Stage
The stage design using solid and liquid phase diffusion bonding in semiconductor devices addresses particle emission, ensuring cleaner wafer environments and improved device characteristics by eliminating brazing material from the gas flow path.
Patent Information
- Application Number
- JP2023056208
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-03-30
AI Technical Summary
The emission of particles from the stage in semiconductor devices contaminates the wafer, leading to deterioration of semiconductor device characteristics.
A stage design with multiple metal plates bonded using solid phase diffusion bonding for the first and second plates and liquid phase diffusion bonding for the second and third plates, forming a gas flow path without brazing material, and incorporating a heater in the third groove.
The design suppresses particle emission by eliminating brazing material from the gas flow path, thereby maintaining the cleanliness of the wafer and enhancing semiconductor device performance.
Smart Images

Figure 2024143492000001_ABST
Abstract
Description
[Technical field]
[0001] An embodiment of the present invention relates to a stage installed in a semiconductor device. [Background technology]
[0002] A semiconductor device for manufacturing semiconductor elements is provided with a stage on which a wafer is placed, and a heater or the like is embedded in the stage to control the temperature of the wafer placed thereon (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2004-165085 A [Patent Document 2] JP 2008-39255 A Summary of the Invention [Problem to be solved by the invention]
[0004] As shown in Patent Document 1, the stage includes a plurality of plate members, and a resistance heating element (heater) is disposed between the plurality of plate members. The plurality of plate members are joined by brazing. Patent Document 2 discloses a heat exchanger in which a plurality of joining plates (plate members) are joined by a combination of brazing, diffusion bonding, and HIP bonding.
[0005] The stage is located close to the wafer, and if particles are released from the stage, the film formed on the wafer will be contaminated and the characteristics of the semiconductor device will deteriorate. For this reason, it is desirable to suppress particles released from the stage.
[0006] In view of the above problems, one object of one embodiment of the present invention is to provide a stage in which particles released to the outside are suppressed. [Means for solving the problem]
[0007] A stage according to one embodiment of the present invention includes a first metal plate, a second metal plate located below the first metal plate and joined to the first metal plate, and a third metal plate located below the second metal plate and joined to the second metal plate, wherein the first metal plate includes a first groove portion exposed to the outside, and the second metal plate includes a second groove portion covered by the first metal plate and communicating with the first groove portion, and a third groove portion covered by the third metal plate, wherein the first groove portion and the second groove portion are gas flow paths, and a heater is disposed in the third groove portion.
[0008] A portion of the heater may be fixed to the third groove by a brazing material.
[0009] The third groove does not have to communicate with the first groove.
[0010] A brazing material may not be included between the first metal plate and the second metal plate, and a brazing material may be included between the second metal plate and the third metal plate.
[0011] A bonding interface including irregularities due to crystal grains may be observed between the second metal plate and the third metal plate.
[0012] The second metal plate may be joined to the first metal plate by solid-phase diffusion bonding, and the third metal plate may be joined to the second metal plate by liquid-phase diffusion bonding. The liquid-phase diffusion bonding may be bonding using a brazing material.
[0013] Each of the first metal plate, the second metal plate, and the third metal plate may be an aluminum alloy including magnesium.
[0014] Each of the first metal plate, the second metal plate, and the third metal plate may be an aluminum alloy containing manganese.
[0015] The stage may further include a shaft located below the third metal plate and joined to the third metal plate, and a gas introduction pipe for supplying gas to the gas flow path and a heater may be disposed within the shaft. Effect of the Invention
[0016] According to the stage of the embodiment of the present invention, the gas flow path connected to the outside is formed by solid-phase diffusion bonding. Therefore, the gas flow path does not contain brazing material that may cause particles. Therefore, the stage 10 can suppress particles from being released to the outside. [Brief description of the drawings]
[0017] [Figure 1] FIG. 2 is a schematic perspective view of a stage according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic top view of a stage according to an embodiment of the present invention. [Diagram 3] FIG. 2 is a schematic cross-sectional view of a stage according to an embodiment of the present invention. [Figure 4] 4 is a flowchart illustrating a method for manufacturing a stage according to an embodiment of the present invention. [Diagram 5] 5A to 5C are schematic cross-sectional views illustrating a manufacturing method of a stage according to an embodiment of the present invention. [Figure 6] 5A to 5C are schematic cross-sectional views illustrating a manufacturing method of a stage according to an embodiment of the present invention. [Figure 7] 5A to 5C are schematic cross-sectional views illustrating a manufacturing method of a stage according to an embodiment of the present invention. [Figure 8] 1 is a schematic cross-sectional view showing a configuration of an etching apparatus according to an embodiment of the present invention. [Figure 9] 1 is a schematic cross-sectional view showing the configuration of a CVD apparatus according to one embodiment of the present invention. [Figure 10] 1 is a schematic cross-sectional view showing a configuration of a sputtering apparatus according to an embodiment of the present invention. [Figure 11]1 is a schematic cross-sectional view illustrating a configuration of a deposition apparatus according to one embodiment of the present invention. [Figure 12] 1 is a cross-sectional SEM image of a bonding interface between a first metal plate and a second metal plate in an example sample. [Figure 13] 1 is a cross-sectional SEM image of a bonding interface between a second metal plate and a third metal plate in an example sample. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Hereinafter, each embodiment of the invention disclosed in this application will be described with reference to the drawings. However, the present invention can be embodied in various forms without departing from the gist of the invention, and the present invention should not be interpreted as being limited to the description of the embodiments exemplified below.
[0019] In the drawings, the width, thickness, shape, etc. of each part may be shown diagrammatically compared to the actual embodiment in order to clarify the explanation, but it is merely an example and does not limit the interpretation of the present invention. In addition, in this specification and each figure, elements having the same function as those explained in the previous figures may be given the same reference numerals and duplicate explanations may be omitted. For convenience of explanation, the words "upper" and "lower" are used in the explanation, but "upper" and "lower" respectively indicate the orientation when the stage is in use (when a wafer is placed on it).
[0020] In this specification and drawings, the same reference numerals are used to collectively represent multiple identical or similar components, and capital letters are used to distinguish between the multiple components. The same reference numerals, hyphens, and natural numbers are used to distinguish between multiple parts of a single component.
[0021] First Embodiment A stage 10 according to one embodiment of the present invention will be described with reference to FIGS.
[0022] Fig. 1 is a schematic perspective view of a stage 10 according to an embodiment of the present invention. Fig. 2 is a schematic top view of the stage 10 according to an embodiment of the present invention. Fig. 3 is a schematic cross-sectional view of the stage 10 according to an embodiment of the present invention. Specifically, Fig. 3 is a cross-sectional view of the stage 10 taken along the line A1-A2 shown in Fig. 2.
[0023] 1, the stage 10 includes a plate portion 100 and a shaft portion 200, and a wafer is placed on a first surface 100a of the plate portion 100. The shaft portion 200 is connected to a second surface 100b of the plate portion 100 opposite to the first surface 100a. For example, the shaft portion 200 is joined to the plate portion 100 by brazing, but is not limited to this.
[0024] The wafer placed on the stage 10 may be, for example, but is not limited to, silicon (Si), silicon carbide (SiC), sapphire, quartz, glass, gallium phosphide (GaP), gallium arsenide (GaAs), indium phosphide (InP), or gallium nitride (GaN). As described above, since the wafer is placed on the first surface 100a of the plate portion 100, it is preferable that the first surface 100a is a flat surface.
[0025] As shown in FIG. 3, the plate portion 100 includes a first metal plate 110, a second metal plate 120, and a third metal plate 130. The first metal plate 110 to the third metal plate 130 are stacked in this order. That is, the second metal plate 120 is located below the first metal plate 110, and the third metal plate 130 is located below the second metal plate 120. The first surface 100a of the plate portion 100 corresponds to the upper surface of the first metal plate 110, and the second surface 100b of the plate portion 100 corresponds to the lower surface of the third metal plate 130. The shaft portion 200 is connected to the third metal plate 130.
[0026] There is no particular limitation on the thickness of each of the first metal plate 110 to the third metal plate 130. The thicknesses of the first metal plate 110 to the third metal plate 130 may be the same or different.
[0027] 2, the first metal plate 110 has a circular shape when viewed from above. The second metal plate 120 and the third metal plate 130 overlapping the first metal plate 110 also have a circular shape. However, the shapes of the first metal plate 110 to the third metal plate 130 are not limited to a circular shape. The shapes of the first metal plate 110 to the third metal plate 130 may be appropriately determined according to the shape of the wafer, and the first metal plate 110 to the third metal plate 130 may have an elliptical or polygonal shape.
[0028] The material of each of the first metal plate 110, the second metal plate 120, and the third metal plate 130 is an aluminum alloy. For example, the aluminum alloy is an aluminum alloy containing copper and magnesium (2000 series), an aluminum alloy containing manganese (3000 series), an aluminum alloy containing silicon (4000 series), an aluminum alloy containing magnesium (5000 series), an aluminum alloy containing magnesium and silicon (6000 series), and an aluminum alloy containing zinc and magnesium (7000 series). In the stage 10 used in the semiconductor device, particularly, an aluminum alloy containing manganese (3000 series) and an aluminum alloy containing magnesium and silicon (6000 series) are used. Specifically, the material of each of the first metal plate 110, the second metal plate 120, and the third metal plate 130 is A6061 or A3003 of the JIS standard. A6061 has excellent corrosion resistance. A3003 has the same machinability and corrosion resistance as pure aluminum.
[0029] The material of each of the first metal plate 110, the second metal plate 120, and the third metal plate 130 is not limited to the above-mentioned aluminum alloy. Also, the first metal plate 110, the second metal plate 120, and the third metal plate 130 may be made of the same material or different materials.
[0030] As shown in FIG. 3, the first metal plate 110 includes a first groove portion 112. The first groove portion 112 is provided on the upper surface of the first metal plate 110 (i.e., the first surface 100a of the plate portion 100). The first groove portion 112 is exposed to the outside of the stage 10. The second metal plate 120 includes a second groove portion 122 and a third groove portion 124. The second groove portion 122 is provided on the upper surface of the second metal plate 120 and is covered by the first metal plate 110. The third groove portion 124 is provided on the lower surface of the second metal plate 120 and is covered by the third metal plate 130.
[0031] 2, in a plan view, the first groove portion 112 may be provided in a circumferential shape or in a linear shape. A plurality of first groove portions 112 may be provided. The plurality of first groove portions 112 may intersect with each other.
[0032] 2 and 3, the second groove portion 122 is connected to the first groove portion 112 via a through hole 114 provided in the first metal plate 110. In other words, the second groove portion 122 communicates with the first groove portion via the through hole 114. Note that it is sufficient that the through hole 114 is provided in a part of the first groove portion 112. Furthermore, the number of through holes 114 may be one or more.
[0033] The first groove 112 and the second groove 122 are gas flow paths. A gas introduction pipe 210 is disposed in the shaft portion 200, and an end of the gas introduction pipe 210 is connected to the second groove 122. The gas supplied from the gas introduction pipe 210 to the second groove 122 flows through the second groove 122 and the first groove 112, and is discharged from the first groove 112 to the outside of the stage 10. For example, the gas is a process gas for forming a film on the wafer, but is not limited thereto. For example, the gas may be a gas that does not contribute to the film formation itself, but is passed to uniformize the temperature of the stage 10.
[0034] The planar shape of the second groove 122 is not particularly limited. The second groove 122 may have the same planar shape as the first groove 112. The second groove 122 only needs to have a planar shape that allows the gas supplied from the gas introduction pipe 210 to flow into the first groove 112, and the planar shape of the second groove 122 is not particularly limited. The gas supplied to the first groove 112 is released to the outside of the stage 10.
[0035] For example, the cross-sectional shape of each of the first groove portion 112 and the second groove portion 122 is rectangular, but is not limited to this. The cross-sectional shape of the first groove portion 112 and the second groove portion 122 may be, for example, semicircular or semi-elliptical. Furthermore, the cross-sectional shape of the first groove portion 112 and the second groove portion 122 may have the same cross-sectional shape or different cross-sectional shapes.
[0036] A heater 220 is disposed in the third groove portion 124, and a terminal 220a of the heater 220 is housed in the shaft portion 200. The heater 220 generates heat when a current is supplied from the terminal 220a, and heats the stage 10. The temperature of the stage 10 can be controlled by adjusting the amount of current supplied to the terminal 220a. For example, the heater 220 is a sheath heater, but is not limited to this. The number of heaters disposed in the third groove portion 124 may be one or more.
[0037] The planar shape of the third groove portion 124 corresponds to the arrangement shape of the heaters 220. It is preferable that the heaters 220 are arranged in such a way that the temperature of the stage 10 is uniform. Therefore, the planar shape of the third groove portion 124 is appropriately determined according to the number and arrangement shape of the heaters 220.
[0038] For example, the cross-sectional shape of the third groove 124 is rectangular, but is not limited to this. The cross-sectional shape of the third groove 124 may be, for example, semicircular or semi-elliptical.
[0039] Although not shown, a return path for flowing a cooling medium may be provided in the plate portion 100. By utilizing not only heating by the heater 220 but also cooling by the cooling medium flowing through the return path, precise temperature control of the stage 10 becomes possible.
[0040] The first metal plate 110 is joined to the second metal plate 120. Moreover, the second metal plate 120 is joined to the third metal plate 130. Here, the joining of the first metal plate 110 and the second metal plate 120, and the joining of the second metal plate 120 and the third metal plate 130 will be described. Details of the joining method will be described in the second embodiment.
[0041] The bonding between the first metal plate 110 and the second metal plate 120 is solid-phase diffusion bonding. That is, the first metal plate 110 and the second metal plate 120 are directly bonded using heat and pressure without being melted. Therefore, no metal elements other than those contained in the materials of the first metal plate 110 and the second metal plate 120 are present near the bonding interface between the first metal plate 110 and the second metal plate 120. In addition, since the first metal plate 110 and the second metal plate 120 do not melt, the bonding interface between the first metal plate 110 and the second metal plate 120 is highly flat, and no irregularities due to crystal grains formed by melting and solidifying are seen at the bonding interface.
[0042] The second metal plate 120 and the third metal plate 130 are joined by liquid phase diffusion bonding. For example, liquid phase diffusion bonding is brazing using a brazing material. The second metal plate 120 and the third metal plate 130 are joined via the brazing material. Therefore, metal elements contained in the brazing material are present near the joint interface between the second metal plate 120 and the third metal plate 130. In addition, since the brazing material melts, irregularities due to crystal grains formed by melting and solidifying the brazing material are seen near the joint interface between the second metal plate 120 and the third metal plate 130.
[0043] For example, the brazing material may be an alloy containing silver, copper, and zinc, an alloy containing copper and zinc, copper containing a trace amount of phosphorus, an alloy containing aluminum, an alloy containing titanium, copper, and nickel, an alloy containing titanium, zirconium, and copper, or an alloy containing titanium, zirconium, copper, and nickel.
[0044] As described above, the bonding between the first metal plate 110 and the second metal plate 120 is different from the bonding between the second metal plate 120 and the third metal plate 130. The bonding between the second metal plate 120 and the third metal plate 130 is liquid phase diffusion bonding. Therefore, at the bonding interface between the second metal plate 120 and the third metal plate 130, irregularities due to solidification of crystal grains are formed. In other words, the bonding interface between the second metal plate 120 and the third metal plate 130 is less flat than the bonding interface between the first metal plate 110 and the second metal plate 120.
[0045] Metal elements near the bonded interface, grain boundaries, and interface irregularities can be observed using cross-sectional SEM and EDX.
[0046] The stage 10 includes a gas flow path formed by a first groove 112 provided in the first metal plate 110 and a second groove 122 provided in the second metal plate 120. The first metal plate 110 and the second metal plate 120 are bonded by solid-state diffusion bonding, so the gas flow path of the stage 10 does not contain brazing material or the like. Therefore, in the stage 10, particles caused by the brazing material are not released to the outside together with the gas flowing through the gas flow path. That is, in the stage 10, it is possible to suppress particles being released to the outside.
[0047] In this embodiment, the stage 10 includes three metal plates, but the number of metal plates included in the stage 10 is not limited to three. The number of metal plates included in the stage 10 may be two, or may be four or more. In addition, the positions and the number of the grooves and the heaters in the stage 10 are not particularly limited. In the stage 10, solid-phase diffusion bonding is used for bonding two metal plates when forming a flow path connected to the outside of the stage 10. In the stage 10, at least solid-phase diffusion bonding is used for bonding between the metal plates when forming a flow path connected to the outside of the stage 10, and solid-phase diffusion bonding can be used instead of liquid-phase diffusion bonding.
[0048] <Second embodiment> A method for manufacturing the stage 10 according to one embodiment of the present invention will be described with reference to FIGS.
[0049] Fig. 4 is a flow chart illustrating a method for manufacturing the stage 10 according to one embodiment of the present invention. Also, Figs. 4 to 7 are schematic cross-sectional views illustrating the method for manufacturing the stage 10 according to one embodiment of the present invention.
[0050] 4 shows a manufacturing process for the plate portion 100 of the stage 10, and includes steps S110 to S140. Steps S110 to S140 will be described below in order.
[0051] In step S110, the first metal plate 110 and the second metal plate 120 are planarized (see FIG. 5). The planarization is performed on the surfaces on which solid-phase diffusion bonding is performed. That is, the lower surface of the first metal plate 110 (the surface opposite to the first surface 100a of the plate portion 100) and the upper surface of the second metal plate 120 (the surface facing the lower surface of the first metal plate 110) are planarized.
[0052] In step S120, the first metal plate 110, the second metal plate 120, and the third metal plate 130 are aligned (see FIG. 6). At this time, a gas introduction pipe is connected to the second groove 122 of the second metal plate 120, and a heater 220 is disposed in the third groove 124 of the second metal plate 120. As shown in FIG. 6, the first metal plate 110 to the third metal plate 130 are stacked in order, and the first metal plate 110 to the third metal plate 130 are aligned. In this embodiment, solid-phase diffusion bonding and liquid-phase diffusion bonding are performed simultaneously. Therefore, in step S120, the alignment of three metal plates, the first metal plate 110 to the third metal plate 130, is performed, instead of the alignment of two metal plates among the first metal plate 110 to the third metal plate 130.
[0053] In the following description, for convenience, the structure in which the first metal plate 110 to the third metal plate 130 are stacked and aligned (that is, the structure before bonding) is referred to as the metal plate stacked structure 105.
[0054] In step S130, the metal plate laminated structure 105 is heated and pressurized (see FIG. 7). Pressurization may be performed in a direction from the first metal plate 110 to the third metal plate 130, or from the third metal plate 130 to the first metal plate 110. The heated and pressurized metal plate laminated structure 105 is held for a predetermined time. As a result, solid-state diffusion bonding is performed between the first metal plate 110 and the second metal plate 120, and the first metal plate 110 and the second metal plate 120 are bonded to each other.
[0055] The lower limit of the heating temperature of the metal plate laminated structure 105 is 400°C or higher, preferably 500°C or higher. The upper limit of the heating temperature of the metal plate laminated structure 105 is lower than the melting point of the material of the first metal plate 110 and the second metal plate 120. If the heating temperature is too low, sufficient solid-phase diffusion bonding is not performed. If the heating temperature is too high, the metal plates melt.
[0056] The load of the pressurization of the metal plate laminated structure 105 is 0.5 MPa or more and 8 MPa or less, preferably 1.0 MPa or more and 4 MPa or less. If the load of the pressurization is too low, it is difficult for the first metal plate 110 and the second metal plate 120 to come into surface contact with each other. If the load of the pressurization is too high, the metal plate laminated structure 105 will be deformed.
[0057] The holding time for heating and pressing is 0.1 to 10 hours, preferably 0.5 to 8 hours. If the holding time is too short, sufficient solid-phase diffusion bonding is not performed. If the holding time is too long, the manufacturing takt time of the stage 10 is reduced.
[0058] In addition, 3000 series aluminum alloys are less susceptible to deformation than 6000 series aluminum, so when the first metal plate 110 and the second metal plate are made of 3000 series aluminum alloys, it is preferable to increase the heating temperature, increase the load applied by pressure, or increase the holding time of heating and pressure.
[0059] In step S140, brazing is performed between the second metal plate 120 and the third metal plate 130 while heating and pressurizing are performed in step S130. As a result, liquid phase diffusion bonding is performed between the second metal plate 120 and the third metal plate 130, and the second metal plate 120 and the third metal plate 130 are bonded together. The brazing material used in brazing may be adjusted so as to flow into the third groove portion 124. In this case, a portion of the heater 220 arranged in the third groove portion 124 is fixed to the third groove portion by the brazing material.
[0060] The brazing filler metal may be pre-placed between the second metal plate 120 and the third metal plate 130 during alignment in step S120, and the brazing filler metal may be inserted between the second metal plate 120 and the third metal plate 130 in step S140.
[0061] The manufacturing process of the plate portion 100 of the stage 10 is completed by releasing the heating and pressure applied to the metal plate laminate structure. Through this manufacturing process, the first metal plate 110 and the second metal plate 120 are bonded together by solid-phase diffusion bonding, and a gas flow path that does not include brazing material is formed. Also, the second metal plate 120 and the third metal plate 130 are bonded together by liquid-phase diffusion bonding. In this manufacturing process, solid-phase diffusion bonding and liquid-phase diffusion bonding are performed simultaneously, thereby improving the manufacturing takt time of the plate portion 100 and reducing the manufacturing cost of the stage 10.
[0062] According to the manufacturing method of the stage 10, the first metal plate 110 and the second metal plate 120 are bonded by solid-state diffusion bonding, so that the gas flow passage of the stage 10 does not contain brazing material or the like. Therefore, in the stage 10, particles caused by the brazing material are not released to the outside together with the gas flowing through the gas flow passage. That is, in the stage 10, it is possible to suppress particles being released to the outside.
[0063] <Third embodiment> An etching apparatus 50 according to one embodiment of the present invention will be described with reference to Fig. 8. The etching apparatus 50 includes a stage 10. Therefore, in the following, a description of the same or similar configuration as the configuration of the stage 10 described in the first embodiment may be omitted.
[0064] FIG. 8 is a schematic cross-sectional view showing the configuration of an etching apparatus 50 according to an embodiment of the present invention.
[0065] The etching apparatus 50 can perform dry etching on various films. The etching apparatus 50 has a chamber 502. The chamber 502 provides a space in which etching is performed on a film such as a conductor, an insulator, or a semiconductor formed on a wafer.
[0066] An exhaust device 504 is connected to the chamber 502, which allows the inside of the chamber 502 to be set to a reduced pressure atmosphere. The chamber 502 is further provided with an inlet pipe 506 for introducing a reactive gas, and a reactive gas for etching is introduced into the chamber 502 via a valve 508. The reactive gas may be, for example, carbon tetrafluoride (CF 4 ), octafluorocyclobutane (cC 4 F8), decafluorocyclopentane (cC 5 F 10 ), or hexafluorobutadiene (C 4 F 6 ) and other fluorine-containing organic compounds can be used.
[0067] A microwave source 512 can be provided at the top of the chamber 502 via a waveguide 510. The microwave source 512 has an antenna for supplying microwaves, and outputs high-frequency microwaves such as 2.45 GHz microwaves or 13.56 MHz radio waves (RF). The microwaves generated by the microwave source 512 are propagated to the top of the chamber 502 by the waveguide 510 and introduced into the chamber 502 via a window 514 made of quartz, ceramic, or the like. The microwaves turn the reactive gas into plasma, and the etching of the film proceeds due to electrons, ions, or radicals contained in the plasma.
[0068] A stage 10 for placing a wafer is provided at the bottom of the chamber 502. A power source 524 is connected to the stage 10, and high-frequency power is applied to the stage 10, and an electric field due to microwaves is formed in a direction perpendicular to the surface of the stage 10 and the surface of the wafer. Magnets 516, 518, and 520 can be further provided at the top and sides of the chamber 502. The magnets 516, 518, and 520 may be permanent magnets or electromagnets having electromagnetic coils. The magnets 516, 518, and 520 generate a magnetic field parallel to the stage 10 and the surface of the wafer. The magnetic field and the electric field due to the microwaves work together to cause the electrons in the plasma to resonate under the Lorentz force and be bound to the stage 10 and the surface of the wafer. As a result, a high-density plasma can be generated on the surface of the wafer.
[0069] Further connected to the stage 10 is a heater power supply 530 that controls the heater 220 provided on the stage 10. Further connected to the stage 10 may be, as optional configurations, a power supply 526 for an electrostatic chuck that fixes the wafer to the stage 10, a temperature controller 528 that controls the temperature of the medium circulated inside the stage 10, and a rotation control device (not shown) that rotates the stage 10.
[0070] <Fourth embodiment> A CVD apparatus 60 according to one embodiment of the present invention will be described with reference to Fig. 9. The CVD apparatus 60 includes a stage 10. Therefore, in the following, a description of the same or similar configuration as the configuration of the stage 10 described in the first embodiment may be omitted.
[0071] FIG. 9 is a schematic cross-sectional view showing the configuration of a CVD apparatus 60 according to one embodiment of the present invention.
[0072] The CVD apparatus 60 includes a chamber 602. The CVD apparatus 60 provides a place where reactive gases are chemically reacted to chemically form various films on a wafer.
[0073] An exhaust device 604 is connected to the chamber 602, and the pressure inside the chamber 602 can be reduced. An inlet pipe 606 for introducing a reactive gas is further provided in the chamber 602, and a reactive gas for film formation is introduced into the chamber 602 via a valve 608. As the reactive gas, various gases can be used depending on the film to be formed. The gas may be liquid at room temperature. For example, a thin film of silicon, silicon oxide, silicon nitride, or the like can be formed by using silane, dichlorosilane, tetraethoxysilane, or the like. In addition, a thin metal film of tungsten, aluminum, or the like can be formed by using tungsten fluoride, trimethylaluminum, or the like.
[0074] As in the etching apparatus 50, a microwave source 612 may be provided at the top of the chamber 602 via a waveguide 610. Microwaves generated by the microwave source 612 are introduced into the chamber 602 through the waveguide 610. The microwaves convert the reactive gas into plasma, and various active species contained in the plasma promote a chemical reaction of the gas, and the product of the chemical reaction is deposited on the wafer to form a thin film. As an optional configuration, a magnet 644 for increasing the density of the plasma may be provided in the chamber 602. A stage 10 is provided at the bottom of the chamber 602, and a thin film can be deposited with the wafer placed on the stage 10. As in the etching apparatus 50, a magnet 616 and a magnet 618 may be further provided on the side of the chamber 602.
[0075] Further connected to the stage 10 is a heater power supply 630 that controls the heater 220 provided on the stage 10. Further connected to the stage 10 as optional configurations may be a power supply 624 for supplying high frequency power to the stage 10, a power supply 626 for the electrostatic chuck, a temperature controller 628 that controls the temperature of the cooling medium circulated inside the stage 10, and a rotation control device (not shown) for rotating the stage 10.
[0076] <Fifth embodiment> A sputtering apparatus 70 according to one embodiment of the present invention will be described with reference to Fig. 10. The sputtering apparatus 70 includes a stage 10. Therefore, in the following, a description of the same or similar configuration as the configuration of the stage 10 described in the first embodiment may be omitted.
[0077] FIG. 10 is a schematic cross-sectional view showing the configuration of a sputtering apparatus 70 according to one embodiment of the present invention.
[0078] The sputtering apparatus 70 includes a chamber 702. The sputtering apparatus 70 provides a field for causing high-speed ions to collide with a target and depositing the target atoms generated during the collision onto a wafer.
[0079] An exhaust device 704 for reducing the pressure inside the chamber 702 is connected to the chamber 702. An introduction pipe 706 and a valve 708 for introducing a sputtering gas such as argon into the chamber 702 are provided in the chamber 702.
[0080] A target stage 710 that holds a target containing a material to be deposited and functions as a cathode is provided at the bottom of the chamber 702, and a target 712 is placed on the target stage 710. A high-frequency power supply 714 is connected to the target stage 710, and plasma can be generated in the chamber 702 by the high-frequency power supply 714.
[0081] A stage 10 may be provided on top of the chamber 702. In this case, thin film formation proceeds with a wafer placed under the stage 10. As with the etching apparatus 50 and the CVD apparatus 60, a heater power supply 730 is connected to the stage 10. The stage 10 may further be connected to a power supply 724 for supplying high frequency power to the stage 10, a power supply 726 for the electrostatic chuck, a temperature controller 728, and a rotation control device (not shown) for rotating the stage 10.
[0082] Argon ions accelerated by the plasma generated in the chamber 702 collide with the target 712, ejecting atoms from the target 712. The ejected atoms fly to and deposit on a wafer placed under the stage 10 while the shutter 716 is open.
[0083] 10 shows a configuration in which the stage 10 is installed at the top of the chamber 702 and the target stage 710 is installed at the bottom of the chamber 702, but the configuration of the sputtering apparatus 70 is not limited to this, and the target 712 may be located above the stage 10. Alternatively, the stage 10 may be installed so that the main surface of the wafer is disposed perpendicular to the horizontal plane, and the target stage 710 may be provided opposite the stage 10.
[0084] Sixth Embodiment A deposition apparatus 80 according to one embodiment of the present invention will be described with reference to Fig. 11. The deposition apparatus 80 includes a stage 10. Therefore, in the following, a description of a configuration that is the same as or similar to the configuration of the stage 10 described in the first embodiment may be omitted.
[0085] FIG. 11 is a schematic cross-sectional view showing the configuration of a vapor deposition apparatus 80 according to one embodiment of the present invention.
[0086] The deposition apparatus 80 includes a chamber 802. The deposition apparatus 80 is provided with a space for evaporating a material in a deposition source 810 and depositing the evaporated material onto a wafer.
[0087] An exhaust device 504 is connected to the chamber 802 to create a high vacuum inside the chamber 802. An introduction pipe 806 is provided to the chamber 802 to return the chamber 802 to atmospheric pressure, and an inert gas such as nitrogen or argon is introduced into the chamber 802 via a valve 808.
[0088] A stage 10 may be provided on the upper portion of the chamber 802. The deposition of material proceeds with the wafer placed under the stage 10. As with the etching apparatus 50, the CVD apparatus 60, and the sputtering apparatus 70, the stage 10 is further connected to a heater power supply 828. The stage 10 may further be connected to an electrostatic chuck power supply 824, a temperature controller 826, and a rotation control device 830 for rotating the stage 10 as optional configurations. The stage 10 may further include a mask holder 816 for fixing a metal mask between the wafer and the deposition source 810. This allows the metal mask to be placed near the wafer so that the opening of the metal mask overlaps with the region where the material is to be deposited.
[0089] An evaporation source 810 is provided at the bottom of the chamber, and the material to be evaporated is filled in the evaporation source 810. A heater for heating the material is provided in the evaporation source 810, and the heater is controlled by a control device 812. The inside of the chamber 802 is made into a high vacuum using an exhaust device 804, and the evaporation source 810 is heated to vaporize the material, thereby starting evaporation. When the evaporation rate becomes constant, a shutter 814 is opened, thereby starting the deposition of the material on the wafer.
[0090] The etching apparatus 50, the CVD apparatus 60, the sputtering apparatus 70, and the deposition apparatus 80 described above in the third to sixth embodiments use the stage 10. In the stage 10, no brazing material is used in the formation of the gas flow passage, so particles resulting from the brazing material are not released to the outside together with the gas flowing through the gas flow passage. Therefore, by using the stage 10, it is possible to suppress particles being released from the gas flow passage into the chamber. EXAMPLES
[0091] The stage 10 described in the first embodiment will be described in more detail based on an example. The first metal plate 110 to the third metal plate 130 were made of aluminum alloy A3003, and the example samples were produced according to the process described in the second embodiment.
[0092] Fig. 12 is a cross-sectional SEM image of the bonding interface between the first metal plate 110 and the second metal plate 120 in the example sample. Fig. 13 is a cross-sectional SEM image of the bonding interface between the second metal plate 120 and the third metal plate 130 in the example sample.
[0093] As shown in Fig. 12 and Fig. 13, no defects were found at any of the bonding interfaces. The first metal plate 110 and the second metal plate 120 are bonded by solid-phase diffusion bonding. As shown in Fig. 12, no irregularities were found at the bonding interface, and the bonding interface was found to be highly flat. On the other hand, the second metal plate 120 and the third metal plate 130 are bonded by brazing. As shown in Fig. 13, it was found that irregularities were formed at the bonding interface due to the solidification of crystal grains.
[0094] The above-described embodiments of the present invention may be combined as appropriate as long as they are not mutually inconsistent. Furthermore, those in which a person skilled in the art appropriately adds or deletes components or modifies the design based on each embodiment are also included in the scope of the present invention as long as they include the gist of the present invention.
[0095] Furthermore, even if there are other effects and advantages different from those brought about by the respective embodiments described above, those which are clear from the description in this specification or which can be easily predicted by a person skilled in the art are naturally understood to be brought about by the present invention. [Explanation of symbols]
[0096] 10: stage, 100: plate portion, 100a: first surface, 100b: second surface, 105: metal plate laminated structure, 110: first metal plate, 112: first groove portion, 114: through hole, 120: second metal plate, 122: second groove portion, 124: third groove portion, 130: third metal plate, 200: shaft portion, 210: gas introduction tube, 220: heater, 220a: terminal, 50: Etching device, 502: Chamber, 504: Exhaust device, 506: Inlet tube, 508: Valve, 510: Waveguide, 512: Microwave source, 514: Window, 516, 518, 520: Magnet, 524, 526: Power supply, 528: Temperature controller, 530: Heater power supply, 60: CVD device, 602: chamber, 604: exhaust device, 606: introduction pipe, 608: valve, 610: waveguide, 612: microwave source, 616, 618: magnet, 624, 626: power supply, 628: temperature controller, 630: heater power supply, 644: magnet, 70: sputtering device, 702: chamber, 704: exhaust device, 706: introduction pipe, 708: valve, 710: target stage, 712: target, 714: high frequency power source, 716: shutter, 724, 726: power source, 728: temperature controller, 730: heater power source, 80: deposition device, 802: chamber, 804: exhaust device, 806: introduction pipe, 808: valve, 810: deposition source, 812: control device, 814: shutter, 816: mask holder, 824: power source, 826: temperature controller, 828: heater power source, 830: rotation control device
Claims
1. A first metal plate; a second metal plate located below the first metal plate and joined to the first metal plate; a third metal plate located below the second metal plate and joined to the second metal plate; the first metal plate includes a first groove portion exposed to the outside, The second metal plate comprises: a second groove portion covered by the first metal plate and communicating with the first groove portion; a third groove portion covered by the third metal plate; the first groove portion and the second groove portion are gas flow paths, A heater is disposed in the third groove.
2. The stage of claim 1 , wherein a portion of the heater is fixed to the third groove by a brazing material.
3. The stage of claim 1 , wherein the third groove is not in communication with the first groove.
4. The stage of claim 1 , wherein there is no braze material between the first metal plate and the second metal plate.
5. The stage of claim 4 , further comprising a braze material between the second metal plate and the third metal plate.
6. The stage according to claim 1 , wherein a bonding interface including irregularities caused by crystal grains is observed between the second metal plate and the third metal plate.
7. the second metal plate is joined to the first metal plate by solid-state diffusion bonding; The stage of claim 1 , wherein the third metal plate is bonded to the second metal plate by liquid phase diffusion bonding.
8. The stage according to claim 7 , wherein the liquid phase diffusion bonding is a bonding using a brazing material. Hmm, the stage.
9. The stage of claim 1 , wherein each of the first metal plate, the second metal plate, and the third metal plate is an aluminum alloy containing magnesium.
10. The stage of claim 1 , wherein the first metal plate, the second metal plate, and the third metal plate are each an aluminum alloy containing manganese.
11. Further, the shaft is located below the third metal plate and joined to the third metal plate, The stage according to claim 1 , wherein a gas introduction pipe for supplying gas to the gas flow passage and the heater are disposed within the shaft.
Citation Information
Patent Citations
Improved heater for substrate processing equipment for depositing tungsten
JP2002513091A
Heating device and manufacturing method of the same
JP2004165085A
Heat exchanger and its manufacturing method
JP2008039255A
Suction chuck and transfer device including suction chuck
JP2014054710A
Electrostatic chuck
JP2015035446A