Cement composition and method of producing the same

A cement composition with controlled ratios of calcined inorganic minerals and Portland cement clinker enhances strength and kneadability, addressing low carbon emissions and strength degradation issues in cement compositions.

JP2024143494APending Publication Date: 2024-10-11MITSUBISHI UBE CEMENT CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023056210
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing cement compositions face challenges in achieving both low carbon emissions and maintaining good kneadability and compressive strength, particularly when replacing Portland cement clinker with limestone, as it can lead to strength degradation and fluidity issues.

Method used

A cement composition comprising specific ratios of calcined inorganic minerals, such as allophane, with controlled BET specific surface areas and mass ratios, along with Portland cement clinker and gypsum, to enhance strength development and kneadability while reducing carbon footprint.

Benefits of technology

The composition achieves excellent compressive strength at both initial and long-term stages with improved kneadability, while reducing carbon emissions by optimizing the replacement ratio of Portland cement clinker.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143494000001
    Figure 2024143494000001
  • Figure 2024143494000002
    Figure 2024143494000002
  • Figure 2024143494000003
    Figure 2024143494000003
Patent Text Reader

Abstract

To provide a low-carbon cement composition which has good kneadability and exhibits excellent compressive strength development in the early stage of hardening and over a long period of time.SOLUTION: A cement composition comprises: a calcined inorganic mineral having a ratio of the mass of SiO2 to the mass of Al2O3 of 0.5 or more and 3.0 or less and having a BET specific surface area of 30 m2 / g or more and 180 m2 / g or less; a carbonate; a Portland cement clinker, and gypsum. The content of the calcined inorganic mineral is 0.5 mass% or more and less than 10.0 mass%. The total content of the carbonate and the calcined inorganic mineral is 5 mass% or more and 15 mass% or less. The total content of the Portland cement clinker and the gypsum is 85 mass% or more and less than 95 mass%.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to cement compositions and methods for making same. [Background technology]

[0002] As part of efforts to promote low carbonization, cement compositions are being used in which part of the ordinary Portland cement, which has a large CO2 emission associated with its production, is replaced with admixtures. Limestone is widely used as an admixture added to cement because it is easy to obtain and inexpensive.

[0003] At present, the amount of admixture added to ordinary Portland cement is set at 5% by mass or less according to JIS R 5210:2009, but from the viewpoint of preventing global warming and reducing carbon, it is desired to further increase the proportion of cement clinker replaced by admixture to create an even lower carbon cement in order to reduce the amount of cement clinker used.On the other hand, it is known that simply adding limestone in excess of the current 5% results in a decrease in strength compared to ordinary Portland cement at present (for example, Non-Patent Document 1).

[0004] Regarding the types of admixtures, the JIS standard allows the use of fly ash, blast furnace slag, and silica fume in addition to limestone as minor admixture components, but it is also important to explore other promising admixtures. For example, metakaolin, which is made by calcining kaolin, a natural material, is known to provide good strength development when added to cement (Non-Patent Document 2). [Prior art documents] [Non-patent literature]

[0005] [Non-Patent Document 1] Ayuka Nakaguchi et al., "Quality evaluation of cement with increased amounts of minor mixed components", Abstracts of the Cement Technology Conference, 2018, pp.270-271 [Non-Patent Document 2] Karen Scrivener et al.: Calcined clay limestone cements (LC3), Cement and Concrete Research,Vol.114,pp.49-56 (2018) Summary of the Invention [Problem to be solved by the invention]

[0006] However, since kaolin, which is the raw material for metakaolin that exhibits good strength development in Non-Patent Document 2, is produced in limited regions and countries, there is a need to find materials other than kaolin that are effective as admixtures.

[0007] In addition, in Non-Patent Document 2, calcined clay containing metakaolin with a large BET specific surface area is added at about 30%, and it is expected that fluidity and kneadability will deteriorate when a large amount of inorganic minerals with such a large specific surface area are included. On the other hand, if an attempt is made to reduce the amount of inorganic minerals that contribute to strength development in order to improve kneadability, it is not clear how strength development will be achieved as a cement composition.

[0008] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a low-carbon cement composition that has good kneadability and exhibits excellent compressive strength development both in the early stage of hardening and over a long period of time, and a method for producing the same. [Means for solving the problem]

[0009] One aspect of the present disclosure is as follows [1] to

[10] . [1] The ratio of the mass of SiO2 to the mass of Al2O3 is 0.5 to 3.0 and the BET specific surface area is 30 m 2 / g or more 180m 21. A cement composition comprising: a calcined inorganic mineral having a calcium carbonate content of 0.5% by mass or more and less than 10.0% by mass; a combined content of the carbonate and the calcined inorganic mineral being more than 5% by mass and less than 15% by mass; and a combined content of the Portland cement clinker and the gypsum being 85% by mass or more and less than 95% by mass. [2] The cement composition according to [1], wherein the calcined inorganic mineral contains calcined allophane. [3] The cement composition according to [1] or [2], wherein the inorganic mineral before calcination has an insoluble residue of 50 mass% or less as measured based on the hydrochloric acid-sodium carbonate method of JIS R 5202:2010. [4] The cement composition according to any one of [1] to [3], wherein the content of the carbonate is 2.0 mass % or more and 9.5 mass % or less based on the total mass of the cement composition. [5] Blaine specific surface area is 3000 cm 2 / g or more 6000cm 2 The cement composition according to any one of [1] to [4], wherein the cement composition has a molecular weight of 1.0 to 1.5 μg / g or less. [6] A hardened paste comprising the cement composition according to any one of [1] to [5] and water. [7] The ratio of the mass of SiO2 to the mass of Al2O3 is 0.5 to 3.0 and the BET specific surface area is 30 m 2 / g or more 180m 2 1. A method for producing a cement composition, comprising: a preparation step of mixing a calcined inorganic mineral having a calcium carbonate content of 0.5% by mass or more and less than 10.0% by mass, a total content of the carbonate and the calcined inorganic mineral being more than 5% by mass and less than 15% by mass, and a total content of the Portland cement clinker and the gypsum being 85% by mass or more and less than 95% by mass. [8] The ratio of the mass of SiO2 to the mass of Al2O3 is 0.5 to 3.0 and the BET specific surface area is 30 m 2 / g or more 180m 2Calcined inorganic minerals with a specific surface area of ​​3000 cm3 or less are ground together with carbonates, Portland cement clinker, and gypsum to obtain a powder with a specific surface area of ​​3000 cm3. 2 / g or more 6000cm 2 / g or less, a content of the calcined inorganic mineral is 0.5% by mass or more and less than 10.0% by mass, a total content of the carbonate and the calcined inorganic mineral is more than 5% by mass and 15% by mass or less, and a total content of the Portland cement clinker and the gypsum is 85% by mass or more and less than 95% by mass. [9] The method according to [7] or [8], further comprising a calcination step of calcining the inorganic mineral before calcination at 500 to 950°C to obtain the calcined inorganic mineral.

[10] The method according to [9], wherein the inorganic mineral contains allophane. Effect of the Invention

[0010] According to the present disclosure, it is possible to provide a low-carbon cement composition that has good kneadability and exhibits excellent compressive strength development both in the early stage of hardening and over a long period of time, and a method for producing the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, embodiments of the present disclosure will be described. However, the following embodiments are merely examples for explaining the present disclosure, and are not intended to limit the present disclosure to the following contents. In the following description, when it is written "X to Y" (X and Y are arbitrary numbers), it means "X or more and Y or less" unless otherwise specified.

[0012] Unless otherwise specified, the materials exemplified in this specification can be used alone or in combination of two or more. When a plurality of substances corresponding to each component are present in the composition, the content of each component in the composition means the total amount of the plurality of substances present in the composition, unless otherwise specified.

[0013] <Cement composition> The cement composition according to one embodiment of the present disclosure has a ratio of the mass of SiO to the mass of AlO of 0.5 or more and 3.0 or less, and a BET specific surface area of ​​30 m 2 / g or more 180m 2 The cement composition according to one embodiment includes a calcined inorganic mineral (calcined inorganic mineral) having a calcium phosphate content of 0.5% by mass or more and less than 10.0% by mass, a total content of the carbonate and the calcined inorganic mineral is more than 5% by mass and less than 15% by mass, and a total content of the Portland cement clinker and the gypsum is 85% by mass or more and less than 95% by mass. The cement composition according to one embodiment can be said to be a composition in which a part of the Portland cement clinker is replaced with the calcined inorganic mineral, and is useful as a cement composition that reduces the environmental load.

[0014] (calcined inorganic minerals) Calcined inorganic minerals are those obtained by calcining inorganic minerals. Calcination increases the compressive strength of inorganic minerals, but does not substantially change the SiO2 content, Al2O3 content, or mass ratio SiO2 / Al2O3 of the inorganic minerals.

[0015] The fact that the inorganic mineral is calcined means that 27 This can be confirmed by analyzing with Al-NMR. Specifically, in inorganic minerals that have been calcined, 27 When the sum of the peak areas of 4-coordinate Al, 5-coordinate Al, and 6-coordinate Al analyzed by Al-NMR is taken as 100%, if the ratio of the peak area of ​​at least one of 4-coordinate Al and 5-coordinate Al is 30% or more and 50% or less, it can be determined that the inorganic mineral has been calcined.

[0016] In the calcined inorganic mineral, the framework of tetracoordinated Al and pentacoordinated Al is unstable, and it is considered that tetracoordinated Al and pentacoordinated Al contribute to increasing the reactivity with Portland cement clinker. When the ratio of the peak area of ​​at least one of tetracoordinated Al and pentacoordinated Al is 30% or more, it is easy to enjoy the effect of this action. When the ratio of tetracoordinated Al and pentacoordinated Al is 50% or less, it is easy to suppress the reaction with Portland cement clinker from progressing rapidly. From these viewpoints, the ratio of the peak area of ​​at least one of tetracoordinated Al and pentacoordinated Al may be 30% or more and 45% or less, or may be 35% or more and 45% or less, and it is preferable that the ratios of the peak areas of tetracoordinated Al and pentacoordinated Al are both 30% or more and 50% or less, more preferably 30% or more and 45% or less, and even more preferably 35% or more and 45% or less.

[0017] The sum of the peak areas of tetracoordinated Al and pentacoordinated Al is preferably 50% or more from the viewpoint of reactivity with Portland cement clinker, and is preferably 90% or less from the viewpoint of reaction rate with Portland cement clinker. From these viewpoints, the sum of the peak areas of tetracoordinated Al and pentacoordinated Al is more preferably 60% to 90% and even more preferably 70% to 80%. The peak area of ​​hexacoordinated Al is preferably 10% to 50%, more preferably 10% to 40%, and even more preferably 20% to 30%.

[0018] In order for an inorganic mineral to have the desired peak areas for 4-coordinate Al, 5-coordinate Al, and 6-coordinate Al, the inorganic mineral may be calcined at a predetermined temperature, more specifically, calcined according to the calcination process described below.

[0019] The peak area ratio is determined as follows: Nuclides of calcined inorganic minerals 27The chemical shift and coordination state of Al-NMR are analyzed using an NMR device JNM-ECZ800R (manufactured by JEOL Ltd.). The analysis method is the MAS (Magic Angle Spinning) method, and a 3.2 mm sample tube is used. The analysis conditions are magnetic field strength: 18.79 T, frequency: 20 kHz, number of accumulations: 256, and pulse width: 90° (0.6 μs). 27 For the Al-NMR spectrum, the waveform of each peak is separated using a Voigt function, which is a convolution function of a Gaussian function and a Lorentzian function.The area of ​​each peak is then calculated using the integral value of each separated peak.

[0020] In addition, calcined inorganic minerals 27 In the Al-NMR spectrum, peak P1 is observed in the chemical shift range of -10 ppm to 15 ppm, peak P2 in the chemical shift range of 50 ppm to 80 ppm, and peak P3 in the chemical shift range of 30 ppm to 40 ppm. Peak P1 corresponds to 6-coordinated Al, which originates from the inorganic mineral skeleton. Peaks P2 and P3 originate from 4-coordinated Al and 5-coordinated Al, respectively, which are thought to be generated by partial collapse of the inorganic mineral skeleton (e.g., decomposition and dehydroxylation of the 6-coordinated Al structure by heat treatment at high temperature). From the obtained peak areas of P1 to P3, the sum of the areas of P1 + P2 + P3 and the ratios of the areas of P2 and P3 based on the sum are calculated.

[0021] The insoluble residue of the inorganic mineral before calcination, measured based on the hydrochloric acid-sodium carbonate method of JIS R 5202:2010, may be 50% by mass or less, 40% by mass or less, or 30% by mass or less. The insoluble residue of the inorganic mineral before calcination may be 20% by mass or more, 25% by mass or more, or 35% by mass or more. The higher the insoluble residue, the higher the amount of minerals with low reactivity in the inorganic mineral. The amount of the insoluble residue can be adjusted by screening, classifying, or other screening of the inorganic mineral. If the insoluble residue of the inorganic mineral before calcination is low, the reactivity and strength expression of the inorganic mineral will be better, and by containing an appropriate amount of insoluble residue, the labor and cost for screening the inorganic mineral can be reduced.

[0022] The inorganic mineral may be a mineral produced by weathering a volcanic ejecta, i.e., a mineral derived from a volcanic ejecta. Examples of the volcanic ejecta include volcanic ash, volcanic lapilli, pumice, pyroclastic flow deposits, and the like. The inorganic mineral may be a mineral produced by weathering an igneous rock. Examples of the igneous rock include granite, and the like. In general, allophane is produced by weathering a volcanic ejecta or an igneous rock, halloysite is produced by further weathering of allophane, and kaolin is produced by further weathering of halloysite. Kaolin, allophane, and halloysite are clay minerals.

[0023] From the viewpoint of easily exhibiting sufficient compressive strength, the content of the calcined clay mineral in the calcined inorganic mineral is preferably 60 mass% or more, more preferably 80 mass% or more, and may be 100 mass% (calcined inorganic mineral essentially consisting of calcined clay mineral).

[0024] Examples of inorganic minerals (before calcination) include kaolin, allophane, halloysite, imogolite, illite, montmorillonite, pyrophyllite, etc. The mass ratio SiO2 / Al2O3 of these inorganic minerals is 0.5 or more and 3.0 or less. Among these inorganic minerals, from the viewpoint of reactivity with Portland cement clinker, the inorganic minerals preferably contain allophane or halloysite, and more preferably contain allophane.

[0025] Allophane is an amorphous inorganic mineral. Allophane generally has a particle size of 0.05 μm to 0.2 μm and can be dissolved in water at temperatures up to 250 m. 2 / g or more 600m 2 Halloysite is a crystalline inorganic mineral. Halloysite generally has a particle size of 0.1 μm to 0.3 μm and a BET specific surface area of ​​40 m 2 / g or more 100m 2 / g or less.

[0026] The calcined inorganic mineral preferably comprises calcined allophane or calcined halloysite, more preferably comprises calcined allophane. The calcined inorganic mineral may be free of metakaolin.

[0027] From the viewpoint of easily exhibiting sufficient compressive strength, the content of calcined allophane or calcined halloysite in the calcined inorganic mineral is preferably 60 mass% or more, more preferably 80 mass% or more, and may be 100 mass% (calcined inorganic mineral substantially consisting of calcined allophane or calcined halloysite). The content of calcined allophane in the calcined inorganic mineral can be measured by an acid-alkali alternating dissolution method, and the content of calcined halloysite can be measured by XRD Rietveld analysis.

[0028] The mass ratio SiO2 / Al2O3 of the calcined inorganic mineral is 0.5 or more, and may be 0.7 or more or 0.9 or more. The mass ratio SiO2 / Al2O3 of the calcined inorganic mineral is 3.0 or less, and may be 2.0 or less, 1.7 or less, or 1.2 or less. When the mass ratio SiO2 / Al2O3 is within these ranges, the reactivity between the calcined inorganic mineral and the Portland cement clinker is easily improved.

[0029] The SiO2 content in the calcined inorganic mineral is preferably 30% by mass or more and 55% by mass or less from the viewpoint of reactivity with Portland cement clinker. The Al2O3 content in the calcined inorganic mineral is preferably 20% by mass or more and 60% by mass or less from the viewpoint of reactivity with Portland cement clinker.

[0030] The BET specific surface area of ​​calcined inorganic minerals is 30m 2 / g or more, and 2 / g or more, 45m 2 / g or more, 70m 2 / g or more or 100m 2 / g or more. The BET specific surface area is 180 m 2 / g or less, 150m 2 / g or less, 120m 2 / g or less, 90m 2 / g or less, 60m 2 / g or less or 50m 2 / g or less. When the BET specific surface area is in this range, the reactivity between the calcined inorganic mineral and the Portland cement clinker is easily improved. The BET specific surface area is a specific surface area measured by a nitrogen gas adsorption method.

[0031] The content of the calcined inorganic mineral based on the total amount of the cement composition is 0.5% by mass or more, and may be 1.0% by mass or more or 2.0% by mass or more. By having the content of the calcined inorganic mineral in these ranges, better compressive strength can be obtained. The content of the calcined inorganic mineral based on the total amount of the cement composition is less than 10.0% by mass, and may be 9.0% by mass or less, 7.0% by mass or less, or 4.0% by mass or less. By having the content of the calcined inorganic mineral in these ranges, better fluidity can be maintained.

[0032] (Carbonates) Carbonates can promote the hydration reaction between Portland cement clinker and calcined inorganic minerals. Examples of carbonates include alkali metal carbonates, alkaline earth metal carbonates, and their hydrates, such as sodium carbonate, sodium carbonate decahydrate (Na2CO3·10H2O), potassium carbonate (K2CO3), calcium carbonate (limestone), and magnesium carbonate. Sodium sesquicarbonate dihydrate (Na3H(CO3)2·NaHCO3·2H2O) can also be used as a carbonate.

[0033] As the limestone, for example, powders mainly composed of calcium carbonate such as limestone powder and kansui stone powder that are generally available on the market can be used. The limestone preferably includes one that conforms to the minor mixing components described in JIS R 5210:2009 "Portland cement".

[0034] The carbonate content in the cement composition may be 2.0 mass% or more, 3.5 mass% or more, or 5.0 mass% or more, based on the total amount of the cement composition, from the viewpoint of fluidity, while it may be 15 mass% or less, 12 mass% or less, or 9.5 mass% or less, from the viewpoint of compressive strength.

[0035] Based on the total amount of the cement composition, the combined content of carbonates and calcined inorganic minerals is greater than 5% by weight, and may be 7% or more, or 9% or more, based on the total amount of the cement composition. Based on the total amount of the cement composition, the combined content of carbonates and calcined inorganic minerals is less than 15% by weight, and may be less than 13% by weight, or less than 11% by weight.

[0036] (Portland cement clinker) The Portland cement clinker may be Portland cement clinker used to prepare various Portland cements as specified in JIS R 5210:2009 "Portland cement". Examples of the Portland cement clinker include ordinary Portland cement clinker, high-early strength Portland cement clinker, moderate-heat Portland cement clinker, low-heat Portland cement clinker, oil well Portland cement clinker, etc. The Portland cement clinker may include at least one selected from the group consisting of ordinary Portland cement clinker and high-early strength Portland cement clinker, and preferably includes ordinary Portland cement clinker.

[0037] Portland cement clinker is made up of tricalcium silicate (3CaO SiO 2、 C3S), dicalcium silicate (2CaO SiO 2、 C2S), tricalcium aluminate (3CaO·Al2O 3、 C3A), tricalcium aluminate (3CaO·Al2O3, C3A), and tetracalcium aluminate ferroferrate (4CaO·Al2O3·Fe2O 3、It may contain C4AF. The content of each of C3S, C2S, C3A, and C4AF in Portland cement clinker can be calculated by the Bogue formula. The Bogue formula is a widely used formula for calculating the content ratio of major minerals in cement clinker from the content ratio of chemical composition. In the chemical formula part of the Bogue formula, chemical analysis values (content ratio (mass%) of each compound) according to JIS R 5204:2019 "Fluorescent X-ray analysis method for cement" are substituted.

[0038] <Bogue formula> C3S [mass%] = (4.07 × CaO [mass%]) - (7.60 × SiO2 [mass%]) - (6.72 × Al2O3 [mass%]) - (1.43 × Fe2O3 [mass%]) - (2.85 × SO3 [mass%]) C2S [mass%] = (2.87 × SiO2 [mass%]) - (0.754 × C3S [mass%]) C3A [mass%] = (2.65 × Al2O3 [mass%]) - (1.69 × Fe2O3 [mass%]) C4AF [mass%] = 3.04 × Fe2O3 [mass%]

[0039] The amount of C3S in Portland cement clinker may be 30.0 mass% or more and 70.0 mass% or less, preferably 40.0 mass% or more and 66.0 mass% or less, more preferably 50.0 mass% or more and 63.0 mass% or less, still more preferably 54.0 mass% or more and 59.0 mass% or less, and particularly preferably 56.0 mass% or more and 57.0 mass% or less. By setting the lower limit value of the C3S amount within the above range, the initial compressive strength in the hardening of the cement composition can be further improved. By setting the upper limit value of the C3S amount within the above range, the heat generation during the hardening of the cement composition can be suppressed.

[0040] The C2S content in the Portland cement clinker may be 5.0% by mass or more and 65.0% by mass or less, preferably 10.0% by mass or more and 50.0% by mass or less, more preferably 12.0% by mass or more and 40.0% by mass or less, even more preferably 15.0% by mass or more and 30.0% by mass or less, and particularly preferably 18.0% by mass or more and 22.0% by mass or less. By setting the lower limit of the C2S content within the above range, the long-term compressive strength during hardening of the cement composition can be further improved. Also, by setting the upper limit of the C2S content within the above range, the initial compressive strength during hardening of the cement composition can be further improved.

[0041] The amount of C3A in the Portland cement clinker may be 7.0% by mass or more, preferably 8.0% by mass or more, more preferably 8.5% by mass or more, even more preferably 9.0% by mass or more, and particularly preferably 9.5% by mass or more. By setting the lower limit of the amount of C3A within the above range, a cement composition can be produced in which the amount of waste and / or by-products such as coal ash, which are raw materials for Portland cement clinker, is further increased. The amount of C3A in the Portland cement clinker may be 13.0% by mass or less, preferably 12.0% by mass or less, more preferably 11.0% by mass or less, even more preferably 10.4% by mass, and particularly preferably 9.8% by mass or less. By setting the upper limit of the amount of C3A within the above range, it becomes easier to suppress the regeneration of ettringite (a compound represented by 3CaO·Al2O3·3CaSO4·32H2O), and the increase in adiabatic temperature rise during hardening of the cement composition can also be further reduced.

[0042] The amount of C4AF in the Portland cement clinker may be 7.0% by mass or more, preferably 8.0% by mass or more, more preferably 9.0% by mass or more, even more preferably 9.5% by mass or more, and particularly preferably 9.8% by mass or more. By setting the lower limit of the amount of C4AF within the above range, a cement composition can be produced in which the amount of waste and / or by-products such as coal ash, which are raw materials for Portland cement clinker, is further increased. The amount of C4AF in the Portland cement clinker may be 14.0% by mass or less, preferably 13.0% by mass or less, more preferably 12.0% by mass or less, even more preferably 11.0% by mass or less, and particularly preferably 10.4% by mass or less. By setting the upper limit of the amount of C4AF within the above range, the increase in adiabatic temperature rise during hardening of the cement composition can be further reduced.

[0043] The content of the Portland cement clinker may be, for example, 80% by mass or more and 93% by mass or less, 83% by mass or more and 91% by mass or less, or 85% by mass or more and 89% by mass or less, with the total amount of the cement composition being 100% by mass. By having the Portland cement clinker content in the cement composition be 80% by mass or more, 83% by mass or more, or 85% by mass or more, better compressive strength can be obtained, and by having the content be 93% by mass or less, 91% by mass or less, or 89% by mass or less, CO2 emissions can be further reduced.

[0044] (plaster) As the gypsum, for example, dihydrate gypsum, hemihydrate gypsum, anhydrous gypsum, etc. can be used. As the gypsum, one of dihydrate gypsum, hemihydrate gypsum, and anhydrous gypsum may be used alone, or a combination of two or more may be used. When the cement composition contains gypsum, the hydration reaction rate can be adjusted.

[0045] The content of gypsum in the cement composition may be equivalent to the content of gypsum in general Portland cement. The content of gypsum in the cement composition may be, for example, 0.5 to 3.5 mass%, 0.7 to 3.0 mass%, or 1.0 to 2.5 mass%, calculated as SO3, with the total amount of the cement composition being 100 mass%.

[0046] The total content of gypsum and Portland cement clinker in the cement composition is 85 mass% or more, and may be 87 mass% or more, or 89 mass% or more, based on the total amount of the cement composition. The total content of gypsum and Portland cement clinker in the cement composition is less than 95 mass%, and may be 93 mass% or less, or 91 mass% or less, based on the total amount of the cement composition. When the total content of gypsum and Portland cement clinker in the cement composition is within these ranges, it is possible to achieve both strength development and low carbonization.

[0047] (Other ingredients) The cement composition may contain other components such as inorganic fine powder, calcium hydroxide, powder containing calcium other than calcium hydroxide, water reducer for concrete, accelerator, retarder, etc. (excluding gypsum, limestone, and calcined inorganic minerals). The content of other components may be 20% by mass or less, 15% by mass or less, or 10% by mass or less based on the total amount of the cement composition.

[0048] When the cement composition contains an inorganic fine powder, the compressive strength is further improved. Examples of the inorganic fine powder include powdery materials such as silica stone and crushed stone. The content of the inorganic fine powder in the cement composition may be more than 0 mass% or 5 mass% or more from the viewpoint of fluidity, and may be 20 mass% or less, 15 mass% or less, or 10 mass% or less from the viewpoint of compressive strength, based on the total amount of the cement composition.

[0049] <Blaine specific surface area> The Blaine specific surface area of ​​the cement composition and its various components can be measured in accordance with the description of JIS R 5201:2015 "Physical Measurement Methods of Cement". The Blaine specific surface area of ​​the cement composition is 3000 cm 2 / g or more, 3250cm 2 / g or more or 3300cm 2 The Blaine specific surface area of ​​the cement composition may be 6000 cm 2 / g or less, 4000cm 2 / g or less or 3400cm 2 When the specific surface area of ​​the cement composition is within this range, it is possible to achieve both strength development and heat suppression, and it is possible to reduce the cost and CO2 emissions due to crushing.

[0050] <Cured body> The hardened body is obtained by hardening a paste containing the above cement composition and water. The hardening conditions are not particularly limited. The hardened body can be prepared in accordance with the method described in JIS R 5201:2015 "Physical test method for cement".

[0051] The amount of water in the paste is preferably 35 parts by mass or more relative to 100 parts by mass of the total amount of the cement composition from the viewpoint of fluidity, and is preferably 80 parts by mass or less from the viewpoint of making it easier to make the pore structure of the hardened body dense. From these viewpoints, the amount of water is preferably 35 parts by mass or more and 80 parts by mass or less, and more preferably 50 parts by mass or more and 70 parts by mass or less.

[0052] <Method of manufacturing cement composition> A method for producing a cement composition according to an embodiment of the present disclosure is a method for producing a cement composition having a ratio of the mass of SiO2 to the mass of Al2O3 of 0.5 or more and 3.0 or less, and a BET specific surface area of ​​30 m 2 / g or more 180m 2The method includes a preparation step of mixing calcined inorganic minerals having a calcined inorganic mineral content of 0.5% by mass or more and less than 10.0% by mass, a total content of carbonates and calcined inorganic minerals being more than 5% by mass and not more than 15% by mass, and a total content of Portland cement clinker and gypsum being 85% by mass or more and less than 95% by mass.

[0053] A method for producing a cement composition according to another embodiment of the present disclosure is a method for producing a cement composition having a ratio of the mass of SiO2 to the mass of Al2O3 of 0.5 or more and 3.0 or less and a BET specific surface area of ​​30 m 2 / g or more 180m 2 Calcined inorganic minerals with a density of 0.01g or less, carbonates, Portland cement clinker, and gypsum are mixed or simultaneously ground to produce a powder with a Blaine specific surface area of ​​3000 cm 2 / g or more 6000cm 2 / g or less, the content of calcined inorganic minerals is 0.5% by mass or more and less than 10.0% by mass, the total content of carbonates and the calcined inorganic minerals is more than 5% by mass and 15% by mass or less, and the total content of Portland cement clinker and gypsum is 85% by mass or more and less than 95% by mass.

[0054] The method for producing a cement composition may further include a calcination step, prior to the preparation step, of calcining an inorganic mineral at 500 to 950° C. to obtain a calcined inorganic mineral. In this case, the inorganic mineral may be a clay mineral.

[0055] (Preparation process) In the preparation step, the calcined inorganic minerals, carbonates, Portland cement clinker and gypsum are mixed and / or ground, and may be mixed and / or ground with the other ingredients mentioned above.

[0056] When pulverization is performed in the preparation process, the order of mixing and pulverization is not particularly limited. That is, each raw material may be mixed and then pulverized, each raw material may be individually pulverized and then mixed, or each raw material may be mixed and pulverized at the same time. A part of the above materials may be mixed and pulverized, and then the other materials may be separately pulverized and / or mixed. Mixing may be performed using a mixer such as a pan mixer, a tilting mixer, or a ribbon mixer, or may be mixed and pulverized using a pulverizer such as a ball mill, a vertical roller mill, or a roller press, or each raw material may be pulverized and then mixed using a mixer such as a mechanical mixer.

[0057] (calcination process) The calcination temperature in the calcination step is preferably 500° C. or higher from the viewpoint of increasing the compressive strength of the inorganic mineral, while it is preferably 950° C. or lower from the viewpoint of suppressing the formation of other minerals (for example, the formation of mullite in the case of allophane). From these viewpoints, the calcination temperature may be 500° C. or higher and 950° C. or lower, 600° C. or higher and 900° C. or lower, or 800° C. or higher and 900° C. or lower. The calcination time is not particularly limited, but may be 0.5 hours or higher and 5 hours or lower, or may be 1 hour or higher and 4 hours or lower, from the viewpoint of the effect on the crystal structure.

[0058] The calcination process is 27 It can be said that the calcination process is a process of calcining an inorganic mineral so that the ratio of the peak area of ​​at least one of tetracoordinated Al and pentacoordinated Al is 30% to 50% when the sum of the peak areas of tetracoordinated Al, pentacoordinated Al, and hexacoordinated Al analyzed by Al-NMR is taken as 100%. It can be said that the calcination process is a process that causes partial collapse of the inorganic mineral framework and generates peaks P2 and P3 derived from tetracoordinated Al and pentacoordinated Al, which can contribute to improving the compressive strength.

[0059] Although the embodiments of the present disclosure have been described above, the present disclosure is not limited to the above embodiments. EXAMPLES

[0060] The present disclosure will be described in more detail below with reference to examples, comparative examples, and reference examples. However, the present disclosure is not limited to the following examples.

[0061] [Raw materials for cement composition] (Portland cement clinker) As the Portland cement clinker, ordinary Portland cement clinker was used whose mineral composition calculated by the Bogue formula is shown in the following Table 1. The chemical composition of the cement used in the Bogue formula calculation was measured in accordance with the method described in JIS R 5204 "Method for fluorescent X-ray analysis of cement."

[0062] [Table 1]

[0063] (plaster) The gypsum used was one that satisfied the requirements set forth in JIS R 9151:2009 "Natural gypsum for cement."

[0064] (limestone) The limestone (LS) is a fine powder of limestone (Blaine specific surface area: 7470 cm) made by crushing limestone that has a calcium carbonate content of 90% by mass or more and an aluminum oxide content of 1.0% by mass or less and meets the requirements for minor mixed components described in JIS R 5210:2019 "Portland cement". 2 / g) was used.

[0065] (Inorganic Minerals) Allophane was used as the inorganic mineral. The trade names of allophane used were SEKADO P1 (manufactured by Shinagawa General Co., Ltd.) and Kanuma-tsuchi (manufactured by Akagi Engei Co., Ltd.). The insoluble residues of the inorganic minerals used are shown in Table 2. The insoluble residues of the inorganic minerals were measured in accordance with JIS R 5202:2010 "Methods for chemical analysis of cement". Calcined inorganic minerals were obtained by heating each of SEKADO P1 and Kanuma-tsuchi before calcination at 900°C for 60 minutes in an electric furnace. The chemical composition of the calcined inorganic minerals is shown in Table 3. The chemical components of the calcined inorganic minerals were determined by chemical analysis using the fundamental parameter method of fluorescent X-rays (equipment used: ZSX-100e manufactured by Rigaku Co., Ltd.). The density, Blaine specific surface area, and BET specific surface area of ​​the inorganic minerals before and after calcination are shown in Table 4.

[0066] [Method for measuring BET specific surface area] The amount of nitrogen gas adsorption was measured for allophane (before calcination) and calcined allophane that had been pretreated for 1 hour at 105°C in a nitrogen gas atmosphere using a BELSORPMINI manufactured by Microtrack-Bel, Inc. The BET specific surface area was calculated based on the results.

[0067] [Blaine specific surface area] The Blaine specific surface area of ​​each component of the cement composition was measured in accordance with JIS R 5201:2015 "Physical measurement method of cement".

[0068] [Table 2]

[0069] [Table 3]

[0070] [Table 4]

[0071] [Preparation of cement composition] Gypsum was added in an amount of 1.0% by mass calculated as the amount of SO3 to Portland cement clinker having the chemical composition shown in Table 1, and mixed and ground to obtain a base cement. Then, limestone powder and allophane (before calcination) or calcined allophane were mixed according to the formulation shown in Table 5 to prepare a cement composition. Reference Example 1 is a cement composition containing 4% by mass of limestone powder and corresponding to ordinary Portland cement of JIS R 5210:2009 "Portland cement".

[0072] [Preparation of hardened body] The prepared cement composition was mixed with standard sand for cement strength testing provided by the Japan Cement Association as fine aggregate and water, and a hardened body was prepared according to the method described in JIS R 5201:2015 "Physical test methods for cement." The prepared hardened body was cured underwater in a thermostatic chamber at 20°C until it was 7 or 28 days old.

[0073] [Measurement of compressive strength ratio] The compressive strength of the above-mentioned hardened body was measured at ages of 7 days and 28 days in accordance with the description of JIS R 5201:2015 "Physical Testing Methods for Cement". The results are shown in Table 5. The compressive strength ratio is the ratio (percentage) of the compressive strength of the hardened body to the compressive strength of the reference hardened body. The reference hardened body was prepared by mixing the cement composition of Reference Example 1, which corresponds to ordinary Portland cement, with standard sand for cement strength testing by the Japan Cement Association as fine aggregate and water in accordance with the method described in JIS R 5201:2015 "Physical Testing Methods for Cement".

[0074] [Table 5]

[0075] From Table 5, it was found that in Examples 1 and 2, unlike Comparative Examples 1 to 3, not only was the compressive strength particularly excellent at 7 days, but also at 28 days. Compared with Reference Example 1, which corresponds to current ordinary Portland cement, Examples 1 and 2 showed roughly equal or greater compressive strength at both 7 and 28 days, while achieving low carbonization by reducing the amount of clinker. In addition, in the cement compositions of all Examples, when the calcined inorganic mineral with a large specific surface area was in the range of 0.5 mass% or more and less than 10.0 mass%, the kneadability was good and the filling property into the mortar formwork was good.

Claims

1. A 2 O 3 SiO 2 The mass ratio of the above is 0.5 to 3.0, and the BET specific surface area is 30 m 2 / g or more 180m 2 / g or less of calcined inorganic minerals, carbonates, Portland cement clinker, and gypsum; The content of the calcined inorganic mineral is 0.5% by mass or more and less than 10.0% by mass; The total content of the carbonate and the calcined inorganic mineral is more than 5% by mass and not more than 15% by mass; A cement composition, wherein the total content of the Portland cement clinker and the gypsum is 85% by mass or more and less than 95% by mass.

2. 2. The cement composition of claim 1, wherein the calcined inorganic mineral comprises calcined allophane.

3. The cement composition according to claim 1 or 2, wherein the inorganic mineral before calcination has an insoluble residue of 50 mass% or less as measured based on the hydrochloric acid-sodium carbonate method of JIS R 5202:2010.

4. 3. The cement composition according to claim 1, wherein the content of the carbonate is 2.0 mass% or more and 9.5 mass% or less based on the total mass of the cement composition.

5. Blaine specific surface area is 3000 cm 2 / g or more 6000cm 2 The cement composition according to claim 1 or 2, wherein the viscosity is 0.05 to 1.0 MPa.

6. A hardened paste comprising the cement composition according to claim 1 or 2 and water.

7. A 2 O 3 SiO 2 The mass ratio of the above is 0.5 to 3.0, and the BET specific surface area is 30 m 2 / g or more 180m 2 1. A method for producing a cement composition, comprising: a preparation step of mixing a calcined inorganic mineral having a calcium phosphate content of 0.5% by mass or more and less than 10.0% by mass, a total content of the carbonate and the calcined inorganic mineral being more than 5% by mass and less than 15% by mass, and a total content of the Portland cement clinker and the gypsum being 85% by mass or more and less than 95% by mass.

8. A 2 O 3 SiO 2 The mass ratio of the above is 0.5 to 3.0, and the BET specific surface area is 30 m 2 / g or more 180m 2 Calcined inorganic minerals with a specific surface area of ​​3000 cm3 / g or less, carbonates, Portland cement clinker, and gypsum are simultaneously mixed and ground to obtain a powder with a specific surface area of ​​3000 cm3 / g or less. 2 / g or more 6000cm 2 / g or less, a content of the calcined inorganic mineral is 0.5% by mass or more and less than 10.0% by mass, a total content of the carbonate and the calcined inorganic mineral is more than 5% by mass and 15% by mass or less, and a total content of the Portland cement clinker and the gypsum is 85% by mass or more and less than 95% by mass.

9. The method according to claim 7 or 8, further comprising a calcination step of calcining the inorganic mineral before calcination at 500 to 950° C. to obtain the calcined inorganic mineral.

10. The method according to claim 9 , wherein the inorganic mineral comprises allophane.