Laminated film, and retort pouch
The laminated film with a high-melting-point base layer and controlled DSC55% temperature sealant layer addresses the need for low-temperature sealing without deformation, ensuring efficient and aesthetically pleasing heat sealing.
Patent Information
- Application Number
- JP2023056198
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
There is a demand for laminated films that can be heat-sealed at relatively low temperatures without shrinking or deforming in the heat-sealed area, while maintaining a good appearance, due to the increased speed of packaging bag formation and reduced heat sealing time.
A laminated film comprising a biaxially stretched base layer with a thermoplastic resin having a melting point of 161°C or higher and an unstretched sealant layer containing a propylene-based polymer, where the DSC55% temperature is between 130°C and 153°C, allowing for controlled melting during sealing.
The laminated film can be heat-sealed at a lower temperature with improved appearance and reduced deformation, enhancing the sealing process efficiency and product quality.
Smart Images

Figure 2024143485000001 
Figure 2024143485000002 
Figure 2024143485000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminate film and a retort pouch comprising the laminate film. [Background technology]
[0002] As various packaging materials, laminated films having a base layer and a sealant layer are widely used. Such laminated films can be formed into packaging bags (bag-making) by heat-sealing them with the sealant layer facing inward to form a storage space.
[0003] Such a packaging bag can be used, for example, as a retort food packaging bag such as a retort pouch. A package formed by heat sealing such a retort food packaging bag with an article contained therein may be heated for the purpose of sterilization or the like. For example, Patent Document 1 discloses a multilayer film with excellent heat resistance as a film used for this type of retort food packaging bag. The multilayer film includes a base layer containing a propylene-based polymer and an ethylene-propylene copolymer in a predetermined ratio, and a sealant layer containing a propylene-based polymer, an ethylene-propylene copolymer, and a predetermined propylene copolymer in a predetermined ratio. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent Publication No. 2022-102606 Summary of the Invention [Problem to be solved by the invention]
[0005] In recent years, the speed at which packaging bags are formed using the above-mentioned laminated film has been increasing, and the time required for heat sealing has been shortened. For this reason, there is a demand for a laminated film having a sealant layer that can be heat-sealed at a relatively low temperature. In addition, there is a demand for a laminated film that has a good appearance and does not shrink or deform at the heat-sealed portion where the sealant layers are opposed to each other when a packaging bag is formed using the laminated film.
[0006] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a laminated film that can be heat-sealed at a relatively low temperature and has a good appearance at the heat-sealed area, and a retort pouch including the laminated film. [Means for solving the problem]
[0007] The laminated film according to the present invention is a laminated film comprising a base layer and a sealant layer, wherein the base layer is a biaxially stretched film containing a thermoplastic resin having a melting point of 161°C or higher, or formed from a thermoplastic resin composition containing the thermoplastic resin and having a melting point of 161°C or higher, and the sealant layer is an unstretched film containing a propylene-based polymer, and the temperature T' at which the cumulative change in heat of fusion from 50°C to temperature T', which accounts for 55% of the cumulative change in heat of fusion from 50°C to 200°C observed by DSC of the unstretched film, is from 130°C to 153°C.
[0008] The retort pouch according to the present invention comprises the above-mentioned laminate film. Effect of the Invention
[0009] According to the present invention, it is possible to provide a laminate film that can be heat-sealed at a relatively low temperature and has a good appearance at the heat-sealed area, and a retort pouch including said laminate film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The following describes embodiments of the present invention, but the present invention is not limited to the following embodiments. The present invention is not limited to the configurations described below, and various modifications are possible within the scope of the claims. The embodiments and examples obtained by appropriately combining the technical means disclosed in the different embodiments and examples are also included in the technical scope of the present invention.
[0011] The laminated film according to this embodiment includes a base layer and a sealant layer.
[0012] <Base material layer> The substrate layer is a biaxially stretched film containing a thermoplastic resin having a melting point of 161°C or higher, or formed from a thermoplastic resin composition containing the thermoplastic resin and having a melting point of 161°C or higher.
[0013] Examples of the thermoplastic resin used in the base layer include polyethylene terephthalate (PET), nylon 6, nylon 6,6, and propylene-based polymers. Among these, the thermoplastic resin is preferably a propylene-based polymer. The thermoplastic resin may be used alone or in combination of two or more kinds.
[0014] The propylene-based polymer is a polymer containing 50% by mass or more of monomer units based on propylene, and may be a propylene homopolymer or a propylene-based copolymer. The propylene-based copolymer may contain monomer units based on ethylene and / or an α-olefin having 4 to 12 carbon atoms. Examples of the α-olefin having 4 to 12 carbon atoms include 1-butene, 1-hexene, and 1-octene, and 1-butene is preferred. From the viewpoint of improving heat resistance, the propylene-based polymer is preferably a propylene homopolymer. The base layer may contain two or more propylene-based polymers having different types and contents of monomer units.
[0015] The melting point of the thermoplastic resin used in the base layer is 161° C. or higher, and from the viewpoint of improving heat resistance, is preferably 163° C. or higher, and more preferably 165° C. or higher.
[0016] From the viewpoint of improving heat resistance, the content of the thermoplastic resin having a melting point of 161° C. or more is preferably 95 mass % or more, and more preferably 98 mass % or more, based on the total mass of the base layer.
[0017] The thermoplastic resin composition having a melting point of 161° C. or more used in the base layer contains the above-mentioned thermoplastic resin having a melting point of 161° C. or more. The content of the thermoplastic resin having a melting point of 161° C. or more is preferably 95% by mass or more, and more preferably 98% by mass or more, based on the total mass of the thermoplastic resin composition, from the viewpoint of improving heat resistance. From the viewpoint of improving heat resistance, the thermoplastic resin composition is preferably a propylene-based polymer composition having a melting point of 161° C. or more, which contains a propylene-based polymer having a melting point of 161° C. or more.
[0018] In one embodiment, from the viewpoint of improving heat resistance, the base layer contains a propylene-based polymer having a melting point of 161°C or higher, or is formed from a propylene-based polymer composition containing the propylene-based polymer and having a melting point of 161°C or higher.
[0019] The melting point of the thermoplastic resin composition is preferably 163° C. or higher, and more preferably 165° C. or higher, from the viewpoint of improving heat resistance.
[0020] <Sealant layer> The sealant layer is an unstretched film containing a propylene-based polymer, and the temperature T' at which the cumulative change in heat of fusion from 50°C to temperature T' accounts for 55% of the cumulative change in heat of fusion from 50°C to 200°C observed by DSC of the unstretched film is from 50°C to temperature T' is 130°C or more and 153°C or less.
[0021] The temperature T' (unit: °C) at which the cumulative heat of fusion change, which accounts for 55% of the cumulative heat of fusion change from 50°C to 200°C observed by DSC of the unstretched film used in the sealant layer, occurs from 50°C to temperature T' is measured by the following measurement method. Hereinafter, temperature T' may be referred to as DSC 55% temperature (unit: °C).
[0022] [Measuring method for DSC 55% temperature (T') (unit: °C)] Using a temperature modulated differential scanning calorimeter (Q100 manufactured by TA Instruments), about 5 mg of the sealant layer is cooled to 0°C under a nitrogen gas atmosphere (nitrogen gas flow rate 50 ml / min). Next, after holding at 0°C for 5 minutes, the temperature is raised to 230°C at an average heating rate of 2°C / min, a temperature modulation amplitude of ±0.5°C, and a temperature modulation period of 1 minute, and the temperature is measured to obtain a reversing heat flow (specific heat component). Using the same differential scanning calorimeter, about 4 mg of indium (In) is heated to an equilibrium temperature of 110°C under a nitrogen gas atmosphere (nitrogen gas flow rate 50 ml / min), and then heated at a heating rate of 5°C / min to 180°C. The maximum peak start temperature of the obtained melting endothermic curve was taken as the onset temperature, which was 156.6°C.
[0023] For the reversing heat flow value Q(T) for a temperature T between 50°C and 200°C, the straight line connecting the amount of heat Q(50) at 50°C and the amount of heat Q(200) at 200°C is taken as the baseline, and the amount of heat Q'(T) of reversing heat flow after baseline correction at a certain temperature T is defined as the following equation (2).
[0024]
number
[0025] Starting from 50°C, the integral of the reversing heat flow after baseline correction up to a temperature T' in the range from 50°C to 200°C is defined as A(T') in the following equation (3).
[0026]
number
[0027] Regarding A(T'), the temperature T' that satisfies the following formula (4) is defined as the temperature T' at which the cumulative change in heat of fusion that accounts for 55% of the cumulative change in heat of fusion is from 50°C to temperature T'.
[0028]
number
[0029] The DSC 55% temperature (T') of the laminate film according to this embodiment is from 130° C. to 153° C., preferably from 130° C. to 150° C., and more preferably from 135° C. to 150° C. When the DSC 55% temperature (T') of the laminate film is in the above range, the surface layer of the film melts effectively during the manufacturing process of the package, making the package easier to seal, and therefore the minimum sealable temperature can be lowered.
[0030] By changing the type and content of the monomer units other than propylene contained in the propylene-based polymer used in the sealant layer, the surface layer of the film becomes easier to melt, and the DSC55% temperature can be controlled. Specifically, ethylene and α-olefins having 4 to 12 carbon atoms can be used as the type of monomer units other than propylene, and the DSC55% temperature can be lowered by using ethylene rather than α-olefins having 5 to 12 carbon atoms, and the DSC55% temperature can be lowered by using α-olefins having 4 carbon atoms rather than ethylene. The DSC55% temperature can also be lowered by increasing the total content of monomer units other than propylene contained in the propylene-based polymer. When a plurality of propylene-based polymers and / or α-olefin-based polymers are contained, the DSC55% temperature can be controlled by changing the type and content of monomer units other than propylene as an average of each polymer. To increase the DSC55% temperature, the opposite operation can be performed, and the DSC55% temperature can be controlled by appropriately adjusting the type and amount of monomer units other than propylene used in the sealant layer as described above.
[0031] Examples of the propylene-based polymer contained in the sealant layer include a propylene-based polymer mainly composed of a structural unit derived from propylene, a propylene-α-olefin copolymer containing a structural unit derived from propylene and a structural unit derived from an α-olefin, and a heterophasic propylene polymer material.
[0032] <Propylene-based polymer containing propylene as the main component (component A)> The propylene-based polymer (component A) mainly composed of structural units derived from propylene contains 98% by mass or more of structural units derived from propylene. The content of the structural units derived from propylene in the propylene-based polymer (component A) is preferably 99% by mass or more and 100% by mass or less, more preferably 100% by mass. That is, the propylene-based polymer (component A) may be a propylene homopolymer.
[0033] The propylene polymer (component A) may contain a structural unit derived from at least one selected from the group consisting of ethylene and an α-olefin having 4 to 12 carbon atoms. The content of the structural unit derived from at least one selected from the group consisting of ethylene and an α-olefin having 4 to 12 carbon atoms in the propylene polymer (component A) is preferably 2 mass% or less, and more preferably more than 0 mass% and 1 mass% or less.
[0034] <Propylene-based random copolymer (component B)> The propylene-based random copolymer (component B) of propylene and a monomer other than propylene may be a propylene-based random copolymer (component B) containing more than 40% by mass and less than 85% by mass of structural units derived from propylene and more than 15% by mass and less than 60% by mass of structural units derived from at least one selected from the group consisting of ethylene and α-olefins having 4 to 12 carbon atoms.
[0035] The content of structural units derived from propylene in the propylene random copolymer (component B) is preferably more than 50% by mass and not more than 85% by mass, more preferably more than 50% by mass and not more than 80% by mass, and even more preferably 60% by mass or more and not more than 80% by mass. The content of structural units derived from at least one selected from the group consisting of ethylene and α-olefins having 4 to 12 carbon atoms is preferably 15% by mass or more and less than 50% by mass, more preferably 20% by mass or more and less than 50% by mass, and even more preferably 20% by mass or more and not more than 40% by mass.
[0036] In one embodiment, the propylene-based random copolymer (component B) preferably contains more than 50% by mass and less than 85% by mass of structural units derived from propylene and more than 15% by mass and less than 50% by mass of structural units derived from ethylene, from the viewpoint of excellent heat seal strength at low temperatures.
[0037] <Heterophasic propylene polymer material (component 1)> The heterophasic propylene polymerization material (component 1) is composed of a propylene-based polymer (component 1-1) containing 98% by mass or more of structural units derived from propylene, and a propylene-α-olefin copolymer (component 1-2) containing more than 50% by mass and 85% by mass or less of structural units derived from propylene and 15% by mass or more and less than 50% by mass of structural units derived from at least one selected from the group consisting of ethylene and α-olefins having 4 to 12 carbon atoms.
[0038] The propylene-based polymer (component 1-1) constituting the heterophasic propylene polymerization material (component 1) contains 98% by mass or more of structural units derived from propylene. The content of the structural units derived from propylene in the propylene-based polymer (component 1-1) is preferably 99% by mass or more and 100% by mass or less, more preferably 100% by mass. That is, the propylene-based polymer (component 1-1) may be a propylene homopolymer.
[0039] The propylene polymer (component 1-1) may contain a structural unit derived from at least one selected from the group consisting of ethylene and an α-olefin having 4 to 12 carbon atoms. The content of the structural unit derived from at least one selected from the group consisting of ethylene and an α-olefin having 4 to 12 carbon atoms in the propylene polymer (component 1-1) is preferably 2 mass% or less, and more preferably more than 0 mass% and 1 mass% or less.
[0040] The propylene-α-olefin copolymer (component 1-2) constituting the heterophasic propylene polymerization material (component 1) contains more than 50 mass% and 85 mass% or less of structural units derived from propylene, and 15 mass% or more and less than 50 mass% of structural units derived from at least one selected from the group consisting of ethylene and α-olefins having 4 to 12 carbon atoms.
[0041] The content of structural units derived from propylene in the propylene-α-olefin copolymer (component 1-2) is preferably more than 50% by mass and not more than 80% by mass, more preferably from 60% by mass to 80% by mass. The content of structural units derived from at least one selected from the group consisting of ethylene and α-olefins having 4 to 12 carbon atoms is preferably from 20% by mass to less than 50% by mass, more preferably from 20% by mass to 40% by mass.
[0042] In one embodiment of the heterophasic propylene polymer material (component 1), the propylene-based polymer (component 1-1) is preferably a propylene homopolymer, and the propylene-α-olefin copolymer (component 1-2) is preferably a propylene-ethylene copolymer. In this case, the content of the propylene homopolymer (component 1-1) is preferably 50% by mass or more and 90% by mass or less, more preferably 60% by mass or more and 90% by mass or less, and even more preferably 60% by mass or more and 80% by mass or less, based on the total mass of the propylene homopolymer (component 1-1) and the propylene-ethylene copolymer (component 1-2), from the viewpoint of excellent balance between heat sealability and blocking resistance. Furthermore, the content of the propylene-ethylene copolymer (component 1-2) relative to the total mass of the propylene homopolymer (component 1-1) and the propylene-ethylene copolymer (component 1-2) is preferably 10% by mass or more and 50% by mass or less, more preferably 10% by mass or more and 40% by mass or less, and even more preferably 20% by mass or more and 40% by mass or less, from the viewpoint of achieving an excellent balance between heat sealability and blocking resistance.
[0043] In one embodiment of a heterophasic propylene polymerization material consisting of a propylene homopolymer (component 1-1) and a propylene-ethylene copolymer (component 1-2), the propylene-ethylene copolymer (component 1-2) preferably has a content of structural units derived from propylene of more than 50% by mass and less than 85% by mass, and a content of structural units derived from ethylene of more than 15% by mass and less than 50% by mass, from the viewpoint of excellent heat seal strength at low temperatures.
[0044] Examples of the α-olefin having 4 to 12 carbon atoms used in the propylene polymer (component A), the propylene random copolymer (component B) and the heterophasic propylene polymerization material (component 1) include 1-butene, 1-hexene, 1-octene, etc., and preferably 1-butene. The structural unit derived from the α-olefin having 4 to 12 carbon atoms may be a structural unit derived from one kind of α-olefin alone, or may be a structural unit derived from two or more kinds of α-olefins.
[0045] The propylene polymer (component A), the propylene random copolymer (component B) and the heterophasic propylene polymerization material (component 1) can be produced by polymerizing the raw material propylene with ethylene and / or an α-olefin using a Ziegler-Natta catalyst, a metallocene catalyst or the like.
[0046] Methods for polymerizing the propylene-based polymer (component A), the propylene-based random copolymer (component B) and the heterophasic propylene polymerization material (component 1) include a method of polymerizing in an inert solvent such as hexane, heptane, toluene, or xylene, a method of polymerizing in liquid propylene or ethylene, a method of adding a catalyst to gaseous propylene or ethylene and polymerizing in the gas phase, or a method of polymerizing by combining these methods.
[0047] From the viewpoint of productivity, the method for producing the heterophasic propylene polymerization material (component 1) is preferably a method in which a first step is carried out to produce a propylene-based polymer (component 1-1) substantially in the absence of an inert solvent, and then a second step is carried out to produce a propylene-α-olefin copolymer (component 1-2) by polymerizing propylene and at least one member selected from the group consisting of ethylene and α-olefins having 4 to 12 carbon atoms in a gas phase in the presence of the propylene-based polymer (component 1-1), thereby obtaining the heterophasic propylene polymerization material (component 1) by multistage polymerization.
[0048] Methods for adjusting the ethylene content of the propylene polymer (component 1-1) and the propylene-α-olefin copolymer (component 1-2) include a method of adding appropriate amounts of hydrogen gas, a molecular weight regulator such as a metal compound, and ethylene in each step of the polymerization, and a method of adjusting the temperature, pressure, etc. during the polymerization.
[0049] The production ratio of the propylene-based polymer (component 1-1) and the propylene-α-olefin copolymer (component 1-2) can be controlled by the polymerization time in the first and second steps, the size of the polymerization tank, the amount of the polymer held in the polymerization tank, the polymerization temperature, the polymerization pressure, etc. If necessary, drying may be performed at a temperature below the melting point of polypropylene in order to remove the residual solvent in polypropylene and ultra-low molecular weight oligomers produced as by-products during production. Examples of the drying method include the methods described in JP-A-55-75410 and JP Patent No. 2565753.
[0050] The melt flow rate (MFR) of the heterophasic propylene polymer material (component 1) obtained in the second step, measured at a temperature of 230° C. and a load of 2.16 kg, is preferably 0.001 g / 10 min to 10 g / 10 min, more preferably 0.01 g / 10 min to 10 g / 10 min, and even more preferably 0.01 g / 10 min to 5 g / 10 min, from the viewpoint of improving the processability and sanitation of the film. The MFR is measured by the method A specified in JIS K7210-1.
[0051] <Propylene-α-olefin copolymer (component 2)> The propylene-α-olefin copolymer (component 2) contains more than 85% by mass and less than 98% by mass of structural units derived from propylene, and more than 2% by mass and less than 15% by mass of structural units derived from at least one selected from the group consisting of ethylene and α-olefins having 4 to 12 carbon atoms.
[0052] The content of structural units derived from propylene in the propylene-α-olefin copolymer (component 2) is preferably 90% by mass or more and less than 98% by mass, more preferably 94% by mass or more and 97% by mass or less. The content of structural units derived from at least one selected from the group consisting of ethylene and α-olefins having 4 to 12 carbon atoms in the propylene-α-olefin copolymer (component 2) is preferably more than 2% by mass and 10% by mass or less, more preferably 3% by mass or more and 6% by mass or less.
[0053] Examples of the α-olefin having 4 to 12 carbon atoms used in the propylene-α-olefin copolymer (component 2) include 1-butene, 1-hexene, 1-octene, etc., and 1-butene is preferred. The structural unit derived from the α-olefin having 4 to 12 carbon atoms may be a structural unit derived from one type of α-olefin alone, or may be a structural unit derived from two or more types of α-olefins.
[0054] The propylene-α-olefin copolymer (component 2) may be one produced using a heterogeneous catalyst, or may be one produced using a homogeneous catalyst (for example, a metallocene catalyst, etc.).
[0055] The melt flow rate (MFR) of the propylene-α-olefin copolymer (component 2) measured at 230° C. under a load of 2.16 kg is preferably 1 g / 10 min to 10 g / 10 min, more preferably 1 g / 10 min to 8 g / 10 min, and even more preferably 2 g / 10 min to 5 g / 10 min. The MFR is measured by Method A specified in JIS K7210-1.
[0056] The melting point of the propylene-α-olefin copolymer (component 2) measured by differential scanning calorimetry (DSC) is preferably 120°C or higher and 165°C or lower, more preferably 120°C or higher and 150°C or lower, and even more preferably 125°C or higher and 150°C or lower.
[0057] <β crystal nucleating agent (ingredient 3)> The β-crystal nucleating agent (component 3) refers to a compound that can form β-crystals having a hexagonal crystal structure in a propylene-based polymer. As the β-crystal nucleating agent, various conventionally known β-crystal nucleating agents can be used. Examples of the pigment include amide compounds represented by N,N'-dicyclohexyl-2,6-naphthalenedicarboxyamide, N,N'-dicyclohexylterephthalamide, N,N'-diphenylhexanediamide, etc.; tetraoxaspiro compounds; quinacridones represented by quinacridone, quinacridonequinone, etc.; iron oxides having nanoscale sizes; calcium pimelate, potassium 1,2-hydroxystearate, alkali or alkaline earth metal salts of carboxylic acids represented by magnesium benzoate, magnesium succinate, magnesium phthalate, etc.; aromatic sulfonic acid compounds represented by sodium benzenesulfonate, sodium naphthalenesulfonate, etc.; diesters or triesters of di- or tribasic carboxylic acids; phthalocyanine pigments represented by phthalocyanine blue, etc.; two-component compounds consisting of component C which is an organic dibasic acid and component D which is an oxide, hydroxide or salt of a metal of Group IIA of the periodic table; and compositions consisting of a cyclic phosphorus compound and a magnesium compound. One or more of these may be used in combination. Among the above-mentioned β-crystal nucleating agents, from the viewpoint of excellent retort adhesion resistance, the amide compounds N,N'-dicyclohexyl-2,6-naphthalenedicarboxyamide, N,N'-dicyclohexylterephthalamide, and N,N'-diphenylhexanediamide are preferred, and N,N'-dicyclohexyl-2,6-naphthalenedicarboxyamide is more preferred. Commercially available products of N,N'-dicyclohexyl-2,6-naphthalenedicarboxyamide include, for example, NU-100 (manufactured by New Japan Chemical Co., Ltd.).
[0058] From the viewpoint of excellent retort welding resistance, the concentration of the β-crystal nucleating agent is preferably 100 ppm by mass or more and 3000 ppm by mass or less, more preferably 300 ppm by mass or more and 2000 ppm by mass or less, even more preferably 300 ppm by mass or more and 1500 ppm by mass or less, and particularly preferably 500 ppm by mass or more and 1500 ppm by mass or less, relative to the total mass of the propylene-based polymer used in the sealant layer.
[0059] In one embodiment, the sealant layer comprises a heterophasic propylene polymeric material (component 1) and further comprises at least one component selected from a propylene-α-olefin copolymer (component 2) and a β crystal nucleating agent (component 3).
[0060] In one embodiment, the sealant layer contains a heterophasic propylene polymerization material (component 1) and a propylene-α-olefin (component 2). In this case, the content of the heterophasic propylene polymerization material (component 1) is preferably 20% by mass or more and 80% by mass or less, more preferably 30% by mass or more and 80% by mass or less, and even more preferably 30% by mass or more and 70% by mass or less, based on the total mass of the heterophasic propylene polymerization material (component 1) and the propylene-α-olefin (component 2) used in the sealant layer. The content of the propylene-α-olefin (component 2) is preferably 20% by mass or more and 80% by mass or less, more preferably 20% by mass or more and 70% by mass or less, and even more preferably 30% by mass or more and 70% by mass or less, based on the total mass of the heterophasic propylene polymerization material (component 1) and the propylene-α-olefin (component 2).
[0061] In one embodiment, the sealant layer includes a heterophasic propylene polymerization material (component 1) and a β crystal nucleating agent (component 3). In another embodiment, the sealant layer includes a heterophasic propylene polymerization material (component 1), a propylene-α-olefin (component 2), and a β crystal nucleating agent (component 3). In this case, the concentration of the β crystal nucleating agent in the sealant layer is preferably 100 ppm by mass or more and 3000 ppm by mass or less from the viewpoint of excellent retort adhesion resistance.
[0062] Additives and other resins may be added to the base layer and sealant layer constituting the laminated film of this embodiment as necessary. Examples of additives include antioxidants, neutralizing agents, ultraviolet absorbers, antistatic agents, lubricants, nucleating agents, adhesives, antifogging agents, antiblocking agents, and melt flow rate regulators. Examples of antioxidants include phenol-based antioxidants, phosphorus-based antioxidants, and sulfur-based antioxidants, and a composite antioxidant having a unit having both a phenol-based antioxidant mechanism and a phosphorus-based antioxidant mechanism in one molecule can also be used. Other resins include elastomers such as styrene-butadiene-styrene copolymers and styrene-isoprene-styrene copolymers hydrogenated styrene-based copolymer rubbers.
[0063] The thermoplastic resin composition forming the biaxially stretched film, which is the base layer, can be formed by melt-kneading the thermoplastic resin used in the base layer and, if necessary, the various additives described above. The propylene-based polymer composition forming the non-stretched film, which is the sealant layer, can be formed by melt-kneading the propylene-based polymer used in the sealant layer and, if necessary, the various additives described above.
[0064] The above melt-kneading can be carried out by using a conventional method and device. For example, the above materials are mixed using a mixing device such as a Henschel mixer, a ribbon blender, or a tumble mixer, and then melt-kneaded. Alternatively, the above materials are continuously fed at a constant rate using a constant-rate feeder to obtain a homogeneous mixture, and then the mixture is melt-kneaded using a single-screw or twin-screw or more extruder, a Banbury mixer, a roll-type kneader, or the like.
[0065] The melt-kneading temperature when the thermoplastic resin composition forming the biaxially stretched film, which is the base layer, is melt-kneaded is preferably 190° C. or more and 320° C. or less, more preferably 210° C. or more and 280° C. or less. The melt-kneading temperature when the propylene-based polymer composition forming the non-stretched film, which is the sealant layer, is melt-kneaded is preferably 190° C. or more and 320° C. or less, more preferably 210° C. or more and 280° C. or less.
[0066] The films used for the base layer and the sealant layer of the laminate film of the present embodiment can be produced by subjecting the thermoplastic resin composition used for the base layer and the propylene-based polymer composition used for the sealant layer to a T-die method or an inflation method.
[0067] The film used for the base layer of the laminated film of the present embodiment can be stretched by, for example, roll stretching, tenter stretching, tubular stretching, etc. The stretching ratio is 1.5 to 20 times, preferably 2 to 15 times.
[0068] The laminated film according to the present embodiment can be formed by laminating a base material layer and a sealant layer. The method of manufacturing the laminated film by laminating the base material layer and the sealant layer may be a method of forming by stacking each layer, or a method of forming by co-extrusion, such as a dry lamination method, a T-die method, a tubular method, etc. Examples of the method of forming by co-extrusion include a method using a feed block type die in which molten resins flowing into a die from multiple extruders are combined in layers in the die, and a method using a multi-manifold type die in which molten resins flowing into a die from multiple extruders are sent to separate manifolds and combined in layers just before the lip of the die.
[0069] The thickness of the base layer is preferably 70% or more and 90% or less, more preferably 70% or more and 85% or less, and even more preferably 75% or more and 85% or less, based on the total thickness of the base layer and the sealant layer. The thickness of the sealant layer is preferably 10% or more and 30% or less, more preferably 15% or more and 30% or less, and even more preferably 15% or more and 25% or less, based on the total thickness of the base layer and the sealant layer. By making the thickness of the base layer and the sealant layer within the above range, the interlayer peeling between the base layer and the sealant layer is less likely to occur, and the laminated film has excellent heat seal strength and bag drop strength, and can suppress the occurrence of unevenness (yellow orange peel) on the surface of the laminated film when the laminated film is heated.
[0070] The thickness of the laminated film is preferably 5 μm or more and 500 μm or less, and more preferably 30 μm or more and 150 μm or less.
[0071] The laminated film may be subjected to a surface treatment such as corona discharge treatment, flame treatment, plasma treatment, or ozone treatment by a method usually adopted industrially.
[0072] The laminated film may be combined with other barrier films, transferable films, etc. to form a composite film. Examples of the barrier film include stretched nylon film, aluminum foil, polyvinylidene chloride film, etc. The thickness of the barrier film is preferably 5 μm or more and 20 μm or less. Examples of the transferable film include nylon film, biaxially stretched polypropylene film, polyethylene terephthalate film, etc. The thickness of the transferable film is preferably 10 μm or more and 20 μm or less. Examples of the method for combining the laminated film with other films include dry lamination and extrusion lamination.
[0073] The laminate film can be used for packaging purposes, such as packaging food, textiles, miscellaneous goods, etc. The laminate film is preferably a laminate film for packaging retort food. The laminate film can also be used as a material for forming a packaging bag for packaging any packaging object such as food, clothing, miscellaneous goods, etc. The packaging bag is preferably a retort pouch. That is, the retort pouch according to this embodiment includes the above-mentioned laminate film.
[0074] In the laminate film according to the present embodiment, when the thermoplastic resin is a propylene-based polymer, both of the base layer and the sealant layer constituting the laminate film contain a propylene-based polymer, and the propylene-based polymer is the main component of the laminate film, and therefore the laminate film has excellent recyclability.
[0075] The present invention includes the following aspects. [1] A laminated film including a base layer and a sealant layer, The substrate layer is a biaxially stretched film that contains a thermoplastic resin having a melting point of 161°C or higher, or is formed from a thermoplastic resin composition containing the thermoplastic resin and having a melting point of 161°C or higher, the sealant layer is an unstretched film containing a propylene-based polymer, and the temperature T' at which a cumulative change in heat of fusion accounting for 55% of a cumulative change in heat of fusion from 50°C to 200°C observed by DSC of the unstretched film is from 50°C to temperature T' is 130°C or more and 153°C or less; Laminated film. [2] The base layer contains a propylene-based polymer having a melting point of 161°C or higher, or is formed from a propylene-based polymer composition containing the propylene-based polymer and having a melting point of 161°C or higher. The laminated film described in [1] above. [3] The sealant layer contains the following heterophasic propylene polymerization material (component 1), and further contains at least one component selected from the following propylene-α-olefin copolymer (component 2) and β crystal nucleating agent (component 3), The laminate film according to the above [1] or [2]. Heterophagic propylene polymer material (component 1) A propylene-based polymer (component 1-1) containing 98% by mass or more of structural units derived from propylene; A propylene-α-olefin copolymer (component 1-2) containing more than 50% by mass and 85% by mass or less of structural units derived from propylene and 15% by mass or more and less than 50% by mass of structural units derived from at least one selected from the group consisting of ethylene and α-olefins having 4 to 12 carbon atoms; Heterophagic propylene polymeric materials. Propylene-α-olefin copolymer (component 2) A propylene-α-olefin copolymer comprising more than 85% by mass and less than 98% by mass of structural units derived from propylene and more than 2% by mass and less than 15% by mass of structural units derived from at least one selected from the group consisting of ethylene and α-olefins having 4 to 12 carbon atoms. [4] The laminated film according to [3] above, wherein the sealant layer comprises the heterophasic propylene polymer material (component 1) and a propylene-α-olefin copolymer (component 2). [5] The laminate film according to [3] or [4] above, wherein the sealant layer contains the β-crystal nucleating agent (component 3), and the concentration of the β-crystal nucleating agent in the sealant layer is 100 ppm by mass or more and 3000 ppm by mass or less. [6] A retort pouch comprising the laminate film according to any one of [1] to [5] above. EXAMPLES
[0076] The present invention will be described in more detail below using examples and comparative examples, but the present invention is not limited to the following examples.
[0077] The measured values of each item in the examples and comparative examples were measured by the following methods.
[0078] The contents of the propylene polymer and the propylene-ethylene copolymer contained in the heterophasic propylene polymerization material are obtained from the material balance during each polymerization.
[0079] The content of the structural unit derived from ethylene contained in the propylene-ethylene copolymer contained in the heterophasic propylene polymerization material is obtained by performing an IR spectrum measurement on the entire heterophasic propylene polymerization material and calculating it according to the following formula (1) in accordance with the "Method for Block Copolymers" described on page 616 of the Polymer Analysis Handbook (published by Kinozoku Shoten in 1995). Here, ET, EA, and EB in formula (1) represent the content of ethylene structural units in the entire heterophasic propylene polymerization material, the content of ethylene structural units in the propylene polymer, and the content of ethylene structural units in the propylene-ethylene copolymer, respectively, and PA and PB represent the contents of the propylene polymer and the propylene-ethylene copolymer, respectively. EB = (ET - EA×PA) / PB Formula (1)
[0080] The content of the monomer unit derived from ethylene in the propylene-ethylene copolymer composition (unit: mass%) was determined by the IR spectrum measurement method described on page 256 of the Polymer Analysis Handbook (published by Asakura Shoten in 1985).
[0081] The contents of the monomer units derived from ethylene and 1-butene in the propylene-ethylene-1-butene terpolymer composition (unit: mass%) were determined by the IR spectrum measurement method described on page 256 of the Polymer Analysis Handbook (published by Asakura Shoten in 1985).
[0082] The melt flow rate of the propylene polymer composition and the heterophasic propylene polymerization material composition was measured at a temperature of 230°C and a load of 2.16 kg according to Method A specified in JIS K7210-1.
[0083] <DSC 55% melting temperature (unit: °C)> Using a temperature modulated differential scanning calorimeter (Q100 manufactured by TA Instruments), approximately 5 mg of the sealant film was cooled to 0°C under a nitrogen gas atmosphere (nitrogen gas flow rate 50 ml / min). Next, after holding at 0°C for 5 minutes, the temperature was raised to 230°C at an average heating rate of 2°C / min, a temperature modulation amplitude of ±0.5°C, and a temperature modulation period of 1 minute, and the reversing heat flow (specific heat component) was obtained. Using the same differential scanning calorimeter, approximately 4 mg of indium (In) was heated in a nitrogen gas atmosphere (nitrogen gas flow rate: 50 ml / min) to an equilibrium temperature of 110°C, and then heated at a heating rate of 5°C / min up to 180°C. The onset temperature of the maximum peak of the obtained melting endothermic curve was determined to be 156.6°C.
[0084] For the reversing heat flow value Q(T) for a temperature T between 50°C and 200°C, the straight line connecting the amount of heat Q(50) at 50°C and the amount of heat Q(200) at 200°C is taken as the baseline, and the amount of heat Q'(T) of reversing heat flow after baseline correction at a certain temperature T is defined as the following equation (2).
[0085]
number
[0086] Starting from 50°C, the integral of the reversing heat flow after baseline correction up to a temperature T' in the range from 50°C to 200°C is defined as A(T') in the following equation (3).
[0087]
number
[0088] Regarding A(T'), the temperature T' that satisfies the following formula (4) is defined as the temperature T'DSC55% temperature, at which the cumulative change in heat of fusion accounting for 55% of the cumulative change in heat of fusion is from 50°C to temperature T'.
[0089]
number
[0090] <Melting point (unit: °C)> Using a differential scanning calorimeter (PerkinElmer), an aluminum pan containing about 10 mg of a pellet-shaped resin composition sample was (1) held at 230°C for 5 minutes under a nitrogen atmosphere, then (2) cooled from 230°C to 0°C at a rate of 5°C / min. Next, (3) held at 0°C for 5 minutes, then (4) heated from 0°C to 230°C at a rate of 5°C / min. The temperature of the maximum peak of the melting endothermic curve obtained by calorimetry in the process (4) was taken as the melting point (Tm). In the above process (4), the melting point of indium (In) measured by the same method as above was 156.6°C.
[0091] <Minimum sealable temperature (unit: ℃)> A laminated film was used in which a sealant layer and a base layer were laminated by a dry lamination method. Using a heat sealer (manufactured by Toyo Tester Kogyo Co., Ltd.), the laminated film was folded in two so that the sealant layer was on the inside, and the ends opposite the folded position were heat-sealed in a strip shape along the extension direction of the folded position under the following conditions. ·Seal bar: Flat double-sided heating Sealing pressure: 1.0kg / cm 2 Sealing time: 1.0sec Seal width: 10mm
[0092] Then, a 15 mm wide test piece was cut out perpendicular to the seal width direction, and a tensile testing machine (Tensilon manufactured by Orientec) was used to determine the heat seal temperature at which the peel resistance was 15 N / 15 mm when peeled at a peel angle of 90° and a tensile speed of 200 mm / min, and this was determined as the minimum temperature at which sealing was possible.
[0093] <Heat seal appearance> A laminated film was used in which a sealant layer and a base layer were laminated by a dry lamination method. Using a heat sealer (manufactured by Toyo Tester Kogyo Co., Ltd.), the laminated film was folded in two so that the sealant layer was on the inside, and the ends opposite the folded position were heat-sealed in a strip shape along the extension direction of the folded position under the following conditions. ·Seal bar: Flat double-sided heating Sealing temperature: 170℃ Sealing pressure: 1.0kg / cm 2 Sealing time: 1.0sec Seal width: 10mm
[0094] The appearance of the laminated film after heat sealing was then checked, and a mark of "O" was given when the laminated film was not deformed, and a mark of "X" was given when the laminated film was deformed due to shrinkage.
[0095] The components used in the examples and comparative examples are as follows.
[0096] [Heterophasic Propylene Polymerization Material Composition A] Using a Ziegler-Natta catalyst, in the first step, propylene was polymerized in the gas phase, and then in the second step, propylene and ethylene were copolymerized in the gas phase to obtain a heterophasic propylene polymerization material A consisting of a propylene homopolymer A-1 and a propylene-ethylene copolymer A-2. 100 parts by mass of the heterophasic propylene polymerization material A were mixed with 0.01 parts by mass of hydrotalcite (manufactured by Kyowa Chemical Industry Co., Ltd.), 0.1 parts by mass of Irganox 1010 (manufactured by BASF), 0.05 parts by mass of Irgafos 168 (manufactured by BASF), and 0.1 parts by mass of NU-100 (β crystal nucleating agent, manufactured by New Japan Chemical Co., Ltd.) in a Henschel mixer, and then melt extrusion was performed to obtain a pellet-shaped heterophasic propylene polymerization material composition A. The obtained pellet-shaped heterophasic propylene polymerization material composition A had a propylene homopolymer A-1 content of 77 parts by mass, a propylene-ethylene copolymer A-2 content of 23 parts by mass, and a structural unit content derived from ethylene in the propylene-ethylene copolymer A-2 of 30% by mass, per 100 parts by mass of the total content of the polymers contained in the heterophasic propylene polymerization material A, and had a melt flow rate measured at 230°C of 2.5 g / 10 min.
[0097] [Heterophasic propylene polymer material composition B] Using a Ziegler-Natta catalyst, in the first step, propylene was polymerized in the gas phase, and then in the second step, propylene and ethylene were copolymerized in the gas phase to obtain a heterophasic propylene polymerization material B consisting of a propylene homopolymer B-1 and a propylene-ethylene copolymer B-2. 100 parts by mass of the heterophasic propylene polymerization material B were mixed with 0.01 parts by mass of hydrotalcite (manufactured by Kyowa Chemical Industry Co., Ltd.), 0.1 parts by mass of Irganox 1010 (manufactured by BASF), and 0.05 parts by mass of Irgafos 168 (manufactured by BASF) in a Henschel mixer, and then the mixture was melt-extruded to obtain a pellet-shaped heterophasic propylene polymerization material composition B. The obtained pellet-shaped heterophasic propylene polymerization material composition B had a propylene homopolymer B-1 content of 77 parts by mass, a propylene-ethylene copolymer B-2 content of 23 parts by mass, and a structural unit content derived from ethylene in the propylene-ethylene copolymer B-2 of 30% by mass, per 100 parts by mass of the total content of the polymers contained in the heterophasic propylene polymerization material B, and had a melt flow rate measured at 230°C of 2.2 g / 10 min.
[0098] [Heterophasic propylene polymer material composition C] Using a Ziegler-Natta catalyst, in the first step, propylene was polymerized in the gas phase, and then in the second step, propylene and ethylene were copolymerized in the gas phase to obtain a heterophasic propylene polymerization material C consisting of a propylene homopolymer C-1 and a propylene-ethylene copolymer C-2. 100 parts by mass of the heterophasic propylene polymerization material C were mixed with 0.01 parts by mass of hydrotalcite (manufactured by Kyowa Chemical Industry Co., Ltd.), 0.1 parts by mass of Irganox 1010 (manufactured by BASF), 0.05 parts by mass of Irgafos 168 (manufactured by BASF), and 0.2 parts by mass of NU-100 (β crystal nucleating agent, manufactured by New Japan Chemical Co., Ltd.) in a Henschel mixer, and then melt extrusion was performed to obtain a pellet-shaped heterophasic propylene polymerization material composition C. The obtained pellet-shaped heterophasic propylene polymerization material composition C had a propylene homopolymer C-1 content of 77 parts by mass, a propylene-ethylene copolymer C-2 content of 23 parts by mass, and a structural unit content derived from ethylene in the propylene-ethylene copolymer C-2 of 30% by mass, per 100 parts by mass of the total content of the polymers contained in the heterophasic propylene polymerization material C, and had a melt flow rate measured at 230°C of 2.6 g / 10 min.
[0099] [Propylene-ethylene copolymer composition D] Propylene and ethylene were copolymerized in the gas phase using a Ziegler-Natta catalyst to obtain a propylene-ethylene copolymer D. 100 parts by mass of the obtained propylene-ethylene copolymer D were mixed with 0.01 parts by mass of hydrotalcite (manufactured by Kyowa Chemical Industry Co., Ltd.), 0.1 parts by mass of Irganox 1010 (manufactured by BASF), and 0.05 parts by mass of Irgafos 168 (manufactured by BASF) in a Henschel mixer, and then melt extrusion was performed to obtain a pellet-shaped propylene-ethylene copolymer composition D. The obtained pellet-shaped propylene-ethylene copolymer composition D had a content of structural units derived from ethylene in the propylene-ethylene copolymer D of 4.4% by mass, and a melt flow rate measured at 230°C of 8.3 g / 10 min.
[0100] [Propylene-ethylene-1-butene terpolymer composition E] Propylene, ethylene, and 1-butene were copolymerized in the gas phase using a Ziegler-Natta catalyst to obtain a propylene-ethylene-1-butene terpolymer E. 100 parts by mass of propylene-ethylene-1-butene terpolymer E were mixed with 0.01 parts by mass of hydrotalcite (Kyowa Chemical Industry Co., Ltd.), 0.1 parts by mass of Irganox 1010 (BASF), and 0.05 parts by mass of Irgafos 168 (BASF) in a Henschel mixer, and then melt extrusion was performed to obtain a pellet-shaped propylene-ethylene-1-butene terpolymer composition E. The pellet-shaped propylene-ethylene-1-butene terpolymer composition E obtained had a content of structural units derived from ethylene of 2.1% by mass and a content of structural units derived from 1-butene of 5.6% by mass in the propylene-ethylene-1-butene terpolymer composition E, and had a melt flow rate measured at 230°C of 7.0 g / 10 min.
[0101] [Propylene homopolymer composition F] Propylene was polymerized in the gas phase using a Ziegler-Natta catalyst to obtain propylene homopolymer F. 100 parts by mass of propylene homopolymer F were mixed with 0.01 parts by mass of hydrotalcite (Kyowa Chemical Industry Co., Ltd.), 0.09 parts by mass of Irganox 1010 (BASF), and 0.05 parts by mass of Sumilizer GP (Sumitomo Chemical Co., Ltd.) in a Henschel mixer, and then melt extrusion was performed to obtain pellet-shaped propylene homopolymer composition F. The obtained pellet-shaped propylene homopolymer composition F had a melting point of 165°C and a melt flow rate measured at 230°C of 2.3 g / 10 min.
[0102] [Propylene-ethylene copolymer composition G] Propylene and ethylene were copolymerized in the gas phase using a Ziegler-Natta catalyst to obtain a propylene-ethylene copolymer G. 100 parts by mass of the obtained propylene-ethylene copolymer G were mixed with 0.01 parts by mass of hydrotalcite (manufactured by Kyowa Chemical Industry Co., Ltd.), 0.1 parts by mass of Irganox 1010 (manufactured by BASF), and 0.05 parts by mass of Irgafos 168 (manufactured by BASF) in a Henschel mixer, and then melt extrusion was performed to obtain a pellet-shaped propylene-ethylene copolymer composition G. The obtained pellet-shaped propylene-ethylene copolymer composition G had a content of structural units derived from ethylene in the propylene-ethylene copolymer G of 0.6% by mass, a melting point of 158°C, and a melt flow rate measured at 230°C of 3.0g / 10 min.
[0103] [Sealant layer (1)] Using a 50 mm T-die film-forming device (Tanabe Plastics Co., Ltd. V-50-F600 film-forming device with a 400 mm wide T-die), 100% by mass of the heterophasic propylene polymer material composition A was melt-kneaded at a resin temperature of 280°C and extruded from the T-die. Next, the mixture was cooled and solidified while being wound up on a chill roll (cooling roll) at a cooling temperature of 80°C, to obtain a sealant layer (1) with a thickness of 70 μm. The obtained sealant layer (1) was used to evaluate the DSC 55% melting temperature. The results are shown in Table 2.
[0104] [Sealant layer (2)] 50% by mass of the heterophasic propylene polymer material composition B and 50% by mass of the propylene-ethylene copolymer composition D were pellet-blended. A sealant layer (2) having a thickness of 70 μm was obtained in the same manner as the sealant layer 1, except that the obtained mixture was used. The evaluation results of the DSC 55% melting temperature of the obtained sealant layer (2) are shown in Table 2.
[0105] [Sealant layer (3)] 50% by mass of the heterophasic propylene polymer material composition B and 50% by mass of the propylene-ethylene-1-butene terpolymer E were pellet-blended. A sealant layer (3) having a thickness of 70 μm was obtained in the same manner as the sealant layer 1, except that the obtained mixture was used. The evaluation results of the DSC 55% melting temperature of the obtained sealant layer (3) are shown in Table 2.
[0106] [Sealant layer (4)] 50% by mass of the heterophasic propylene polymer material composition C and 50% by mass of the propylene-ethylene copolymer composition D were pellet-blended. A sealant layer (4) having a thickness of 70 μm was obtained in the same manner as the sealant layer 1, except that the obtained mixture was used. The evaluation results of the DSC 55% melting temperature of the obtained sealant layer (4) are shown in Table 2.
[0107] [Sealant layer (5)] 50% by mass of the heterophasic propylene polymer material composition C and 50% by mass of the propylene-ethylene-1-butene terpolymer E were pellet-blended. A sealant layer (5) having a thickness of 70 μm was obtained in the same manner as the sealant layer 1, except that the obtained mixture was used. The evaluation results of the DSC 55% melting temperature of the obtained sealant layer (5) are shown in Table 2.
[0108] [Sealant layer (6)] A sealant layer (6) having a thickness of 70 μm was obtained in the same manner as for the sealant layer 1, except that 100% by mass of the heterophasic propylene polymerization material composition B was used. The evaluation results of the DSC 55% melting temperature of the obtained sealant layer (6) are shown in Table 2.
[0109] [Base material layer (1)] 100 parts by mass of the propylene homopolymer composition F was used, and after melt kneading with three extruders, it was introduced into one coextrusion T-die (die width 300 mm, lip opening 2 mm) and melt extrusion was performed at a die temperature of 260 ° C. The extruded molten film was cooled with a cooling roll at 30 ° C. to obtain a cast sheet with a thickness of about 1 mm. The obtained cast sheet was stretched 5 times in the longitudinal direction at 147 ° C. by the peripheral speed difference between a low-speed roll rotating at 4 m / min and a high-speed roll rotating at 20 m / min. Subsequently, it was stretched 8 times in the transverse direction at a preheating temperature of 190 ° C. and a stretching temperature of 170 ° C. in a heating furnace, and the width in the transverse direction was relaxed by 19.5% while performing heat treatment at 165 ° C. The film coming out of the heating furnace was cooled with a cooling roll at 20 ° C. to obtain a base layer (1) with a thickness of 20 μm.
[0110] [Base material layer (2)] 100 parts by mass of propylene-ethylene copolymer composition G was used, melt-kneaded with three extruders, and then introduced into one coextrusion T-die (die width 300 mm, lip opening 2 mm) and melt-extruded at a die temperature of 260 ° C. The extruded molten film was cooled with a cooling roll at 30 ° C. to obtain a cast sheet with a thickness of about 1 mm. The obtained cast sheet was stretched 5 times in the longitudinal direction at 140 ° C. due to the difference in peripheral speed between a low-speed roll rotating at 4 m / min and a high-speed roll rotating at 20 m / min. Subsequently, it was stretched 8 times in the transverse direction at a preheating temperature of 175 ° C. and a stretching temperature of 157 ° C. in a heating furnace, and the width in the transverse direction was relaxed by 6.5% while performing heat treatment at 165 ° C. The film coming out of the heating furnace was cooled with a cooling roll at 20 ° C. to obtain a base layer (2) with a thickness of 20 μm.
[0111] [Example 1] The sealant layer (1) and the base layer (1) obtained above were laminated by dry lamination to obtain a laminate film (1). The physical properties of the obtained laminate film (1) are shown in Table 2. The obtained laminate film (1) was a laminate film excellent in the minimum sealable temperature and in the appearance after sealing.
[0112] [Example 2] The sealant layer (2) and the base layer (1) obtained above were laminated by dry lamination to obtain a laminate film (2). The physical properties of the obtained laminate film (2) are shown in Table 2. The obtained laminate film (2) was a laminate film excellent in the minimum sealable temperature and in the appearance after sealing.
[0113] [Example 3] The sealant layer (3) and the base layer (1) obtained above were laminated by dry lamination to obtain a laminate film (3). The physical properties of the obtained laminate film (3) are shown in Table 2. The obtained laminate film (3) was a laminate film excellent in the minimum sealable temperature and in the appearance after sealing.
[0114] [Example 4] The sealant layer (4) and the base layer (1) obtained above were laminated by dry lamination to obtain a laminate film (4). The physical properties of the obtained laminate film (4) are shown in Table 2. The obtained laminate film (4) was a laminate film excellent in the minimum sealable temperature and in the appearance after sealing.
[0115] [Example 5] The sealant layer (5) and the base layer (1) obtained above were laminated by dry lamination to obtain a laminate film (5). The physical properties of the obtained laminate film (5) are shown in Table 2. The obtained laminate film (5) was a laminate film excellent in the minimum sealable temperature and in the appearance after sealing.
[0116] [Comparative Example 1] The sealant layer (1) and the base layer (2) obtained above were laminated by a dry lamination method to obtain a laminate film (6). The physical properties of the obtained laminate film (6) are shown in Table 2. The obtained laminate film (6) had a high minimum sealable temperature and was a laminate film with poor appearance after sealing.
[0117] [Comparative Example 2] The sealant layer (6) and the base layer (2) obtained above were laminated by dry lamination to obtain a laminate film (7). The physical properties of the obtained laminate film (7) are shown in Table 2. The obtained laminate film (7) had a high minimum sealable temperature and was a laminate film with poor appearance after sealing.
[0118] [Table 1]
[0119] [Table 2]
[0120] The results in Table 2 show that the laminated films of the examples which satisfy all of the constituent requirements of the present invention can be heat-sealed at relatively low temperatures and have a good appearance at the heat-sealed areas.
Claims
1. A laminated film including a base layer and a sealant layer, The substrate layer is a biaxially stretched film that contains a thermoplastic resin having a melting point of 161°C or higher, or is formed from a thermoplastic resin composition containing the thermoplastic resin and having a melting point of 161°C or higher, the sealant layer is an unstretched film containing a propylene-based polymer, and a temperature T' at which a cumulative change in heat of fusion accounting for 55% of a cumulative change in heat of fusion from 50°C to 200°C observed by DSC of the unstretched film is from 50°C to temperature T' is 130°C or more and 153°C or less; Laminated film.
2. The base layer contains a propylene-based polymer having a melting point of 161° C. or more, or is formed from a propylene-based polymer composition containing the propylene-based polymer and having a melting point of 161° C. or more. The laminated film according to claim 1 .
3. The sealant layer contains the following heterophasic propylene polymer material (component 1), and further contains at least one component selected from the following propylene-α-olefin copolymer (component 2) and a β-crystal nucleating agent (component 3): The laminated film according to claim 1 or 2. Heterophagic Propylene Polymerization Material (Component 1) A propylene-based polymer (component 1-1) containing 98% by mass or more of structural units derived from propylene; a propylene-α-olefin copolymer (component 1-2) containing more than 50% by mass and not more than 85% by mass of structural units derived from propylene and 15% by mass or more and less than 50% by mass of structural units derived from at least one selected from the group consisting of ethylene and α-olefins having 4 to 12 carbon atoms; Heterophagic propylene polymeric materials. Propylene-α-olefin copolymer (component 2) A propylene-α-olefin copolymer comprising more than 85% by mass and less than 98% by mass of structural units derived from propylene and more than 2% by mass and less than 15% by mass of structural units derived from at least one selected from the group consisting of ethylene and α-olefins having 4 to 12 carbon atoms.
4. 4. The laminate film of claim 3, wherein the sealant layer comprises the heterophasic propylene polymer material (component 1) and a propylene-α-olefin copolymer (component 2).
5. The laminate film according to claim 3 , wherein the sealant layer contains the β-crystal nucleating agent (component 3), and the concentration of the β-crystal nucleating agent in the sealant layer is 100 ppm by mass or more and 3000 ppm by mass or less.
6. A retort pouch comprising the laminate film according to claim 1.
Citation Information
Patent Citations
Multilayer film, and, packaging bag
JP2022102606A