Block copolymer and use thereof
A block copolymer of aromatic polyamide and polyether sulfone addresses the solubility issues of aromatic polyether sulfone in electrolytes, enhancing stability and performance in non-aqueous electrolyte secondary batteries.
Patent Information
- Application Number
- JP2023056112
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Aromatic polyether sulfone exhibits high solubility in electrolytes, particularly those containing carbonate, limiting its practicality as a component in non-aqueous electrolyte secondary batteries.
A block copolymer is developed, comprising blocks A and B connected by an amide or ester bond, where block A is primarily aromatic polyamide and block B is primarily aromatic polyether sulfone, with specific structural components and proportions to enhance stability and improve battery characteristics.
The block copolymer demonstrates improved stability in electrolytes and enhances various battery characteristics, such as higher capacity retention and discharge rates, compared to traditional aromatic polyether sulfones.
Smart Images

Figure 2024143434000001 
Figure 2024143434000002 
Figure 2024143434000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a block copolymer and its use. [Background technology]
[0002] Non-aqueous electrolyte secondary batteries such as lithium ion secondary batteries have a high energy density and are therefore widely used as batteries for personal computers, mobile phones, personal digital assistants, etc. Recently, development has also progressed for use as in-vehicle batteries.
[0003] In non-aqueous electrolyte secondary batteries, components containing resin materials, such as separators, are used. Therefore, the resin materials themselves are also the subject of research and development. Among them, aromatic polyethersulfone is one of the resin materials that has attracted attention. Patent Document 1 is an example of a document that discloses the use of aromatic polyethersulfone as a material for secondary battery separators. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent Publication No. 2005-317494 Summary of the Invention [Problem to be solved by the invention]
[0005] However, aromatic polyethersulfone has high solubility in electrolytes (particularly electrolytes containing carbonate), and there is still room for improvement in its practicality as a component for non-aqueous electrolyte secondary batteries.
[0006] An embodiment of the present invention has been made in view of the above, and has an object to provide a novel block copolymer, which can be used, for example, in a porous layer for a non-aqueous electrolyte secondary battery. [Means for solving the problem]
[0007] An embodiment of the present invention includes the following configuration. <1> A block copolymer having a structure in which a block A mainly composed of a unit represented by the following formula (1) and a block B mainly composed of a unit represented by the following formula (2) are linked by an amide bond or an ester bond: -(NH-Ar1-NHCO-Ar2-CO)-...Formula (1) -(Ar3-SO2-Ar4-O)-··· formula (2) In formula (1) and formula (2), Ar1, Ar2, Ar3, and Ar4 each independently represent a divalent group having one or more aromatic rings. Between different units, the structure of each of Ar1, Ar2, Ar3 or Ar4 may be different. <2> At least one of the blocks A has 30 or more units represented by formula (1); <1> The block copolymer according to claim 1. <3> <1> or <2> The block copolymer according to claim 1, A porous layer for a non-aqueous electrolyte secondary battery, further comprising a filler as an optional component. <4> Further comprising a filler, <3> 2. The porous layer for a non-aqueous electrolyte secondary battery according to claim 1 . <5> On one or both sides of the polyolefin porous film, <3> or <4> 2. A laminate separator for a non-aqueous electrolyte secondary battery, comprising the porous layer for a non-aqueous electrolyte secondary battery according to claim 1 laminated thereon. <6> 6. The separator for a non-aqueous electrolyte secondary battery according to claim 5, further comprising an adhesive layer in addition to the porous layer for a non-aqueous electrolyte secondary battery. <7> A positive electrode and <5> or <6> 13. A nonaqueous electrolyte secondary battery member comprising the laminated separator for a nonaqueous electrolyte secondary battery according to claim 12 and a negative electrode arranged in this order. <8> <5> A non-aqueous electrolyte secondary battery comprising the laminated separator for non-aqueous electrolyte secondary batteries according to claim 1. <9> <7> A non-aqueous electrolyte secondary battery comprising the member for a non-aqueous electrolyte secondary battery according to claim 1. <10> <1> or <2> A method for producing the block copolymer according to claim 1, comprising the following step (a): (a) polymerizing a monomer represented by NH2-Ar1-NH2, a monomer represented by XOC-Ar2-COX, and a terminal-modified aromatic polyethersulfone; Where: The terminal-modified aromatic polyethersulfone has a terminal modified with -OH or -NH2, and is mainly composed of a unit represented by formula (2), The two X's contained in the monomer represented by XOC-Ar2-COX above are each independently a hydroxyl group or a halogen. <11> <1> or <2> A method for producing the block copolymer according to claim 1, comprising the following step (b): (b) polymerizing a terminal-modified aromatic polyethersulfone, an aromatic polyamide, and a monomer represented by XOC-Ar2-COX; Where: The terminal-modified aromatic polyethersulfone has a terminal modified with -OH or -NH2, and is mainly composed of a unit represented by formula (2), The aromatic polyamide has a unit represented by the formula (1) as a main component, The two X's contained in the monomer represented by XOC-Ar2-COX above are each independently a hydroxyl group or a halogen. Effect of the Invention
[0008] An object of one embodiment of the present invention is to provide a novel block copolymer, which can be used, for example, in a porous layer for a non-aqueous electrolyte secondary battery. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] [1. Block Copolymers] [Block copolymer structure] A block copolymer according to one embodiment of the present invention has a block A and a block B. The block A mainly contains a unit represented by the following formula (1). The block B mainly contains a unit represented by the following formula (2). -(NH-Ar1-NHCO-Ar2-CO)-...Formula (1) -(Ar3-SO2-Ar4-O)-··· formula (2)
[0010] Block A is an aromatic polyamide block. The ratio of the units represented by formula (1) to all the units contained in block A is preferably 80% or more, more preferably 90% or more, and even more preferably 95% or more. In one embodiment, the entire block A except for the terminals is represented by the units represented by formula (1).
[0011] Block B is an aromatic polyethersulfone block. The ratio of the units represented by formula (2) to all the units contained in block B is preferably 80% or more, more preferably 90% or more, and even more preferably 95% or more. In one embodiment, the entire block B except for the terminals is represented by the units represented by formula (2).
[0012] A block copolymer having a block A and a block B has properties different from those of aromatic polyethersulfone and aromatic polyamide. For example, the block copolymer can have improved stability against an electrolyte compared to aromatic polyethersulfone. In addition, the block copolymer can have various improved battery properties compared to aromatic polyamide.
[0013] Ar1, Ar2, Ar3 and Ar4 are each independently a divalent group having one or more aromatic rings. The block copolymer contains a plurality of units represented by formula (1) and formula (2). In this case, the specific structures of Ar1, Ar2, Ar3 and Ar4 may be different between different units.
[0014] Ar1, Ar2, Ar3 and Ar4 may have an unsubstituted aromatic ring, a substituted aromatic ring, or a combination of an unsubstituted aromatic ring and a substituted aromatic ring. An aromatic ring refers to a cyclic compound that satisfies the Hückel rule. Examples of aromatic rings include benzene, naphthalene, anthracene, azulene, pyrrole, pyridine, furan, and thiophene. In one embodiment of the present invention, the aromatic ring is composed of only carbon atoms and hydrogen atoms. In one embodiment of the present invention, the aromatic ring is a benzene ring or a condensed ring of two or more benzene rings (such as naphthalene and anthracene).
[0015] Examples of the substituent that the aromatic ring may have include an alkyl group, an alkenyl group, an alkynyl group, a cycloalkyl group, a cycloalkenyl group, a cycloalkynyl group, a hydroxyl group, a carboxyl group, a nitro group, an amino group, a halogen group, and a sulfonic acid group. When the substituent has a carbon atom, the number of carbon atoms contained in one substituent may be 1 to 20, 1 to 15, or 1 to 10.
[0016] In one embodiment, Ar1 and Ar2 are benzene rings, and the amide group is located at the para position relative to the benzene ring. In this case, block A is a block mainly composed of poly(paraphenylene terephthalamide). In one embodiment, block A is a block composed of poly(paraphenylene terephthalamide).
[0017] In one embodiment, Ar3 and Ar4 are benzene rings, and the sulfonyl group and the ether group are located at the para position relative to the benzene ring. In this case, block B is a block mainly composed of polyethersulfone. In one embodiment, block B is a block made of polyethersulfone.
[0018] Block A and block B are linked by an amide bond or an ester bond. For example, when a block copolymer is synthesized using an NH2-terminated modified aromatic polyethersulfone, block A and block B are linked by an amide bond. For example, when a block copolymer is synthesized using an OH-terminated modified aromatic polyethersulfone, block A and block B are linked by an ester bond.
[0019] The block configuration of the block copolymer is not particularly limited. In one embodiment, the block copolymer is a diblock copolymer of block A-block B. In one embodiment, the block copolymer is a triblock copolymer of block A-block B-block A or block B-block A-block B. In one embodiment, the block copolymer has four or more blocks (e.g., a tetrablock copolymer of block A-block B-block A-block B).
[0020] The lower limit of the proportion of block A in the entire block copolymer may be 5 mol% or more, 10 mol% or more, 15 mol% or more, 20 mol% or more, or 25 mol% or more. The upper limit of the proportion of block A in the entire block copolymer may be 95 mol% or less, 90 mol% or less, 85 mol% or less, 80 mol% or less, or 75 mol% or less. The lower limit of the proportion of block B in the entire block copolymer may be 5 mol% or more, 10 mol% or more, 15 mol% or more, 20 mol% or more, or 25 mol% or more. The upper limit of the proportion of block B in the entire block copolymer may be 95 mol% or less, 90 mol% or less, 85 mol% or less, 80 mol% or less, or 75 mol% or less. When the proportions of block A and block B are within the above-mentioned ranges, the polymer tends to be suitable for use in a porous layer for a non-aqueous electrolyte secondary battery.
[0021] The lower limit of the ratio of the unit represented by formula (1) to all units of the block copolymer may be 5 mol% or more, 10 mol% or more, 15 mol% or more, 20 mol% or more, or 25 mol% or more. The upper limit of the ratio of the unit represented by formula (1) to all units of the block copolymer may be 95 mol% or less, 90 mol% or less, 85 mol% or less, 80 mol% or less, or 75 mol% or less. The lower limit of the ratio of the unit represented by formula (2) to all units of the block copolymer may be 5 mol% or more, 10 mol% or more, 15 mol% or more, 20 mol% or more, or 25 mol% or more. The upper limit of the ratio of the unit represented by formula (2) to all units of the block copolymer may be 95 mol% or less, 90 mol% or less, 85 mol% or less, 80 mol% or less, or 75 mol% or less. When the proportion of the unit represented by formula (1) and the unit represented by formula (2) is within the above-mentioned range, the polymer tends to be suitable for use in a porous layer for a non-aqueous electrolyte secondary battery.
[0022] The block A has preferably 30 or more units represented by formula (1), more preferably 33 or more units, even more preferably 36 or more units, even more preferably 38 or more units, and particularly preferably 40 or more units. In a preferred embodiment, the block A has preferably 30 or more consecutive units represented by formula (1), more preferably 33 or more consecutive units, even more preferably 36 or more consecutive units, even more preferably 38 or more consecutive units, and particularly preferably 40 or more consecutive units. The upper limit of the number of units represented by formula (1) contained in one block A is, for example, 100 or less, 80 or less, or 60 or less. In one embodiment, at least one of the blocks A contained in the block copolymer is a block A that satisfies the above-mentioned conditions. In one embodiment, all of the blocks A contained in the block copolymer are blocks A that satisfy the above-mentioned conditions. When the block copolymer satisfies the above-mentioned conditions, the block copolymer tends to have excellent coatability when producing a porous layer for a nonaqueous electrolyte secondary battery.
[0023] Block B has preferably 10 or more, more preferably 15 or more, and even more preferably 20 or more units represented by formula (2). In a preferred embodiment, block B has preferably 10 or more consecutive units represented by formula (2), more preferably 15 or more consecutive units, and even more preferably 20 or more consecutive units. The upper limit of the number of units represented by formula (2) contained in one block B is, for example, 100 or less, 80 or less, or 60 or less. In one embodiment, at least one of the blocks B contained in the block copolymer is a block B that satisfies the above-mentioned conditions. In one embodiment, all of the blocks B contained in the block copolymer are blocks B that satisfy the above-mentioned conditions.
[0024] [Method of manufacturing block copolymer] The above-mentioned block copolymer can be produced by Production Method 1 or Production Method 2 described below. However, the method for producing the block copolymer is not limited to Production Method 1 or Production Method 2. Those skilled in the art of polymer science can produce the block copolymer by various methods with reference to the description in this specification and common technical knowledge.
[0025] (Manufacturing method 1) In the production method 1, a terminal-modified aromatic polyethersulfone and a monomer serving as a raw material for an aromatic polyamide are polymerized. Specifically, the production method 1 includes step (a): polymerizing a monomer represented by NH2-Ar1-NH2, a monomer represented by XOC-Ar2-COX, and a terminal-modified aromatic polyethersulfone.
[0026] In step (a), the terminally modified aromatic polyethersulfone has a terminal modified to -OH or -NH2, and is mainly composed of a unit represented by formula (2). The terminally modified aromatic polyethersulfone can be synthesized by known techniques (see, for example, WO 2021 / 261391). Alternatively, commercially available terminally modified aromatic polyethersulfone may be used. The terminally modified aromatic polyethersulfone can be block B in a block copolymer. In one embodiment, the main chain of the terminally modified aromatic polyethersulfone is mainly composed of polyethersulfone.
[0027] In step (a), the two X's contained in the monomer represented by XOC-Ar2-COX are each independently a hydroxyl group or a halogen. A halogen is fluorine, chlorine, bromine, iodine or a combination thereof.
[0028] In step (a), the monomer represented by NH2-Ar1-NH2 and the monomer represented by XOC-Ar2-COX can both be block A in the block copolymer. Thus, Ar1 and Ar2 follow the above definitions. In one embodiment, the monomer represented by NH2-Ar1-NH2 is paraphenylenediamine. In one embodiment, the monomer represented by XOC-Ar2-COX is terephthalic acid dichloride.
[0029] The polymerization conditions in step (a) can be appropriately determined by those skilled in the art depending on the raw materials used and the structure of the block copolymer to be obtained.
[0030] Production method 1 is suitable for producing a block copolymer having a relatively short block A. A relatively short block A is, for example, a block A containing 26 or less units represented by formula (1).
[0031] (Manufacturing method 2) In the production method 2, a terminal-modified aromatic polyethersulfone and an aromatic polyamide are linked together. Specifically, the production method 2 includes step (b): polymerizing a terminal-modified aromatic polyethersulfone, an aromatic polyamide, and a monomer represented by XOC-Ar2-COX.
[0032] In step (b), the terminal-modified aromatic polyethersulfone has terminals modified to -OH or -NH2 and mainly comprises a unit represented by formula (2). The terminal-modified aromatic polyethersulfone is as described in relation to Production Method 1.
[0033] In step (b), the aromatic polyamide is based on the unit represented by formula (1). The aromatic polyamide can be synthesized by known techniques. Alternatively, a commercially available aromatic polyamide product can be used. The aromatic polyamide can be block A in a block copolymer. In one embodiment, the main chain of the aromatic polyamide is based on poly(paraphenylene terephthalamide).
[0034] In step (b), the monomer represented by XOC-Ar2-COX is as described in relation to Production Method 1. Regardless of whether the terminals of the terminal-modified aromatic polyethersulfone are modified to -OH or -NH2, the monomer represented by XOC-Ar2-COX is added to the polymerization system.
[0035] The polymerization conditions in step (b) can be appropriately determined by those skilled in the art depending on the raw materials used and the structure of the block copolymer to be obtained.
[0036] Production method 2 is suitable for producing a block copolymer having a relatively long block A. A relatively long block A is, for example, a block A containing 27 or more units represented by formula (1).
[0037] [2. Porous layer for non-aqueous electrolyte secondary batteries] A porous layer for a non-aqueous electrolyte secondary battery according to one embodiment of the present invention contains the above-mentioned block copolymer.
[0038] In this specification, the porous layer for a nonaqueous electrolyte secondary battery may be abbreviated simply as a "porous layer." Also, in this specification, the laminate separator for a nonaqueous electrolyte secondary battery may be abbreviated simply as a "laminated separator."
[0039] [Filler] The porous layer may contain a filler, which may be an organic filler or an inorganic filler.
[0040] Examples of organic fillers include styrene, vinyl ketone, acrylonitrile, methyl methacrylate, ethyl methacrylate, glycidyl methacrylate, glycidyl acrylate, methyl acrylate, and the like, alone or in copolymers of two or more kinds; fluororesins such as polytetrafluoroethylene, tetrafluoroethylene-hexafluoropropylene copolymer, tetrafluoroethylene-ethylene copolymer, and polyvinylidene fluoride; melamine resin; urea resin; polyolefin; and polymethacrylate. The organic fillers may be used alone or in combination of two or more kinds. Among these organic fillers, polytetrafluoroethylene powder is preferred in terms of chemical stability.
[0041] Examples of inorganic fillers include materials made of inorganic substances such as metal oxides, metal nitrides, metal carbides, metal hydroxides, carbonates, and sulfates. Specific examples include powders of aluminum oxide (such as alumina), boehmite, silica, titania, magnesia, barium titanate, aluminum hydroxide, and calcium carbonate; as well as minerals such as mica, zeolite, kaolin, and talc. The inorganic fillers may be used alone or in combination of two or more. Among these inorganic fillers, aluminum oxide is preferred in terms of chemical stability.
[0042] The shape of the filler may be, for example, approximately spherical, plate-like, columnar, needle-like, whisker-like, fibrous, etc., and any of these particles may be used. Approximately spherical particles are preferred because they are more likely to form uniform pores.
[0043] The average particle size of the filler contained in the porous layer is preferably 0.01 to 1 μm. In this specification, the "average particle size of the filler" refers to the volume-based average particle size (D50) of the filler. D50 refers to the particle size at which the cumulative distribution based on the volume is 50%. D50 can be measured, for example, using a laser diffraction particle size distribution analyzer (manufactured by Shimadzu Corporation, product names: SALD2200, SALD2300, etc.).
[0044] The filler content in the porous layer is preferably 20 to 90% by weight, and more preferably 40 to 80% by weight, based on 100% by weight of the porous layer. If the filler content is within the above range, a porous layer having sufficient ion permeability can be obtained.
[0045] [Other ingredients] The porous layer may contain components other than the block copolymer and the filler, for example, a resin other than the block copolymer.
[0046] Examples of such resins include polyolefins; (meth)acrylate resins; fluorine-containing resins; polyamide resins; polyimide resins; polyamideimide resins; polyester resins; rubbers; resins having a melting point or glass transition temperature of 180°C or higher; water-soluble polymers; polycarbonate, polyacetal, polyether ether ketone, and the like.
[0047] Of the above-mentioned resins, (meth)acrylate resins, fluorine-containing resins, polyamide resins, polyimide resins, polyamideimide, polyester resins and water-soluble polymers are preferred.
[0048] As the polyolefin, polyethylene, polypropylene, polybutene, ethylene-propylene copolymer, and the like are preferable.
[0049] Examples of fluorine-containing resins include polyvinylidene fluoride (PVDF), polytetrafluoroethylene, vinylidene fluoride-hexafluoropropylene copolymer, tetrafluoroethylene-hexafluoropropylene copolymer, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, vinylidene fluoride-tetrafluoroethylene copolymer, vinylidene fluoride-trifluoroethylene copolymer, vinylidene fluoride-trichloroethylene copolymer, vinylidene fluoride-vinyl fluoride copolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene copolymer, and ethylene-tetrafluoroethylene copolymer, as well as fluorine-containing rubbers having a glass transition temperature of 23° C. or lower among the above-mentioned fluorine-containing resins.
[0050] As the polyamide-based resin, aramid resins such as aromatic polyamides and wholly aromatic polyamides are preferred.
[0051] Specific examples of the aramid resin include poly(paraphenylene terephthalamide), poly(metaphenylene isophthalamide), poly(parabenzamide), poly(metabenzamide), poly(4,4'-benzanilide terephthalamide), poly(paraphenylene-4,4'-biphenylene dicarboxylic acid amide), poly(metaphenylene-4,4'-biphenylene dicarboxylic acid amide), poly(paraphenylene-2,6-naphthalene dicarboxylic acid amide), poly(metaphenylene-2,6-naphthalene dicarboxylic acid amide), poly(2-chloroparaphenylene terephthalamide), paraphenylene terephthalamide / 2,6-dichloroparaphenylene terephthalamide copolymer, metaphenylene terephthalamide / 2,6-dichloroparaphenylene terephthalamide copolymer, etc. Among these, poly(paraphenylene terephthalamide) is more preferable.
[0052] As the polyester-based resin, aromatic polyesters such as polyarylates and liquid crystal polyesters are preferred.
[0053] Examples of rubbers include styrene-butadiene copolymers and hydrogenated products thereof, methacrylate copolymers, acrylonitrile-acrylate copolymers, styrene-acrylate copolymers, ethylene propylene rubber, and polyvinyl acetate.
[0054] Examples of resins having a melting point or glass transition temperature of 180° C. or higher include polyphenylene ether, polysulfone, polyethersulfone, polyphenylene sulfide, polyetherimide, polyamideimide, and polyetheramide.
[0055] Examples of the water-soluble polymer include polyvinyl alcohol, polyethylene glycol, cellulose ether, sodium alginate, polyacrylic acid, polyacrylamide, and polymethacrylic acid.
[0056] The resin used in the porous layer may be of one type alone or of two or more types in combination.
[0057] [3. Laminated separator for non-aqueous electrolyte secondary batteries] One aspect of the present invention is a laminate separator for a non-aqueous electrolyte secondary battery, in which the above-mentioned porous layer is laminated on one or both sides of a polyolefin porous film.
[0058] [Polyolefin porous film] The laminated separator for a non-aqueous electrolyte secondary battery according to one embodiment of the present invention includes a polyolefin porous film. The polyolefin porous film has many interconnected pores inside, allowing gas and liquid to pass from one side to the other side. The polyolefin porous film can be a substrate for the laminated separator for a non-aqueous electrolyte secondary battery. The polyolefin porous film can be melted when the battery generates heat, rendering the laminated separator for a non-aqueous electrolyte secondary battery non-porous, thereby imparting a shutdown function to the laminated separator for a non-aqueous electrolyte secondary battery.
[0059] Here, the term "polyolefin porous film" refers to a porous film mainly composed of polyolefin resin. Also, "mainly composed of polyolefin resin" means that the proportion of polyolefin resin in the porous film is 50% by volume or more, preferably 90% by volume or more, and more preferably 95% by volume or more of the total material constituting the porous film.
[0060] The polyolefin resin, which is the main component of the polyolefin porous film, is not particularly limited, and examples thereof include homopolymers and copolymers obtained by polymerizing monomers such as ethylene, propylene, 1-butene, 4-methyl-1-pentene, and / or 1-hexene, which are thermoplastic resins. That is, examples of homopolymers include polyethylene, polypropylene, and polybutene, and examples of copolymers include ethylene-propylene copolymers. The polyolefin porous film may be a layer containing these polyolefin resins alone, or a layer containing two or more of these polyolefin resins. Among these, polyethylene is more preferable because it can prevent (shut down) the flow of excessive current at a lower temperature, and in particular, polyethylene with a high molecular weight mainly composed of ethylene is preferable. The polyolefin porous film may contain components other than polyolefins as long as the function is not impaired.
[0061] Examples of polyethylene include low-density polyethylene, high-density polyethylene, linear polyethylene (ethylene-α-olefin copolymer), and ultra-high molecular weight polyethylene. Among these, ultra-high molecular weight polyethylene is more preferred, and has a weight average molecular weight of 5×10 5 ~15×10 6 It is more preferable that the polyolefin resin contains a high molecular weight component having a weight average molecular weight of 1,000,000 or more. In particular, it is more preferable that the polyolefin resin contains a high molecular weight component having a weight average molecular weight of 1,000,000 or more, since the strength of the polyolefin porous film and the laminate separator for non-aqueous electrolyte secondary batteries is improved.
[0062] The thickness of the polyolefin porous film is preferably 5 to 20 μm, more preferably 7 to 15 μm, and even more preferably 9 to 15 μm. If the thickness is 5 μm or more, the functions required of the polyolefin porous film (such as a shutdown function) can be sufficiently obtained. If the thickness is 20 μm or less, a thin laminate separator for a nonaqueous electrolyte secondary battery can be obtained.
[0063] The pore size of the pores in the polyolefin porous film is preferably 0.1 μm or less, and more preferably 0.06 μm or less, which allows sufficient ion permeability to be obtained and further prevents particles constituting the electrode from entering the film.
[0064] The weight per unit area of the polyolefin porous film is usually 4 to 20 g / m2 so as to increase the gravimetric energy density and volumetric energy density of the battery. 2 is preferably 5 to 12 g / m 2 It is more preferable that:
[0065] The polyolefin porous film preferably has an air permeability of 30 to 500 s / 100 mL, more preferably 50 to 300 s / 100 mL, in Gurley value, which allows the laminated separator for non-aqueous electrolyte secondary batteries to have sufficient ion permeability.
[0066] The porosity of the polyolefin porous film is preferably 20 to 80% by volume, and more preferably 30 to 75% by volume, which increases the amount of electrolyte retained and reliably prevents (shuts down) the flow of excessive current at a lower temperature.
[0067] The method for producing the polyolefin porous film can be a known method and is not particularly limited. For example, as described in Japanese Patent No. 5476844, a method in which a filler is added to a thermoplastic resin, a film is formed, and then the filler is removed can be mentioned.
[0068] Specifically, for example, when the polyolefin porous film is formed from a polyolefin resin containing ultra-high molecular weight polyethylene and a low molecular weight polyolefin having a weight average molecular weight of 10,000 or less, from the viewpoint of production costs, it is preferable to produce it by a method including the following steps (1) to (4).
[0069] (1) A process for obtaining a polyolefin-based resin composition by kneading 100 parts by weight of ultra-high molecular weight polyethylene, 5 to 200 parts by weight of a low molecular weight polyolefin having a weight average molecular weight of 10,000 or less, and 100 to 400 parts by weight of an inorganic filler such as calcium carbonate; (2) forming a sheet from the polyolefin resin composition; (3) removing the inorganic filler from the sheet obtained in step (2); (4) A step of stretching the sheet obtained in the step (3). In addition, the methods described in the above-mentioned patent documents may be used.
[0070] Moreover, as the polyolefin porous film, a commercially available product having the above-mentioned characteristics may be used.
[0071] [Physical properties of laminated separators for non-aqueous electrolyte secondary batteries] The laminate separator has an air permeability of preferably 500s / 100mL or less, more preferably 300s / 100mL or less, in Gurley value. The porous layer in the laminate separator has an air permeability of preferably 400s / 100mL or less, more preferably 200s / 100mL or less, in Gurley value. If the air permeability is in the above range, it can be said to have sufficient ion permeability.
[0072] The air permeability of the porous layer is calculated by YX, where X is the air permeability of the polyolefin porous film and Y is the air permeability of the laminated separator. The air permeability of the porous layer can be adjusted, for example, by the intrinsic viscosity of the resin and the basis weight of the porous layer. In general, when the intrinsic viscosity of the resin is small, the Gurley value tends to be small. Also, when the basis weight of the porous layer is small, the Gurley value tends to be small.
[0073] The thickness of the porous layer provided in the laminate separator is preferably 10 μm or less, more preferably 7 μm or less, and even more preferably 5 μm or less.
[0074] The separator according to an embodiment of the present invention may include another porous layer other than the porous film and the porous layer, if necessary, within a range that does not impair the object of the present invention. Examples of the other porous layer include known porous layers such as a heat-resistant layer, an adhesive layer, and a protective layer.
[0075] The other porous layer may be provided on one or both sides of the laminate separator. When the laminate separator has an insulating porous layer on both sides of a porous film, the other porous layer may be provided on the insulating porous layer on both sides, or on the insulating porous layer on one side. When the laminate separator has an insulating porous layer on only one side of a porous film, the other porous layer may be provided on the insulating porous layer, or on the side of the porous film where the insulating porous layer is not provided. It can also be said that the other porous layer may be provided on the outermost layer of the laminate separator.
[0076] For example, the laminated separator further includes an adhesive layer in addition to the insulating porous layer. In this specification, the adhesive layer means a porous layer having adhesive properties. The adhesive layer may be provided on the surface of the laminated separator that contacts the electrode.
[0077] [Method for manufacturing laminated separator for non-aqueous electrolyte secondary battery] The porous layer can be formed by using a coating liquid in which the block copolymer, the filler, and optionally other components are dissolved or dispersed in a solvent. Methods for forming the coating liquid include, for example, mechanical stirring, ultrasonic dispersion, high pressure dispersion, and media dispersion. For example, N-methylpyrrolidone, N,N-dimethylacetamide, and N,N-dimethylformamide can be used as the solvent.
[0078] An example of a method for forming the porous layer is a method in which the above-mentioned coating liquid is prepared, the coating liquid is applied to a polyolefin porous film, and the film is dried to form a porous layer.
[0079] The coating liquid can be applied to the polyolefin porous film by a known coating method such as a knife, blade, bar, gravure, or die coating method.
[0080] The method of removing the solvent (dispersion medium) is generally by drying. Examples of drying methods include natural drying, air drying, heat drying, and reduced pressure drying, but any method may be used as long as the solvent (dispersion medium) can be sufficiently removed. In addition, the solvent (dispersion medium) contained in the paint may be replaced with another solvent before drying. A specific example of a method of replacing the solvent (dispersion medium) with another solvent and then removing it is to replace it with a poor solvent with a low boiling point such as water, alcohol, or acetone, precipitate it, and then dry it.
[0081] 4. Non-aqueous electrolyte secondary battery components and non-aqueous electrolyte secondary batteries A nonaqueous electrolyte secondary battery member according to one embodiment of the present invention comprises a positive electrode, the above-mentioned laminated separator for nonaqueous electrolyte secondary batteries, and a negative electrode arranged in this order. A nonaqueous electrolyte secondary battery according to one embodiment of the present invention includes the above-mentioned laminated separator for nonaqueous electrolyte secondary batteries. The nonaqueous electrolyte secondary battery generally has a structure in which a negative electrode and a positive electrode face each other via the above-mentioned laminated separator for nonaqueous electrolyte secondary batteries. In the nonaqueous electrolyte secondary battery, a battery element in which the structure is impregnated with an electrolyte is enclosed in an exterior material. For example, the nonaqueous electrolyte secondary battery is a lithium ion secondary battery that obtains electromotive force by doping and dedoping lithium ions.
[0082] [Positive electrode] As the positive electrode, for example, a positive electrode sheet having a structure in which an active material layer containing a positive electrode active material and a binder is formed on a current collector can be used. The active material layer may further contain a conductive agent.
[0083] The positive electrode active material may be, for example, a material capable of doping / dedoping lithium ions.
[0084] Examples of the material include lithium composite oxides containing at least one transition metal such as V, Ti, Cr, Mn, Fe, Co, Ni, and Cu. Examples of the lithium composite oxide include lithium composite oxides having a layered structure, lithium composite oxides having a spinel structure, and solid solution lithium-containing transition metal oxides made of lithium composite oxides having both a layered structure and a spinel structure. Other examples include lithium cobalt composite oxides and lithium nickel composite oxides. Furthermore, examples of the lithium composite oxides in which a part of the transition metal atoms that are the main components of these lithium composite oxides are replaced with other elements such as Na, K, B, F, Al, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Mg, Ca, Ga, Zr, Si, Nb, Mo, Sn, and W are also included.
[0085] Examples of the lithium composite oxide in which a part of the transition metal atoms constituting the main part of the lithium composite oxide are substituted with other elements include a lithium cobalt composite oxide having a layered structure represented by the following formula (3), a lithium nickel composite oxide represented by the following formula (4), a lithium manganese composite oxide having a spinel structure represented by the following formula (5), and a solid solution lithium-containing transition metal oxide represented by the following formula (6).
[0086] Li[Lix(Co 1-a M 1 a ) 1-x ]O2···(3) (In formula (3), M1 is at least one metal selected from the group consisting of Na, K, B, F, Al, Ti, V, Cr, Mn, Fe, Ni, Cu, Zn, Mg, Ga, Zr, Si, Nb, Mo, Sn, and W, and satisfies -0.1≦x≦0.30 and 0≦a≦0.5.)
[0087] Li[Liy(Ni 1-b M 2 b )1-y]O2···(4) (In the formula (4), M2 is at least one metal selected from the group consisting of Na, K, B, F, Al, Ti, V, Cr, Mn, Fe, Co, Cu, Zn, Mg, Ga, Zr, Si, Nb, Mo, Sn, and W, and satisfies -0.1≦y≦0.30 and 0≦b≦0.5.)
[0088] LizMn 2-c M 3 c O4···(5) (In formula (5), M 3 is at least one metal selected from the group consisting of Na, K, B, F, Al, Ti, V, Cr, Fe, Co, Ni, Cu, Zn, Mg, Ga, Zr, Si, Nb, Mo, Sn, and W, and satisfies 0.9≦z, 0≦c≦1.5.
[0089] Li 1+w M 4 d M 5 e O2···(6) (In formula (6), M 4 and M 5 are at least one metal selected from the group consisting of Al, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Mg, and Ca, and satisfy 0 < w ≦ 1 / 3, 0 ≦ d ≦ 2 / 3, 0 ≦ e ≦ 2 / 3, and w + d + e = 1.)
[0090] Specific examples of the lithium composite oxide represented by the above formulas (3) to (6) include LiCoO2, LiNiO2, LiMnO2, LiNi 0.8 Co 0.2 O2, LiNi 0.5 Mn 0.5 O2, LiNi 0.85 Co 0.10 Al 0.05 O2, LiNi 0.8 Co 0.15 Al 0.05 O2, LiNi 0.5 Co 0.2 Mn 0.3 O2, LiNi 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.33 Co 0.33 Mn 0.33 O2, LiMn2O4, LiMn 1.5 Ni 0.5 O4, LiMn 1.5 Fe 0.5 O4, LiCoMnO4, Li 1.21 Ni 0.20 Mn 0.59 O2, Li 1.22 Ni 0.20 Mn 0.58 O2, Li 1.22 Ni 0.15 Co 0.10 Mn 0.53 O2, Li 1.07 N i0.35 Co 0.08 Mn 0.50 O2, Li 1.07 Ni 0.36 Co 0.08 Mn 0.49 O2, etc. can be mentioned.)
[0091] In addition, lithium composite oxides other than the lithium composite oxides represented by the above formulas (3) to (6) can also be preferably used as the positive electrode active material. Examples of such lithium composite oxides include LiNiVO4, LiV3O6, Li 1.2 Fe 0.4 Mn 0.4 O2, etc.
[0092] Examples of materials other than lithium composite oxides that can be preferably used as the positive electrode active material include phosphates having an olivine structure, such as phosphates having an olivine structure represented by the following formula (7).
[0093] Liv(M 6 f M 7 g M 8 h M 9 i ) j PO4 ···(7) (In the formula (7), M6 is Mn, Co, or Ni; M 7 is Ti, V, Cr, Mn, Fe, Co, Ni, Zr, Nb, or Mo, and M 8 is a transition metal or main group element, optionally excluding elements of groups VIA and VIIA, and M 9 is a transition metal or a typical group element, optionally excluding the elements of groups VIA and VIIA, and satisfies 1.2 ≧ a ≧ 0.9, 1 ≧ b ≧ 0.6, 0.4 ≧ c ≧ 0, 0.2 ≧ d ≧ 0, 0.2 ≧ e ≧ 0, 1.2 ≧ f ≧ 0.9.
[0094] The positive electrode active material preferably has a coating layer on the surface of the lithium metal composite oxide particles constituting the positive electrode active material. Examples of materials constituting the coating layer include metal composite oxides, metal salts, boron-containing compounds, nitrogen-containing compounds, silicon-containing compounds, and sulfur-containing compounds, and among these, metal composite oxides are preferably used.
[0095] As the metal composite oxide, an oxide having lithium ion conductivity is preferably used. For example, a metal composite oxide of Li and at least one element selected from the group consisting of Nb, Ge, Si, P, Al, W, Ta, Ti, S, Zr, Zn, V and B can be mentioned. When the positive electrode active material has a coating layer, the coating layer suppresses side reactions at the interface between the positive electrode active material and the electrolyte under high voltage, and the obtained secondary battery can have a long life. In addition, the formation of a high resistance layer at the interface between the positive electrode active material and the electrolyte can be suppressed, and the obtained secondary battery can have a high output.
[0096] Examples of the conductive agent include carbonaceous materials such as natural graphite, artificial graphite, cokes, carbon black, pyrolytic carbons, carbon fibers, and baked organic polymer compounds.
[0097] Examples of the binder include polyvinylidene fluoride, vinylidene fluoride copolymer, polytetrafluoroethylene, vinylidene fluoride-hexafluoropropylene copolymer, tetrafluoroethylene-hexafluoropropylene copolymer, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, ethylene-tetrafluoroethylene copolymer, vinylidene fluoride-tetrafluoroethylene copolymer, vinylidene fluoride-trifluoroethylene copolymer, vinylidene fluoride-trichloroethylene copolymer, vinylidene fluoride-vinyl fluoride copolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene copolymer, thermoplastic polyimide, polyethylene, and thermoplastic resin such as polypropylene, acrylic resin, and styrene butadiene rubber. The binder also functions as a thickener.
[0098] Examples of the positive electrode current collector include conductors such as Al, Ni, stainless steel, etc. Among them, Al is more preferable because it is easy to process into a thin film and is inexpensive.
[0099] Examples of methods for producing a sheet-like positive electrode include a method in which a positive electrode active material, a conductive agent, and a binder that constitute a positive electrode mixture are pressure-molded on a positive electrode current collector; a method in which a positive electrode active material, a conductive agent, and a binder are made into a paste using an appropriate organic solvent to obtain a positive electrode mixture, and then the positive electrode mixture is applied to a positive electrode current collector and dried to obtain a sheet-like positive electrode mixture, which is then pressed to be fixed to the positive electrode current collector.
[0100] [Negative electrode] As the negative electrode, for example, a negative electrode sheet having a structure in which an active material layer containing a negative electrode active material and a binder is formed on a current collector can be used. The active material layer may further contain a conductive agent.
[0101] Examples of the negative electrode active material include carbon materials, chalcogen compounds (oxides, sulfides, etc.), nitrides, metals, and alloys that can be doped and dedoped with lithium ions at a lower potential than the positive electrode.
[0102] Examples of carbon materials that can be used as the negative electrode active material include graphite such as natural graphite and artificial graphite, cokes, carbon black, pyrolytic carbons, carbon fiber, and fired organic polymer compounds.
[0103] Examples of oxides that can be used as the negative electrode active material include oxides represented by the formula SiO x (where x is a positive real number); TiO2, TiO, etc., are oxides of silicon represented by the formula TiO x (where x is a positive real number); oxide of titanium represented by the formula V, such as V2O5 or VO2 x O y (where x and y are positive real numbers); oxides of vanadium with the formula Fe, such as Fe3O4, Fe2O3, and FeO x O y (where x and y are positive real numbers); oxide of iron, such as SnO2, SnO, etc., with the formula SnO x (where x is a positive real number); WO3, WO2, etc., are oxides of tin represented by the general formula WO xTungsten oxide represented by (where x is a positive real number); composite metal oxides containing lithium and titanium or vanadium such as Li4Ti5O 12 and LiVO2; and the like can be mentioned.
[0104] Examples of sulfides that can be used as the negative electrode active material include titanium sulfides represented by the formula Ti x Sy (where x and y are positive real numbers); vanadium sulfides represented by the formula VS x (where x is a positive real number); iron sulfides represented by the formula FexSy (where x and y are positive real numbers) such as Fe3S4, FeS2, and FeS; molybdenum sulfides represented by the formula Mo x S y (where x and y are positive real numbers); tin sulfides represented by the formula SnS x (where x is a positive real number); tungsten sulfides represented by the formula WS x (where x is a positive real number); antimony sulfides represented by the formula Sb x S y (where x and y are positive real numbers); selenium sulfides represented by the formula Se x S y (where x and y are positive real numbers); and the like can be mentioned.
[0105] Examples of nitrides that can be used as the negative electrode active material include Li3N, Li 3-x A x N (where A is either one or both of Ni and Co, and 0 < x < 3). Lithium-containing nitrides such as these can be mentioned.
[0106] These carbon materials, oxides, sulfides, and nitrides may be used alone or in combination of two or more. Also, these carbon materials, oxides, sulfides, and nitrides may be either crystalline or amorphous. These carbon materials, oxides, sulfides, and nitrides are mainly supported on the negative electrode current collector and used as an electrode.
[0107] Examples of metals that can be used as the negative electrode active material include lithium metal, silicon metal, and tin metal.
[0108] Also, there is a composite material containing Si or Sn as the first constituent element, as well as the second and third constituent elements. The second constituent element is, for example, at least one of cobalt, iron, magnesium, titanium, vanadium, chromium, manganese, nickel, copper, zinc, gallium, and zirconium. The third constituent element is, for example, at least one of boron, carbon, aluminum, and phosphorus.
[0109] In particular, the metal material is preferably silicon or tin (which may contain a trace amount of impurities), SiO v (0 <v≦2)、SnO w (0≦w≦2), Si—Co—C composite material, Si—Ni—C composite material, Sn—Co—C composite material, and Sn—Ni—C composite material are preferred.
[0110] Examples of the negative electrode current collector include Cu, Ni, stainless steel, etc. Among them, Cu is more preferable, particularly in lithium ion secondary batteries, because it is difficult to form an alloy with lithium and it is easy to process into a thin film.
[0111] Examples of the method for producing a sheet-shaped negative electrode include a method of pressurizing a negative electrode active material to be a negative electrode mixture on a negative electrode current collector, a method of making a negative electrode active material into a paste using an appropriate organic solvent to obtain a negative electrode mixture, applying the negative electrode mixture to a negative electrode current collector, drying the mixture, and pressing the sheet-shaped negative electrode mixture obtained to fix it to the negative electrode current collector, etc. The paste preferably contains the conductive agent and the binder.
[0112] [Nonaqueous electrolyte] The non-aqueous electrolyte may be, for example, a non-aqueous electrolyte obtained by dissolving a lithium salt in an organic solvent. Examples of the lithium salt include LiClO4, LiPF6, LiAsF6, LiSbF6, LiBF4, LiSO3F, LiCF3SO3, LiN(SO2CF3)2, LiN(SO2C2F5)2, LiN(SO2CF3)(COCF3), Li(C4F9SO3), LiC(SO2CF3)3, Li2B 10 Cl 10 , LiBOB (here, BOB stands for bis(oxalato)borate), lithium salts of lower aliphatic carboxylates, LiAlCl4, etc. These may be used alone or as a mixture of two or more. Among them, as the lithium salt, it is preferable to use at least one selected from the group consisting of fluorine-containing LiPF6, LiAsF6, LiSbF6, LiBF4, LiSO3F, LiCF3SO3, LiN(SO2CF3)2, and LiC(SO2CF3)3.
[0113] Examples of the organic solvent include carbonates such as propylene carbonate, ethylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, 4-trifluoromethyl-1,3-dioxolan-2-one, and 1,2-di(methoxycarbonyloxy)ethane; 1,2-dimethoxyethane, 1,3-dimethoxypropane, pentafluoropropyl methyl ether, 2,2,3,3-tetrafluoropropyl difluoromethyl ether, tetrahydrofuran, and 2-methyltetrahydrofuran. ethers; esters such as methyl formate, methyl acetate, and γ-butyrolactone; nitriles such as acetonitrile and butyronitrile; amides such as N,N-dimethylformamide and N,N-dimethylacetamide; carbamates such as 3-methyl-2-oxazolidone; sulfur-containing compounds such as sulfolane, dimethyl sulfoxide, and 1,3-propane sultone; or organic solvents such as these with a fluoro group further introduced therein (organic solvents in which one or more hydrogen atoms have been replaced with fluorine atoms).
[0114] The organic solvent is preferably used as a mixed solvent by mixing two or more kinds. Among them, a mixed solvent containing carbonates is preferable, and a mixed solvent of a cyclic carbonate and an acyclic carbonate and a mixed solvent of a cyclic carbonate and an ether are more preferable. As a mixed solvent of a cyclic carbonate and an acyclic carbonate, a mixed solvent containing ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate is preferable. A nonaqueous electrolyte using such a mixed solvent has an advantage that it has a wide operating temperature range, is not easily deteriorated even when used at a high voltage, is not easily deteriorated even when used for a long time, and is difficult to decompose even when a graphite material such as natural graphite or artificial graphite is used as the active material of the negative electrode.
[0115] In addition, it is preferable to use a nonaqueous electrolyte solution containing a fluorine-containing lithium salt such as LiPF6 and an organic solvent having a fluorine substituent, since this increases the safety of the resulting nonaqueous electrolyte secondary battery. A mixed solvent containing an ether having a fluorine substituent, such as pentafluoropropyl methyl ether or 2,2,3,3-tetrafluoropropyl difluoromethyl ether, and dimethyl carbonate is more preferable, since it has a high capacity retention rate even when discharged at a high voltage.
[0116] [Members for non-aqueous electrolyte secondary batteries and methods for producing non-aqueous electrolyte secondary batteries] As a method for producing a member for a non-aqueous electrolyte secondary battery, for example, there is a method in which a positive electrode, the above-mentioned laminated separator for a non-aqueous electrolyte secondary battery, and a negative electrode are arranged in this order.
[0117] In addition, the method for producing a nonaqueous electrolyte secondary battery may be, for example, the following method. First, a nonaqueous electrolyte secondary battery member is placed in a container that will become the housing of the nonaqueous electrolyte secondary battery. Next, the container is filled with a nonaqueous electrolyte, and then the container is sealed while reducing the pressure. In this way, a nonaqueous electrolyte secondary battery can be produced.
[0118] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention. EXAMPLES
[0119] [Synthesis Example] [Synthesis Example 1: Synthesis of amine-modified polyethersulfone] An amine-modified polyethersulfone having a -NH2 group at the end was synthesized by the method described in International Publication No. 2021 / 261391. The weight average molecular weight of the amine-modified polyethersulfone was 11,600 (polystyrene equivalent value measured by SEC).
[0120] [Synthesis Example 2: Synthesis of block copolymer (1) based on Production Method 2] A block copolymer was synthesized based on Preparation Method 2 by the following procedure. 1. A 500 mL separable flask equipped with a stirring blade, a thermometer, a nitrogen inlet, and a powder addition port was thoroughly dried. 2. 426 g of N-methylpyrrolidone was charged into a flask. 32.8 g of calcium chloride (dried at 200°C for 2 hours) was added, and the temperature was raised to 100°C to completely dissolve the calcium chloride. This resulted in a calcium chloride solution. The calcium chloride concentration in the calcium chloride solution was 7.14% by weight. The moisture content in the calcium chloride solution was adjusted to 200 ppm. 3. 8.02 g of paraphenylenediamine was added to the calcium chloride solution and completely dissolved by stirring for 30 minutes. During this process, the liquid temperature was maintained at 25°C. 4. The liquid temperature was cooled to 20°C. Then, 12.5 g of terephthalic acid dichloride was added and reacted for 1 hour. In this way, block A composed of poly(paraphenylene terephthalamide) was synthesized. 5. The liquid temperature was raised to 40° C. 17.2 g of amine-modified polyethersulfone (synthesized in Synthesis Example 1) was added and completely dissolved over 1 hour. 6. The liquid temperature was cooled to 20°C. Then, 2.66 g of terephthalic acid dichloride was added and reacted for 1.5 hours. In this way, a block copolymer (1) was synthesized in which block A composed of poly(paraphenylene terephthalamide) and block B composed of polyethersulfone were linked by an amide bond. The content of the block copolymer in the solution, which was the synthesis system, was 7% by weight.
[0121] In the block copolymer (1), 50 mol % of all units was occupied by block A, and the remaining 50 mol % was occupied by block B. The number of paraphenylene terephthalamide units (the number of units represented by formula (1)) per block A, calculated from the amount of monomer charged, was 40.
[0122] [Synthesis Example 3: Synthesis of block copolymer (2) based on Production Method 2] Block copolymer (2) was synthesized by changing the following points in Synthesis Example 2. In step 2, the amount of N-methylpyrrolidone used was 424 g. In step 2, the amount of calcium chloride added was 32.6 g. In step 3, the amount of paraphenylenediamine added was 12.0 g. In step 4, the amount of terephthalic acid dichloride added was 20.5 g. In step 5, the amount of amine-modified polyethersulfone added was 8.58 g. In step 6, the amount of terephthalic acid dichloride added was 1.63 g.
[0123] In the block copolymer (2), 75 mol % of all units was occupied by block A, and the remaining 25 mol % was occupied by block B. The number of paraphenylene terephthalamide units per block A (the number of units represented by formula (1)) calculated from the amount of monomer charged was 54.
[0124] [Synthesis Examples 4 to 6: Synthesis of block copolymers (3) to (5) based on Production Method 2] Similarly to Synthesis Examples 1 and 2, block copolymers (3) to (5) were synthesized based on Production Method 2 by appropriately changing the amounts of materials used. In block copolymers (3) to (5), the number of paraphenylene terephthalamide units (the number of units represented by formula (1)) per block A was as follows. Block copolymer (3): 29 units Block copolymer (4): 36 units Block copolymer (5): 47 units
[0125] [Synthesis Example 7: Synthesis of block copolymer (6) based on Production Method 1] A block copolymer was synthesized based on Preparation Method 1 by the following procedure. 1. A 500 mL separable flask equipped with a stirring blade, a thermometer, a nitrogen inlet, and a powder addition port was thoroughly dried. 2. 424 g of N-methylpyrrolidone was charged into a flask. 32.6 g of calcium chloride (dried at 200°C for 2 hours) was added, and the temperature was raised to 100°C to completely dissolve the calcium chloride. This resulted in a calcium chloride solution. The calcium chloride concentration in the calcium chloride solution was 7.14% by weight. The moisture content in the calcium chloride solution was adjusted to 170 ppm. 3. The calcium chloride solution was heated to 40° C., and 24.8 g of amine-modified polyethersulfone (synthesized in Synthesis Example 1) was added and completely dissolved by stirring for 30 minutes. 4. The liquid temperature was cooled to 20°C. 5. 11.5 g of paraphenylenediamine was added and stirred for 30 minutes to completely dissolve. 6. 21.4 g of terephthalic acid dichloride was added and reacted for 1 hour. In this way, a block copolymer (6) was synthesized in which block A composed of poly(paraphenylene terephthalamide) and block B composed of polyethersulfone were linked by an amide bond. The content of the block copolymer in the solution, which was the synthesis system, was 10% by weight.
[0126] In the block copolymer (6), 50 mol % of all units was occupied by block A, and the remaining 50 mol % was occupied by block B. The number of paraphenylene terephthalamide units (the number of units represented by formula (1)) per block A, calculated from the amount of monomer charged, was 23.
[0127] [Synthesis Example 8: Synthesis of block copolymer (7) based on Production Method 1] Similarly to Synthesis Example 7, a block copolymer (7) was synthesized based on Production Method 1 by appropriately changing the amounts of materials used. In block copolymer (7), the number of paraphenylene terephthalamide units (the number of units represented by Formula (1)) per block A was 26.
[0128] [Comparative Synthesis Example 1: Synthesis of poly(paraphenylene terephthalamide)] Poly(paraphenylene terephthalamide) was synthesized according to the following procedure. 1. A 500 mL separable flask equipped with a stirring blade, a thermometer, a nitrogen inlet, and a powder addition port was thoroughly dried. 2. 428 g of N-methylpyrrolidone was charged into a flask. 32.9 g of calcium chloride (dried at 200°C for 2 hours) was added, and the temperature was raised to 100°C to completely dissolve the calcium chloride. This resulted in a calcium chloride solution. The calcium chloride concentration in the calcium chloride solution was 7.14% by weight. The moisture content in the calcium chloride solution was adjusted to 450 ppm. 3. 13.9g of paraphenylenediamine was added to the calcium chloride solution and dissolved completely. During this process, the liquid temperature was maintained at 30±2°C. 4. The liquid temperature was cooled to 20°C. 5. 25.2 g of terephthalic acid dichloride was added in three portions and reacted for 1 hour. In this process, the liquid temperature was maintained at 20±2°C. In this way, poly(paraphenylene terephthalamide) was synthesized. The content of poly(paraphenylene terephthalamide) in the solution, which was the synthesis system, was 6% by weight.
[0129] [Comparative Synthesis Example 2: Preparation of polyethersulfone solution] A polyethersulfone solution was prepared by the following procedure: The polyethersulfone used in Comparative Synthesis Example 2 was unmodified, and had Cl atoms located at its terminals. 1. A 500 mL separable flask equipped with a stirring blade, a thermometer, a nitrogen inlet, and a powder addition port was thoroughly dried. 2. 470 g of N-methylpyrrolidone was placed in a flask. 3. 30 g of polyethersulfone (Sumikaexcel 3600P, Sumitomo Chemical Co., Ltd.) was added to the flask, and the liquid temperature was raised to 100°C. 4. The mixture was stirred for 1 hour while keeping the temperature at 100°C ± 5°C until the polyethersulfone was completely dissolved. The liquid was then cooled to 20°C.
[0130] [Comparative Synthesis Example 3: Preparation of a mixed solution of poly(paraphenylene terephthalamide) and polyethersulfone] The mixed solution was prepared according to the following procedure. 1. Poly(paraphenylene terephthalamide) was synthesized in the same manner as in Comparative Synthesis Example 1. The weight of the solution used in the synthesis was 500 g. 2. A polyethersulfone solution was prepared in the same manner as in Comparative Synthesis Example 2. The weight of the solution was 500 g. 3. A 500 mL separable flask equipped with a stirring blade, a thermometer, a nitrogen inlet, and a powder addition port was thoroughly dried. 200 g of the solution obtained in step 1 and 200 g of the solution obtained in step 2 were charged into the flask. 4. The mixture was stirred for 1 hour while maintaining the temperature at 20±2°C to obtain a mixed solution.
[0131] [Evaluation of polymer properties] [Molecular weight measurement] The measurement was carried out according to the following procedure. 1. The solutions obtained in Synthesis Examples 1 and 2 and Comparative Synthesis Examples 1 and 2 were diluted with N-methylpyrrolidone so that the polymer concentration was 0.1% by weight. 2. The solution was filtered through a PTFE membrane filter (pore size: 0.45 μm). 3. The filtrate was analyzed by size exclusion chromatography (SEC) under the following analytical conditions:
[0132] Equipment: Equipment equivalent to LC-20A (Shimadzu Corporation) Column: Two TSK-GEL SUPER AWM-H columns (Tosoh Corporation) Eluent: 30 mM LiBr dissolved in N-methylpyrrolidone Flow rate: 0.4mL / min Column temperature: 40℃ Detection: UV310nm 4. Based on the obtained chromatogram, the polystyrene equivalent molecular weight was obtained.
[0133] [Solubility in electrolyte] The measurement was carried out according to the following procedure.
[0134] (Preparation of sample solution) Sample solutions from block copolymers of synthesis examples 2 and 3 1. 50 g of the solutions obtained in Synthesis Examples 2 and 3 were weighed out and added to 500 mL of ion-exchanged water. In this manner, a polymer was precipitated. The precipitated polymer was separated by filtration. 2. The polymer precipitated in step 1 was washed with 100 mL of ion-exchanged water and then filtered. The resulting powder was dried in an oven at 150° C. for 2 hours. 3. 0.20 g of the powder obtained in step 2 was weighed out. This powder was immersed in 99.8 g of an electrolyte (EC / EMC / DMC=3 / 5 / 2) in an LC vial. While immersed, extraction was performed for 5 days while appropriately stirring. 4. The extract obtained in step 3 was filtered through a PTFE membrane filter (pore size: 0.45 μm) to obtain a sample solution. The sample solution mainly contains polyethersulfone that was unreacted in the block copolymer synthesis reaction. Sample solution from polyethersulfone in Comparative Synthesis Example 2 1. 0.20 g of the polyethersulfone (Sumikaexcel 3600P, Sumitomo Chemical Co., Ltd.) used in Comparative Synthesis Example 2 was weighed out. This polyethersulfone was immersed in 99.8 g of electrolyte (EC / EMC / DMC=3 / 5 / 2) in an LC vial. While immersed, extraction was performed for 5 days while stirring appropriately. 2. The extract obtained in step 1 was filtered through a PTFE membrane filter (pore size: 0.45 μm) to obtain a sample solution. A portion of polyethersulfone was dissolved in the sample solution. ● Sample solution from the mixed solution of Comparative Synthesis Example 3 1. 50 g of the solution obtained in Comparative Synthesis Example 3 was weighed out and added to 500 mL of ion-exchanged water. In this manner, a polymer was precipitated. The precipitated polymer was separated by filtration. 2. The polymer precipitated in step 1 was washed with 100 mL of ion-exchanged water and then filtered. The resulting powder was dried in an oven at 150° C. for 2 hours. 3. 0.20 g of the powder obtained in step 2 was weighed out. This powder was immersed in 99.8 g of an electrolyte (EC / EMC / DMC=3 / 5 / 2) in an LC vial. While immersed, extraction was performed for 5 days while appropriately stirring. 5. The extract obtained in step 3 was filtered through a PTFE membrane filter (pore size: 0.45 μm) to obtain a sample solution. In the sample solution, a part of the polyethersulfone contained in the mixed solution was dissolved.
[0135] (Preparation of reference solution) Reference solution for synthesis examples 2 and 3 1. 0.20 g of amine-modified polyethersulfone was immersed in 99.8 g of N-methylpyrrolidone for 1 day until it was completely dissolved. 2. The solution obtained in step 1 was filtered through a PTFE membrane filter (pore size: 0.45 μm) to obtain a reference solution. Reference solution for comparative synthesis examples 2 and 3 1. 0.20 g of polyethersulfone (Sumikaexcel 3600P, Sumitomo Chemical Co., Ltd.) was immersed in 99.8 g of N-methylpyrrolidone for one day until it was completely dissolved. 2. The solution obtained in step 1 was filtered through a PTFE membrane filter (pore size: 0.45 μm) to obtain a reference solution.
[0136] (Size Exclusion Chromatography) 1. The sample solution and the reference solution were analyzed by size exclusion chromatography (SEC). The analytical conditions were as follows: Equipment: Equipment equivalent to LC-20A (Shimadzu Corporation) Column: Two TSK-GEL SUPER AWM-H columns (Tosoh Corporation) Eluent: 30 mM LiBr dissolved in N-methylpyrrolidone Flow rate: 0.4mL / min Column temperature: 40℃ Detection: UV310nm 2. The area value of the peak corresponding to polyethersulfone was calculated for each of the chromatograms obtained from the sample solution and the reference solution. The area value calculated from the sample solution was designated as area value A, and the area value calculated from the reference solution was designated as area value B. 3. The elution rate of polyethersulfone into the electrolyte was calculated based on the following formula. In the formula, p is a correction coefficient and represents the proportion (wt%) of polyethersulfone in the polymer obtained in the Synthesis Example or Comparative Synthesis Example. For example, the value of p in Synthesis Example 2 is 0.492.
[0137] Percentage of polyethersulfone dissolved in electrolyte (wt%) = area value A / (area value B × p)
[0138] [result] The results are shown in Table 1 below. [Table 1]
[0139] The polymers obtained in Synthesis Examples 2 and 3 had a significantly lower elution rate in the electrolyte compared to polyethersulfone, and therefore had significantly improved stability in the electrolyte. These results suggest that block copolymers of poly(paraphenylene terephthalamide) and polyethersulfone were synthesized in Synthesis Examples 2 and 3.
[0140] In relation to this result, it is worth noting that amine-modified polyethersulfone was used in Synthesis Examples 2 and 3, whereas general Cl-terminated polyethersulfone was used in Comparative Synthesis Examples 2 and 3. General polyethersulfone has a drawback of low stability against electrolyte. To address this drawback, a method of mixing with poly(paraphenylene terephthalamide), which has high stability against electrolyte, was considered, but the stability against electrolyte was still insufficient. The solution that the present inventors finally found was to modify the terminals of polyethersulfone and form a block copolymer with poly(paraphenylene terephthalamide). In this respect, it can be said that the present invention is a highly inventive and creative approach to the prior art.
[0141] [Evaluation of polymer battery characteristics] [Preparation of porous layer and laminated separator] The porous layer and the laminated separator were produced according to the following procedure. 1. The solutions obtained in Synthesis Examples 2 and 3 or Comparative Synthesis Examples 1 to 3 were mixed with N-methylpyrrolidone. As a result, solutions in which the polymer was dissolved or dispersed were obtained. The amounts of the solutions obtained in Synthesis Examples 2 and 3 or Comparative Synthesis Examples 1 to 3 used were all 400 g. The amounts of N-methylpyrrolidone used for the polymers of Synthesis Examples 2 and 3 were 687 g, and for the polymers of Comparative Synthesis Examples 1 to 3 were 637 g. 2. Aluminum oxide (average particle size: 0.013 μm) was added to the solution obtained in step 1, and uniformly dispersed using a pressure type disperser. Thus, a coating liquid was prepared. The solid concentration of the coating liquid (total concentration of polymer and aluminum oxide) was 5 wt %. The amount of aluminum oxide used was 28.0 g for the polymers of Synthesis Examples 2 and 3, and 24.0 g for the polymers of Comparative Synthesis Examples 1 to 3. 3. Polyethylene porous film (thickness: 10.7 μm, weight per unit area: 6.0 g / m 2 ) was coated with the coating liquid. In this manner, a coated product was obtained. 4. The coated product obtained in step 3 was treated in an oven at 50°C and humidity of 70% for 2 minutes. This formed a porous layer on the polyethylene porous film. 5. The porous layer was washed with water and dried to obtain a laminated separator having a porous layer. In the polymer obtained in Comparative Synthesis Example 2, most of the porous layer peeled off in the water washing step, and sufficient film formation was not possible.
[0142] [Cycle characteristics] (Preparation of non-aqueous electrolyte secondary battery) A non-aqueous electrolyte secondary battery for testing incorporating the laminated separator was fabricated according to the following procedure. 1. (Positive electrode) Thickness: 49.9 μm, Density: 2.97 g / cm 3 The positive electrode active material layer had a composition of LiNi 0.78 Co 0.19 Al 0.03 The ratio of O2:conductive material:polyvinylidene fluoride was 92:4:4. 2. (Negative electrode) Thickness: 71.2 μm, Density: 1.45 g / cm 3 A negative electrode agent having a void volume of 41.3 μL was prepared. The composition of the negative electrode active material layer was artificial graphite:styrene butadiene rubber:carboxymethyl cellulose=96.5:2.0:1.5 in weight ratio. 3. A nonaqueous electrolyte secondary battery member was fabricated by laminating the negative electrode, the laminated separator, and the positive electrode in this order. At this time, the negative electrode active material layer was laminated so as to face the polyolefin substrate side of the laminated separator, and the positive electrode active material layer was laminated so as to face the porous layer side of the laminated separator. 4. The nonaqueous electrolyte secondary battery components were placed in a bag made of laminated aluminum layers and heat seal layers, and a nonaqueous electrolyte was injected. The amount of nonaqueous electrolyte injected was 2.8 times the total void volume of the electrodes and laminated separator. The composition of the nonaqueous electrolyte was a mixed solvent of ethylene carbonate: ethyl methyl carbonate: diethyl carbonate = 3: 5: 2 (volume ratio), in which 1 wt% vinylene carbonate and 1 mol / L LiPF6 were dissolved. 5. The bag was heat sealed while the pressure inside the bag was reduced, thereby completing a non-aqueous electrolyte secondary battery for testing.
[0143] (Capacity retention rate measurement) The discharge capacity of the prepared battery was measured according to the following procedure. 1. One initial charge / discharge cycle was performed under the following conditions: temperature: 25°C, voltage range: 2.7 to 4.2 V, and current value: 0.1 C (when charging) or 0.2 C (when discharging). Here, 1 C is the current value at which the rated capacity based on the 1-hour rate of discharge capacity is discharged in 1 hour. 2. The nonaqueous electrolyte secondary battery was aged by performing 10 cycles of charge and discharge at a temperature of 25° C., a voltage range of 2.7 to 4.2 V, and a current value of 1 C (when charging) or 5 C (when discharging). 3. 200 cycles of charge and discharge were performed under the following conditions: temperature: 45°C, voltage range: 2.5 to 4.2 V, current value: 1 C (when charging) or 5 C (when discharging). The capacity retention rate after 200 cycles was calculated by dividing the discharge capacity (mAh) after 200 cycles by the discharge capacity (mAh) at the first cycle.
[0144] [result] The results are shown in Table 2. [Table 2]
[0145] The nonaqueous electrolyte secondary batteries using the polymers according to Synthesis Examples 2 and 3 had a higher capacity retention rate after 200 cycles compared to the nonaqueous electrolyte secondary batteries using the polymers according to Comparative Synthesis Examples 1 to 3. At least in this respect, the nonaqueous electrolyte secondary batteries using the polymers according to Synthesis Examples 2 and 3 have better cycle characteristics than the nonaqueous electrolyte secondary batteries according to the prior art.
[0146] [Rate characteristics] (Preparation of non-aqueous electrolyte secondary battery) A non-aqueous electrolyte secondary battery for testing was fabricated by the above-mentioned procedure, incorporating the laminated separator. As the polymer constituting the heat-resistant layer, those synthesized in Synthesis Examples 2 and 3 or Comparative Synthesis Example 1 were used.
[0147] (Capacity retention rate measurement) The discharge capacity of the prepared battery was measured according to the following procedure. 1. One initial charge / discharge cycle was performed under the following conditions: temperature: 25°C, voltage range: 2.7 to 4.2 V, and current value: 0.1 C (when charging) or 0.2 C (when discharging). Here, 1 C is the current value at which the rated capacity based on the 1-hour rate of discharge capacity is discharged in 1 hour. 2. The nonaqueous electrolyte secondary battery was aged by performing 10 cycles of charge and discharge at a temperature of 25° C., a voltage range of 2.7 to 4.2 V, and a current value of 1 C (when charging) or 5 C (when discharging). 3. One cycle of charge and discharge was performed under the following conditions: temperature: 45°C, voltage range: 2.5 to 4.2V, current value: 1C (when charging) or 1C, 3C, 4C or 5C (when discharging). The capacity retention rate after discharging at 3C, 4C or 5C was determined by dividing the discharge capacity (mAh) when the discharge current value was 3C, 4C or 5C by the discharge capacity (mAh) when the discharge current value was 1C.
[0148] [result] The results are shown in Table 3 below. [Table 3]
[0149] The nonaqueous electrolyte secondary batteries using the polymers according to Synthesis Examples 2 and 3 had higher capacity retention rates after 3C, 4C, and 5C discharges than the nonaqueous electrolyte secondary battery using the polymer according to Comparative Synthesis Example 1. At least in this respect, the nonaqueous electrolyte secondary batteries using the polymers according to Synthesis Examples 2 and 3 have better rate characteristics than the nonaqueous electrolyte secondary batteries according to the prior art.
[0150] [Evaluation of Coatability] The coatability of the coating liquid was evaluated according to the following procedure. 1. Coating solutions were prepared from the solutions obtained in Synthesis Examples 2, 4, and 5 according to the method described above. 2. The obtained coating liquid was applied to a polyethylene porous film (thickness: 10.7 μm, weight per unit area: 6.0 g / m 2 The coatability during coating was evaluated based on the following criteria. ++: Neither powder falling nor uneven coating was observed. +: Either powder falling or uneven coating was observed, but it was not a problem for the product.
[0151] [result] The results are shown in Table 4. [Table 4]
[0152] All of the coating solutions using the polymers according to Synthesis Examples 2, 4, and 5 exhibited good coatability. In particular, the coating solutions using the polymers according to Synthesis Examples 2 and 5, in which the number of paraphenylene terephthalamide units per block is 40 or more, exhibited particularly good coatability. [Industrial Applicability]
[0153] The present invention can be used for non-aqueous electrolyte secondary batteries and the like.
Claims
1. A block copolymer having a structure in which a block A mainly composed of a unit represented by the following formula (1) and a block B mainly composed of a unit represented by the following formula (2) are linked by an amide bond or an ester bond: -(NH-Ar1-NHCO-Ar2-CO)-...Formula (1) -(Ar3-SO 2 -Ar4-O)- Formula (2) In formula (1) and formula (2), Ar1, Ar2, Ar3, and Ar4 each independently represent a divalent group having one or more aromatic rings. Between different units, the structure of each of Ar1, Ar2, Ar3 or Ar4 may be different.
2. 2. The block copolymer according to claim 1, wherein at least one of the blocks A has 30 or more units represented by formula (1).
3. A porous layer for a non-aqueous electrolyte secondary battery, comprising the block copolymer according to claim 1 or 2.
4. The porous layer for a non-aqueous electrolyte secondary battery according to claim 3 , further comprising a filler.
5. A laminate separator for a non-aqueous electrolyte secondary battery, comprising the porous layer for a non-aqueous electrolyte secondary battery according to claim 3 laminated on one or both sides of a polyolefin porous film.
6. 6. The separator for a non-aqueous electrolyte secondary battery according to claim 5, further comprising an adhesive layer in addition to the porous layer for a non-aqueous electrolyte secondary battery.
7. A member for a non-aqueous electrolyte secondary battery, comprising a positive electrode, the laminate separator for a non-aqueous electrolyte secondary battery according to claim 5, and a negative electrode arranged in this order.
8. A nonaqueous electrolyte secondary battery comprising the laminated separator for nonaqueous electrolyte secondary batteries according to claim 5.
9. A nonaqueous electrolyte secondary battery comprising the member for a nonaqueous electrolyte secondary battery according to claim 7.
10. A method for producing the block copolymer according to claim 1 or 2, comprising the following step (a): (a) NH 2 -Ar1-NH 2 a step of polymerizing a monomer represented by the formula (I) and a terminal-modified aromatic polyethersulfone; Where: The terminally modified aromatic polyethersulfone has an —OH or —NH 2 and has a unit represented by formula (2) as a main component, The two X's contained in the monomer represented by XOC-Ar2-COX are each independently a hydroxyl group or a halogen.
11. A method for producing the block copolymer according to claim 1 or 2, comprising the following step (b): (b) polymerizing a terminal-modified aromatic polyethersulfone, an aromatic polyamide, or a monomer represented by XOC-Ar2-COX; Where: The terminally modified aromatic polyethersulfone has an —OH or —NH 2 and has a unit represented by formula (2) as a main component, The aromatic polyamide has a unit represented by the formula (1) as a main component, The two X's contained in the monomer represented by XOC-Ar2-COX are each independently a hydroxyl group or a halogen.
Citation Information
Patent Citations
Porous membrane, its manufacturing method, and secondary battery using this
JP2005317494A