled off. As a result, the peeling of the tantalum carbide coating film 11 progresses further. As a result, the tantalum carbide coating material falls into a vicious cycle of peeling of the tantalum carbide coating film 11 and damage to the substrate 12. Therefore, if the number of intersections of cracks present on the surface of tantalum carbide coating film 11 per unit area is small, the promotion of damage to the substrate caused by the two cracks is suppressed, and peeling of tantalum carbide coating film 11 is suppressed.

[0016] Here, in the case where there are two cracks per unit area on the surface of the tantalum carbide coating film 11, we consider a case where the two cracks have an intersection (see FIG. 3) and a case where they do not have an intersection (see FIG. 4). When each tantalum carbide coating material 1 is exposed to a high-temperature corrosive environment, the substrate 12 is damaged from the vicinity of the crack 31, but when there is an intersection 30 of the cracks 31, it is expected that the size of the damage 32 near the intersection 30 will be larger than when there is no intersection of the cracks 31 (see FIGS. 3(b) and 4(b)). For this reason, peeling of the tantalum carbide coating film is more likely to occur near the crack intersection 30 than near a normal crack 31.

[0017] 5 is an image of the surface of the tantalum carbide-coated carbon material after it has been used in a SiC single crystal growth environment, observed with a scanning electron microscope (SEM), and it can be seen that peeling of the tantalum carbide coating film has occurred at the intersections of the cracks. Therefore, if the number of intersections of the cracks on the surface of the tantalum carbide coating film 11 per unit area is small, i.e., the number of intersections of the cracks on the surface of the tantalum carbide coating film 11 per unit area is less than 25 / cm. 2 If it is equal to or less than this, peeling of the tantalum carbide coating film is unlikely to occur when the tantalum carbide coating material is exposed to a high-temperature corrosive environment.

[0018] The number of intersections of cracks present on the surface of the tantalum carbide coating film 11 per unit area can be measured as follows. Since the cracks occurring in the tantalum carbide coating material are too large to be seen with the naked eye, the number of intersections of cracks present on the surface of the tantalum carbide coating film 11 per unit area is measured by one or both of the following two methods.

[0019] (1) Measurement using a scanning electron microscope (SEM) The sample is processed to a size that can be observed by SEM, and its surface is observed. In this case, the information obtained from one image is about 6 mm at maximum. 2 (=2mm×3mm), so 1cm 2 To observe a range of 1000 mm, it is necessary to obtain about 17 images. In addition, to avoid bias due to local observation, it is necessary to obtain about 17 images at another location that is sufficiently distant. This operation is repeated 10 times to obtain a total of 170 or more images, and the number of crack intersections is counted from this total of 170 or more images. The value obtained by dividing the number of crack intersections by the area of ​​the portion observed using the total of 170 or more images obtained is the number of crack intersections per unit area (number / cm2) present on the surface of the tantalum carbide coating film 11. 2 )

[0020] (2) Measurement using flaw detection agents Depending on the shape of the sample, processing may be required for SEM observation, and during this processing, cracks may appear on the surface of the tantalum carbide coating. To eliminate this possibility, cracks are visualized using a flaw detection agent that can detect cracks on the order of μm, and the cracks are then detected visually or using an optical microscope to measure the cracks on a 1cm scale. 2 The number of crack intersections per hit may be measured.

[0021] <Average length of roughness curve element Rsm> The average length Rsm of the surface roughness curve element of the tantalum carbide coating film 11 is preferably 10 μm or less. When the average length Rsm of the surface roughness curve element of the tantalum carbide coating film 11 is 10 μm or less, it is possible to suppress adhesion of dust particles in the air to the surface of the tantalum carbide coating film 11. From this viewpoint, the average length Rsm of the surface roughness curve element of the tantalum carbide coating film 11 is more preferably 9.8 μm or less, and even more preferably 6.5 μm or less. The lower limit of the range of the average length Rsm of the surface roughness curve element of the tantalum carbide coating film 11 is not particularly limited, but is usually 1.1 μm.

[0022] The average length Rsm of the roughness curve element at the interface between the substrate 12 and the tantalum carbide coating film 11 is preferably 0.1 mm or more and 5.0 mm or less. When the average length Rsm of the roughness curve element at the interface between the substrate 12 and the tantalum carbide coating film 11 is 0.1 mm or more and 5.0 mm or less, the adhesion strength between the substrate 12 and the tantalum carbide coating film 11 can be further increased. In addition, when the average length Rsm of the roughness curve element at the interface between the substrate 12 and the tantalum carbide coating film 11 is 0.1 mm or more and 5.0 mm or less, the number of intersections of cracks present on the surface of the tantalum carbide coating film 11 per unit area can be further reduced. From this viewpoint, the average length Rsm of the roughness curve element at the interface between the substrate 12 and the tantalum carbide coating film 11 is more preferably 0.5 mm or more and 5.0 mm or less, even more preferably 1.0 mm or more and 5.0 mm or less, and even more preferably 2.0 mm or more and 5.0 mm or less. The average length Rsm of the roughness curve elements at the interface between the substrate 12 and the tantalum carbide coating film 11 is the same value as the average length Rsm of the roughness curve elements on the surface of the substrate 12. Therefore, by setting the average length Rsm of the roughness curve elements on the surface of the substrate 12 within the above range, the average length Rsm of the roughness curve elements at the interface between the substrate 12 and the tantalum carbide coating film 11 can be set within the above range. The average length Rsm of the roughness curve elements on the surface of the substrate 12 may be due to an intentionally created pattern, or may be due to marks of a cutting tool during machining.

[0023] The average length of the roughness curve element RSm can be measured using a commercially available surface roughness meter or a microscopic image of the fracture cross section, and is the average length of the roughness curve element specified in JIS B0601:2013 and ISO 4287:1997. The average length of the roughness curve element RSm is the distance x from the i-th peak to the i+1-th peak on the cross-sectional profile. i Using the spacing m between the peaks, this is expressed by the following formula. Rsm = (1 / m) × Σx i (i=1~m) Furthermore, the minimum height for determining a mountain is 10% of the average height Rz of the cross-sectional profile curve. It can be said that the larger the value of the average length Rsm of the roughness curve element, the larger the periodic interval of the roughness is, and the smaller the value of the average length Rsm of the roughness curve element, the smaller the periodic interval of the roughness is.

[0024] The adhesion strength between the tantalum carbide coating film 11 and the substrate 12 is preferably 5 MPa or more. If the adhesion strength between the tantalum carbide coating film 11 and the substrate 12 is 5 MPa or more, peeling of the tantalum carbide coating film in a high-temperature corrosive environment can be further suppressed. From this viewpoint, the adhesion strength between the tantalum carbide coating film 11 and the substrate 12 is more preferably 5.1 MPa or more, and further preferably 6.5 MPa or more. The upper limit of the range of the adhesion strength between the tantalum carbide coating film 11 and the substrate 12 is not particularly limited, but is usually 18.5 MPa.

[0025] The adhesion strength between the tantalum carbide coating film 11 and the substrate 12 was measured, for example, using a thin film adhesion strength measuring device (manufactured by Quad Group, product name "Romulus"), by adhering the tantalum carbide coating film 11 and a pin 46 with adhesive 45, pressing down with a pressing jig 44 and pulling the pin 46, as shown in Fig. 6, to measure the stress at which the tantalum carbide coating film 41 peeled off. Five measurements were made, and the average of the five calculations was taken as the adhesion strength.

[0026] <Method of manufacturing tantalum carbide coated material> The tantalum carbide coating material according to one embodiment of the present invention can be produced by forming a tantalum carbide coating film on the surface of a substrate. The tantalum carbide coating film can be formed on the surface of the substrate by, for example, a chemical vapor deposition (CVD) method, a sintering method, a carbonization method, or the like. Among these, the CVD method is preferred as a method for forming a tantalum carbide layer, since it can form a uniform and dense film.

[0027] Furthermore, the CVD method includes a thermal CVD method, a photo-CVD method, a plasma CVD method, and the like, and the thermal CVD method, for example, can be used to form a tantalum carbide coating film. The thermal CVD method has advantages such as a relatively simple apparatus configuration and no damage caused by plasma. The formation of a tantalum carbide coating film by the thermal CVD method can be performed, for example, using an externally heated low-pressure CVD apparatus 20 as shown in FIG. 2. In the externally heated low-pressure CVD apparatus 20, the substrate 12 is supported by a support means 25 in a reaction chamber 24 equipped with a heater 21, a raw material supply unit 22, an exhaust unit 23, and the like.

[0028] A method for producing a tantalum carbide coating material according to one embodiment of the present invention will be described with reference to FIGS. First, the substrate 12 is placed in the reaction chamber 24 of the external heat type low pressure CVD apparatus 20. The substrate 12 is supported by a supporting means 25 having a supporting portion with a pointed tip. Next, heating is performed by the heater 21. For example, the heater 21 is heated under reduced pressure at a temperature of 1000 to 2500°C. Next, a tantalum carbide coating film is formed on the surface of the substrate 12. As raw material gases, a gas of a compound containing carbon atoms such as methane (CH4) and a tantalum halide gas such as tantalum pentachloride (TaCl5) are supplied from the raw material supply unit 22 to the reaction chamber 24. Next, the raw material gas supplied from the raw material supply unit 22 is subjected to a thermal CVD reaction at a high temperature of 1000 to 2500°C under reduced pressure, to form a tantalum carbide coating film on the surface of the substrate 12.

[0029] The tantalum carbide coating material of one embodiment of the present invention is merely one example of the tantalum carbide coating material of the present invention, and therefore does not limit the tantalum carbide coating material of the present invention.

[0030] [Compound semiconductor growth equipment] The compound semiconductor growth apparatus of the present invention uses the tantalum carbide coating material of the present invention. The tantalum carbide coating material of the present invention is used as a component of a compound semiconductor growth apparatus for compound semiconductors such as SiC (silicon carbide), GaN (gallium nitride), and AlN (aluminum nitride). EXAMPLES

[0031] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these.

[0032] Tantalum carbide-coated carbon materials of Examples 1 to 17 and Comparative Examples 1 to 6 were produced as follows.

[0033] Example 1 The substrate 12 has a linear thermal expansion coefficient of 3.5×10 -6 Two isotropic carbon materials were prepared, each having a surface roughness curve element average length Rsm of 4.3 mm and a linear thermal expansion coefficient of 1.0 μm / °C. The linear thermal expansion coefficient of the same carbon material sample was measured using a thermomechanical analyzer (manufactured by Hitachi High-Tech Science Corporation, product name "TMA7300"). The average length Rsm of the surface roughness curve element of the substrate 12 was measured using a surface roughness meter (manufactured by Mitutoyo Corporation, product name "SJ201"). Next, the substrate 12 was placed in a reaction chamber of an external heat type low pressure CVD apparatus 20 shown in Fig. 2. The substrate 12 was supported by a supporting means 25 having three supporting parts each having a pointed tip. Next, after heating the reaction chamber 24 to a temperature of 1500°C, TaCl5 gas, CH4 gas and Ar gas were mixed and the resulting mixed gas was supplied to the reaction chamber 24 to form a tantalum carbide coating film on the surface of the carbon substrate 12, thereby producing the tantalum carbide-coated carbon material of Example 1. The flow rates of the CH4 gas and the carrier gas (Ar) were controlled by mass flow controllers to be 1.0 SLM and 1.0 SLM, respectively.

[0034] Of the two tantalum carbide-coated carbon materials prepared, one was used for the various measurements described below, and the other was used to produce SiC single crystals, and the number of uses was counted until peeling of the tantalum carbide coating film was visible to the naked eye.

[0035] The number of crack intersections per unit area present on the surface of the tantalum carbide coating film, the average length Rsm of the roughness curve element of the surface of the tantalum carbide coating film, and the adhesion strength between the tantalum carbide coating film and the substrate of one of the prepared tantalum carbide-coated carbon materials were measured. The method for measuring the number of crack intersections per unit area present on the surface of the tantalum carbide coating film was as described above, and an SEM (manufactured by Keyence Corporation, product name "VE8800") and a flaw detector (Microcheck cleaning solution, Microcheck penetrant solution, and Microcheck developer, manufactured by Ichinen Chemicals Corporation) were used. The surface roughness of the tantalum carbide coating film was measured with a surface roughness meter (manufactured by Mitutoyo Corporation, product name "SJ201"). The adhesion strength between the substrate 12 and the tantalum carbide coating film 11 was measured with a thin film adhesion strength measuring device (manufactured by Quad Group, product name "Romulus").

[0036] Example 2 The base material 12 has a thermal expansion coefficient of 4.2×10 -6 Two isotropic carbon materials having a surface roughness of 4.2 mm, a surface roughness curve element average length Rsm of 4.2 mm, and a surface roughness of 4.2 mm were prepared.

[0037] Example 3 The base material 12 has a thermal expansion coefficient of 4.5×10 -6 Two isotropic carbon materials having a surface roughness of 4.6 mm Rsm and a surface roughness curve element average length Rsm of 4.6 mm were prepared.

[0038] Example 4 The base material 12 has a thermal expansion coefficient of 5.1×10 -6 Two isotropic carbon materials having a surface roughness of 4.1 mm Rsm were prepared.

[0039] Example 5 The base material 12 has a thermal expansion coefficient of 5.6×10 -6 Two isotropic carbon materials having a surface roughness of 4.5 mm, a surface roughness curve element average length Rsm of 4.5 mm, and a surface roughness of 4.5 mm were prepared.

[0040] Example 6 The base material 12 has a thermal expansion coefficient of 6.0×10 -6 Two isotropic carbon materials having a surface roughness of 4.4 mm, a surface roughness curve element average length Rsm of 4.4 mm, and a surface roughness of 4.4 mm were prepared.

[0041] Example 7 The base material 12 has a thermal expansion coefficient of 6.4×10 -6 Two isotropic carbon materials having a surface roughness of 4.4 mm, a surface roughness curve element average length Rsm of 4.4 mm, and a surface roughness of 4.4 mm were prepared.

[0042] Example 8 The base material 12 has a thermal expansion coefficient of 6.9×10 -6 Two isotropic carbon materials having a surface roughness of 4.3 mm, a surface roughness curve element average length Rsm of 4.3 mm, and a surface roughness of 4.3 mm were prepared.

[0043] Example 9 The base material 12 has a thermal expansion coefficient of 7.5×10 -6 Two isotropic carbon materials having a surface roughness of 4.2 mm, a surface roughness curve element average length Rsm of 4.2 mm, and a surface roughness of 4.2 mm were prepared.

[0044] Example 10 The substrate 12 has a linear thermal expansion coefficient of 4.2×10 -6 Two isotropic carbon materials having a surface roughness of 0.1 mm, a viscosity of 1000 s / ° C., and an average length Rsm of the surface roughness curve element of 0.1 mm, were prepared.

[0045] Example 11 The substrate 12 has a linear thermal expansion coefficient of 4.2×10 -6 Two isotropic carbon materials having a surface roughness of 0.9 mm, a surface roughness curve element average length Rsm of 0.9 mm, and a surface roughness of 0.5 mm were prepared.

[0046] Example 12 The substrate 12 has a linear thermal expansion coefficient of 4.2×10 -6 Two isotropic carbon materials having a surface roughness of 2.1 mm, a surface roughness curve element average length Rsm of 2.1 mm, and a surface roughness of 2.1 mm were prepared.

[0047] (Example 13) The substrate 12 has a linear thermal expansion coefficient of 4.2×10 -6 Two isotropic carbon materials having a surface roughness of 3.5 mm, a surface roughness curve element average length Rsm of 3.5 mm, and a surface roughness of 3.5 mm were prepared.

[0048] Example 14 The substrate 12 has a linear thermal expansion coefficient of 4.2×10 -6 Two isotropic carbon materials having a surface roughness of 0.05 to 0.25 mm and an average length Rsm of the surface roughness curve element of 5.0 mm were prepared.

[0049] Example 15 The substrate 12 has a linear thermal expansion coefficient of 6.4×10 -6 Two isotropic carbon materials having a surface roughness of 0.04 mm Rsm and a surface roughness curve element average length Rsm of 0.04 mm were prepared.

[0050] (Example 16) The substrate 12 has a linear thermal expansion coefficient of 6.9×10 -6 Two isotropic carbon materials having a surface roughness of 0.02 mm Rsm and a surface roughness curve element average length Rsm of 0.02 mm were prepared.

[0051] (Example 17) The substrate 12 has a linear thermal expansion coefficient of 7.5×10 -6 Two isotropic carbon materials having a surface roughness of 0.06 mm Rsm were prepared.

[0052] Comparative Example 1 The substrate 12 has a linear thermal expansion coefficient of 3.5×10 -6Two isotropic carbon materials having a surface roughness of 0.04 mm Rsm and a surface roughness curve element average length Rsm of 0.04 mm were prepared.

[0053] Comparative Example 2 The substrate 12 has a linear thermal expansion coefficient of 4.2×10 -6 Two isotropic carbon materials having a surface roughness of 0.06 mm Rsm were prepared.

[0054] Comparative Example 3 The substrate 12 has a linear thermal expansion coefficient of 4.5×10 -6 Two isotropic carbon materials having a surface roughness curve element average length Rsm of 0.03 mm were prepared.

[0055] Comparative Example 4 The substrate 12 has a linear thermal expansion coefficient of 5.1×10 -6 Two isotropic carbon materials having a surface roughness of 0.03 mm Rsm and a surface roughness curve element average length Rsm of 0.03 mm were prepared.

[0056] Comparative Example 5 The substrate 12 has a linear thermal expansion coefficient of 5.6×10 -6 Two isotropic carbon materials having a surface roughness of 0.06 mm Rsm were prepared.

[0057] Comparative Example 6 The substrate 12 has a linear thermal expansion coefficient of 6.0×10 -6 Two isotropic carbon materials having a surface roughness of 0.07 mm, a viscosity of 1000 s / ° C., and an average length Rsm of the surface roughness curve element of 0.07 mm were prepared.

[0058] The evaluation results of Examples 1 to 17 and Comparative Examples 1 to 6 are shown in Table 1. [Table 1]

[0059] <Evaluation result 1> Examples 1 to 17 and Comparative Examples 1 to 6 are compared. The number of intersections of cracks on the surface of the tantalum carbide coating film per unit area was 25 / cm 2 If the crack intersections on the surface of the tantalum carbide coating are less than 25 / cm2, the number of intersections per unit area is 25 / cm2. 2 In comparison with the case where the number of uses is larger than that of ... From this, it was found that the number of intersections of cracks on the surface of the tantalum carbide coating per unit area was 25 / cm 2 It can be seen that if the temperature is below this range, peeling of the tantalum carbide coating film is unlikely to occur.

[0060] <Evaluation result 2> Comparing Examples 1 to 14 with Examples 15 to 17 and Comparative Examples 1 to 6, when the average length Rsm of the surface roughness curve element of the tantalum carbide coating film is 10 μm or less, the number of uses until the tantalum carbide coating film of the tantalum carbide coating material peels off in a SiC single crystal growth environment is greater than when the average length Rsm of the surface roughness curve element of the tantalum carbide coating film is greater than 10 μm. This shows that when the average length Rsm of the roughness curve elements on the surface of the tantalum carbide coating is 10 μm or less, peeling of the tantalum carbide coating becomes even less likely to occur.

[0061] <Evaluation result 3> For Example 2, Examples 10 to 14, and Comparative Example 2, the linear thermal expansion coefficient was 4.2 × 10 -6 / °C is used as the substrate 12. When the average length Rsm of the roughness curve elements of the substrate surface is 0.1 mm or more and 5 mm or less (Example 2 and Examples 10 to 14), the number of intersections of cracks present on the surface of the tantalum carbide coating film per unit area is smaller and the number of uses until peeling of the tantalum carbide coating film occurs is greater than when the average length Rsm of the roughness curve elements of the substrate surface is 0.06 mm (Comparative Example 2). Therefore, it is clear that it is preferable for the average length Rsm of the roughness curve elements of the surface of the substrate to be 0.1 mm or more and 5 mm or less.

[0062] <Evaluation result 4> Comparisons are made between Example 1 and Comparative Example 1, Example 2 and Comparative Example 2, Example 3 and Comparative Example 3, Example 4 and Comparative Example 4, Example 5 and Comparative Example 5, Example 6 and Comparative Example 6, Example 7 and Example 15, Example 8 and Example 16, and Example 9 and Example 17. When using carbon materials with the same linear thermal expansion coefficient, when the average length Rsm of the roughness curve elements of the surface of the carbon material is 0.1 mm or more and 5 mm or less, the number of intersections of cracks present on the surface of the tantalum carbide coating film per unit area is smaller, the adhesion strength is large at 5 MPa or more, and the number of uses until peeling of the tantalum carbide coating film occurs is greater, compared to when the average length Rsm of the roughness curve elements of the surface of the carbon material is less than 0.1 mm. Therefore, it is preferable that the average length Rsm of the roughness curve element of the surface of the substrate is 0.1 mm or more and 5 mm or less. Therefore, it is preferable that the average length Rsm of the roughness curve element of the interface between the substrate and the tantalum carbide coating is 0.1 mm or more and 5.0 mm or less. [Explanation of symbols]

[0063] 1. Tantalum carbide coating material 11. Tantalum carbide coating 12...Base material 20. External heating type low pressure CVD equipment 21. Heater 22...Raw material supply department 23 Exhaust section 24...Reaction chamber 25...Support means 30. Crack intersection 31. Crack 32...Damage 44... Holding jig 45...Adhesive 46···pin

Claims

1. A tantalum carbide coating material comprising a substrate and a tantalum carbide coating film coating at least a portion of the substrate, The number of intersections of cracks on the surface of the tantalum carbide coating film per unit area is 25 / cm 2 Tantalum carbide coated material, which is:

2. 2. The tantalum carbide coating material according to claim 1, wherein the average length Rsm of the roughness profile elements on the surface of the tantalum carbide coating film is 10 μm or less.

3. 2. The tantalum carbide coating material according to claim 1, wherein the average length Rsm of the roughness profile elements at the interface between the substrate and the tantalum carbide coating film is 0.1 mm or more and 5.0 mm or less.

4. 2. The tantalum carbide coating material according to claim 1, wherein the substrate is a carbon substrate composed primarily of carbon.

5. 2. The tantalum carbide coated material according to claim 1, wherein the adhesive strength between the tantalum carbide coating film and the substrate is 5 MPa or more.

6. The linear thermal expansion coefficient of the substrate is 3.5×10 -6 / ℃ or more 7.5 x 10 -6 2. The tantalum carbide coating material according to claim 1, wherein the temperature is 0.15 to 1.5° C.

7. A compound semiconductor growth device using the tantalum carbide coating material according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Graphite member coated with silicon carbide

    JP1994305861A

  • Carbon composite material for reducing atmosphere furnace, and its production

    JP1998245285A

  • Carbon composite material

    JP2004084057A

  • Tantalum carbide-coated carbon material for heating, production method of tantalum carbide-coated carbon material for heating, silicon carbide epitaxial wafer growth equipment and gallium nitride epitaxial wafer fabrication and growth equipment

    JP2022120773A

  • Tantalum carbide coating carbon material and method of manufacturing the same, and member for semiconductor single-crystal manufacturing apparatus

    JP2019099453A