Resin composition, coating, and plastic molded product

A resin composition with polycarbonate and acrylic polyols, enhanced by an aromatic solvent, addresses storage stability and appearance issues in high-crystallinity polycarbonate diols, achieving stable and flexible coating films.

JP2024143417APending Publication Date: 2024-10-11MITSUBISHI CHEM CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023056083
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing resin compositions based on polycarbonate diols with high crystallinity, while improving chemical resistance and stain resistance, suffer from poor storage stability, crystallization issues, and undesirable film appearance such as gloss or haze.

Method used

A resin composition comprising polycarbonate polyol, acrylic polyol, and an aromatic hydrocarbon solvent, with specific ratios and components like 1,10-decanediol and 1,4-butanediol, enhances storage stability and film appearance by improving chemical resistance and flexibility.

Benefits of technology

The composition forms a coating film with excellent appearance and good storage stability, maintaining chemical resistance and flexibility, suitable for long-term use in various applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143417000001
    Figure 2024143417000001
  • Figure 2024143417000002
    Figure 2024143417000002
  • Figure 2024143417000003
    Figure 2024143417000003
Patent Text Reader

Abstract

To provide a resin composition which is capable of forming a coating film with a superior appearance and demonstrates superior storage stability, to provide a coating, and to provide a plastic molded product.SOLUTION: A resin composition comprises a polycarbonate polyol (A) made from a polyhydric alcohol, an acrylic polyol (B), and a solvent, where the polyhydric alcohol comprises an alcohol (1a) represented by the formula (1a), and the solvent comprises an aromatic hydrocarbon solvent (C). HO-R1-OH (1a). (In the formula (1a), R1 is a substituted or unsubstituted C8-20 alkylene group).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition, a coating material, and a plastic molded article. [Background technology]

[0002] (Meth)acrylic resins are widely used in paints, taking advantage of their excellent chemical resistance and coating appearance. However, when applying to plastic substrates, it is difficult to ensure adhesion and flexibility using (meth)acrylic resin alone.

[0003] In order to solve this problem, it has been proposed to use a mixture of different resins that have high adhesion to plastic substrates and high flexibility, and among these, polycarbonate diols are often used. For example, Patent Document 1 discloses that a polycarbonate-modified acrylic resin made from a specific polycarbonate diol and an acrylic resin derived from a limited monomer provides good adhesion, water-resistant adhesion, and resistance to fragrances. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2020 / 044487 Summary of the Invention [Problem to be solved by the invention]

[0005] However, the coating film formed from the resin composition described in Patent Document 1 was insufficient in chemical resistance and stain resistance. As in Patent Document 1, polycarbonate diols with low crystallinity have often been used, but it is necessary to use polycarbonate diols with high crystallinity in order to maximize performance such as chemical resistance, stain resistance, flexibility, etc. On the other hand, polycarbonate diols with high crystallinity have extremely poor storage stability, such as crystallization in solution, whether used alone or mixed with acrylic polyol, and further have problems such as poor appearance, such as gloss and haze, when a coating film is formed.

[0006] An object of the present invention is to provide a resin composition, a paint, and a plastic molded article which are capable of forming a coating film with excellent appearance and have good storage stability. [Means for solving the problem]

[0007] That is, the present invention relates to the following items [1] to

[10] . [1] A resin composition comprising a polycarbonate polyol (A) made from a polyhydric alcohol, an acrylic polyol (B), and a solvent, The polyhydric alcohol includes an alcohol (1a) represented by the following formula (1a): The resin composition, wherein the solvent comprises an aromatic hydrocarbon solvent (C). H.O.R. 1 -OH (1a) (In formula (1a), R 1 represents a substituted or unsubstituted alkylene group having 8 to 20 carbon atoms. [2] The resin composition according to [1], wherein the polyhydric alcohol comprises one or more diols derived from biomass. [3] The resin composition according to [1] or [2], wherein the alcohol (1a) contains 1,10-decanediol. [4] The resin composition according to any one of [1] to [3] above, wherein the polyhydric alcohol comprises 1,10-decanediol and 1,4-butanediol. [5] The resin composition according to any one of the above [1] to [4], wherein a mass ratio (A) / (B) of the polycarbonate polyol (A) to the acrylic polyol (B) is 5 / 95 to 90 / 10. [6] The resin composition according to any one of the above [1] to [5], wherein the acrylic polyol (B) has a glass transition temperature of -50 to 150°C. [7] The resin composition according to any one of the above [1] to [6], wherein the content of the aromatic hydrocarbon solvent (C) is 35 to 100 mass % based on the total mass of the solvents. [8] The resin composition according to any one of [1] to [7] above, wherein the aromatic hydrocarbon solvent (C) comprises at least one of toluene and xylene. [9] A paint containing the resin composition according to any one of [1] to [8] above.

[10] A plastic molded product painted with the paint described in [9] above. Effect of the Invention

[0008] According to the present invention, it is possible to provide a resin composition, a paint, and a plastic molded article which are capable of forming a coating film with excellent appearance and have good storage stability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The present invention will be described in further detail below by presenting preferred embodiments of the invention. However, the following description is one example of an embodiment of the present invention, and the present invention is not limited to the contents described below as long as it does not go beyond the gist of the invention. In this specification, the use of "to" indicating a range of values ​​means that the values ​​before and after it are included as the lower limit and upper limit. In addition, in this specification, "(meth)acrylic" is a general term for acrylic or methacrylic. In the following specification, the term "coating film" refers to a cured coating film formed from the coating material of the present invention.

[0010] [Resin composition] Hereinafter, one embodiment of the resin composition of the present invention will be described. The resin composition of the present embodiment contains the following polycarbonate polyol (A), acrylic polyol (B), and a solvent. The resin composition may further contain components other than the polycarbonate polyol (A), the acrylic polyol (B), and the solvent (hereinafter also referred to as "optional components"), as necessary, within a range that does not impair the effects of the present invention.

[0011] <Polycarbonate polyol (A)> The polycarbonate polyol (A) is a compound produced from a polyhydric alcohol, which contains an alcohol (1a) represented by the following formula (1a). By using the alcohol (1a) as a raw material, the chemical resistance and low-temperature flexibility of the coating film are improved. H.O.R. 1 -OH (1a) (In formula (1a), R 1 represents a substituted or unsubstituted alkylene group having 8 to 20 carbon atoms.

[0012] The polycarbonate polyol (A) can be produced by polycondensing a polyhydric alcohol containing at least the alcohol (1a) with a carbonate compound through an ester exchange reaction.

[0013] From the viewpoint of improving the chemical resistance of the coating film, the polycarbonate polyol (A) is more preferably a polycarbonate diol containing a structural unit derived from a polyhydric alcohol containing an alcohol (2a) represented by the following formula (2a) and at least one of the alcohols (1a), and a structural unit derived from a dicarbonate compound, the polycarbonate diol having a hydroxyl value of 38.0 to 145 mgKOH / g and a molar ratio of the structural unit derived from the alcohol (2a) to the structural unit derived from the alcohol (1a) of (2a) / (1a)=90 / 10 to 0 / 100. H.O.R. 2 -OH (2a) (In formula (2a), R 2 represents a substituted or unsubstituted alkylene group having 4 carbon atoms.

[0014] An example of the structural unit derived from the alcohol (1a) is a structural unit represented by the following formula (11a).

[0015] [ka]

[0016] In formula (11a), R 11 represents a substituted or unsubstituted alkylene group having 8 to 20 carbon atoms. In formula (11a), R 11 may be one type or multiple types. In formula (11a), R 11 represents a substituted or unsubstituted alkylene group having 8 to 20 carbon atoms, and from the viewpoint of improving the chemical resistance and low-temperature flexibility of the coating film, if a substituent is present, it is preferable that the substituent has fewer carbon atoms, more preferably the substituent has 2 or less carbon atoms, even more preferably 1 or less carbon atoms, and particularly preferably is unsubstituted.

[0017] An example of the structural unit derived from the alcohol (2a) is a structural unit represented by the following formula (21a).

[0018] [ka]

[0019] In formula (21a), R 21 represents a substituted or unsubstituted alkylene group having 4 carbon atoms. In formula (21a), R 21 may be one type or multiple types. In formula (21a), R 21 is a substituted or unsubstituted alkylene group having 4 carbon atoms, but is preferably unsubstituted from the viewpoint of improving the chemical resistance and low-temperature flexibility of the coating film.

[0020] When the polycarbonate polyol (A) has a structural unit derived from the alcohol (2a) and a structural unit derived from the alcohol (1a), when it is made into a polyurethane, the solution stability, chemical resistance, and low-temperature flexibility of the resin composition and the coating material described later become good.

[0021] The molar ratio (2a) / (1a) of the structural units derived from the alcohol (2a) to the structural units derived from the alcohol (1a) is preferably from 90 / 10 to 0 / 100, more preferably from 89 / 11 to 10 / 90, further preferably from 85 / 15 to 20 / 80, particularly preferably from 80 / 20 to 25 / 75, and most preferably from 75 / 25 to 27 / 73. When the molar ratio of (2a) / (1a) is within the above range, the resin composition has good solution stability when made into a polyurethane, and the resin composition and the cured coating film of the coating have good low-temperature flexibility and chemical resistance.

[0022] (Polyhydric alcohol) The polyhydric alcohol is a raw material for the polycarbonate polyol (A). The polyhydric alcohol includes the alcohol (1a). Examples of the alcohol (1a), which is a dihydroxy compound serving as a raw material for the polycarbonate polyol (A), include 1,8-octanediol, 2-methyl-1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,16-hexadecanediol, 1,18-octadecanediol, 1,12-octadecanediol, and 1,20-eicosanediol. Among these, from the viewpoint of achieving an excellent balance of solution stability, chemical resistance, and low-temperature flexibility when formed into a polyurethane, 1,8-octanediol, 2-methyl-1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, and 1,12-dodecanediol are preferred, 2-methyl-1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, and 1,12-dodecanediol are more preferred, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, and 1,12-dodecanediol are even more preferred, 1,10-decanediol, 1,11-undecanediol, and 1,12-dodecanediol are particularly preferred, and 1,10-decanediol is most preferred. That is, the alcohol (1a) preferably contains 1,10-decanediol. The alcohol (1a) may be used alone or in combination of two or more kinds.

[0023] From the viewpoint of reducing the environmental load, the alcohol (1a) is preferably derived from a renewable organic resource biosynthesized from one or more of animals, plants, microorganisms, and bacteria. That is, from the viewpoint of reducing the environmental load, the polyhydric alcohol preferably contains one or more diols derived from biomass. Examples of the alcohol (1a) derived from a renewable organic resource and biosynthesized from one or more of animals, plants, microorganisms, and bacteria include 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,12-octadecanediol, and 1,20-eicosanediol.

[0024] For example, when 1,10-decanediol is used as a dihydroxy compound derived from a renewable organic resource that is biosynthesized from one or more of animals, plants, microorganisms, and bacteria, 1,10-decanediol can be biosynthesized by synthesizing sebacic acid from castor oil by alkali fusion, and then hydrogenating the sebacic acid directly or after an esterification reaction.

[0025] The polyhydric alcohol preferably further contains the alcohol (2a) in addition to the alcohol (1a). Examples of the alcohol (2a) which is a dihydroxy compound used as a raw material for the polycarbonate polyol (A) include 2-methyl-1,3-propanediol and 1,4-butanediol. Among these, 1,4-butanediol is preferred from the viewpoint of the balance between chemical resistance and low-temperature flexibility when made into polyurethane. In other words, the alcohol (2a) preferably contains 1,4-butanediol. The alcohol (2a) may be used alone or in combination of two or more kinds.

[0026] From the viewpoint of reducing the environmental load, the alcohol (2a) is preferably derived from a renewable organic resource, that is, biosynthesized from one or more of animals, plants, microorganisms, and bacteria. An example of the alcohol (2a) derived from a renewable organic resource and biosynthesized from one or more of animals, plants, microorganisms, and bacteria is 1,4-butanediol.

[0027] When using, for example, 1,4-butanediol as a dihydroxy compound derived from a renewable organic resource biosynthesized from one or more of animals, plants, microorganisms, and bacteria, 1,4-butanediol may be produced by chemical synthesis from succinic acid, succinic anhydride, succinic acid esters, maleic acid, maleic anhydride, maleic acid esters, tetrahydrofuran, γ-butyrolactone, etc. obtained by a fermentation method, 1,4-butanediol may be produced directly by a fermentation method, or 1,4-butanediol may be produced from 1,3-butadiene obtained by a fermentation method. Among these, the method of directly producing 1,4-butanediol by a fermentation method and the method of obtaining 1,4-butanediol by hydrogenating succinic acid with a reduction catalyst are efficient and preferable.

[0028] From the viewpoint of achieving an excellent balance of solution stability, chemical resistance, and low-temperature flexibility when formed into a polyurethane, it is preferable that the polyhydric alcohol contains 1,10-decanediol. Furthermore, from the viewpoint of providing a polyurethane with an excellent balance of solution stability, chemical resistance, and low-temperature flexibility, and reducing the environmental load, the polyhydric alcohol in the resin composition of the present invention preferably contains 1,10-decanediol and 1,4-butanediol. That is, the polycarbonate polyol (A) preferably has a structural unit derived from 1,10-decanediol and a structural unit derived from 1,4-butanediol.

[0029] When the alcohol (1a) and the alcohol (2a) are used in combination, the molar ratio thereof, (2a) / (1a), is preferably from 90 / 10 to 0 / 100, more preferably from 89 / 11 to 10 / 90, further preferably from 85 / 15 to 20 / 80, particularly preferably from 80 / 20 to 25 / 75, and most preferably from 75 / 25 to 27 / 73.

[0030] The polyhydric alcohol may contain a dihydric alcohol (3a), which is a dihydroxy compound other than the alcohol (1a) and the alcohol (2a), or a trihydric or higher alcohol (4a), as long as the effects of the present invention are not impaired. The alcohol (3a) may be an alcohol represented by the following formula (3a): H.O.R. 3 -OH (3a) (In formula (3a), R 3 represents a substituted or unsubstituted alkylene group having 1 to 3 or 5 to 7 carbon atoms.

[0031] Examples of the alcohol (3a) include methanediol, 1,2-ethanediol, 1,2-propanediol, 1,3-propanediol, 1,2-pentanediol, 1,5-pentanediol, 1,2-hexanediol, 1,6-hexanediol, 1,2-heptanediol, and 1,7-heptanediol. Examples of the alcohol (4a) include trimethylolpropane, sorbitol, 1,4-sorbitan, erythritol, pentaerythritol, dipentaerythritol, tripentaerythritol, 1,2,4-butanetriol, 1,2,5-pentanetriol, 2-methyl-1,2,3-propanetriol, 2-methyl-1,2,4-butanetriol, and glycerin. The alcohol (3a) and the alcohol (4a) may each be used alone or in combination of two or more kinds.

[0032] The amount of the alcohol (3a) used is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 1% by mass or less, based on the total mass of the polyhydric alcohol. The amount of the alcohol (4a) used is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 1% by mass or less, based on the total mass of the polyhydric alcohol.

[0033] (Carbonate compounds) The carbonate compound (hereinafter sometimes referred to as "carbonic acid diester") is a raw material for the polycarbonate polyol (A). The carbonate compound is not limited as long as it does not impair the effects of the present invention, and examples thereof include dialkyl carbonates, diaryl carbonates, and alkylene carbonates. Among these, diaryl carbonates are preferred from the viewpoint of reactivity.

[0034] Specific examples of the carbonate compound include dimethyl carbonate, diethyl carbonate, dibutyl carbonate, diphenyl carbonate, and ethylene carbonate. Among these, diphenyl carbonate is preferred from the viewpoint of good reactivity. The carbonate compounds may be used alone or in combination of two or more.

[0035] (Transesterification catalyst) When producing the polycarbonate polyol (A), an ester exchange catalyst (hereinafter sometimes simply referred to as "catalyst") can be used as necessary for the purpose of promoting polymerization. However, when an ester exchange catalyst is used, if an excessively large amount of the catalyst remains in the obtained polycarbonate polyol (A), the catalyst may inhibit or excessively promote the urethanization reaction when the polycarbonate polyol (A) is used to produce a polyurethane. For this reason, the amount of catalyst remaining in the polycarbonate polyol (A) is not particularly limited, but the content in terms of catalyst metal relative to the total mass of the polycarbonate polyol (A) is preferably 100 ppm by mass or less, more preferably 50 ppm by mass or less, and even more preferably 10 ppm by mass or less.

[0036] As the transesterification catalyst, any compound that is generally considered to have transesterification ability can be used without any particular limitation. Examples of the transesterification catalyst include compounds of metals in Group 1 of the periodic table, such as lithium, sodium, potassium, rubidium, and cesium; compounds of metals in Group 2 of the periodic table, such as magnesium, calcium, strontium, and barium; compounds of metals in Group 4 of the periodic table, such as titanium and zirconium; compounds of metals in Group 5 of the periodic table, such as hafnium; compounds of metals in Group 9 of the periodic table, such as cobalt; compounds of metals in Group 12 of the periodic table, such as zinc; compounds of metals in Group 13 of the periodic table, such as aluminum; compounds of metals in Group 14 of the periodic table, such as germanium, tin, and lead; compounds of metals in Group 15 of the periodic table, such as antimony and bismuth; and compounds of lanthanide metals, such as lanthanum, cerium, europium, and ytterbium. The transesterification catalyst may be used alone or in combination of two or more kinds.

[0037] Among these, from the viewpoint of increasing the reaction rate of the ester exchange reaction, preferred are compounds of metals of Group 1 on the periodic table, compounds of metals of Group 2 on the periodic table, compounds of metals of Group 4 on the periodic table, compounds of metals of Group 5 on the periodic table, compounds of metals of Group 9 on the periodic table, compounds of metals of Group 12 on the periodic table, compounds of metals of Group 13 on the periodic table, and compounds of metals of Group 14 on the periodic table, more preferred are compounds of metals of Group 1 on the periodic table and compounds of metals of Group 2 on the periodic table, and even more preferred are compounds of metals of Group 2 on the periodic table. Among the compounds of Group 1 metals of the periodic table, compounds of lithium, potassium and sodium are preferred, compounds of lithium and sodium are more preferred, and compounds of sodium are even more preferred. Among the compounds of Group 2 metals of the periodic table, compounds of magnesium, calcium and barium are preferred, compounds of calcium and magnesium are more preferred, and compounds of magnesium are even more preferred.

[0038] These metal compounds are mainly used as hydroxides, salts, etc. Examples of salts when used as salts include halide salts such as chlorides, bromides, iodides, etc.; carboxylates such as acetates, formates, benzoates, etc.; sulfonates such as methanesulfonic acid, toluenesulfonic acid, trifluoromethanesulfonic acid, etc.; phosphorus-containing salts such as phosphates, hydrogen phosphates, dihydrogen phosphates, etc.; and acetylacetonate salts. The metal compounds can also be used as alkoxides such as methoxides, ethoxides, etc.

[0039] From the viewpoint of increasing the reaction rate of the transesterification reaction, acetates, nitrates, sulfates, carbonates, phosphates, hydroxides, halides, and alkoxides of at least one metal selected from Group 2 metals of the periodic table are preferred, acetates, carbonates, and hydroxides of Group 2 metals of the periodic table are more preferred, acetates, carbonates, and hydroxides of magnesium and calcium are even more preferred, acetates of magnesium and calcium are particularly preferred, and magnesium acetate is most preferred.

[0040] From the viewpoint of obtaining sufficient polymerization activity, the amount of the transesterification catalyst used is preferably 500 mass ppm or less, more preferably 100 mass ppm or less, even more preferably 50 mass ppm or less, and particularly preferably 10 mass ppm or less, as a mass ratio of the metal compound to the mass of the raw material polyhydric alcohol, and is preferably 0.01 mass ppm or more, more preferably 0.1 mass ppm or more, and even more preferably 1 mass ppm or more.

[0041] (Reaction conditions) The reaction temperature during the transesterification reaction can be arbitrarily selected as long as it is a temperature at which a practical reaction rate can be obtained. Usually, the reaction temperature of the transesterification reaction is preferably 70°C or higher, more preferably 100°C or higher, and even more preferably 130°C or higher. Also, it is preferably 250°C or lower, more preferably 230°C or lower, and even more preferably 200°C or lower. If the reaction temperature is within the above range, the transesterification reaction can proceed at a practical rate. In addition, by setting the reaction temperature of the transesterification reaction within the above range, it is possible to prevent quality problems such as coloration of the resulting polycarbonate polyol (A) or by-production of an ether structure.

[0042] Furthermore, the reaction temperature throughout all steps of the ester exchange reaction for producing the polycarbonate polyol (A) is preferably 180° C. or less, more preferably 170° C. or less, and even more preferably 160° C. or less. By keeping the reaction temperature throughout all steps at 180° C. or less, it is possible to prevent the polycarbonate polyol (A) from being easily discolored due to high temperature conditions.

[0043] The reaction can be carried out at normal pressure, but the transesterification reaction is an equilibrium reaction, and the reaction can be biased toward the product system by distilling off the light-boiling components produced outside the system. Therefore, in the latter half of the reaction process, it is usually preferable to adopt reduced pressure conditions and carry out the reaction while distilling off the light-boiling components. It is also possible to gradually reduce the pressure from the middle of the reaction and carry out the reaction while distilling off the light-boiling components produced. In particular, it is preferable to carry out the reaction by increasing the degree of reduced pressure at the end of the reaction, since by-products such as monoalcohols, phenols, and cyclic carbonates can be distilled off. The reaction pressure at the end of the ester exchange reaction is preferably 10 kPa or less, more preferably 5 kPa or less, and even more preferably 1 kPa or less.

[0044] In order to effectively distill off the low boiling components, the transesterification reaction can also be carried out while passing an inert gas such as nitrogen, argon or helium through the reaction system. When a low-boiling carbonate compound or polyhydric alcohol is used in the transesterification reaction, the reaction can be carried out at a temperature close to the boiling point of the carbonate compound or polyhydric alcohol in the early stage of the reaction, and the temperature can be gradually increased as the reaction proceeds to further proceed. By adopting this method, it is possible to prevent the distillation of unreacted carbonate compound in the early stage of the reaction. Furthermore, in order to prevent the raw materials from distilling out of the reaction system during the reaction, a reflux tube is attached to the reactor and the reaction is carried out while refluxing the carbonate compound and the polyhydric alcohol, whereby the charged raw materials are not lost outside the reaction system and polycarbonate polyol (A) can be obtained in high yield.

[0045] The polymerization reaction can be carried out in a batch or continuous manner, but is preferably carried out in a continuous manner from the viewpoint of product stability, etc. The apparatus used may be any of tank, tube, and tower types, and known polymerization tanks equipped with various stirring blades, etc. can be used. There are no particular limitations on the atmosphere during the temperature rise of the apparatus, but from the viewpoint of product quality, it is preferable to carry out the reaction in an inert gas such as nitrogen gas at normal pressure or reduced pressure.

[0046] The polymerization reaction in producing the polycarbonate polyol (A) can be terminated when a target molecular weight is reached while measuring the molecular weight of the polycarbonate polyol (A) produced, thereby enabling control of the molecular weight of the polycarbonate polyol (A). The reaction time required for the polymerization reaction varies greatly depending on the polyhydric alcohol, carbonate compound, and catalyst used, and the type of catalyst used, and therefore cannot be generally specified. From the viewpoint of shortening the polymerization process, however, the reaction time is usually preferably 50 hours or less, more preferably 20 hours or less, and even more preferably 10 hours or less.

[0047] (Catalyst deactivator) As described above, when a catalyst is used in the polymerization reaction for producing the polycarbonate polyol (A), the catalyst usually remains in the resulting polycarbonate polyol (A). When the polycarbonate polyol (A) is heated in the polyurethane-forming reaction, the remaining catalyst may cause an increase in the molecular weight of the polyurethane, a change in composition, a deterioration in color tone, or a decrease in the yield of the polyurethane-forming reaction. In order to suppress the above-mentioned adverse effects of the remaining catalyst, it is preferable to add, for example, a catalyst deactivator in an amount approximately equimolar to the amount of the transesterification catalyst used to deactivate the transesterification catalyst. Furthermore, after adding the catalyst deactivator, the transesterification catalyst can be efficiently deactivated by heat treatment or the like as described below.

[0048] Catalyst deactivators used to inactivate the transesterification catalyst include phosphorus-based compounds. Examples of phosphorus-based compounds include inorganic phosphoric acids such as phosphoric acid and phosphorous acid, and organic phosphoric acid esters such as dibutyl phosphate, tributyl phosphate, trioctyl phosphate, triphenyl phosphate, triphenyl phosphite, etc. Among these, phosphoric acid and phosphorous acid are preferred, and phosphoric acid is more preferred, from the viewpoint of their large catalyst deactivation effect even in small amounts. The phosphorus-based compounds may be used alone or in combination of two or more.

[0049] The amount of phosphorus-based compound used is not particularly limited, but as described above, it may be approximately equimolar to the transesterification catalyst used. The amount of phosphorus-based compound used is preferably 5 mol or less, more preferably 2 mol or less, per mol of the transesterification catalyst used. Also, it is preferably 0.6 mol or more, more preferably 0.8 mol or more, and even more preferably 1.0 mol or more. If the amount of phosphorus-based compound used is within the above range, when the polycarbonate polyol (A) is heated, polyurethane can be produced without causing an increase in the molecular weight of the polycarbonate polyol (A), a change in composition, deterioration in color tone, or a decrease in the yield of polyurethane.

[0050] The inactivation of the transesterification catalyst by adding a phosphorus-based compound can be carried out at room temperature, but the inactivation can be carried out more efficiently by heat treatment. The temperature of the heat treatment is not particularly limited, but is preferably 180°C or lower, more preferably 150°C or lower, even more preferably 120°C or lower, and particularly preferably 100°C or lower. Also, it is preferably 50°C or higher, more preferably 60°C or higher, and even more preferably 70°C or higher. When the heat treatment temperature is within the above range, the transesterification catalyst can be efficiently inactivated. Also, coloration of the resulting polycarbonate polyol (A) can be prevented. The time for the heat treatment for the reaction with the phosphorus-based compound is not particularly limited, but is usually preferably 0.1 to 5 hours.

[0051] (purification) The reaction product obtained after the polymerization reaction for producing the polycarbonate polyol (A) and, if necessary, after inactivation of the transesterification catalyst, contains impurities such as the above-mentioned impurities not having hydroxyl groups at the polymer terminals, phenols, the starting dihydroxy compounds, carbonate compounds, the by-produced low-boiling cyclic carbonates, and the added catalysts, and can be purified to remove these impurities. For purification at that time, a method of removing low-boiling compounds by distillation can be adopted. As a specific method of distillation, there is no particular limitation on the form, and any method can be adopted, such as reduced pressure distillation, steam distillation, and thin film distillation, among which thin film distillation is preferred from the viewpoint of obtaining a polycarbonate polyol (A) with high purity and little coloration.

[0052] There are no particular limitations on the conditions for thin-film distillation, but the temperature during thin-film distillation is preferably 250°C or lower, more preferably 200°C or lower. Also, it is preferably 120°C or higher, more preferably 150°C or higher. If the temperature during thin-film distillation is within the above range, the effect of removing low-boiling components is sufficient. Also, if the temperature during thin-film distillation is within the above range, it is possible to prevent the polycarbonate polyol (A) obtained after thin-film distillation from being colored.

[0053] The pressure during thin-film distillation is preferably 500 Pa or less, more preferably 150 Pa or less, further preferably 70 Pa or less, and particularly preferably 60 Pa or less. When the pressure during thin-film distillation is within the above range, the effect of removing low-boiling components can be sufficiently obtained.

[0054] The temperature at which the polycarbonate polyol (A) is kept warm immediately before the thin-film distillation is preferably 250° C. or lower, more preferably 150° C. or lower, and is preferably 80° C. or higher, more preferably 120° C. or higher. If the temperature at which the polycarbonate polyol (A) is kept warm immediately before the thin-film distillation is within the above range, it is possible to prevent the fluidity of the polycarbonate polyol (A) from decreasing immediately before the thin-film distillation. Also, if the temperature at which the polycarbonate polyol (A) is kept warm immediately before the thin-film distillation is within the above range, it is possible to prevent the polycarbonate polyol (A) obtained after the thin-film distillation from being colored.

[0055] In order to remove water-soluble impurities, the polycarbonate polyol (A) may be washed with water, alkaline water, acidic water, a solution containing a chelating agent, etc. In this case, the compound dissolved in water can be selected arbitrarily.

[0056] (molecular chain end) The polycarbonate polyol (A) may have a hydroxyl group at the molecular chain end. The polycarbonate polyol (A) obtained by the reaction of the polyhydric alcohol with the carbonate compound may contain a polycarbonate polyol that does not have a hydroxyl group at the molecular chain end as an impurity. A specific example of a polycarbonate polyol that does not have a hydroxyl group at the molecular chain end is a polycarbonate polyol whose molecular chain end is an alkyloxy group or an aryloxy group, and most of them have a structure derived from a carbonate compound. For example, when diphenyl carbonate is used as the carbonate compound, a phenoxy group may remain as the aryloxy group; when dimethyl carbonate is used, a methoxy group may remain as the alkyloxy group; when diethyl carbonate is used, an ethoxy group may remain; and when ethylene carbonate is used, a hydroxyethoxy group may remain as the molecular chain terminal.

[0057] The ratio of the total number of terminal structures derived from the alcohol (2a) and the alcohol (1a) to the total number of terminal structures of the polycarbonate polyol (A) is preferably 80 mol% or more, more preferably 90 mol% or more, even more preferably 95 mol% or more, particularly preferably 97 mol% or more, and most preferably 99 mol% or more. If the ratio of the total number of terminal structures derived from the alcohol (2a) and the alcohol (1a) to the total number of terminal structures of the polycarbonate polyol is within the above range, it becomes easy to achieve a desired molecular weight when made into polyurethane, and it becomes possible to become a raw material for polyurethane having an excellent balance of solution stability, chemical resistance, and low-temperature flexibility.

[0058] (Hydroxyl value) The hydroxyl value of the polycarbonate polyol (A) is preferably 37.4 mgKOH / g or more, more preferably 38.7 mgKOH / g or more, even more preferably 40 mgKOH / g or more, particularly preferably 42 mgKOH / g or more, more particularly preferably 44.8 mgKOH / g or more, and most preferably 45 mgKOH / g or more. Also, it is preferably 140 mgKOH / g or less, more preferably 135 mgKOH / g or less, even more preferably 130 mgKOH / g or less, and particularly preferably 125 mgKOH / g or less. If the hydroxyl value is within the above range, the viscosity is not too high and handling during polyurethane formation is good. Also, the physical properties such as chemical resistance and low temperature flexibility of the cured film of the resin composition and coating of the present invention are good. The above upper and lower limits of the hydroxyl value of the polycarbonate polyol (A) can be combined in any combination. For example, the hydroxyl value of the polycarbonate polyol (A) is preferably 37.4 to 140 mgKOH / g, more preferably 38.7 to 135 mgKOH / g, even more preferably 40 to 130 mgKOH / g, particularly preferably 42 to 125 mgKOH / g, more particularly preferably 44.8 to 125 mgKOH / g, and most preferably 45 to 125 mgKOH / g.

[0059] The hydroxyl value of the polycarbonate polyol (A) is a value calculated by a method using an acetylation reagent in accordance with JIS K 1557-1.

[0060] (Molecular weight / molecular weight distribution) The number average molecular weight (Mn) of the polycarbonate polyol (A) calculated from the hydroxyl value is preferably 700 or more, more preferably 800 or more, and even more preferably 900 or more. Also, it is preferably 3500 or less, more preferably 3000 or less, and even more preferably 2500 or less. If the Mn of the polycarbonate polyol (A) is within the above range, the low-temperature flexibility is good when it is made into a urethane. Also, if the Mn of the polycarbonate polyol (A) is within the above range, the viscosity of the resin composition and coating material of the present invention is reduced, and handling during polyurethane formation is easy. The above upper and lower limits of Mn of the polycarbonate polyol (A) can be combined in any combination. For example, Mn of the polycarbonate polyol (A) is preferably 700 to 3,500, more preferably 800 to 3,000, and further preferably 900 to 2,500.

[0061] The molecular weight distribution of the polycarbonate polyol (A), weight average molecular weight / number average molecular weight (Mw / Mn), is preferably 1.1 or more, more preferably 1.3 or more. Also, it is preferably 3.5 or less, more preferably 3.0 or less. If the molecular weight distribution is within the above range, the physical properties of the polyurethane produced using the polycarbonate polyol (A) are good in low-temperature flexibility and elongation are improved. Also, if the molecular weight distribution is within the above range, advanced purification operations such as removing oligomers are not required when producing the polycarbonate polyol (A). The above upper and lower limits of the molecular weight distribution of the polycarbonate polyol (A) can be combined in any manner. For example, the molecular weight distribution (Mw / Mn) of the polycarbonate polyol (A) is preferably from 1.1 to 3.5, more preferably from 1.3 to 3.0.

[0062] The weight average molecular weight and number average molecular weight of the polycarbonate polyol (A) in the molecular weight distribution of the polycarbonate polyol (A) are the weight average molecular weight and number average molecular weight in terms of polystyrene, respectively, and can usually be determined by measurement using gel permeation chromatography (hereinafter also referred to as GPC).

[0063] (Residual by-products, etc.) When producing a polycarbonate diol as the polycarbonate polyol (A), if an aromatic carbonate diester such as diphenyl carbonate is used as a raw material, phenols are produced as by-products during the production of the polycarbonate diol. Since phenols are monofunctional compounds, they may be an inhibitor in the production of polyurethane, and the urethane bond formed by phenols has a weak bond strength, so it may dissociate due to heat in the subsequent process, and isocyanate and phenols may be regenerated, causing problems. In addition, since phenols are irritating substances, it is preferable that the amount of phenols remaining in the polycarbonate diol is as small as possible. Specifically, the amount of phenols remaining in the polycarbonate diol is preferably 1000 ppm or less, more preferably 500 ppm or less, further preferably 300 ppm or less, and particularly preferably 100 ppm or less, as a mass ratio. In order to reduce the amount of phenols in the polycarbonate diol, it is effective to set the pressure of the polymerization reaction of the polycarbonate diol to a high vacuum of 1 kPa or less as an absolute pressure, or to perform thin film distillation after the polymerization of the polycarbonate diol, as described later.

[0064] In the polycarbonate diol, the carbonate diester used as a raw material during production may remain. The amount of the carbonate diester remaining in the polycarbonate diol is not limited, but it is preferable that it is small. The amount of the carbonate diester remaining relative to the polycarbonate diol is preferably 5% by mass or less, more preferably 3% by mass or less, and even more preferably 1% by mass or less, as a mass ratio. Also, it is preferably 0% by mass or more, more preferably 0.01% by mass or more, and even more preferably 0.1% by mass or more. If the amount of the carbonate diester remaining relative to the polycarbonate diol is within the above range, it is possible to prevent the reaction during polyurethane formation from being inhibited. The upper and lower limits of the residual amount of the carbonate diester relative to the polycarbonate diol can be combined in any combination. For example, the residual amount of the carbonate diester relative to the polycarbonate diol is preferably 0 to 5 mass%, more preferably 0.01 to 3 mass%, and even more preferably 0.1 to 1 mass%, in terms of mass ratio.

[0065] In the polycarbonate diol, the dihydroxy compound used in the production may remain. The amount of the dihydroxy compound remaining in the polycarbonate diol is not limited, but it is preferable that it is small. The amount of the dihydroxy compound remaining relative to the polycarbonate diol is preferably 1% by mass or less, more preferably 0.1% by mass or less, and even more preferably 0.05% by mass or less, in terms of mass ratio. If the amount of the dihydroxy compound remaining in the polycarbonate diol is within the above range, the length of the molecule of the soft segment portion when made into polyurethane is sufficient, and desired physical properties can be obtained.

[0066] The polycarbonate diol may contain a cyclic carbonate (cyclic oligomer) produced as a by-product during production. For example, when 1,4-butanediol is used as the alcohol (2a), 1,3-dioxepan-2-one or a compound in which two or more molecules of these form a cyclic carbonate may be produced as a by-product and contained in the polycarbonate diol. The by-product compound may cause a side reaction in the polyurethane reaction and may cause turbidity, so it is preferable to remove the by-product compound as much as possible by making the pressure of the polymerization reaction of the polycarbonate diol a high vacuum of 1 kPa or less as an absolute pressure or by performing thin film distillation after the synthesis of the polycarbonate diol. From the viewpoint of reducing the cause of side reactions and turbidity, the content of these cyclic carbonates contained in the polycarbonate diol is preferably 3% by mass or less, more preferably 1% by mass or less, and even more preferably 0.5% by mass or less, as a mass ratio to the polycarbonate diol.

[0067] (Content) The content of the polycarbonate polyol (A) in the resin composition is preferably 3 to 80 mass%, more preferably 5 to 60 mass%, and even more preferably 10 to 40 mass%, based on the total mass of the solid content (hereinafter, simply referred to as "solid content") corresponding to the remainder after removing the solvent from the resin composition. If the content of the polycarbonate polyol (A) is within the above range, the stability of the resin composition is further improved.

[0068] <Acrylic polyol (B)> The acrylic polyol (B) may be used alone or in combination of two or more kinds.

[0069] The acrylic polyol can be produced, for example, by copolymerizing a polymerizable unsaturated monomer having a hydroxyl group with another polymerizable unsaturated monomer copolymerizable with the polymerizable unsaturated monomer having a hydroxyl group (hereinafter also referred to as "another polymerizable unsaturated monomer") in a conventional manner.

[0070] (monomer) The polymerizable unsaturated monomer having a hydroxyl group is a compound having one or more hydroxyl groups and one or more polymerizable unsaturated groups in one molecule. As the polymerizable unsaturated monomer having a hydroxyl group, specifically, a monoester of acrylic acid or methacrylic acid with a dihydric alcohol having 2 to 10 carbon atoms is suitable, and examples thereof include polymerizable monomers having a hydroxyl group such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 3-chloro-2-hydroxypropyl (meth)acrylate, polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, PLACCEL FM (manufactured by Daicel Corporation, caprolactone addition monomer), and PLACCEL FA (manufactured by Daicel Corporation, caprolactone addition monomer). Among these, 2-hydroxyethyl (meth)acrylate and hydroxypropyl (meth)acrylate are preferred in terms of further improving the scratch resistance and abrasion resistance of the coating film. The polymerizable unsaturated monomer having a hydroxyl group may be used alone or in combination of two or more kinds.

[0071] Examples of other polymerizable unsaturated monomers include (meth)acrylic acid; alkyl esters or cycloalkyl esters of (meth)acrylic acid having 1 to 18 carbon atoms, such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, hexyl (meth)acrylate, octyl (meth)acrylate, lauryl (meth)acrylate, cyclohexyl (meth)acrylate, octyl (meth)acrylate, lauryl (meth)acrylate, and cyclohexyl (meth)acrylate; alkoxyalkyl esters of (meth)acrylic acid, such as methoxybutyl (meth)acrylate, methoxyethyl (meth)acrylate, and ethoxybutyl (meth)acrylate; glycidyl acrylate or glycidyl methacrylate, and a monocarboxylic acid compound having 3 to 18 carbon atoms (for example, acetic acid, propionic acid, , oleic acid, stearic acid or lauric acid); an adduct of Cardura E-10 and an unsaturated acid such as acrylic acid; an ethylenically unsaturated monomer having an alkoxysilane group such as 1-methacryloxytrimethoxysilane; 1-ethylenically unsaturated carboxylic acid such as crotonic acid, itaconic acid, maleic acid, maleic anhydride and fumaric acid; a vinyl monomer having a glycidyl group such as glycidyl (meth)acrylate and allyl glycidyl ether; an amide of (meth)acrylic acid such as acrylamide, N-methylolacrylamide and N-butoxymethylacrylamide; styrene; and (meth)acrylonitrile. The other polymerizable unsaturated monomers may be used alone or in combination of two or more kinds.

[0072] (Solubility parameter) The solubility parameter (SP value) of the acrylic polyol (B) is 8.1 to 12.5 (J / cm 3 ) 1 / 2 is preferable, and 8.3 to 11.5 (J / cm 3 ) 1 / 2 More preferably, 8.5 to 10.0 (J / cm 3 ) 1 / 2is more preferable. When the SP value of the acrylic polyol (B) is equal to or higher than the lower limit, the compatibility with the polycarbonate polyol (A), particularly the polycarbonate polyol (A) made from 1,10-decanediol, is good. When the SP value of the acrylic polyol (B) is equal to or lower than the upper limit, the water resistance of the coating film is good.

[0073] The SP value is an abbreviation for solubility parameter, and is a measure of solubility. The larger the SP value, the higher the polarity, and conversely, the smaller the SP value, the lower the polarity. The SP value can be measured, for example, by the following method [Reference: SUH, CLARKE [JPSA-1, 5, 1671-1681 (1967)].

[0074] As a sample, 0.5 g of acrylic polyol (B) is weighed into a 100 mL beaker, 10 mL of a good solvent is added using a whole pipette, and the mixture is dissolved using a magnetic stirrer. Acetone is used as the solvent. A 50 mL burette is used to drop a poor solvent into the obtained sample at a measurement temperature of 20°C, and the point at which the solution becomes turbid (cloudy point) is defined as the amount of the drop. Ion-exchanged water is used as a high SP poor solvent, and n-hexane is used as a low SP poor solvent, and the cloudy point is measured for each poor solvent. From the following formulas (2-1) to (2-5), the SP value (δ) of the acrylic polyol (B) (unit: (J / cm 3 ) 1 / 2 ) is required. V ml =(V l ×V a ) / (φ l ×V a +φ a1 ×V l ) ···(2-1) δ ml =φ l ×δ l +φ a1 ×δ a (2-2) V mh =(V h ×Va ) / (φ h ×V a +φ a2 ×V h ) ···(2-3) δ mh =φ h ×δ h +φ a2 ×δ a (2-4) δ = {(V ml ) 1 / 2 ×δ ml +(V mh ) 1 / 2 ×δ mh} / {(V ml ) 1 / 2 +(V mh ) 1 / 2} ···(2-5)

[0075] The abbreviations in formulas (2-1) to (2-5) have the following meanings. ·V l : Molar volume of n-hexane (cm 3 / mol) ·V h : Molar volume of ion-exchanged water (cm 3 / mol) ·V a : Molar volume of good solvent (cm 3 / mol) φ l : Volume fraction of n-hexane to the sum of good solvent and n-hexane at the cloudiness point = Amount of n-hexane dropped / (amount of good solvent used + amount of n-hexane dropped) φ h : Volume fraction of ion-exchanged water relative to the sum of good solvent and ion-exchanged water at the turbidity point = Amount of ion-exchanged water dropped / (amount of good solvent used + amount of ion-exchanged water dropped) φ a1 : Volume fraction of good solvent to the sum of good solvent and n-hexane at the cloudiness point = amount of good solvent used / (amount of good solvent used + amount of n-hexane dropped) φ a2 : Volume fraction of good solvent to the sum of good solvent and ion-exchanged water at the cloudiness point = amount of good solvent used / (amount of good solvent used + amount of ion-exchanged water dropped) δ l: SP value of n-hexane δ h : SP value of ion-exchanged water δ a :SP value of good solvent

[0076] (molecular weight) The weight average molecular weight of the acrylic polyol (B) is preferably 900 to 50,000. When the weight average molecular weight of the acrylic polyol (B) is equal to or higher than the lower limit, the hardness of the coating film is good. When the weight average molecular weight of the acrylic polyol (B) is equal to or lower than the upper limit, the viscosity of the resin composition and the coating material described below is appropriately low, and the handling is good. The weight average molecular weight of the acrylic polyol (B) is preferably 1,000 to 25,000.

[0077] The weight average molecular weight of the acrylic polyol (B) is a value calculated as a standard polystyrene by gel permeation chromatography (GPC) under the following detailed measurement conditions. (GPC measurement conditions) Columns: "TSK-gel superHZM-M", "TSK-gel HZM-M", "TSK-gel HZ2000" ·Eluent:THF ·Flow rate: 0.35mL / min ·Injection volume: 10μL Column temperature: 40℃ Detector: UV-8020

[0078] (Hydroxyl value) The hydroxyl value of the acrylic polyol (B) is preferably 10 to 300 mgKOH / g, more preferably 25 to 220 mgKOH / g. If the hydroxyl value of the acrylic polyol (B) is equal to or greater than the lower limit, a preferred crosslink density as a coating film is obtained, and the hardness of the coating film is good. If the hydroxyl value of the acrylic polyol (B) is equal to or less than the upper limit, the solubility in a resin composition or a paint described below and the flexibility of the coating film when made into a coating film are good. The hydroxyl value of the acrylic polyol (B) is a value calculated by the following formula (3). Hydroxyl number (mgKOH / g) = (fb ×M1 b / Mn b / M2 b ×〔KOH〕×1000) ···(3)

[0079] The abbreviations in formula (3) have the following meanings. f b : the number of hydroxyl groups in the monomer having a hydroxyl group (the polymerizable unsaturated monomer having a hydroxyl group) constituting the acrylic polyol (B) · [KOH]: Molecular weight of KOH M1 b : Mass of monomer having hydroxyl group (g) M2 b : Solid content mass (g) of acrylic polyol (B) Mn b : Molecular weight of monomer having hydroxyl group (number average molecular weight)

[0080] (glass transition temperature) The lower limit of the glass transition temperature of the acrylic polyol (B) is preferably -60°C, more preferably -50°C. The upper limit of the glass transition temperature of the acrylic polyol (B) is preferably 180°C, more preferably 150°C, and even more preferably 140°C. If the glass transition temperature of the acrylic polyol (B) is equal to or higher than the lower limit, the hardness of the coating film becomes good. If the glass transition temperature of the acrylic polyol (B) is equal to or lower than the upper limit, the coating material described below is less likely to gel, and good handling can be maintained. The upper and lower limits of the glass transition temperature of the acrylic polyol (B) can be combined in any combination. For example, the glass transition temperature of the acrylic polyol (B) is preferably -60 to 180°C, more preferably -50 to 150°C, and even more preferably -50 to 140°C. The glass transition temperature (Tg) (unit: ° C.) of the acrylic polyol (B) is a value calculated by the Fox formula shown in the following formula (4).

[0081]

number

[0082] The abbreviations in formula (4) have the following meanings. · Wi: mass fraction of monomer i Tgi: Tg of the homopolymer of monomer i (℃) For the Tg of a homopolymer, the values ​​described in "Polymer Handbook, 4th Edition, John Wiley & Sons" can be used. For the Tg of homopolymers not described in "Polymer Handbook, 4th Edition, John Wiley & Sons," an actual measured value measured by the method described in JIS standard K-7121-1987 "Method for measuring transition temperature of plastics" can be used.

[0083] (Content) The content of the acrylic polyol (B) in the resin composition is preferably 5 to 90 mass%, more preferably 20 to 85 mass%, and even more preferably 50 to 80 mass%, based on the total mass of the solid content corresponding to the remainder after removing the solvent from the resin composition. If the content of the acrylic polyol (B) is within the above range, the stability of the resin composition is further improved.

[0084] (mass ratio) From the viewpoint of obtaining a good appearance of the coating film, the mass ratio (A) / (B) of the polycarbonate polyol (A) to the acrylic polyol (B) is preferably 5 / 95 to 90 / 10, more preferably 10 / 90 to 70 / 30, and even more preferably 15 / 85 to 50 / 50.

[0085] <Solvent> The solvent includes an aromatic hydrocarbon solvent (C). The solvent may further contain a solvent other than the aromatic hydrocarbon solvent (C) (hereinafter also referred to as "other solvent").

[0086] (Aromatic Hydrocarbon Solvents (C)) Examples of the aromatic hydrocarbon solvent (C) include toluene, xylene, benzene, trimethylbenzene, cumene, and T-SOL. TM 100FLUID (ENEOS Corporation), T-SOL TM150FLUID (manufactured by ENEOS Corporation), SS200, IPZOL 100 (manufactured by Idemitsu Kosan Co., Ltd.), IPZOL 150 (manufactured by Idemitsu Kosan Co., Ltd.), and high boiling point aromatic solvent S100 (manufactured by Ando Parachemie Co., Ltd.). Among these, from the viewpoint of producing less aggregates in the paint and improving the appearance of the coating film, toluene, xylene, T-SOL are preferred as aromatic hydrocarbon solvents (C). TM Preferred are 100FLUID (manufactured by ENEOS Corporation) and high boiling point aromatic solvent S100 (manufactured by Ando Parachemie Co., Ltd.), and from the viewpoint of reducing aggregates in the paint and improving the appearance of the coating film, it is more preferred that the aromatic hydrocarbon solvent (C) contains one or more of toluene and xylene. The aromatic hydrocarbon solvent (C) may be used alone or in combination of two or more kinds.

[0087] The content of the aromatic hydrocarbon solvent (C) is preferably 35 to 100 mass % based on the total mass of the solvent, more preferably 50 to 100 mass %, and even more preferably 70 to 100 mass %. When the content of the aromatic hydrocarbon solvent (C) is within the above range, the compatibility between the polycarbonate polyol (A), particularly the polycarbonate polyol (A) made from 1,10-decanediol as a raw material, and the acrylic polyol (B) becomes good, and the appearance of the coating film and the stability of the resin composition become good.

[0088] In addition, the polycarbonate polyol (A) and the acrylic polyol (B) may use an aromatic hydrocarbon solvent (C) as a reaction solvent in the production process. In that case, the obtained reaction product contains the polycarbonate polyol (A) and the aromatic hydrocarbon solvent (C) or the acrylic polyol (B) and the aromatic hydrocarbon solvent (C), and the reaction product can be used as it is for the production of a resin composition or a coating material without removing the aromatic hydrocarbon solvent (C). When a reaction product containing the polycarbonate polyol (A) and the aromatic hydrocarbon solvent (C) is used for producing a coating material, the aromatic hydrocarbon solvent (C) derived from the polycarbonate polyol (A), i.e., the aromatic hydrocarbon solvent (C) contained in the reaction product, is also included in the content of the aromatic hydrocarbon solvent (C) in the resin composition or coating material. In addition, when a reaction product containing the acrylic polyol (B) and the aromatic hydrocarbon solvent (C) is used for producing a coating material, the aromatic hydrocarbon solvent (C) derived from the acrylic polyol (B), i.e., contained in the reaction product, is also included in the content of the aromatic hydrocarbon solvent (C) in the resin composition or coating material.

[0089] (Other solvents) Other solvents include, for example, alcohol-based solvents such as methanol, isopropyl alcohol, n-butanol, diacetone alcohol, 2-methoxyethanol (methyl cellosolve), 2-ethoxyethanol (ethyl cellosolve), 2-butoxyethanol (butyl cellosolve), and tertiary amyl alcohol; carboxylic acid ester-based solvents such as ethyl acetate, n-propyl acetate, butyl acetate, and butyl formate; ketone-based solvents such as methyl ethyl ketone, methyl isobutyl ketone, acetone, and cyclohexanone; amide-based solvents such as dimethylformamide and dimethylacetamide; ether-based solvents such as diethyl ether, methoxytoluene, 1,2-dimethoxyethane, 1,2-dibutoxyethane, 1,1-dimethoxymethane, 1,1-dimethoxyethane, 1,4-dioxane, tetrahydrofuran, and propylene glycol monomethyl ether acetate; and methylene glycol monomethyl ether acetate. Examples of the alkylene glycol alkyl ether acetate solvent include alkylene glycol alkyl ether acetate solvents such as methylene glycol monoethyl ether acetate, methylene glycol monopropyl ether acetate, methylene glycol monobutyl ether acetate, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monopropyl ether acetate, ethylene glycol monobutyl ether acetate, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol monopropyl ether acetate, propylene glycol monobutyl ether acetate, butylene glycol monomethyl ether acetate, butylene glycol monoethyl ether acetate, butylene glycol monopropyl ether acetate, and butylene glycol monobutyl ether acetate. The other solvents may be used alone or in combination of two or more.

[0090] The content of the other solvent is preferably from 0 to 65 mass %, more preferably from 0 to 50 mass %, and further preferably from 0 to 30 mass %, based on the total mass of the solvents.

[0091] <Optional ingredients> The resin composition of the present invention may contain optional components as listed below, if necessary. From the viewpoint of imparting various properties, it is preferable to add optional components when using the resin composition as a coating material. Examples of optional components contained in the resin composition include a crosslinking agent (D), a weather resistance imparting agent, a surface conditioner, a curing acceleration catalyst, an antioxidant, an anti-yellowing agent, a bluing agent, a pigment, a leveling agent, an antifoaming agent, a thickener, an anti-settling agent, an antistatic agent, and an anti-fogging agent. The optional components may be used alone or in combination of two or more.

[0092] <Method of producing resin composition> The resin composition can be produced by uniformly mixing the polycarbonate polyol (A), the acrylic polyol (B) and a solvent. During mixing, one or more optional components may be added, if necessary. As described above, when at least one of a reaction product containing the polycarbonate polyol (A) and an aromatic hydrocarbon solvent and a reaction product containing the acrylic polyol (B) and an aromatic hydrocarbon solvent is used, one or more optional components may be added as necessary to produce a resin composition, or the resin composition may be further diluted with a solvent to a desired solid content concentration.

[0093] <Solid content concentration> The solid content concentration of the resin composition is preferably 30% by mass or more and less than 100% by mass, more preferably 35 to 70% by mass, and even more preferably 40 to 65% by mass, based on the total mass of the resin composition. If the solid content concentration of the resin composition is equal to or more than the lower limit, sagging during application of the resin composition when used as a coating material can be suppressed, resulting in a good appearance. If the solid content concentration of the resin composition is equal to or less than the upper limit, stability is good. The solid content of the resin composition is the mass ratio of the remainder after removing the solvent from the resin composition to the total mass of the resin composition, and is also called the net concentration. In other words, the sum of the content of the solvent in the resin composition and the solid content of the resin composition is 100 mass%.

[0094] <Action and effect> The resin composition of the present embodiment described above contains a specific polycarbonate polyol (A), so that the coating film has excellent chemical resistance, stain resistance, and flexibility. In addition, the resin composition of the present embodiment contains an aromatic hydrocarbon solvent, so that a coating film with good appearance can be obtained. In addition, the storage stability of the resin composition and its coating material is improved. Therefore, the resin composition of the present embodiment has good storage stability. Furthermore, by using the resin composition of the present embodiment, it is possible to form a coating film that can maintain various performance properties such as chemical resistance, stain resistance, flexibility, and appearance of the coating film, and these performance properties can be well maintained even under conditions of long-term use in exterior building materials, road materials, vehicles including automobiles, aircraft, etc.

[0095] [paint] Hereinafter, one embodiment of the coating material of the present invention will be described. The coating material of the present embodiment is a composition (coating material composition) containing the resin composition of the present invention. The coating material preferably contains a crosslinking agent (D) described below. The coating material may further contain components other than the resin composition of the present invention and the crosslinking agent (D) (hereinafter also referred to as "optional components"), if necessary, within a range that does not impair the effects of the present invention.

[0096] <Resin composition> The resin composition contained in the coating material is the resin composition of the present invention described above, and therefore a description thereof will be omitted. The content of polycarbonate polyol (A) in the coating material is preferably 1 to 70 mass%, more preferably 5 to 50 mass%, and even more preferably 10 to 30 mass%, based on the total mass of the components that form the coating film (hereinafter also referred to as "coating film-forming components"). When the content of polycarbonate polyol (A) is equal to or higher than the lower limit, the chemical resistance of the coating film is good. When the content of polycarbonate polyol (A) is equal to or lower than the upper limit, the appearance of the coating film is good, and the coating film is less likely to crack. Here, the "components that form the coating film" refers to the remainder after removing the solvent from the coating material (i.e., the solid content of the coating material).

[0097] The content of the acrylic polyol (B) in the coating material is preferably 1 to 90 mass%, more preferably 20 to 80 mass%, and even more preferably 40 to 70 mass%, based on the total mass of the coating film-forming components. When the content of the acrylic polyol (B) is equal to or higher than the lower limit, the appearance of the coating film is good. When the content of the acrylic polyol (B) is equal to or lower than the upper limit, cracks are less likely to occur in the coating film.

[0098] <Crosslinking agent (D)> For the purpose of forming a coating film that is tough, strong, and has excellent abrasion resistance, chemical resistance, and weather resistance, the coating material of the present invention preferably contains a crosslinking agent (D). Examples of the crosslinking agent (D) include polyisocyanates, melamine resins, epoxy resins, and alkyl silicates. Among these, polyisocyanates and melamine resins that are highly reactive with the acrylic polyol (B) are preferred, and polyisocyanates are even more preferred because they have a low curing temperature, can shorten the curing time, and can reduce the energy required for curing. The crosslinking agent (D) may be used alone or in combination of two or more kinds.

[0099] (Polyisocyanate) The polyisocyanate is preferably a bifunctional or higher isocyanate compound. Known bifunctional or higher isocyanate compounds can be used. Examples of bifunctional isocyanate compounds (hereinafter also referred to as "diisocyanate compounds") include hexamethylene diisocyanate, dicyclohexylmethane diisocyanate, isophorone diisocyanate, and 1,3-bis(isocyanatomethyl)cyclohexane 4,4-dicyclohexyl diisocyanate. The diisocyanate compounds may be used alone or in combination of two or more kinds.

[0100] The tri- or higher functional isocyanate compounds are synthesized using the above-mentioned diisocyanate compounds as a starting material, and examples thereof include biuret compounds, trimethylolpropane adduct compounds, isocyanurate compounds, and allophanate compounds. Specific examples of trifunctional or higher isocyanate compounds include hexamethylene diisocyanate biuret (manufactured by Asahi Kasei Corporation under the trade name "Duranate 24A-100"), hexamethylene diisocyanate adduct (manufactured by Asahi Kasei Corporation under the trade name "Duranate P-301-75E"), hexamethylene diisocyanate isocyanurate (manufactured by Asahi Kasei Corporation under the trade name "Duranate TPA-100"), blocked isocyanate (manufactured by Asahi Kasei Corporation under the trade name "Duranate MF-K60X"); 1,3-bis(isocyanatomethylene Examples of such compounds include a trimethylolpropane adduct of 1,3-bis(isocyanatomethyl)cyclohexane (manufactured by Mitsui Chemicals, Inc. under the trade name "Takenate D-120N"), an isocyanurate of 1,3-bis(isocyanatomethyl)cyclohexane (manufactured by Mitsui Chemicals, Inc. under the trade name "Takenate D-127N"), a trimethylolpropane adduct of isophorone diisocyanate (manufactured by Mitsui Chemicals, Inc. under the trade name "Takenate D-140N"); and an allophanate of hexamethylene diisocyanate (manufactured by Sumika Bayer Urethane Co., Ltd. under the trade name "Desmodur XP2679"). The tri- or higher functional isocyanate compounds may be used alone or in combination of two or more kinds. From the viewpoint of increasing the crosslink density of the coating film and improving the water resistance of the coating film, the polyisocyanate is preferably a tri- or higher functional isocyanate compound.

[0101] In addition, as the polyisocyanate, it is also possible to use blocked polyisocyanate compounds, which are compounds in which the isocyanate groups in the above-mentioned difunctional or higher isocyanate compounds and derivatives thereof are blocked with a blocking agent. The blocked polyisocyanate compounds may be used alone or in combination of two or more kinds.

[0102] Examples of blocking agents include phenolic compounds such as phenol, cresol, xylenol, nitrophenol, ethylphenol, hydroxydiphenyl, butylphenol, isopropylphenol, nonylphenol, octylphenol, and methyl hydroxybenzoate; lactam compounds such as ε-caprolactam, δ-valerolactam, γ-butyrolactam, and β-propiolactam; aliphatic alcohol compounds such as methanol, ethanol, propyl alcohol, butyl alcohol, amyl alcohol, and lauryl alcohol; ether compounds such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol monomethyl ether, and methoxymethanol; benzyl alcohol, glycolic acid, methyl glycolate, ethyl glycolate, butyl glycolate, lactic acid, methyl lactate, ethyl lactate, butyl lactate, methylol urea, methylol melamine, diacetone alcohol, and 2-hydroxyethyl Alcohol compounds such as acrylates and 2-hydroxyethyl methacrylate; oxime compounds such as formamide oxime, acetamide oxime, acetoxime, methyl ethyl ketoxime, diacetyl monooxime, benzophenone oxime, and cyclohexane oxime; active methylene compounds such as dimethyl malonate, diethyl malonate, ethyl acetoacetate, methyl acetoacetate, and acetylacetone; butyl mercaptan, t-butyl mercaptan, hexyl mercaptan, t-dodecyl mercaptan, and 2-mercaptobenzothiazole mercaptan compounds such as thiophenol, methylthiophenol, and ethylthiophenol; acid amide compounds such as acetanilide, acetaniside, acetotoluide, acrylamide, methacrylamide, acetate amide, stearic acid amide, and benzamide; imide compounds such as succinimide, phthalic acid amide, and maleic acid amide; amine compounds such as diphenylamine, phenylnaphthylamine, xylidine, N-phenylxylidine, carbazole, aniline, naphthylamine, butylamine, dibutylamine, and butylphenylamine;Examples of the compounds include imidazole-based compounds such as imidazole and 2-ethylimidazole; urea-based compounds such as urea, thiourea, ethyleneurea, ethylenethiourea, and diphenylurea; carbamate esters such as N-phenylcarbamate phenyl; imine-based compounds such as ethyleneimine and propyleneimine; sulfite-based compounds such as sodium bisulfite and potassium bisulfite; and azole-based compounds. Examples of the azole compounds include pyrazoles or pyrazole derivatives such as pyrazole, 3,5-dimethylpyrazole, 3-methylpyrazole, 4-benzyl-3,5-dimethylpyrazole, 4-nitro-3,5-dimethylpyrazole, 4-bromo-3,5-dimethylpyrazole, and 3-methyl-5-phenylpyrazole; imidazoles or imidazole derivatives such as imidazole, benzimidazole, 2-methylimidazole, 2-ethylimidazole, and 2-phenylimidazole; and imidazoline derivatives such as 2-methylimidazoline and 2-phenylimidazoline.

[0103] When blocking (reacting with a blocking agent), a solvent may be added as necessary. The solvent used in the blocking reaction is preferably a solvent that has low reactivity or does not react with the isocyanate group, such as ketones such as acetone and methyl ethyl ketone, esters such as ethyl acetate, and N-methyl-2-pyrrolidone (NMP). The solvent used in the blocking reaction may be one type alone or two or more types in combination.

[0104] The compounding ratio of polyisocyanate, polycarbonate polyol (A) and acrylic polyol (B) is preferably 0.5 to 2.0, more preferably 0.7 to 1.8, and even more preferably 0.8 to 1.5, in terms of the performance of the coating film, in terms of NCO / OH [molar number of isocyanate groups in polyisocyanate / molar number of hydroxyl groups in polycarbonate polyol (A) and acrylic polyol (B)]. When NCO / OH is equal to or greater than the lower limit, the curing speed of the coating material can be increased. In addition, the crosslinking density of the coating film increases, and the hardness and water resistance of the coating film are likely to be improved. When NCO / OH is equal to or less than the upper limit, the drying property after coating the coating material on the substrate and the adhesion of the coating film to the substrate are likely to be improved.

[0105] (Melamine resin) The melamine resin is a resin obtained by addition condensation of an amine compound such as melamine, guanamine, or urea with formaldehyde, or a resin obtained by further addition condensation of such a resin with an alcohol. Examples of melamine resins include methylated melamine, butylated melamine, methylated benzoguanamine, butylated benzoguanamine, etc. In particular, from the viewpoint of improving the chemical resistance of the cured coating film, fully or partially methylolated melamine resins such as hexamethylol melamine, pentamethylol melamine, tetramethylol melamine, and mixtures thereof are preferred.

[0106] Specific examples of melamine resins include those manufactured by Cytec Corporation under the trade names "CYMEL 303," "CYMEL 325," and "CYMEL 1156"; those manufactured by Mitsui Chemicals, Inc. under the trade names "YUBAN 20N," "YUBAN 20SB," and "YUBAN 128"; and those manufactured by Sumitomo Chemical Co., Ltd. under the trade names "SUMIMAL M-50W," "SUMIMAL M-40N," and "SUMIMA L M-30W." The melamine resin may be used alone or in combination of two or more kinds.

[0107] (Epoxy resin) The epoxy resin is an epoxy compound or epoxy resin, and any conventionally known epoxy resin can be used without limitation as long as it has two or more glycidyl groups (epoxy groups) on average in the molecule. Examples of epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, novolac type epoxy resins (such as phenol novolac type epoxy resins and cresol novolac type epoxy resins), alicyclic epoxy resins (such as 3',4'-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate), nitrogen-containing cyclic epoxy resins (such as triglycidyl isocyanurate and hydantoin type epoxy resins), hydrogenated bisphenol A type epoxy resins, aliphatic epoxy resins, glycidyl ether type epoxy resins, bisphenol S type epoxy resins, biphenyl type epoxy resins, dicyclocyclic type epoxy resins, naphthalene type epoxy resins, and halogenated epoxy resins. The epoxy resin may be used alone or in combination of two or more kinds.

[0108] The content of the crosslinking agent (D) in the coating material is preferably 1 to 90 mass%, more preferably 5 to 70 mass%, and even more preferably 10 to 50 mass%, based on the total mass of the coating film-forming components. If the content of the crosslinking agent (D) is equal to or greater than the lower limit, the coating film is less likely to crack. If the content of the crosslinking agent (D) is equal to or less than the upper limit, the appearance of the coating film is good.

[0109] The content of the crosslinking agent (D) in the coating material is preferably 5 to 100 parts by mass, more preferably 15 to 90 parts by mass, based on the total mass (100 parts by mass) of the polycarbonate polyol (A) and the acrylic polyol (B). When the content of the crosslinking agent is within the above range, the drying property after the coating material is applied to a substrate and the adhesion of the coating film to the substrate tend to be improved.

[0110] <Optional ingredients> Optional components contained in the coating material include weather resistance imparting agents, surface conditioners, curing acceleration catalysts, antioxidants, anti-yellowing agents, bluing agents, pigments, leveling agents, defoamers, thickeners, anti-settling agents, antistatic agents, and anti-fogging agents. The optional components may be used alone or in combination of two or more.

[0111] (Weather resistance agent) The weather resistance imparting agent is a component that imparts weather resistance to the coating film. Examples of weather resistance imparting agents include ultraviolet absorbers and light stabilizers. The weather resistance imparting agent may be used alone or in combination of two or more kinds.

[0112] <<Ultraviolet absorbing agent>> As the ultraviolet absorber, compounds derived from triazine-based compounds, benzophenone-based compounds, benzotriazole-based compounds, phenyl salicylate-based compounds, phenyl benzoate-based compounds, or the like are preferred, with benzophenone-based compounds being preferred since they can be contained in large amounts in the coating material, and triazine-based compounds and benzotriazole-based compounds being preferred since they can prevent yellowing of substrates such as polycarbonate. From the viewpoint of preventing yellowing of the cured coating film over a long period of time, it is more preferable that the ultraviolet absorbing agent has a maximum absorption wavelength in the range of 240 to 380 nm.

[0113] Specific examples of ultraviolet absorbers include a mixture of 2-[4-(2-hydroxy-3-dodecyloxy-propyl)oxy-2-hydroxyphenyl]-4,6-[bis(2,4-dimethylphenyl)-1,3,5-triazine] and 2-[4-(2-hydroxy-3-tridecyloxy-propyl)oxy-2-hydroxyphenyl]-4,6-[bis(2,4-dimethylphenyl)-1,3,5-triazine] (BASF's trade name "Tinuvin 400"); 2-[4-(octyl-2-methylethanoate)oxy-2- hydroxyphenyl]-4,6-[bis(2,4-dimethylphenyl)]-1,3,5-triazine (BASF's trade name "Tinuvin 479"), tris[2,4,6-[2-{4-(octyl-2-methylethanoate)oxy-2-hydroxyphenyl}]-1,3,5-triazine] (BASF's trade name "Tinuvin 777"), 2-hydroxybenzophenone, 5-chloro-2-hydroxybenzophenone, 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2- Hydroxy-4-octyloxybenzophenone, 4-dodecyloxy-2-hydroxybenzophenone, 2-hydroxy-4-octadecyloxybenzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, phenyl salicylate, p-tert-butylphenyl salicylate, p-(1,1,3,3-tetramethylbutyl)phenyl salicylate, 3-hydroxyphenyl benzoate, phenylene-1,3-dibenzoate, 2-( 2-hydroxy-5'-methylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-butylphenyl)-5-chlorobenzotriazole, 2-(2-hydroxy-3,5-di-tert-butylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-butylphenyl)benzotriazole, 2-(2-hydroxy-4-octylphenyl)benzotriazole, 2-(2'-hydroxy-5'-methacryloxyethylphenyl)-2H-benzotriazole and the like. The ultraviolet absorbents may be used alone or in combination of two or more.

[0114] The content of the ultraviolet absorber in the coating material is preferably 0.1 to 40 parts by mass, more preferably 0.5 to 30 parts by mass, based on the total mass (100 parts by mass) of the polycarbonate polyol (A), the acrylic polyol (B), and the crosslinking agent (D). If the content of the ultraviolet absorber is equal to or greater than the lower limit, the weather resistance of the coating film tends to improve. If the content of the ultraviolet absorber is equal to or less than the upper limit, the curability of the coating material, the hardness of the coating film, and the scratch resistance tend to be further improved.

[0115] <<Light stabilizers>> Examples of the light stabilizer include hindered amine light stabilizers. The hindered amine light stabilizer can further improve the weather resistance of the coating film by using it in combination with an ultraviolet absorber.

[0116] Specific examples of the light stabilizer include a condensation product of 1,2,3,4-butanetetracarboxylic acid, 1,2,2,6,6-pentamethyl-4-piperidinol, and β,β,β,β-tetramethyl-3,9-(2,4,8,10-tetraoxaspiro[5,5])undecane)diethanol (trade name "ADEKA STAB (registered trademark, hereinafter the same) LA-63P" manufactured by ADEKA Corporation); ,2,6,6-Pentamethyl-4-piperidinol and β,β,β,β-tetramethyl-3,9-(2,4,8,10-tetraoxaspiro[5,5])undecane)diethanol condensation product (ADEKA CORPORATION trade name "ADEKA STAB LA-68P"), 1,1-dimethylethyl hydroperoxide and octane condensation product, decanedioic acid bis(2,2,6,6-tetramethyl-1-(octyloxy)-4-piperidinol) tert-butyl)-2-[3,5-di(tert-butyl)-4-hydroxybenzyl]malonate bis(1,2,2,6,6-pentamethyl-4-piperidyl) (BASF product name "Tinuvin 144"), 2,4-bis[N-butyl-N-(1-cyclohexyloxy-2,

[0113] 2,6,6-tetramethylpiperidin-4-yl)amino]-6-(2-hydroxyethylamine)-1,3,5-triazine (BASF's trade name "Tinuvin 152"), a mixture of bis(1,2,2,6,6-pentamethylpiperidin-4-yl) sebacate and methyl(1,2,2,6,6-pentamethylpiperidin-4-yl) sebacate (BASF's trade name "Tinuvin 292"), and the like. The light stabilizer may be used alone or in combination of two or more kinds.

[0117] The content of the light stabilizer in the coating material is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 5 parts by mass, based on the total mass (100 parts by mass) of the polycarbonate polyol (A), the acrylic polyol (B), and the crosslinking agent (D). If the content of the light stabilizer is equal to or greater than the lower limit, the weather resistance of the coating film is likely to be improved. If the content of the light stabilizer is equal to or less than the upper limit, the curability of the coating material, the hardness of the coating film, and the scratch resistance are likely to be improved.

[0118] (Surface conditioner) Examples of the surface conditioner (leveling agent) include silicone-based surface conditioners (silicone-based leveling agents), acrylic-based surface conditioners (acrylic-based leveling agents), and fluorine-based surface conditioners (fluorine-based leveling agents). Among these, silicone-based surface conditioners are preferred. Examples of silicone surface conditioners include polyether-modified siloxanes, polyester-modified polymethylalkylsiloxanes, polyether-modified polydimethylsiloxanes, and acrylic group-containing polyether-modified polydimethylsiloxanes. The surface conditioner may be used alone or in combination of two or more kinds.

[0119] (curing accelerating catalyst) The coating material can be cured at room temperature or by heating, and may contain a curing-accelerating catalyst, if necessary, for the purpose of accelerating curing. Cure-accelerating catalysts include, for example, triethylamine, tetra(2-ethylhexyl) titanate, di-n-butyltin dilaurate, and 1,4-diazabicyclo[2.2.2]octane. The curing-accelerating catalyst may be used alone or in combination of two or more kinds.

[0120] <Paint manufacturing method> The coating material of the present invention can also be produced by uniformly mixing the resin composition of the present invention, which contains the polycarbonate polyol (A), the acrylic polyol (B), and a solvent. When mixing, the crosslinker (D) and one or more optional components may be added, if necessary. In addition, if necessary, the coating material may be further diluted with a solvent to a desired solid content concentration. Examples of the solvent used for dilution include the solvents exemplified above in the explanation of the resin composition.

[0121] <Solid content concentration> The solid content of the paint is preferably 30% by mass or more and less than 100% by mass, more preferably 35 to 90% by mass, even more preferably 35 to 80% by mass, and particularly preferably 40 to 70% by mass, based on the total mass of the paint. If the solid content of the paint is equal to or more than the lower limit, sagging during painting can be suppressed and the appearance can be improved. If the solid content of the paint is equal to or less than the upper limit, it is easy to adjust the film thickness in a general painting method such as spray painting. The solids concentration of a paint is the mass ratio of the remainder of the paint after removing the solvent from the paint to the total mass of the paint, and is also called the net concentration. In other words, the sum of the solvent content in the paint and the solids concentration of the paint is 100 mass%.

[0122] <Action and effect> The coating material of the present embodiment described above contains the resin composition of the present invention and the crosslinking agent (D), and therefore can form a coating film that can maintain various performance properties such as chemical resistance, stain resistance, flexibility, and appearance of the coating film, and these performance properties can be well maintained even under conditions of long-term use in exterior building materials, road materials, vehicles including automobiles, aircraft, etc.

[0123] [Cured product] One embodiment of the cured product will now be described. The cured product of this embodiment is a cured product of the resin composition of the present invention or the coating material of the present invention. The coating film formed from the coating material of the present invention is a cured product of the coating material of the present invention, that is, a cured coating film.

[0124] The cured product can be obtained by curing the coating material of the present invention. Specifically, the coating material is applied to a substrate as described below, and then the coating material on the substrate is cured to obtain the cured product. The coating method can be a known method such as brush coating, bar coating, spray coating, dip coating, spin coating, curtain coating, or the like. The temperature for curing the coating material may be appropriately set in consideration of the heat resistance and thermal deformation property of the substrate, and is preferably 20 to 200°C, and more preferably 60 to 150°C, for example. From the viewpoint of shortening the coating time, the time for curing the paint is preferably from several minutes to several hours.

[0125] The cured product is obtained by curing the resin composition of the present invention or the coating material of the present invention, and can maintain various properties such as chemical resistance and appearance.

[0126] [Plastic molded products] Hereinafter, one embodiment of the plastic molded product of the present invention will be described. An example of the plastic molded product of the present embodiment has a substrate and a layer made of the cured product (hereinafter also referred to as a "cured product layer" or a "coating film") laminated on the substrate. The plastic molded product may be a laminate or an injection molded product. Because this results in a good appearance of the cured coating film, the plastic molded article is preferably a molded article painted with the paint of the present invention, and more preferably a laminate in which the surface of a substrate is painted with the paint of the present invention and a cured layer is formed on the substrate. The cured layer is a coating film formed from the coating material of the present invention.

[0127] The shape of the substrate may be, for example, a film, a plate, or a three-dimensional shape. Examples of materials for the substrate include metals such as zinc-plated steel, zinc alloy-plated steel, stainless steel, and tin-plated steel; and resins such as polymethyl methacrylate resin, polycarbonate resin, polyester resin, polystyrene resin, ABS resin, AS resin, polyamide resin, polyarylate resin, polymethacrylimide resin, and polyallyl diglycol carbonate resin. The surface of the substrate on which the cured material layer is to be laminated may be subjected to a primer treatment.

[0128] The laminate can be obtained by applying the coating material of the present invention to the surface of a substrate, and then curing the coating material on the substrate to form a cured layer on the substrate. The coating method and curing conditions for the coating material are the same as those described above in the explanation of the cured product.

[0129] The thickness of the cured layer is preferably 1 to 50 μm. When the thickness of the cured layer is equal to or greater than the lower limit, the effect of the coating material of the present invention is easily obtained. When the thickness of the cured layer is equal to or less than the upper limit, cracks can be reduced.

[0130] The laminate, which is an example of the plastic molded article of this embodiment, may have a plurality of cured material layers. For example, a laminate having two cured material layers can be obtained by applying the coating material (α) of the present invention to the surface of a substrate, curing it to laminate a first cured material layer (α), and then applying the coating material (β) of the present invention, which has a different composition from the coating material (α), to the surface of the first cured material layer (α) opposite the substrate, curing it, and laminating a second cured material layer (β).

[0131] The laminate may further have a coating film other than the cured product layer, i.e., a coating film other than the coating film formed from the coating material of the present invention (hereinafter also referred to as "other coating film"). Hereinafter, the cured product layer and the other coating film are collectively referred to as "multilayer coating film". The cured product layer is suitable as the outermost layer of a multi-layer coating film because it has excellent properties such as scratch resistance and appearance. Therefore, when the laminate has another coating film, it is preferable that the other coating film and the cured product layer are laminated in this order on the substrate.

[0132] Examples of the multilayer coating film include a multilayer coating film consisting of a colored base coating film and a clear coating film, and a multilayer coating film consisting of a first colored base coating film, a second colored base coating film, and a clear coating film. As described above, the cured product layer is suitable for the outermost layer of the multilayer coating film, and the coating material of the present invention is particularly useful as a clear coating material that forms a clear coating film among the coating films of these multilayer coating films. EXAMPLES

[0133] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited thereto. In addition, "parts" and "%" respectively indicate "parts by mass" and "% by mass" unless otherwise specified.

[0134] [evaluation] <Evaluation of storage stability of resin composition> (Evaluation of low temperature stability) The resin composition was left to stand in a thermostatic chamber at -5°C, and after a certain period of time, the appearance of the resin composition and the state of separation were visually observed, and the storage stability of the resin composition at low temperatures was evaluated according to the following evaluation criteria. A to D were considered to be acceptable. A: No change from the initial state even after 4 weeks. B: After 4 weeks, separation, cloudiness, and crystals were observed. C: After 2 weeks, separation, cloudiness, and crystals were observed. D: After one week, separation, cloudiness, and crystals were observed. E: After 24 hours, separation, cloudiness, and crystals were observed.

[0135] (Evaluation of high temperature stability) The resin composition was left to stand in a thermostatic chamber at 50°C, and after a certain period of time, the appearance of the resin composition and the state of separation were visually observed, and the storage stability of the resin composition at high temperatures was evaluated according to the following evaluation criteria. A to D were considered to be acceptable. A: No change from the initial state even after 4 weeks. B: After 4 weeks, separation, cloudiness, crystallization, and yellowing were observed. C: After 2 weeks, separation, cloudiness, crystallization, and yellowing were observed. D: After one week, separation, cloudiness, crystallization, and yellowing were observed. E: After 24 hours, separation, cloudiness, crystallization, and yellowing were observed.

[0136] <Evaluation of the appearance of the coating> The appearance of the coating film was visually observed and evaluated according to the following criteria, with A being acceptable. A: There is no abnormality in the coating. B: Bumps are observed on the coating. C: Whitening or cracks are observed on the coating.

[0137] <Evaluation of haze of coating film> The haze of the coating film was evaluated according to the following criteria by measuring the diffuse transmittance (haze value) using a haze meter (HM-65W, manufactured by Murakami Color Research Laboratory Co., Ltd.) in accordance with JIS K7136:2000. A and B are considered to be acceptable. A: Haze is less than 1%. B: Haze is 1% or more and less than 3%. C: Haze is 3% or more.

[0138] [Polycarbonate polyol (A)] <Production Example 1: Production of Polycarbonate Diol (A-1)> 926.6g of 1,4-butanediol, 696.9g of 1,10-decanediol derived from biomass, 2376.5g of diphenyl carbonate, and 6.6mL of magnesium acetate tetrahydrate aqueous solution (concentration: 8.4g / L, magnesium acetate tetrahydrate: 56mg) were placed in a 5L glass separable flask equipped with a stirrer, a distillate trap, and a pressure regulator, and the mixture was replaced with nitrogen gas to create a nitrogen atmosphere. The internal temperature was raised to 160°C under stirring, and the contents were heated and dissolved. After that, the pressure was lowered to 24kPa over 2 minutes, and the reaction was carried out for 90 minutes while removing phenol from the system. Next, the pressure was lowered to 9.3kPa over 90 minutes, and further lowered to 0.4kPa over 30 minutes to continue the reaction, and the temperature was raised to 170°C and the reaction was carried out for 60 minutes while removing phenol and unreacted dihydroxy compounds from the system, to obtain a polycarbonate diol-containing composition. Thereafter, 2.6 mL of a 0.85 mass % aqueous phosphoric acid solution (22 mg as phosphoric acid) was added to deactivate the magnesium acetate used as the catalyst, thereby obtaining a polycarbonate diol-containing composition. The obtained polycarbonate diol-containing composition was sent to a thin-film distillation apparatus at a flow rate of about 20 g / min, and thin-film distillation (temperature: 170° C., pressure: 53 to 67 Pa) was carried out to obtain polycarbonate diol (A-1). The thin-film distillation apparatus has a diameter of 50 mm, a height of 200 mm, and an area of ​​0.0314 m. 2 The molecular distillation apparatus used was the "MS-300 Special Model" manufactured by Shibata Scientific Co., Ltd., equipped with an internal condenser and a jacket. The polycarbonate diol (A-1) obtained by thin-film distillation had a phenol content of 100 mass ppm or less, and a magnesium content of 100 mass ppm or less. The polycarbonate diol (A-1) had a number average molecular weight (Mn) of 990, a molecular weight distribution (Mw / Mn) of 2.1, and a hydroxyl value of 114 mgKOH / g. The number average molecular weight (Mn) and weight average molecular weight (Mw) were determined by GPC, and the hydroxyl value was determined by a method using an acetylating agent in accordance with JIS K 1557-1.

[0139] <Polycarbonate diols (A-2) to (A-4)> As the polycarbonate diols (A-2) to (A-4), the following compounds were used. A-2: Polycarbonate diol copolymerized with 1,10-decanediol and 1,4-butanediol (manufactured by Mitsubishi Chemical Corporation, product name "BENEBiOL NL1055DB", number average molecular weight 1000, molecular weight distribution (Mw / Mn) 2.0, hydroxyl value 110mgKOH / g) A-3: Polycarbonate diol copolymerized with 1,10-decanediol and 1,4-butanediol (manufactured by Mitsubishi Chemical Corporation, product name "BENEBiOL NL1070DB", number average molecular weight 1000, molecular weight distribution (Mw / Mn) 2.0, hydroxyl value 110mgKOH / g) A-4: Polycarbonate diol polymerized from 1,10-decanediol (manufactured by Mitsubishi Chemical Corporation, product name "BENEBiOL NL1000D", number average molecular weight 1000, molecular weight distribution (Mw / Mn) 2.0, hydroxyl value 110mgKOH / g)

[0140] [Acrylic polyol (B)] <Production Example 2: Production of acrylic polyol-containing material (B-1)> Into a four-neck flask equipped with a stirrer, a thermometer, a cooling tube, and a nitrogen gas inlet, 60 parts of a high-boiling aromatic hydrocarbon solvent S100 (manufactured by Ando Parachemie Co., Ltd., hereinafter abbreviated as "S100") was charged as an initial solvent, and heated under nitrogen gas aeration so that the internal temperature was 140 ° C. After the internal temperature stabilized, a mixture (drop-feed) of 65 parts of isobornyl methacrylate, 10 parts of methyl methacrylate, 24 parts of 2-hydroxyethyl methacrylate, and 1 part of methacrylic acid as monomers, and 5 parts of tert-butylperoxy 2-ethylhexanoate (manufactured by Nippon Oil & Fats Co., Ltd., trade name "Perbutyl (registered trademark) O") as a polymerization initiator was added dropwise over 3 hours. After holding for 1 hour after the end of the drop-feed, 0.4 parts of Perbutyl (registered trademark) O was dissolved in 7 parts of S100 and added. Thereafter, the mixture was kept for 1 hour and then cooled to room temperature to obtain an acrylic polyol-containing material (B-1) containing 60% acrylic polyol. The glass transition temperature (Tg) of the acrylic polyol in the acrylic polyol-containing material (B-1) was calculated from the above formula (4), the SP value was calculated from the above formulas (2-1) to (2-5), the hydroxyl value (OHV) was calculated from the above formula (3), and the weight average molecular weight (Mw) was calculated by the GPC method. The GPC measurement conditions were as described above. These results are shown in Table 1.

[0141] <Production Examples 3 to 11: Production of Acrylic Polyol-Containing Materials (B-2) to (B-11)> Acrylic polyol-containing materials (B-2) to (B-10) containing 60% or 65% of acrylic polyol were produced in the same manner as in Production Example 2, except that the monomers and polymerization initiators shown in Table 1 were used and the polymerization temperature was changed to the temperature shown in Table 1, and various property values ​​were measured. The results are shown in Table 1.

[0142] [Table 1]

[0143] The abbreviations in Table 1 have the following meanings. Note that blank spaces in the table mean that the component is not blended (0 parts blended). IBXMA: Isobornyl methacrylate (manufactured by Mitsubishi Chemical Corporation, product name "Acryester IBX") MMA: Methyl methacrylate (manufactured by Mitsubishi Chemical Corporation, product name "Acryester M") MA: Methyl acrylate (manufactured by Mitsubishi Chemical Corporation, product name "Methyl acrylate") IBMA: Isobutyl methacrylate (manufactured by Mitsubishi Chemical Corporation, product name "Acryester IB") St: Styrene (NS Styrene Monomer Co., Ltd., product name "Styrene Monomer") EHA: 2-Ethylhexyl acrylate (manufactured by Mitsubishi Chemical Corporation, product name "Ethyl acrylate") HEMA: 2-hydroxyethyl methacrylate (manufactured by Mitsubishi Chemical Corporation, product name "Acryester HO") HEA: 2-hydroxyethyl acrylate (Osaka Organic Chemical Industry Co., Ltd., product name "Hydroxyethyl acrylate") Plaxel FM3: Caprolactone addition monomer (manufactured by Daicel Corporation, product name "Plaxel FM3") · MAA: Methacrylic acid (manufactured by Mitsubishi Chemical Corporation, product name "methacrylic acid") AA: Acrylic acid (manufactured by Mitsubishi Chemical Corporation, product name "100% acrylic acid") Luperox DTA: Di-t-amyl peroxide (manufactured by Arkema Yoshitomi Co., Ltd., product name "Luperox DTA") S100: High boiling point aromatic hydrocarbon solvent S100 (manufactured by Ando Parachemie Co., Ltd., product name "High boiling point aromatic solvent S100") ·PMA: Propylene glycol monomethyl ether acetate

[0144] [Example 1] <Preparation of Resin Composition> 25 parts of polycarbonate diol (A-2) as polycarbonate diol (A) and 125 parts of acrylic polyol-containing material (B-1) as acrylic polyol (B) were uniformly mixed, and the solution was diluted with 50 parts of S100 as a solvent to obtain a resin composition. The storage stability of the resulting resin composition at low and high temperatures was evaluated, and the results are shown in Table 2.

[0145] [Examples 2 to 10, Comparative Examples 1 to 9] Resin compositions were prepared in the same manner as in Example 1, except that the amounts of each component were changed to the compositions shown in Tables 2 and 3. The storage stability of the resulting resin compositions at low and high temperatures was evaluated. The results are shown in Tables 2 and 3.

[0146] [Table 2]

[0147] [Table 3]

[0148] The abbreviations in Tables 2 and 3 have the following meanings. A blank in the table means that the component is not blended (0 parts blended). The content of polycarbonate polyol (A) in the solid content is the content (%) of polycarbonate polyol relative to the total mass of the solid content corresponding to the remainder after removing the solvent from the resin composition. The content of acrylic polyol (B) in the solid content is the content (%) of acrylic polyol relative to the total mass of the solid content. (A) / (B) is the mass ratio of polycarbonate polyol (A) to acrylic polyol (B). S100: High boiling point aromatic solvent S100 (manufactured by Ando Parachemie Co., Ltd., product name "High boiling point aromatic solvent S100") ·PMA: Propylene glycol monomethyl ether acetate

[0149] As is clear from Table 2, the resin compositions obtained in the respective Examples had excellent storage stability at both low and high temperatures. On the other hand, as is clear from Table 3, the resin compositions obtained in each Comparative Example did not contain an aromatic hydrocarbon solvent in the solvent, and therefore the compatibility between the polycarbonate polyol (A) and the acrylic polyol (B) was poor, and the resin was prone to separation, crystallization, and yellowing, and the storage stability at low temperatures was poor. In particular, the resin compositions obtained in Comparative Examples 3 to 9 were also poor in storage stability at high temperatures.

[0150] [Example 11] <Paint preparation> 25 parts of polycarbonate diol (A-2) as polycarbonate diol (A), 125 parts of acrylic polyol-containing material (B-1) as acrylic polyol (B), 32.9 parts of polyisocyanate (isocyanurate of hexamethylene diisocyanate, manufactured by Asahi Kasei Corporation, product name "Duranate TPA-100") as crosslinking agent (D), and 0.39 parts of silicone-based leveling agent (manufactured by BYK, product name "BYK-333") as surface conditioner were uniformly mixed, and the solution was diluted with 50 parts of S100 and 10 parts of butyl acetate as solvents to obtain a coating material.

[0151] <Formation of coating film> The obtained paint was applied onto an ABS resin test piece and a glass plate as substrates so that the dry film thickness was 30 to 40 μm, and after pre-drying for 10 minutes at room temperature (25°C), it was dried and cured for 30 minutes in a dryer at 80°C to obtain a laminate in which a coating film (cured layer) made of the cured product of the paint was formed on the substrate. The coating film of the obtained laminate was evaluated for appearance using an ABS resin test piece and for haze using a glass plate. The results are shown in Table 4.

[0152] [Examples 12 to 20, Comparative Examples 10 to 12] A coating material was prepared in the same manner as in Example 1, except that the blending amounts of each component were changed to the compositions shown in Tables 4 and 5. A laminate was produced using the resulting coating material, and the appearance and haze were evaluated. The results are shown in Tables 4 and 5. [Table 4]

[0153] [Table 5]

[0154] The abbreviations in Tables 4 and 5 have the following meanings. A blank in the table means that the component is not blended (0 parts blended). The content of polycarbonate polyol (A) in the solid content is the content (%) of polycarbonate polyol relative to the total mass of the coating film-forming components (i.e., the solid content corresponding to the remainder after removing the solvent from the paint). The content of acrylic polyol (B) in the solid content is the content (%) of acrylic polyol relative to the total mass of the coating film-forming components (solid content). The content of crosslinker (D) in the solid content is the content (%) of crosslinker (D) relative to the total mass of the coating film-forming components (solid content). (A) / (B) is the mass ratio of polycarbonate polyol (A) to acrylic polyol (B). S100: High boiling point aromatic solvent S100 (manufactured by Ando Parachemie Co., Ltd., product name "High boiling point aromatic solvent S100") ·PMA: Propylene glycol monomethyl ether acetate

[0155] As is clear from Table 4, the coating films formed from the paints obtained in each Example had good appearance. On the other hand, as is clear from Table 5, the paints obtained in the comparative examples did not contain aromatic hydrocarbon solvents in the solvent, and therefore the polycarbonate polyol (A) and the acrylic polyol (B) that form the coating film were not compatible with each other during drying, which tended to cause whitening and high haze in the coating film, resulting in poor appearance of the coating film. [Industrial Applicability]

[0156] According to the present invention, it is possible to provide a resin composition, paint, and plastic molded article that can form a coating film with excellent appearance and have good storage stability. Therefore, the resin composition, paint, and plastic molded article of the present invention are useful as compositions for painting exterior building materials, road materials, vehicles including automobiles, aircraft, etc.

Claims

1. A resin composition comprising a polycarbonate polyol (A) made from a polyhydric alcohol, an acrylic polyol (B), and a solvent, The polyhydric alcohol includes an alcohol (1a) represented by the following formula (1a): The resin composition, wherein the solvent comprises an aromatic hydrocarbon solvent (C). HO-R 1 -OH ・・・(1a) (In formula (1a), R 1 represents a substituted or unsubstituted alkylene group having 8 to 20 carbon atoms.

2. The resin composition according to claim 1 , wherein the polyhydric alcohol comprises one or more diols derived from biomass.

3. The resin composition according to claim 1 or 2, wherein the alcohol (1a) comprises 1,10-decanediol.

4. The resin composition according to claim 1 or 2, wherein the polyhydric alcohol comprises 1,10-decanediol and 1,4-butanediol.

5. The resin composition according to claim 1 or 2, wherein the mass ratio (A) / (B) of the polycarbonate polyol (A) to the acrylic polyol (B) is 5 / 95 to 90 / 10.

6. The resin composition according to claim 1 or 2, wherein the acrylic polyol (B) has a glass transition temperature of -50 to 150°C.

7. The resin composition according to claim 1 or 2, wherein the content of the aromatic hydrocarbon solvent (C) is 35 to 100 mass% based on the total mass of the solvent.

8. The resin composition according to claim 1 or 2, wherein the aromatic hydrocarbon solvent (C) comprises at least one of toluene and xylene.

9. A paint comprising the resin composition according to claim 1 or 2.

10. A plastic molded product coated with the paint according to claim 9.

Citation Information

Patent Citations

  • Polyurethane resin coating agent

    JP2006182904A

  • Coating composition

    JP2019137840A

  • Paint composition

    WO2019131617A1

  • Urethane resin composition, adhesive, and synthetic leather

    WO2021084955A1

  • Polycarbonate-modified acrylic resin, paint, and plastic molded article painted by said paint

    WO2020044487A1