Polarizer, polarizing plate, and image display device
A PVA resin film with a gelled thixotropic material layer addresses dimensional changes in high-temperature environments, ensuring polarizer stability and optical performance in image display devices.
Patent Information
- Application Number
- JP2023055940
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Image display devices face significant dimensional changes in high-temperature environments due to the use of polyvinyl alcohol (PVA) resin-based polarizers, which are stretched films.
A polarizer composed of a polyvinyl alcohol resin film containing a dichroic substance, with a dimensional change suppression layer made of a gelled thixotropic material, typically a metal compound colloid such as alumina colloid, applied to one main surface to restrain dimensional changes.
The solution effectively suppresses dimensional changes in high-temperature environments, maintaining the polarizer's integrity and optical properties without additional processing steps like heating or ultraviolet irradiation, contributing to a thinner polarizing plate and image display device.
Smart Images

Figure 2024143324000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a polarizer, a polarizing plate, and an image display device. [Background technology]
[0002] In many image display devices (e.g., liquid crystal display devices, organic EL display devices, inorganic EL display devices), a polarizing plate is arranged on at least one side of the image display panel due to the image formation method. The polarizing plate typically includes a polarizer made of a polyvinyl alcohol (PVA)-based resin containing a dichroic material. Since the polarizer is a stretched film of a PVA-based resin film, there is a persistent problem of large dimensional change in a high-temperature environment. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2018-091980 A Summary of the Invention [Problem to be solved by the invention]
[0004] The present invention has been made to solve the above-mentioned problems in the conventional art, and a main object of the present invention is to provide a polarizer in which dimensional changes in a high-temperature environment are suppressed. [Means for solving the problem]
[0005] [1] A polarizer according to an embodiment of the present invention is made of a polyvinyl alcohol-based resin film containing a dichroic material and has a dimensional change suppressing layer on one of its main surfaces. The dimensional change suppressing layer is a gelling layer of a thixotropic material. [2] In the above [1], the thixotropic material is a colloidal solution. [3] In the above [2], the colloid is a metal compound colloid, a phyllosilicate colloid or an amide colloid. [4] In the above [2] or [3], the colloid is a metal compound colloid, and the metal compound colloid is at least one selected from the group consisting of an alumina colloid, a silica colloid, a zirconia colloid, a titania colloid, and a tin oxide colloid. [5] In the above [3] or [4], the metal compound colloid is an alumina colloid. [6] In any one of the above [1] to [5], the dimensional change inhibiting layer has a thickness of 30 nm to 1000 nm. [7] According to another aspect of the present invention, there is provided a polarizing plate comprising the polarizer according to any one of [1] to [6] above and a protective layer disposed on at least one main surface of the polarizer. [8] According to yet another aspect of the present invention, there is provided an image display device comprising the polarizer according to any one of [1] to [6] above or the polarizing plate according to [7] above. Effect of the Invention
[0006] According to the embodiment of the present invention, a polarizer in which dimensional change in a high-temperature environment is suppressed can be realized. [Brief description of the drawings]
[0007] [Figure 1] 1 is a schematic cross-sectional view of a polarizer according to one embodiment of the present invention. [Diagram 2] 1 is a schematic cross-sectional view of a polarizing plate according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to these embodiments.
[0009] A. Polarizer Representative embodiments of the present invention will be described below with reference to the drawings, but the present invention is not limited to these embodiments. In addition, in order to make the drawings easier to see and understand, the drawings are drawn typically or conceptually, and thickness, length, width, shape, size, ratio, etc. may differ from the actual ones, and there may be no correspondence between the drawings.
[0010] A-1. Overview of polarizers FIG. 1 is a schematic cross-sectional view of a polarizer according to one embodiment of the present invention. The polarizer 10 in the illustrated example has a polarizer body 11 having two main surfaces and a dimensional change suppressing layer 12 formed on one of the main surfaces of the polarizer body 11. The dimensional change suppressing layer 12 is a gelling layer of a thixotropic material. With such a configuration, dimensional changes in the polarizer in a high-temperature environment can be suppressed. Since the gelling layer of the thixotropic material is strong, it is presumed that it can appropriately restrain the polarizer body in a high-temperature environment, and as a result, dimensional changes in the polarizer in a high-temperature environment can be suppressed. However, such a mechanism is merely presumed, and the presumption is not intended to limit the interpretation of the embodiment of the present invention, and the embodiment of the present invention is not bound by such a mechanism.
[0011] A-2. Polarizer body The polarizer body (hereinafter sometimes simply referred to as polarizer) 11 is typically made of a polyvinyl alcohol (PVA)-based resin film containing a dichroic material (e.g., iodine). Examples of PVA-based resins include polyvinyl alcohol, partially formalized polyvinyl alcohol, ethylene-vinyl alcohol copolymer, and partially saponified ethylene-vinyl acetate copolymer.
[0012] The PVA-based resin preferably contains an acetoacetyl-modified PVA-based resin. With this configuration, a polarizer having desired mechanical strength can be obtained. The amount of the acetoacetyl-modified PVA-based resin is preferably 5% by weight to 20% by weight, and more preferably 8% by weight to 12% by weight, based on 100% by weight of the entire PVA-based resin. If the amount is within this range, a polarizer having better mechanical strength can be obtained.
[0013] The polarizer preferably contains iodide or sodium chloride (sometimes collectively referred to as halide). Examples of iodide include potassium iodide, sodium iodide, and lithium iodide. The content of the halide in the polarizer is preferably 5 to 20 parts by weight, more preferably 10 to 15 parts by weight, based on 100 parts by weight of the PVA-based resin. In the manufacturing method described below, the halide can be blended in a coating liquid that forms a PVA-based resin layer, which is a precursor of the polarizer, and finally introduced into the polarizer. By introducing a halide into the polarizer, the orientation of the PVA molecules in the polarizer can be increased, and therefore a polarizer having excellent optical properties (typically, both a high polarization degree and a high single transmittance) can be realized.
[0014] The polarizer preferably exhibits absorption dichroism at any wavelength of 380 nm to 780 nm. The single transmittance of the polarizer is preferably 41.0% to 46.0%, and more preferably 42.0% to 45.0%. The degree of polarization of the polarizer is preferably 97.0% or more, more preferably 99.0% or more, and even more preferably 99.9% or more. According to the embodiment of the present invention, even if the single transmittance is in the above range, the degree of polarization can be maintained in such a range.
[0015] The thickness of the polarizer is, for example, 15 μm or less, preferably 12 μm or less, more preferably 1 μm to 8 μm, and further preferably 3 μm to 7 μm. By combining such a thin polarizer with a liquid crystal alignment solidified layer, it is possible to significantly reduce the thickness of the optical laminate. Furthermore, if the thickness of the polarizer is within the above range, curling during heating can be well suppressed, and good appearance durability during heating can be obtained.
[0016] The polarizer can be produced by any appropriate method. For example, the resin film forming the polarizer may be a single-layer resin film or a laminate of two or more layers.
[0017] Specific examples of polarizers made of a single-layer resin film include hydrophilic polymer films such as PVA films, partially formalized PVA films, and partially saponified ethylene-vinyl acetate copolymer films that have been dyed with iodine or a dichroic substance such as a dichroic dye and stretched, and polyene-based oriented films such as dehydrated PVA films and dehydrochlorinated polyvinyl chloride films. A polarizer obtained by dyeing a PVA film with iodine and uniaxially stretching it is preferably used because of its excellent optical properties.
[0018] The dyeing with iodine is carried out, for example, by immersing the PVA-based film in an aqueous iodine solution. The stretching ratio of the uniaxial stretching is preferably 3 to 7 times. The stretching may be carried out after the dyeing treatment, or may be carried out while dyeing. Alternatively, the film may be stretched and then dyed. If necessary, the PVA-based film may be subjected to a swelling treatment, a crosslinking treatment, a washing treatment, a drying treatment, or the like. For example, by immersing the PVA-based film in water and washing it with water before dyeing, it is possible to wash off dirt and antiblocking agents on the surface of the PVA-based film, and also to swell the PVA-based film and prevent uneven dyeing.
[0019] Specific examples of polarizers obtained using a laminate include a laminate of a resin substrate and a PVA-based resin layer (PVA-based resin film) laminated on the resin substrate, or a polarizer obtained using a laminate of a resin substrate and a PVA-based resin layer formed by coating on the resin substrate. A polarizer obtained using a laminate of a resin substrate and a PVA-based resin layer formed by coating on the resin substrate can be produced by, for example, applying a PVA-based resin solution to the resin substrate and drying the resin substrate to form a PVA-based resin layer on the resin substrate to obtain a laminate of the resin substrate and the PVA-based resin layer; stretching and dyeing the laminate to make the PVA-based resin layer into a polarizer. In this embodiment, a polyvinyl alcohol-based resin layer containing a halide and a polyvinyl alcohol-based resin is preferably formed on one side of the resin substrate. The stretching typically includes immersing the laminate in an aqueous boric acid solution to stretch it. Furthermore, the stretching may further include, as necessary, stretching the laminate in air at a high temperature (for example, 95° C. or higher) before stretching in the aqueous boric acid solution. In addition, in this embodiment, the laminate is preferably subjected to a drying shrinkage treatment in which the laminate is heated while being transported in the longitudinal direction to shrink the laminate by 2% or more in the width direction. Typically, the manufacturing method of this embodiment includes subjecting the laminate to an air-assisted stretching treatment, a dyeing treatment, an underwater stretching treatment, and a drying shrinkage treatment in this order. By introducing the auxiliary stretching, even when PVA is applied onto a thermoplastic resin, it is possible to increase the crystallinity of the PVA, and to achieve high optical properties. In addition, by simultaneously increasing the orientation of the PVA in advance, problems such as a decrease in the orientation of the PVA or dissolution when immersed in water in the subsequent dyeing and stretching steps can be prevented, and high optical properties can be achieved. Furthermore, when the PVA-based resin layer is immersed in a liquid, the orientation of the polyvinyl alcohol molecules can be disturbed and the orientation can be reduced, compared to when the PVA-based resin layer does not contain a halide. This can improve the optical properties of a polarizer obtained by immersing the laminate in a liquid through a treatment process such as a dyeing treatment and an underwater stretching treatment. Furthermore, the optical properties can be improved by shrinking the laminate in the width direction through a drying shrinkage treatment.The obtained resin substrate / polarizer laminate may be used as it is (i.e., the resin substrate may be used as a protective layer for the polarizer), or any suitable protective layer may be laminated on the peeled surface of the resin substrate / polarizer laminate after peeling the resin substrate from the resin substrate / polarizer laminate, or on the surface opposite to the peeled surface, depending on the purpose. Details of the method for producing such a polarizer are described in, for example, JP2012-73580A and JP6470455A. The entire disclosures of these publications are incorporated herein by reference.
[0020] A-3. Dimensional change suppression layer As described above, the dimensional change inhibiting layer 12 is a gelling layer of a thixotropic material. Thixotropy refers to a phenomenon in which when a fluid is subjected to shear (e.g., stirring, pumping, coating), the viscosity decreases over time, and when the shear is stopped and the fluid is left stationary, the viscosity returns to the original value. Therefore, a thixotropic material is a material whose viscosity decreases under shear stress to become a highly fluid sol (liquid state), and when left stationary, becomes a gel (solid state). As is clear from the nature of a thixotropic material, when a sol under shear (e.g., by stirring) is applied to a polarizer body, the applied film spontaneously gels to become a gelling layer. Therefore, by using a thixotropic material, no additional steps or operations such as heating, ultraviolet irradiation (crosslinking or curing), lamination, or transfer are required when forming the dimensional change inhibiting layer. Therefore, the dimensional change inhibiting layer can be formed very simply and efficiently. Furthermore, the dimensional change inhibiting layer can be formed without adversely affecting the polarizer body (e.g., by heat or ultraviolet light). In addition, since no adhesive layer is required for lamination or transfer, this can contribute to making polarizers (ultimately polarizing plates and image display devices) thinner.
[0021] A thixotropic material is typically a colloidal solution, which typically is a sol under shear and gels on standing. A colloidal solution typically contains a liquid medium (dispersion medium) and colloidal particles dispersed in the liquid medium.
[0022] Representative examples of the dispersion medium include water or an organic solvent. Specific examples of the organic solvent include alcohols such as methanol, ethanol, propanol, butanol, ethylene glycol, propylene glycol, butanediol, pentanediol, 2-methyl-2,4-pentanediol, diethylene glycol, dipropylene glycol, and ethylene glycol monopropyl ether; ketones such as methyl ethyl ketone and methyl isobutyl ketone; aromatic hydrocarbons such as toluene and xylene; amides such as dimethylformamide, dimethylacetamide, and N-methylpyrrolidone; esters such as ethyl acetate, butyl acetate, and γ-butyrolactone; and ethers such as tetrahydrofuran and 1,4-dioxane.
[0023] Examples of colloids (colloid particles) include metal compound colloids, phyllosilicate colloids, and amide (acid amide) colloids. The colloids (colloid particles) are preferably metal compound colloids. Examples of metal compound colloids include alumina colloids, silica colloids, zirconia colloids, titania colloids, and tin oxide colloids. These may be used alone or in combination. The metal compound colloids are preferably alumina colloids.
[0024] The concentration of colloid particles in the colloid solution is preferably 0.1% to 30.0% by weight, more preferably 0.15% to 20.0% by weight, and even more preferably 0.15% to 15.0% by weight. If the concentration of colloid particles is within this range, a gelling layer (dimensional change suppression layer) having appropriate mechanical strength can be formed.
[0025] The colloidal particles may have any suitable shape, including, for example, a spherical shape, an oval spherical shape, a needle shape, a rod shape, a fibrous shape, and an amorphous shape.
[0026] The size of the colloidal particles can be appropriately set depending on the purpose, shape, etc. For example, when the colloidal particles are spherical, the average primary particle diameter is preferably 1 nm to 200 nm, more preferably 20 nm to 180 nm, and further preferably 50 nm to 120 nm. For example, when the colloidal particles are elongated (e.g., needle-like, rod-like, fibrous), the average aspect ratio (major axis / minor axis) is preferably 30 to 5000, more preferably 100 to 3000; the average minor axis is preferably 1 nm to 10 nm, more preferably 2 nm to 5 nm; and the average major axis is preferably 100 nm to 10000 nm, more preferably 500 nm to 7000 nm. If the size of the colloidal particles is too large, the transparency and fluidity may be insufficient. If the size of the colloidal particles is too small, the storage stability may be insufficient.
[0027] The pH of the colloidal solution may be, for example, 2.5 to 4.0, or, for example, 3.0 to 3.6. If necessary, a pH adjuster may be used. The colloidal solution can be made neutral by using a pH adjuster. As a result, chemical adverse effects on the polarizer body can be suppressed. Examples of pH adjusters include sodium hydroxide, potassium hydroxide, sodium carbonate, sodium bicarbonate, ammonia, ethylamine, tetramethylammonium hydroxide, and urea.
[0028] The viscosity of the colloidal solution (25° C.) is preferably 300 mPa·s or less, and more preferably 1 mPa·s to 200 mPa·s. If the viscosity of the colloidal solution is within this range, a gelled layer (dimensional change-suppressing layer) having a desired thickness can be formed.
[0029] The colloidal solution may contain additives. Examples of additives include dispersion stabilizers, coupling agents, and antistatic agents. The type, number, combination, and amount of additives may be appropriately set depending on the purpose.
[0030] The colloidal solution typically does not contain a binder resin. In other words, the colloidal solution typically does not have an adhesive function. The colloidal solution, which is a thixotropic material, has a spontaneous film-forming function (gelling function), so there is no need to use a binder resin. As a result, there is no need to apply heat and / or active energy rays (e.g., ultraviolet rays) to harden the binder resin, so that adverse effects on the polarizer body can be avoided when forming the dimensional change suppression layer.
[0031] The metal compound colloid is preferably an alumina colloid as described above. Therefore, the thixotropic material is preferably an alumina sol. Alumina includes aluminum hydroxides (alumina hydrates) such as gibbsite, bayerite, boehmite, pseudoboehmite, diaspore, and amorphous, as well as alumina crystals of γ, η, δ, ρ, κ, θ, χ, and α types. The alumina is preferably boehmite or pseudoboehmite.
[0032] Commercially available colloidal solutions may be used. Specific examples of commercially available products include "Aluminasol-F1000" (alumina colloid) manufactured by Kawaken Fine Chemicals Co., Ltd., "BYK-AQUAGEL 7100" (phyllosilicate colloid) manufactured by BYK, and "Disparlon" (amide colloid) manufactured by Kusumoto Chemicals Co., Ltd.
[0033] The thickness of the dimensional change inhibiting layer is preferably 30 nm to 1000 nm, more preferably 50 nm to 700 nm, even more preferably 70 nm to 500 nm, particularly preferably 80 nm to 400 nm, and particularly preferably 100 nm to 300 nm. When the thickness of the dimensional change inhibiting layer is within this range, it is possible to simultaneously achieve a thin polarizer (and thus a polarizing plate) and inhibit dimensional change of the polarizer.
[0034] B. Polarizing plate FIG. 2 is a schematic cross-sectional view of a polarizing plate according to one embodiment of the present invention. The polarizing plate 100 has a polarizer 10, a first protective layer 20 arranged on one main surface of the polarizer 10, and a second protective layer 30 arranged on the other main surface of the polarizer 10. The polarizer 10 is the polarizer according to the embodiment of the present invention described in the above section A. One of the first protective layer 20 and the second protective layer 30 may be omitted. In this case, the protective layer on the dimensional change suppressing layer side may be omitted, or the protective layer on the opposite side to the dimensional change suppressing layer may be omitted. One of the first protective layer and the second protective layer may be a resin substrate used in the manufacture of the above polarizer.
[0035] The first protective layer and the second protective layer are made of any suitable resin film. Representative materials for the resin film include cellulose resins such as triacetyl cellulose (TAC), cycloolefin resins such as polynorbornene, (meth)acrylic resins, polyester resins such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), polyolefin resins such as polyethylene, and polycarbonate resins. Representative examples of (meth)acrylic resins include (meth)acrylic resins having a lactone ring structure. (Meth)acrylic resins having a lactone ring structure are described in, for example, JP-A-2000-230016, JP-A-2001-151814, JP-A-2002-120326, JP-A-2002-254544, and JP-A-2005-146084. These publications are incorporated herein by reference. From the viewpoint of ease of processing into irregular shapes, etc., cellulose-based resins are preferred, and TAC is more preferred. From the viewpoint of obtaining a polarizing plate having low moisture permeability and excellent durability, cycloolefin-based resins and (meth)acrylic resins are preferred.
[0036] The thickness of each of the first protective layer and the second protective layer is preferably from 10 μm to 80 μm, more preferably from 12 μm to 40 μm, and further preferably from 15 μm to 35 μm.
[0037] In one embodiment, the protective layer (inner protective layer) disposed on the image display panel side when the polarizing plate 100 is applied to an image display device has optical isotropy. In this specification, "optically isotropic" means that the in-plane retardation Re(550) is 10 nm or less, preferably 7 nm or less, more preferably 5 nm or less; and the thickness direction retardation Rth(550) is -10 nm to 10 nm, preferably -7 nm to 7 nm, more preferably -5 nm to 5 nm. In another embodiment, the inner protective layer is a retardation layer having any appropriate retardation value. In this case, the in-plane retardation Re(550) of the retardation layer is, for example, 120 nm to 160 nm. "Re(550)" is the in-plane retardation measured with light having a wavelength of 550 nm at 23°C, and is calculated by the formula: Re=(nx-ny)×d. "Rth(550)" is the thickness direction retardation measured with light of 550 nm wavelength at 23°C, and is calculated by the formula: Re = (nx - nz) x d. Here, "nx" is the refractive index in the direction in which the in-plane refractive index is maximum (i.e., the slow axis direction), "ny" is the refractive index in the direction perpendicular to the slow axis in the plane (i.e., the fast axis direction), "nz" is the refractive index in the thickness direction, and "d" is the thickness (nm) of the layer (film).
[0038] C. Image display device The polarizer described in the above item A or the polarizing plate described in the above item B can be applied to an image display device. Therefore, an image display device including such a polarizer or polarizing plate can also be included in the embodiment of the present invention. Representative examples of the image display device include a liquid crystal display device, an organic electroluminescence (EL) display device, and an inorganic EL display device. EXAMPLES
[0039] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The methods for measuring the various properties in the examples are as follows. In the examples and comparative examples, "parts" and "%" are by weight unless otherwise specified.
[0040] (1) Thickness The polarizer obtained in the examples was cut, and the cross section of the polarizing plate was observed using a scanning electron microscope (manufactured by JEOL Ltd., "JSM7100F") to measure the thickness of the dimensional change suppression layer. The thickness of the polarizer body was measured using an interference film thickness meter (manufactured by Otsuka Electronics Co., Ltd., product name "MCPD-3000").
[0041] (2) Polarizer shrinkage rate The polarizers obtained in the examples and comparative examples were subjected to a heating TMA test. Specifically, the polarizer was cut to 20 mm (absorption axis direction) x 4 mm (transmission axis direction) to prepare a measurement sample. Using a thermomechanical analyzer (Hitachi High-Tech Science Corporation, model number "TMA7100"), the measurement sample was heated from 30°C to 120°C and cooled back to 30°C for three cycles, and then the dimensional change rate (shrinkage rate) in the length direction (absorption axis direction) of the measurement sample was measured. The heating rate was 5°C / min, and the holding time at each temperature was 10 minutes. The dimensional change rate (shrinkage rate) of the measurement sample in the width direction (transmission axis direction) was measured in the same manner as above, except that the heating temperature was changed from 120°C to 80°C.
[0042] [Example 1] As a thermoplastic resin substrate, a long amorphous isophthalic copolymerized polyethylene terephthalate film (thickness: 100 μm) having a Tg of about 75° C. was used, and one side of the resin substrate was subjected to a corona treatment. A PVA aqueous solution (coating solution) was prepared by adding 13 parts by weight of potassium iodide to 100 parts by weight of a PVA-based resin made by mixing polyvinyl alcohol (polymerization degree 4200, saponification degree 99.2 mol%) and acetoacetyl-modified PVA (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., product name "GOHSEFFIMER") in a ratio of 9:1, and dissolving the mixture in water. The above PVA aqueous solution was applied to the corona-treated surface of a resin substrate and dried at 60° C. to form a PVA-based resin layer with a thickness of 13 μm, thereby producing a laminate. The obtained laminate was uniaxially stretched 2.4 times in the machine direction (longitudinal direction) in an oven at 130° C. (auxiliary air stretching treatment). Next, the laminate was immersed in an insolubilizing bath (a boric acid aqueous solution obtained by mixing 4 parts by weight of boric acid with 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (insolubilizing treatment). Next, the film was immersed in a dye bath (an aqueous iodine solution obtained by mixing iodine and potassium iodide in a weight ratio of 1:7 with 100 parts by weight of water) at a liquid temperature of 30°C for 60 seconds while adjusting the concentration so that the single transmittance (Ts) of the finally obtained polarizer would be the desired value (dyeing treatment). Next, the piece was immersed in a crosslinking bath (a boric acid aqueous solution obtained by mixing 3 parts by weight of potassium iodide and 5 parts by weight of boric acid with respect to 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (crosslinking treatment). Thereafter, the laminate was immersed in an aqueous boric acid solution (boric acid concentration: 4% by weight, potassium iodide concentration: 5% by weight) at a liquid temperature of 70°C and uniaxially stretched in the longitudinal direction (longitudinal direction) between rolls with different peripheral speeds to a total stretch ratio of 5.5 times (underwater stretching treatment). Thereafter, the laminate was immersed in a cleaning bath (an aqueous solution obtained by mixing 4 parts by weight of potassium iodide with 100 parts by weight of water) at a liquid temperature of 20° C. (cleaning treatment). Thereafter, the film was dried in an oven maintained at about 90° C. while being brought into contact with a SUS heated roll whose surface temperature was maintained at about 75° C. (drying shrinkage treatment). In this manner, a polarizer having a thickness of about 5 μm was formed on the resin substrate, and a laminate of the resin substrate and the polarizer was obtained. The single transmittance Ts of the polarizer was 43.3%.
[0043] An alumina colloid solution (manufactured by Kawaken Fine Chemicals Co., Ltd., product name "Aluminasol-F1000") was applied to the polarizer surface of the obtained laminate using a bar coater. The applied film gelled spontaneously, forming a dimensional change inhibiting layer as a gelling layer. The thickness of the dimensional change inhibiting layer was 146 nm. The shrinkage rate of the polarizer on which the dimensional change inhibiting layer was formed was measured as described above in (2). The results are shown in Table 1.
[0044] [Comparative Example 1] The laminate of resin substrate / polarizer obtained in Example 1 was subjected to the measurement of the shrinkage percentage in the above item (2) as it was (i.e., without forming a dimensional change-suppressing layer). The results are shown in Table 1.
[0045] [Example 2] A long roll of polyvinyl alcohol (PVA) resin film (manufactured by Kuraray, product name "PE3000") with a thickness of 30 μm was uniaxially stretched in the longitudinal direction to 5.9 times its original size using a roll stretching machine while simultaneously undergoing swelling, dyeing, crosslinking, and washing processes, and finally a drying process to produce a polarizer with a thickness of 12 μm. Specifically, the film was stretched 2.2 times during the swelling treatment in pure water at 20°C. Next, the film was stretched 1.4 times during the dyeing treatment in an aqueous solution at 30°C in which the weight ratio of iodine to potassium iodide was 1:7, and the iodine concentration was adjusted so that the single transmittance of the resulting polarizer was 45.0%. Furthermore, a two-stage crosslinking treatment was adopted, and the film was stretched 1.2 times during the first stage crosslinking treatment in an aqueous solution at 40°C in which boric acid and potassium iodide were dissolved. The aqueous solution in the first stage crosslinking treatment had a boric acid content of 5.0% by weight and a potassium iodide content of 3.0% by weight. The film was stretched 1.6 times during the second stage crosslinking treatment in an aqueous solution at 65°C in which boric acid and potassium iodide were dissolved. The aqueous solution in the second stage crosslinking treatment had a boric acid content of 4.3% by weight and a potassium iodide content of 5.0% by weight. The cleaning treatment was performed with an aqueous potassium iodide solution at 20° C. The aqueous solution used for the cleaning treatment had a potassium iodide content of 2.6% by weight. Finally, the film was dried at 70° C. for 5 minutes to obtain a polarizer.
[0046] An alumina colloid solution (manufactured by Kawaken Fine Chemicals Co., Ltd., product name "Aluminasol-F1000") was applied to the surface of the obtained polarizer using a bar coater. The applied film gelled spontaneously, forming a dimensional change inhibiting layer as a gelling layer. The thickness of the dimensional change inhibiting layer was 62.5 nm. The shrinkage rate of the polarizer on which the dimensional change inhibiting layer was formed was measured as described above in (2). The results are shown in Table 1.
[0047] [Comparative Example 2] The polarizer obtained in Example 2 was directly subjected to the measurement of the shrinkage rate in the above item (2) (i.e., without forming a dimensional change-suppressing layer). The results are shown in Table 1.
[0048] [Table 1]
[0049] As is clear from Table 1, the polarizers of the examples of the present invention are suppressed in dimensional change (thermal shrinkage) in a high-temperature environment. In particular, the dimensional change in the transmission axis direction is suppressed well. It is also clear that the effect of suppressing dimensional change is more remarkable when the thickness of the dimensional change suppressing layer is large. [Industrial Applicability]
[0050] The polarizer and polarizing plate according to the embodiment of the present invention are suitable for use in image display devices. [Explanation of symbols]
[0051] 10 Polarizer 11 Polarizer body 12 Dimensional change suppression layer 20 First protective layer 30 Second layer of protection 100 Polarizing Plate
Claims
1. A polarizer comprising a polyvinyl alcohol-based resin film containing a dichroic material and having a dimensional change suppression layer on one of its main surfaces, The dimensional change inhibiting layer is a gelling layer of a thixotropic material. Polarizer.
2. The polarizer of claim 1 , wherein the thixotropic material is a colloidal solution.
3. The polarizer of claim 2 , wherein the colloid is a metal compound colloid, a phyllosilicate colloid, or an amide colloid.
4. 4. The polarizer according to claim 3, wherein the colloid is a metal compound colloid, and the metal compound colloid is at least one selected from the group consisting of an alumina colloid, a silica colloid, a zirconia colloid, a titania colloid, and a tin oxide colloid.
5. 5. The polarizer according to claim 4, wherein the metal compound colloid is an alumina colloid.
6. 2. The polarizer according to claim 1, wherein the dimensional change inhibiting layer has a thickness of 30 nm to 1000 nm.
7. A polarizing plate comprising the polarizer according to claim 1 and a protective layer disposed on at least one main surface of the polarizer.
8. An image display device comprising the polarizing plate according to claim 7 .
Citation Information
Patent Citations
Polarizing film and manufacturing method of polarized laminate film
JP2018091980A