Vane, compressor comprising vane, and method for manufacturing vane
The vane design for rotary compressors, with a nitrided base material and sputtered hard coating, addresses the wear and seizure issues on the tip surface, improving durability and reducing piston wear.
Patent Information
- Application Number
- JP2023056185
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing rotary compressors face issues with insufficient wear resistance and seizure resistance on the tip surface of vanes due to high surface pressure, leading to potential wear and damage of the piston.
A vane design featuring a nitrided base material with a hard coating formed by a sputtering method, ensuring adequate wear resistance and seizure resistance on the tip surface, while preventing the formation of protrusions that could cause excessive piston wear.
The vane design effectively reduces piston wear and maintains necessary wear resistance and seizure resistance, enhancing the durability and performance of the compressor.
Smart Images

Figure 2024143476000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a vane, a compressor equipped with the vane, and a method for manufacturing the vane. [Background technology]
[0002] The compression section of the rotary compressor includes a cylinder, a piston that revolves along the inner circumferential surface of the cylinder, and a pair of end plates that close both ends of the cylinder. A cylinder chamber is formed by the inner circumferential surface of the cylinder, the outer circumferential surface of the piston, and the pair of end plates, and a vane that divides the cylinder chamber into a suction chamber and a compression chamber is disposed in a vane groove formed in the cylinder. The outer circumferential surface of this type of vane has a tip surface that slides against the outer circumferential surface of the piston, a side surface that slides against the inner surface of the vane groove, and an end surface that slides against the end plate. Therefore, the sliding surfaces of the vane (tip surface, side surface, end surface) are required to have wear resistance that makes them less likely to wear even when they repeatedly slide against the piston or end plate, and seizure resistance that makes them less likely to change even when the temperature of the vane itself rises due to frictional heat caused by sliding. In particular, the tip surface of the vane is required to have high hardness (wear resistance) that can withstand the pressure that it receives from the outer circumferential surface of the piston when sliding against the piston. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 60-26195 [Patent Document 2] Japanese Patent Application Publication No. 10-159774 Summary of the Invention [Problem to be solved by the invention]
[0004] In the rotary compressor described in Patent Document 1, vanes formed from a steel material with a high Cr content as a base material are nitrided to form a nitride diffusion layer on the surface of the vane, thereby ensuring wear resistance and seizure resistance. However, although the vane described in Patent Document 1 has sufficient wear resistance and seizure resistance on the side and end faces, it lacks the hardness required for the tip face of the vane, which receives a large force from the piston and receives a large surface pressure because the contact area during sliding with the piston is small, and there is a risk that wear on the tip face will progress.
[0005] In the rotary compressor described in Patent Document 2, the vanes are nitrided and a CrN film is formed thereon to improve the vane's wear resistance and seizure resistance. However, when a CrN film or the like is formed on the surface of a steel material by ion plating (arc method) as described in Patent Document 2, droplets of several tens of microns in size are generated when the material to be formed is turned into plasma, and the droplets may be taken into the film to form protrusions. If protrusions such as CrN are formed on the tip of the vane, they may be highly aggressive to the piston that slides against the vane, causing wear on the surface of the piston.
[0006] The disclosed technology has been made in consideration of the above, and aims to provide a vane that reduces piston wear while ensuring the necessary wear resistance and seizure resistance on the tip surface of the vane, a compressor equipped with the vane, and a method for manufacturing the vane. [Means for solving the problem]
[0007] One aspect of the vane disclosed in the present application is a vane used in a compressor including a cylinder, a piston that revolves along the inner surface of the cylinder, and an end plate that closes the end of the cylinder, and divides a cylinder chamber surrounded by the cylinder, the piston, and the end plate into a suction chamber and a compression chamber, and includes a nitrided base material and a hard coating that covers a tip surface of the base material, the hard coating being formed by a sputtering method. Effect of the Invention
[0008] According to one aspect of the vane disclosed in the present application, it is possible to reduce piston wear while ensuring the necessary wear resistance and seizure resistance in the tip surface of the vane. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a vertical cross-sectional view showing a compressor equipped with a vane according to a first embodiment. [Diagram 2] FIG. 2 is an exploded perspective view showing a compression unit of the compressor of the first embodiment. [Diagram 3] FIG. 3 is a perspective view showing the vane of the first embodiment. [Figure 4] FIG. 4 is a cross-sectional view showing the hard coating and the nitride layer of the vane of the first embodiment. [Diagram 5] FIG. 5 is an enlarged cross-sectional view showing the tip of the vane of the first embodiment. [Figure 6] FIG. 6 is a schematic diagram for explaining a manufacturing method of the vane of the first embodiment. [Figure 7] FIG. 7 is a cross-sectional view showing the surface of the base material immediately after the nitriding treatment. [Figure 8] FIG. 8 is a cross-sectional view showing a film forming apparatus for forming a hard film on the tip end face of a base material by a sputtering method. [Figure 9] FIG. 9 is a schematic diagram for explaining an example of a hard coating forming step in Example 1. [Figure 10] FIG. 10 is a cross-sectional view showing another film forming apparatus for forming a hard film on the tip surface of a vane of a comparative example by an arc ion plating method. [Figure 11] FIG. 11 is a perspective view showing the surface of the hard coating of the vane of the comparative example. [Figure 12] FIG. 12 is an enlarged cross-sectional view of the tip of the vane according to the second embodiment. [Figure 13] FIG. 13 is a schematic diagram for explaining an example of a hard coating forming step in Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, a vane, a compressor including the vane, and a manufacturing method of the vane according to the embodiments disclosed in the present application will be described with reference to the drawings. Note that the following description does not limit the technology of the present disclosure. In addition, in the following description, the same components are given the same reference numerals, and duplicated descriptions will be omitted. EXAMPLES
[0011] (Compressor configuration) Fig. 1 is a vertical cross-sectional view showing a compressor equipped with a vane of Example 1. As shown in Fig. 1, the compressor 1 is a rotary compressor that accommodates a compression section 12 that draws in a refrigerant from an accumulator 25 and compresses the refrigerant and discharges the compressed refrigerant into the main container 10, and a motor 11 that drives the compression section 12, inside the main container 10, and discharges the high-pressure refrigerant compressed by the compression section 12 into the main container 10 and further into a refrigeration cycle through a discharge pipe 107. The compressor 1 also includes a rotating shaft 15 that transmits the driving force of the motor 11 to the compression section 12, and an accumulator 25 fixed to the outer circumferential surface of the main container 10.
[0012] An upper compression section suction pipe 102T and a lower compression section suction pipe 102S are provided penetrating the main container 10 for sucking low-pressure refrigerant of the refrigeration cycle into the compression section 12. In detail, an upper guide pipe 101T is fixed to the main container 10 by brazing, for example, and the upper compression section suction pipe 102T passes through the inside of the upper guide pipe 101T and is fixed to the upper guide pipe 101T by brazing, for example. Similarly, a lower guide pipe 101S is fixed to the main container 10 by brazing, for example, and the lower compression section suction pipe 102S passes through the inside of the lower guide pipe 101S and is fixed to the lower guide pipe 101S by brazing, for example.
[0013] A discharge pipe 107 for discharging the high-pressure refrigerant compressed in the compression section 12 from inside the main container 10 to the refrigeration cycle is provided penetrating the upper part of the main container 10. A base member 310 that supports the entire compressor 1 is fixed to the lower part of the main container 10 by welding.
[0014] The accumulator 25 includes an accumulator suction pipe 27 that draws refrigerant from the refrigeration cycle into the accumulator 25, and an upper gas-liquid separation pipe 31T and a lower gas-liquid separation pipe 31S for sending gaseous refrigerant to the compression section 12. The accumulator suction pipe 27 is connected to an upper portion of the accumulator 25. The upper gas-liquid separation pipe 31T is connected to the upper compression section suction pipe 102T via an upper connecting pipe 104T. The lower gas-liquid separation pipe 31S is connected to the lower compression section suction pipe 102S via a lower connecting pipe 104S.
[0015] FIG. 2 is an exploded perspective view showing the compression section 12 of the compressor 1 of the first embodiment. As shown in FIG. 1 and FIG. 2, the compression section 12 has an upper cylinder 121T, a lower cylinder 121S, an intermediate partition plate 140, an upper end plate 160T, and a lower end plate 160S. The upper end plate 160T, the upper cylinder 121T, the intermediate partition plate 140, the lower cylinder 121S, and the lower end plate 160S are stacked in this order and fixed by a plurality of bolts 175. The upper end plate 160T is provided with a main bearing portion 161T. The lower end plate 160S is provided with a sub-bearing portion 161S. The rotating shaft 15 is provided with a main shaft portion 153, an upper eccentric portion 152T, a lower eccentric portion 152S, and a sub-shaft portion 151. The rotating shaft 15 has the main shaft portion 153 and the sub-shaft portion 151 supported by the compression section 12. The main shaft portion 153 of the rotating shaft 15 is fitted into the main bearing portion 161T of the upper end plate 160T, and the sub shaft portion 151 of the rotating shaft 15 is fitted into the sub bearing portion 161S of the lower end plate 160S, so that the rotating shaft 15 is rotatably supported by the main bearing portion 161T and the sub bearing portion 161S.
[0016] The motor 11 has a stator 111 disposed on the outside and a rotor 112 disposed on the inside. The stator 111 is fixed to the inner circumferential surface 10a of the main container 10 by, for example, shrink fitting or welding. The rotor 112 is fixed to the rotating shaft 15 by shrink fitting.
[0017] The inside of the main container 10 is filled with lubricating oil 18 in an amount sufficient to almost completely immerse the compression section 12, for lubricating the sliding members of the compression section 12 and for sealing between the high pressure and low pressure sections within the cylinder chamber.
[0018] Next, the compression section 12 will be described in detail with reference to Fig. 2. The upper cylinder 121T has a cylindrical upper hollow section 130T therein, and an upper piston 125T is disposed in the upper hollow section 130T. The upper piston 125T is fitted into an upper eccentric section 152T of the rotating shaft 15. The lower cylinder 121S has a cylindrical lower hollow section 130S therein, and a lower piston 125S is disposed in the lower hollow section 130S. The lower piston 125S is fitted into a lower eccentric section 152S of the rotating shaft 15.
[0019] The upper cylinder 121T is provided with an upper vane groove 128T extending from the upper hollow portion 130T to the outer periphery, and an upper vane 127T is disposed in the upper vane groove 128T. The upper cylinder 121T is provided with an upper spring hole 124T leading from the outer periphery to the upper vane groove 128T, and an upper spring 126T is disposed in the upper spring hole 124T. The lower cylinder 121S is provided with a lower vane groove 128S extending from the lower hollow portion 130S to the outer periphery, and a lower vane 127S is disposed in the lower vane groove 128S. The lower cylinder 121S is provided with a lower spring hole 124S leading from the outer periphery to the lower vane groove 128S, and a lower spring 126S is disposed in the lower spring hole 124S.
[0020] One end of the upper vane 127T is pressed against the upper piston 125T by the upper spring 126T, so that the space outside the upper piston 125T in the upper hollow portion 130T of the upper cylinder 121T is divided into an upper suction chamber 131T and an upper compression chamber 133T, which are upper cylinder chambers. The upper cylinder 121T is provided with an upper suction hole 135T that communicates with the upper suction chamber 131T from the outer periphery. The upper suction hole 135T is connected to the upper compression section suction pipe 102T. One end of the lower vane 127S is pressed against the lower piston 125S by the lower spring 126S, so that the space outside the lower piston 125S in the lower hollow portion 130S of the lower cylinder 121S is divided into a lower suction chamber 131S and a lower compression chamber 133S, which are lower cylinder chambers. The lower cylinder 121S is provided with a lower suction hole 135S that communicates with the lower suction chamber 131S from the outer periphery. A lower compression section suction pipe 102S is connected to the lower suction hole 135S.
[0021] The upper end plate 160T is provided with an upper discharge hole 190T that penetrates the upper end plate 160T and communicates with the upper compression chamber 133T. An upper discharge valve 200T, which is a reed valve that opens and closes the upper discharge hole 190T, and an upper discharge valve holder 201T that regulates the warping of the upper discharge valve 200T are fixed to the upper end plate 160T by an upper rivet 202T. An upper end plate cover 170T that covers the upper discharge hole 190T is disposed on the upper side of the upper end plate 160T, and an upper end plate cover chamber 180T that is closed by the upper end plate 160T and the upper end plate cover 170T is formed. The upper end plate cover 170T is fixed to the upper end plate 160T by a plurality of bolts 175 that fix the upper end plate 160T and the upper cylinder 121T. The upper end plate cover 170T is provided with an upper end plate cover discharge hole 172T that communicates between the upper end plate cover chamber 180T and the inside of the main body container 10. When the compression section 12 is provided in the main body container 10, the inner peripheral surface 10a of the main body container 10 is shrink-fitted to the outer peripheral surface 182a of the upper end plate 160T, and is joined to the main body container 10 by a plurality of welded parts. The structure of the upper end plate 160T in this embodiment 1 will be described in detail later.
[0022] The lower end plate 160S is provided with a lower discharge hole 190S that penetrates the lower end plate 160S and communicates with the lower compression chamber 133S. A lower discharge valve 200S, which is a reed valve that opens and closes the lower discharge hole 190S, and a lower discharge valve holder 201S that regulates the warping of the lower discharge valve 200S are fixed to the lower end plate 160S by a lower rivet 202S. A lower end plate cover 170S that covers the lower discharge hole 190S is disposed below the lower end plate 160S, and a lower end plate cover chamber 180S that is closed by the lower end plate 160S and the lower end plate cover 170S is formed (see FIG. 1). The lower end plate cover 170S is fixed to the lower end plate 160S by a plurality of bolts 175 that fix the lower end plate 160S and the lower cylinder 121S.
[0023] In addition, the compression section 12 is provided with a refrigerant passage hole 136 (see Figure 2) that penetrates the lower end plate 160S, the lower cylinder 121S, the intermediate partition plate 140, the upper end plate 160T and the upper cylinder 121T and connects the lower end plate cover chamber 180S and the upper end plate cover chamber 180T.
[0024] The flow of refrigerant caused by the rotation of the rotary shaft 15 will be described below. The rotation of the rotary shaft 15 causes the upper piston 125T fitted in the upper eccentric portion 152T of the rotary shaft 15 and the lower piston 125S fitted in the lower eccentric portion 152S to revolve, so that the upper suction chamber 131T and the lower suction chamber 131S expand in volume and draw in refrigerant. As a refrigerant intake path, the low-pressure refrigerant of the refrigeration cycle is drawn into the accumulator 25 through the accumulator suction pipe 27, and only the gaseous refrigerant is drawn into the upper gas-liquid separation pipe 31T and the lower gas-liquid separation pipe 31S. The gaseous refrigerant drawn into the upper gas-liquid separation pipe 31T is drawn into the upper suction chamber 131T through the upper connecting pipe 104T and the upper compression section suction pipe 102T. Similarly, the gas refrigerant sucked into the lower gas-liquid separation pipe 31S passes through the lower connecting pipe 104S and the lower compression section suction pipe 102S, and is sucked into the lower suction chamber 131S.
[0025] Next, the flow of the refrigerant discharged by the rotation of the rotary shaft 15 will be described. The rotation of the rotary shaft 15 causes the upper piston 125T fitted to the upper eccentric portion 152T of the rotary shaft 15 to revolve, compressing the refrigerant in the upper compression chamber 133T while reducing its volume, and when the pressure of the compressed refrigerant becomes higher than the pressure in the upper end plate cover chamber 180T outside the upper discharge valve 200T, the upper discharge valve 200T opens and discharges the refrigerant from the upper compression chamber 133T to the upper end plate cover chamber 180T. The refrigerant discharged to the upper end plate cover chamber 180T is discharged into the main body container 10 from the upper end plate cover discharge hole 172T provided in the upper end plate cover 170T.
[0026] Furthermore, as the rotary shaft 15 rotates, the lower piston 125S fitted in the lower eccentric portion 152S of the rotary shaft 15 revolves, compressing the refrigerant in the lower compression chamber 133S while reducing its volume, and when the pressure of the compressed refrigerant becomes higher than the pressure in the lower end plate cover chamber 180S outside the lower discharge valve 200S, the lower discharge valve 200S opens and discharges the refrigerant from the lower compression chamber 133S to the lower end plate cover chamber 180S. The refrigerant discharged to the lower end plate cover chamber 180S passes through the refrigerant passage hole 136 and the upper end plate cover chamber 180T, and is discharged into the main body container 10 from the upper end plate cover discharge hole 172T provided in the upper end plate cover 170T.
[0027] The refrigerant discharged into the main container 10 is guided above the motor 11 through a notch (not shown) that connects the top and bottom of the outer periphery of the stator 111, or a gap (not shown) in the winding portion of the stator 111, or a gap 115 (see Figure 1) between the stator 111 and the rotor 112, and is discharged from a discharge pipe 107 located at the top of the main container 10.
[0028] Next, the flow of the lubricating oil 18 will be described. The lubricating oil 18 sealed in the lower part of the main container 10 is supplied to the compression section 12 through the inside of the rotating shaft 15 (not shown) by the centrifugal force of the rotating shaft 15. The lubricating oil 18 supplied to the compression section 12 is mixed with the refrigerant and is discharged into the inside of the main container 10 together with the refrigerant in a mist form. The mist-formed lubricating oil 18 discharged into the inside of the main container 10 is separated from the refrigerant by the centrifugal force of the rotational force of the motor 11, and returns to the lower part of the main container 10 as oil droplets. However, some of the lubricating oil 18 is not separated and is discharged into the refrigerant together with the refrigerant to the refrigeration cycle. The lubricating oil 18 discharged into the refrigeration cycle circulates through the refrigeration cycle and returns to the accumulator 25, where it is separated inside the accumulator 25 and accumulates in the lower part of the accumulator 25. The lubricating oil 18 accumulated in the lower part of the accumulator 25 is sucked into the upper suction chamber 131T and the lower suction chamber 131S together with the suctioned refrigerant.
[0029] (Characteristic configuration of compressor 1) Next, the characteristic configuration of the vane of the first embodiment will be described. FIG. 3 is a perspective view showing the vane of the first embodiment. The upper vane 127T and the lower vane 127S (hereinafter also referred to as vane 127) have the same structure, so the upper vane 127T will be described below, and the description of the lower vane 127S will be omitted. The upper vane 127T has a tip surface 129a that slides against the outer circumferential surface of the upper piston 125T, and a first side surface 129b and a second side surface 129c that slide against the inner surface of the upper vane groove 128T. The upper vane 127T also has a first end surface 129d that slides against the end surface of the upper end plate 160T, a second end surface 129e that slides against the end surface of the intermediate partition plate 140 as an end plate, and a back surface 129f that is pressed by the upper spring 126T. In addition, to supplement the description of the lower vane 127S, the lower vane 127S has a first end face 129d that slides against an end face of the intermediate partition plate 140 as an end plate, and a second end face 129e that slides against an end face of the lower end plate 160S. The first side face 129b and the second side face 129c, the first end face 129d and the second end face 129e are each formed in a flat plate shape.
[0030] The tip end surface 129a of the upper vane 127T is formed in an arc shape when viewed from a direction perpendicular to the first end surface 129d and the second end surface 129e. An engagement portion 138 with which an end of the upper spring 126T engages is formed on the back surface 129f of the upper vane 127T by cutting out a part of the flat back surface 129f.
[0031] The upper vane 127T includes a base material 210 and a hard coating 220. The base material 210 has a base layer 211 (described later) formed of a material with a chromium (Cr) content exceeding 4.5 [wt%]. Examples of the material include SUS440C (a type of martensitic stainless steel) with a chromium (Cr) content of about 16 [wt%] to 18 [wt%], SKD61 (a type of die steel) with a chromium (Cr) content of about 4.8 [wt%] to 5.5 [wt%], and SKD11 (a type of die steel) with a chromium (Cr) content of about 11.0 [wt%] to 13.0 [wt%]. In this way, the upper vane 127T has an appropriate wear resistance and seizure resistance because the base layer 211 of the base material 210 is formed of a material with a chromium (Cr) content exceeding 4.5 [wt%]. Furthermore, when the base material layer 211 of the base material 210 of the upper vane 127T is formed from stainless steel having a chromium (Cr) content exceeding 10 wt%, the upper vane 127T can sufficiently ensure wear resistance and seizure resistance, particularly of the first side surface 129b and the second side surface 129c, which have a large sliding area.
[0032] Fig. 4 is a cross-sectional view showing the hard coating 220 of the vane 127 of Example 1. Fig. 4 shows a cross section perpendicular to the first end face 129d and the second end face 129e of the vane 127. Fig. 5 is an enlarged cross-sectional view showing the tip of the vane 127 of Example 1. Fig. 5 shows a cross section perpendicular to the first side face 129b and the second side face 129c of the vane 127.
[0033] 4, a hard coating 220 is formed on a tip end surface 129a of the upper vane 127T. A nitride diffusion layer 212 is formed on the entire outer circumferential surface of the base material 210 so as to cover the base material layer 211, and a dense layer 213 is formed on the nitride diffusion layer 212.
[0034] As shown in Fig. 5, a hard coating 220 is formed on the entire tip surface 129a of the upper vane 127T. The hard coating 220 is formed on the surface side of the dense layer 213 of the base material 210 and is in close contact with the dense layer 213. The hard coating 220 is formed of, for example, dichromium nitride (Cr2N) having a Vickers hardness of 1500 HV or more. Since the hard coating 220 is provided on the tip surface 129a of the upper vane 127T, the wear resistance of the tip surface 129a is appropriately ensured.
[0035] (Method of manufacturing vanes) The manufacturing method of the vane of Example 1 is a method for manufacturing the vane 127 of Example 1 configured as described above. Figure 6 is a schematic diagram for explaining the manufacturing method of the vane of Example 1. Figure 6 shows that the properties of the vane 127 change in the order of Figure 6(a) to Figure 6(d) by the manufacturing method of the vane of Example 1.
[0036] As shown in Fig. 6(a), the base material 210 of the vane 127 before nitriding is entirely made of a material with a chromium (Cr) content exceeding 4.5 [wt%]. In the embodiment, a region of the base material 210 having the same composition as the base material 210 before nitriding is referred to as a base material layer 211. The high chromium (Cr) content in the base material layer 211 of the base material 210 ensures the vane 127 to have adequate wear resistance and seizure resistance. In the vane 127 of the embodiment 1, for example, the base material layer 211 of the base material 210 is made of martensitic stainless steel with a chromium (Cr) content of about 16 [wt%] to 18 [wt%]. The vane 127 has a base material layer 211 of a base material 210 formed from stainless steel having a chromium (Cr) content exceeding 10 wt%, thereby ensuring sufficient wear resistance and seizure resistance, particularly on the first side surface 129b and the second side surface 129c, which have a large sliding area.
[0037] After the base material 210 is formed, the base material 210 is quenched (a heat treatment in which a metal is heated until it becomes an austenitic structure, and then rapidly cooled to obtain a martensite structure). This quenching improves the wear resistance and mechanical strength of the base material 210. After the base material 210 is quenched, the base material 210 is tempered (a heat treatment in which a metal having an unstable structure due to quenching or the like is held at an appropriate temperature to stabilize the metal structure). This tempering improves the toughness of the base material 210.
[0038] After the base material 210 is tempered, the base material 210 is subjected to a nitriding treatment (step S1). Examples of the nitriding treatment include gas nitriding, gas soft nitriding, and ion nitriding. As shown in FIG. 6(b), in the nitriding treatment, nitrogen atoms N penetrate and diffuse from the surface of the base material 210 to the inside, and a nitride layer 214 is formed on the surface of the base material 210. Therefore, the nitride layer 214 is formed so as to surround the base material layer 211. The nitride layer 214 here refers to a layer formed by changing the structure of the base material layer 211 by the nitriding treatment. Note that, in the base material 210, a portion formed with the same composition as the base material layer 211 of the base material 210 at a stage immediately before the nitriding treatment is referred to as the base material layer 211 even after the nitriding treatment.
[0039] FIG. 7 is an enlarged cross-sectional view showing the surface of the base material 210 immediately after the nitriding process. In this embodiment, the nitride layer 214 is formed of a nitride diffusion layer 212 and a nitride compound layer 216 (white layer). The nitride diffusion layer 212 is formed on the outer surface side of the base material layer 211. The nitride diffusion layer 212 is formed of an α (alpha) phase having a body-centered cubic crystal structure. The nitride diffusion layer 212 is formed of a material in which nitrogen atoms N are dissolved in a solid solution in the metal forming the base material layer 211, or a material in which chromium (Cr) nitrides are dispersed and precipitated in a material in which nitrogen atoms N are dissolved in a solid solution. Furthermore, the nitrogen atoms N are diffused into the nitride diffusion layer 212 so that a concentration gradient is formed in which the concentration of the nitrogen atoms N decreases as it approaches the base material layer 215.
[0040] The nitride compound layer 216 (white layer) is formed from a material having a higher nitrogen concentration than the material from which the nitride diffusion layer 212 is formed, and is formed from a material that is harder and more brittle than the nitride diffusion layer 212. The nitride compound layer 216 is formed from a dense layer 213 and a porous layer 217. The dense layer 213 is formed on the outer surface side of the nitride diffusion layer 212. The dense layer 213 is mainly composed of iron nitride Fe4N and is formed from a γ' (gamma prime) phase with a face-centered cubic crystal structure. The porous layer 217 is formed on the outer surface side of the dense layer 213 and is formed on the outermost surface of the nitride layer 214 of the nitrided base material 210. The porous layer 217 is mainly composed of iron nitride Fe2N, Fe3N and is formed from an ε (epsilon) phase with a close-packed hexagonal crystal structure. Therefore, immediately after the nitriding process, the surface of the base material 210 has the porous layer 217, the dense layer 213, the nitrided diffusion layer 212, and the base material layer 211 arranged in this order from the outside.
[0041] After the base material 210 is nitrided, the surface of the base material 210 is scraped (step S2). In this step, the surface layers of the nitride compound layer 216 formed on the tip surface 129a, the first side surface 129b, the second side surface 129c, the first end surface 129d, and the second end surface 129e are scraped. As a result, the surface layer having minute bulges and minute recesses generated on the surface of the base material 210 due to the nitriding process is scraped, and the first side surface 129b, the second side surface 129c, the first end surface 129d, and the second end surface 129e are flattened, so that the dimensional accuracy and surface accuracy (flatness) of the vane 127 sliding against the inner surface of the upper vane groove 128T (lower vane groove 128S), the upper end plate 160T (lower end plate 160S), and the end surface of the intermediate partition plate 140 can be ensured. In this embodiment, at least the porous layer 217 of the nitride layer 216 (white layer) is removed so that the dense layer 213 is exposed on the surface of the tip end face 129a of the base material 210.
[0042] After the surface of the base material 210 is scraped, a hard coating 220 is formed on the tip surface 129a of the base material 210 by a sputtering method (step S3). The hard coating 220 is formed of, for example, dichromium nitride (Cr2N) having a Vickers hardness of 1500 HV or more. This improves the wear resistance of the tip surface 129a of the vane 127. In the embodiment, the hard coating 220 is formed so as to adhere closely to the dense layer 213 of the tip surface 29a. Note that the hard coating 220 formed by the sputtering method is not limited to dichromium nitride (Cr2N) and may be, for example, chromium nitride (CrN).
[0043] The hard coating 220 is formed on the front end surface 129a of the base material 210 by a sputtering method using a film forming apparatus 230, as shown in Fig. 8. Fig. 8 is a cross-sectional view showing the film forming apparatus 230 that forms the hard coating 220 on the front end surface 129a of the base material 210 by a sputtering method. The film forming apparatus 230 includes a furnace 231 and a target 232. A processing chamber 233 is formed inside the furnace 231. The target 232 is made of metallic chromium Cr.
[0044] 9 is a schematic diagram for explaining an example of a forming process of the hard coating 220 in Example 1. In the forming process (step S3) of forming the hard coating 220, a plurality of base materials 210 are arranged in a processing chamber 233 provided in a film forming apparatus 230. At this time, the plurality of base materials 210 are arranged so that the side surfaces 129b, 129c of the base materials 210 placed next to each other, i.e., the opposing first side surface 129b and second side surface 129c, contact each other, and the end surfaces 129d, 129e of the base materials 210 placed next to each other, i.e., the opposing first end surface 129d and second end surface 129e contact each other.
[0045] After the plurality of base materials 210 are arranged in the processing chamber 233, the film forming apparatus 230 reduces the pressure inside the processing chamber 233 and introduces an inert gas (for example, argon Ar) and nitrogen gas N2 into the processing chamber 233. After the inert gas and nitrogen gas N2 are introduced into the processing chamber 233, the film forming apparatus 230 applies a high voltage to the target 232 and the plurality of base materials 210 so that the target 232 is negatively charged and the plurality of base materials 210 is positively charged, as shown in FIG. 8. By applying a high voltage between the target 232 and the plurality of base materials 210, plasma is generated in the processing chamber 233, the inert gas becomes ions 234, and the ions 234 collide with the target 232. By the collision of the ions 234 with the target 232, a sputtering phenomenon occurs in which chromium atoms Cr forming the target 232 are released from the target 232.
[0046] The chromium atoms Cr emitted from the target 232 are attached to the tip surfaces 129a of the plurality of base materials 210 together with the nitrogen atoms N. As a result, the hard coating 220 made of dichromium nitride (Cr2N) is formed on the tip surfaces 129a of the plurality of base materials 210. That is, the film forming device 230 collectively forms the hard coating 220 on each tip surface 129a of the plurality of base materials 210 arranged as shown in Fig. 9. As a result, the number of base materials 210 on which the hard coating 220 is formed in one formation process can be increased, and the manufacturing cost of the vane 127 can be reduced.
[0047] Furthermore, by arranging the side surfaces 129b, 129c and end surfaces 129d, 129e of adjacent base materials 210 so that they are in contact with each other, it is possible to mask the side surfaces 129b, 129c and end surfaces 129d, 129e so that the hard coating 220 is not formed on the side surfaces 129b, 129c and end surfaces 129d, 129e. In this way, by using another vane 127 as a masking member for coating the vane 127, it is not necessary to provide a separate process for masking the surfaces of the base material 210 on which the hard coating 220 is not formed, and the masking process can be reduced. The vane manufacturing method can reduce the manufacturing cost of the vane 127 by eliminating the masking process.
[0048] The adhesion when the hard coating 220 is in close contact with the dense layer 213 is better than the adhesion when the hard coating 220 is in close contact with the porous layer 217. Therefore, the vane 127 manufactured so that the hard coating 220 is in close contact with the dense layer 213 can more strongly adhere the hard coating 220 to the base material 210 than other vanes in which the hard coating 220 is in close contact with the base material 210 via the porous layer 217, and can prevent the hard coating 220 from peeling off from the tip end surface 127a.
[0049] In addition, the porous layer 217 has the characteristics of being hard but brittle. Therefore, the vane 127 of Example 1 in which the dense layer 213 is exposed on the surface of the base material 210 by removing the porous layer 217 and then the hard coating 220 is formed so as to adhere to the dense layer 213 can prevent abnormal wear caused by the porous layer 217 falling off during sliding at high surface pressure, compared to other vanes in which the hard coating 220 and the base material 210 are adhered to each other via the porous layer 217.
[0050] When the hard film 220 is formed by sputtering using metallic chromium Cr as the target 232, the hard film 220 made of chromium nitride (CrN) may be difficult to form depending on the film forming apparatus 240. On the other hand, the hard film 220 made of dichromium nitride (Cr2N) is likely to be formed stably regardless of the film forming apparatus 240. Therefore, by using dichromium nitride (Cr2N) as the hard film 220 as in the embodiment, the hard film 220 can be formed stably even by using the sputtering method.
[0051] In the vane of the comparative example, the hard coating 220 is formed by an arc ion plating method different from the sputtering method, and other parts are formed in the same manner as the vane 127 of the above-mentioned Example 1. Fig. 10 is a cross-sectional view showing another film forming apparatus 230 for forming the hard coating 220 on the tip surface 129a of the vane 127 of the comparative example by the arc ion plating method. The film forming apparatus 240 includes a furnace 241 and a target 232. A processing chamber 243 is formed inside the furnace 241. The target 242 is made of metallic chromium Cr.
[0052] After the plurality of base materials 210 are arranged in the processing chamber 243, the film forming apparatus 240 reduces the pressure inside the processing chamber 243 and introduces nitrogen gas N2 into the processing chamber 243. After the nitrogen gas N2 is introduced into the processing chamber 243, the film forming apparatus 240 generates an arc in the processing chamber 243 and heats the target 242. The metal chromium Cr forming the target 242 evaporates when the target 242 is heated. At this time, the target 242 (metal chromium Cr) melted by the heating does not ionize, and droplets having a size of several tens of μ units may be generated in the processing chamber 243. The droplets are formed, for example, from chromium nitride CrN, or dichromium nitride Cr2N, or a mixture thereof. The film forming apparatus 240 applies a voltage so that the evaporated metal chromium Cr is positively charged and the plurality of base materials 210 are negatively charged. When a voltage is applied, the evaporated metallic chromium Cr adheres to the tip surfaces 129a of the plurality of base materials 210 together with nitrogen atoms N. As a result, a hard coating 220 made of dichromium nitride CrN is formed on the tip surfaces 129a of the plurality of base materials 210.
[0053] At this time, the droplets generated in the treatment chamber 243 may not be ionized, but may adhere to the tip surface 129a of the base material 210 together with the evaporated metallic chromium Cr, and may be taken into the hard coating 220. For this reason, as shown in FIG. 11, the hard coating 220 of the vane of the comparative example may have protrusions 245 formed from the droplets. FIG. 11 is a perspective view showing the surface of the hard coating 220 of the vane of the comparative example. When the protrusions 245 are formed on the tip surface 129a of the vane of the comparative example, the vane of the comparative example is highly aggressive to the sliding counterpart that slides against the tip surface 129a of the vane of the comparative example. For this reason, in the compressor equipped with the vane of the comparative example, the protrusions 245 come into contact with the upper piston 125T or the lower piston 125S, so that the upper piston 125T or the lower piston 125S is easily worn. Therefore, the amount of wear on the surface of the upper piston 125T or the lower piston 125S caused by the vane of the comparative example is greater than the amount of wear on the surface of the upper piston 125T or the lower piston 125S caused by the vane 127 of the first embodiment described above.
[0054] The vane 127 of Example 1, in which the hard coating 220 is formed by a sputtering method, can prevent droplets from being generated in the processing chamber 243 and can prevent the protrusions 245 from being formed on the tip end surface 129a. Therefore, the vane 127 of Example 1 can reduce wear on the surface of the upper piston 125T or the lower piston 125S compared to the vane of the comparative example.
[0055] (Effect of vane 127 in embodiment 1) The vane 127 of embodiment 1 is used in a compressor 1 that includes an upper cylinder 121T (lower cylinder 121S), an upper piston 125T (lower piston 125S) that revolves along the inner surface of the upper cylinder 121T (lower cylinder 121S), and an upper end plate 160T (lower end plate 160S, intermediate partition plate 140) that closes the end of the upper cylinder 121T (lower cylinder 121S), and divides the upper cylinder chamber (lower cylinder chamber) surrounded by the upper cylinder 121T (lower cylinder 121S), the upper piston 125T (lower piston 125S), and the upper end plate 160T (lower end plate 160S, intermediate partition plate 140) into an upper suction chamber 131T (lower suction chamber 131S) and an upper compression chamber 133T (lower compression chamber 133S). The vane 127 includes a nitrided base material 210 and a hard coating 220 that covers a tip surface 129a of the base material 210. The hard coating 220 is formed by a sputtering method. This makes it possible for the vane 127 to prevent droplet-derived protrusions 245 formed on another hard coating formed by an arc ion plating method from being formed on the tip surface 129a. Therefore, the vane 127 of the first embodiment can reduce wear of the upper piston 125T (lower piston 125S) that contacts the tip surface 129a while ensuring the hardness of the tip surface 129a by the hard coating 220.
[0056] Furthermore, the Vickers hardness of the hard coating 220 of the vane 127 of Example 1 is 1500 HV or more. This allows the vane 127 to properly ensure the wear resistance of the tip surface 129a. For example, the hard coating 220 is made of dichromium nitride Cr2N. This allows the vane 127 to properly ensure the wear resistance of the tip surface 129a against the upper piston 125T (lower piston 125S).
[0057] Moreover, the base material 210 of the vane 127 of the first embodiment is formed from a material with a chromium content of more than 4.5 wt%, for example, stainless steel with a chromium content of 10.5 wt% or more. For example, the base material 210 of the vane 127 of the first embodiment is formed from martensitic stainless steel with a chromium (Cr) content of about 16 [wt%] to 18 [wt%]. In this way, the vane 127 can ensure sufficient wear resistance and seizure resistance especially for the first side surface 129b, the second side surface 129c, the first end surface 129d, and the second end surface 129e, which have a large sliding area, because the base material layer 211 of the base material 210 has a high chromium (Cr) content.
[0058] Moreover, the base material 210 of the vane 127 of Example 1 is formed with a base material layer 211, a nitride diffusion layer 212 formed outside the base material layer 211, and a dense layer 213 made of a gamma prime phase mainly composed of iron nitride Fe4N formed outside the nitride diffusion layer 212. At this time, the hard coating 220 is formed on the surface of the dense layer 213. Such a vane 127 can strongly adhere the hard coating 220 to the base material 210 and can prevent the hard coating 220 from peeling off from the tip end surface 127a.
[0059] In addition, the base material 210 of the vane 127 of the first embodiment further includes a first side surface 129b and a second side surface 129c that slide against the upper cylinder 121T (lower cylinder 121S), and a first end surface 129d (second end surface 129e) that slides against the upper end plate 160T (lower end plate 160S, intermediate partition plate 140). The first side surface 129b and the second side surface 129c and the first end surface 129d (second end surface 129e) of the base material 210 have a dense layer 213 made of a gamma prime phase mainly composed of iron nitride Fe4N exposed on the outer surface. Such a vane 127 can also sufficiently ensure wear resistance and seizure resistance for the sliding surfaces other than the tip surface 129a (the first side surface 129b, the second side surface 129c, the first end surface 129d, and the second end surface 129e).
[0060] The manufacturing method of the vane of Example 1 is a manufacturing method used when manufacturing the vane 127 of Example 1, and includes a step of nitriding the base material 210 (step S1), and a step of forming the hard coating 220 by a sputtering method after nitriding the base material 210 (step S3). According to this manufacturing method of the vane, it is possible to prevent the projections 245 derived from the droplets from being formed on the tip surface 129a. Therefore, the vane 127 manufactured by this manufacturing method of the vane can reduce wear of the upper piston 125T (lower piston 125S) that contacts the tip surface 129a.
[0061] Moreover, the vane manufacturing method of Example 1 further includes a step (step S2) of exposing the dense layer 213 made of the gamma prime phase mainly made of iron nitride Fe4N at the tip end surface 129a of the base material 210 by removing the porous layer 217 made of the epsilon phase mainly made of iron nitride Fe2N, Fe3N, prior to the step (step S3) of forming the hard coating 220 on the tip end surface 129a of the base material 210. Such a vane manufacturing method can form the hard coating 220 on the surface of the dense layer 213, and can appropriately manufacture the vane 127 that can prevent the hard coating 220 from peeling off the tip end surface 129a.
[0062] Moreover, the vane manufacturing method of Example 1 further includes a step (step S2) of exposing dense layer 213 made of gamma prime phase mainly composed of iron nitride Fe4N on the outer surfaces of first side surface 129b, second side surface 129c, first end face 129d, and second end face 129e of base material 210. Such a vane manufacturing method can appropriately manufacture vane 127 that can ensure sufficient wear resistance and seizure resistance also for first side surface 129b, second side surface 129c, first end face 129d, and second end face 129e, which are sliding surfaces other than tip face 129a.
[0063] The base material 210 further includes a first side surface 129b and a second side surface 129c that slide against the upper cylinder 121T (lower cylinder 121S), and a first end surface 129d (second end surface 129e) that slides against the upper end plate 160T (lower end plate 160S, intermediate partition plate 140). In the vane manufacturing method of the first embodiment, in the step (step S3) of forming the hard coating 220 on the base material 210, the multiple base materials 210 are arranged so that the first side surfaces 129b and the second side surfaces 129c or the first end surfaces 129d (second end surfaces 129e) of the adjacent base materials 210 are in contact with each other, and the hard coating 220 is formed on each tip surface 129a of the multiple base materials 210 at once. In such a vane manufacturing method, the manufacturing cost of the vane 127 can be reduced. EXAMPLES
[0064] As shown in Figures 12 and 13, the vane of Example 2 is the same as the vane 127 of Example 1 described above, except that the dense layer 213 of the vane 127 of Example 1 described above is omitted. Figure 12 is a cross-sectional view showing the vane of Example 2. Figure 13 is a schematic diagram for explaining the manufacturing method of the vane of Example 2. Figure 13 shows that the properties of the vane 127 change in the order of Figures 13(a) to 13(d) by the manufacturing method of the vane of Example 2.
[0065] The vane of Example 2 has a hard coating 220 formed over the entire tip surface 129a, similar to the vane 127 of Example 1 described above. The hard coating 220 is formed on the surface of the nitrided diffusion layer 212 of the base material 210 and is in close contact with the nitrided diffusion layer 212. The vane of Example 2 differs from the vane of Example 1 in that the hard coating 220 is in close contact with the nitrided diffusion layer 212 as a result of not only the porous layer 217 but also the dense layer 213 being removed in a process of scraping the surface of the base material 210, which will be described later.
[0066] The manufacturing method of the vane of Example 2 is a method for manufacturing the vane 127 of Example 2, and as shown in FIG. 13, steps S2 and S3 of the manufacturing method of the vane of Example 1 described above are replaced with steps S4 and S5, respectively, and the other parts are the same as the manufacturing method of the vane of Example 1 described above. FIG. 13 is a schematic diagram for explaining an example of a forming process of the hard coating 220 in Example 2. Step S1 of the manufacturing method of the vane of Example 2 is the same as step S1 of the manufacturing method of the vane of Example 1 described above, as shown in FIG. 13(a) and FIG. 13(b). As shown in FIG. 13(c), after the base material 210 is nitrided in step S1, the surface of the base material 210 is scraped, and the dense layer 213 and the porous layer 217 are removed so that the nitrided diffusion layer 212 is exposed on the surface of the base material 210 (step S4). That is, in step S4, the entire nitride compound layer 216 (white layer) of the nitride layer 214 is removed. As shown in Fig. 13(d), after the surface of the base material 210 is scraped in step S4, a hard coating 220 is formed on the nitride diffusion layer 212 of the tip end face 129a of the base material 210 (step S5). According to such a vane manufacturing method, the vane 127 of Example 2 is appropriately manufactured so that the hard coating 220 is formed on the surface of the nitride diffusion layer 212 of the base material 210 and adheres closely to the nitride diffusion layer 212.
[0067] The adhesion of the hard coating 220 to the nitride diffusion layer 212 is roughly equivalent to the adhesion of the hard coating 220 to the dense layer 213, and is better than the adhesion of the hard coating 220 to the porous layer 217. For this reason, like the vane 127 of the above-described embodiment 1, the vane of embodiment 2 can more strongly adhere the hard coating 220 to the base material 210 and can prevent the hard coating 220 from peeling off from the tip end surface 127a, compared to other vanes in which the hard coating 220 and the base material 210 are in close contact with each other via the porous layer 217.
[0068] In the vane of Example 2, the nitride diffusion layer 212 is exposed on the surface on which the hard coating 220 is not formed, and the first side surface 129b, the second side surface 129c, the first end surface 129d, and the second end surface 129e are formed from the nitride diffusion layer 212. Like the dense layer 213, the nitride diffusion layer 212 has better wear resistance and seizure resistance than the base material layer 211. Therefore, like the vane 127 of Example 1 described above, the vane of Example 2 can ensure wear resistance and seizure resistance even on the surface on which the hard coating 220 is not formed.
[0069] In the vane manufacturing method of the second embodiment described above, the entire surface of the base material 210 is scraped off so that both the dense layer 213 and the porous layer 217 are removed in step S4, but the surface of the base material 210 may be scraped off so that the dense layer 213 remains on a surface (side surface / end surface) other than the tip surface 129a. In the vane manufactured by such a vane manufacturing method, as in the vane of the second embodiment described above, the hard coating 220 is in close contact with the nitride diffusion layer 212 of the tip surface 129a, so that the hardness of the tip surface 129a, which requires particularly high wear resistance, is ensured by the hard coating 220, while peeling of the hard coating 220 from the tip surface 129a can be prevented, and furthermore, the wear resistance and seizure resistance of the sliding surfaces (side surface / end surface) other than the tip surface 129a on which the hard coating 220 is not formed can be ensured by the dense layer 213.
[0070] In the vane manufacturing method of the above-mentioned embodiment, in step S2 in embodiment 1 and in step S4 in embodiment 2, the entire surface of the base material 210 is scraped off so as to remove the porous layer 217, but the base material 210 may be scraped off so as to leave the porous layer 217 on a surface (side surface / end surface) other than the tip surface 129a. In the vane manufactured by such a vane manufacturing method, as in the vane of the above-mentioned embodiment, the hard coating 220 is in close contact with the dense layer 213 or the nitride diffusion layer 212 on the tip surface 129a where particularly high wear resistance is required, so that the hard coating 220 can be prevented from peeling off from the tip surface 129a, and further, the wear resistance and seizure resistance of the surface on which the hard coating 220 is not formed can be ensured by the porous layer 217 (nitride compound layer 216).
[0071] In the vane manufacturing method of the embodiment described above, the hard coating 220 is formed on the tip surfaces 129a of the plurality of base materials 210 with the side surfaces and end surfaces in close contact with each other, but the hard coating 220 may be formed on the tip surfaces 129a of the plurality of base materials 210 with the side surfaces and end surfaces not in close contact with each other. In this case, the surfaces (side surfaces and end surfaces) of the plurality of base materials 210 different from the tip surfaces 129a may be masked so that the hard coating 220 is not formed.
[0072] Incidentally, in the vanes of the previously described embodiments, the hard coating 220 is formed on the surface of the dense layer 213 or the nitride diffusion layer 212, but the hard coating 220 may be formed on the surface of the base material layer 211 in close contact with the base material layer 211. In such a vane, the hard coating 220 is formed by sputtering, which prevents the formation of protrusions 245 on the tip end surface 129a, and reduces wear on the surface of the upper piston 125T or the lower piston 125S, just like in the vanes of the previously described embodiments.
[0073] In the above-described embodiment, a two-cylinder rotary compressor having two cylinders 121, an upper cylinder 121T and a lower cylinder 121S, has been exemplified as the compressor 1, but it may also be a one-cylinder rotary compressor having only one cylinder 121.
[0074] Although the embodiments have been described above, the embodiments are not limited to the above. The above-described components include those that can be easily imagined by a person skilled in the art, those that are substantially the same, and those that are within the so-called equivalent range. Furthermore, the above-described components can be appropriately combined. Furthermore, at least one of various omissions, substitutions, and modifications of the components can be made without departing from the gist of the embodiments. [Explanation of symbols]
[0075] 1 Compressor 121T Upper cylinder (cylinder) 121S Lower Cylinder (Cylinder) 125T Upper piston (piston) 125S Lower piston (piston) 127 Vane 127T Upper vane (vane) 127S Lower vane (vane) 129a Tip surface 129b 1st side 129c 2nd side 129d 1st end face 129e 2nd end face 160T Upper end plate (end plate) 160S Lower end plate (end plate) 210 Base material 211 Base material layer 212 Nitrided layer 213 Layer compacta 214 Nitrided layer 216 Nitride layer 217 Porous Layer 220 Hard Coating
Claims
1. A cylinder; A piston that revolves along an inner circumferential surface of the cylinder; an end plate that closes an end of the cylinder; The compressor is used in a compressor having a vane that divides a cylinder chamber surrounded by the cylinder, the piston, and the end plate into a suction chamber and a compression chamber, A nitrided base material; A hard coating covering a tip surface of the base material, The hard coating is a hard coating formed by a sputtering method. Vane.
2. The hard coating has a Vickers hardness of 1500 HV or more. The vane of claim 1 .
3. The hard coating is made of Cr 2 Formed from N The vane of claim 1 .
4. The base material is formed from a material having a chromium content of more than 4.5 wt %. The vane of claim 1 .
5. The base material is made of stainless steel having a chromium content of 10.5 wt % or more.
5. The vane of claim 4.
6. The base material is made of martensitic stainless steel.
6. The vane of claim 5.
7. The base material has a base layer and a nitride diffusion layer formed outside the base layer, The hard coating is formed on the surface of the nitride diffusion layer. The vane of claim 1 .
8. The base material includes a base layer, a nitride diffusion layer formed outside the base layer, and an FeNb layer formed outside the nitride diffusion layer. 4 A dense layer consisting of a gamma prime phase mainly composed of N is formed, The hard coating is formed on the surface of the dense layer. The vane of claim 1 .
9. The base material further includes a side surface that slides against the cylinder and an end surface that slides against the end plate, The side and end faces of the base material are formed of the nitride diffusion layer or the Fe 4 A dense layer consisting of a gamma prime phase mainly composed of N, or Fe 2 N, Fe 3 Any one of the porous layers containing N as a main component is exposed on the outer surface of each of the side surface and the end surface. The vane of claim 8.
10. A vane according to any one of claims 1 to 9; The cylinder; The piston; The end plate; A compressor comprising:
11. A cylinder; A piston that revolves along an inner circumferential surface of the cylinder; an end plate that closes an end of the cylinder; The compressor is used in a compressor having a cylinder chamber surrounded by the cylinder, the piston and the end plate is divided into a suction chamber and a compression chamber, A base material; A hard coating covering a tip surface of the base material; Equipped with A method for manufacturing a vane, comprising: A step of subjecting the base material to a nitriding treatment; a step of forming the hard coating by a sputtering method after nitriding the base material; Equipped A method for manufacturing a vane.
12. the base material of the vane is formed from a material having a chromium content of greater than 4.5 wt. %; Prior to the step of forming the hard coating on the tip surface of the base material, the base material is subjected to a nitriding treatment to form a nitride layer on the base material, the nitride layer being at least Fe 2 N, Fe 3 By removing the porous layer made of the epsilon phase mainly composed of N, a nitride diffusion layer or an Fe diffusion layer is formed on the tip surface of the base material. 4 The method further includes a step of exposing any layer of a dense layer consisting of a gamma prime phase mainly composed of N, In the step of forming the hard coating on the tip end surface of the base material, the hard coating is formed on the tip end surface of the base material where the nitride diffusion layer or the dense layer is exposed. A method for manufacturing a vane according to claim 11.
13. The base material further includes a side surface that slides against a vane groove formed in the cylinder, and an end surface that slides against the end plate, A nitride diffusion layer or an Fe diffusion layer is formed on the side surface and the end surface of the base material. 4 A dense layer consisting of a gamma prime phase mainly composed of N, or Fe 2 N, Fe 3 The method further includes a step of exposing any one of the porous layers made of an epsilon phase mainly composed of N on the outer surfaces of the side surface and the end surface, A method for manufacturing a vane according to claim 12.
14. The base material further includes a side surface that slides against the cylinder and an end surface that slides against the end plate, In the step of forming the hard coating on the base material, A plurality of base materials are arranged so that the side surfaces or the end surfaces of adjacent base materials are in contact with each other, and the hard coating is formed on each tip surface of the plurality of base materials at once. A method for manufacturing a vane according to claim 11.
Citation Information
Patent Citations
Rotary type fluid compressor
JP1993078792A
Vane for rotary compressor
JP2000136784A
Nitrided vane for rotary compressor and its manufacturing method
JP2005016386A
Vane for refrigerant compressors, method of manufacturing the same and refrigerant compressor
JP2005048687A
Coating film deposition method, and coating base material
JP2007191751A