Flux and cartridge

A flux with a rosin, thixotropic bisamide, and solvent composition, combined with a syringe cartridge, addresses voids and cracks in fluxes, ensuring reliable coating for electronic component bonding.

JP2024143495APending Publication Date: 2024-10-11KOKI COMPANY LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023056211
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing fluxes used in electronic component bonding can develop voids and cracks when cooled, leading to poor coating and discard, especially in three-dimensional packaging, necessitating a solution to suppress these issues and maintain applied shape.

Method used

A flux formulation comprising a rosin component, thixotropic component with bisamide compounds, and solvent component, with specific content ranges and properties, and a syringe-shaped cartridge to contain and apply the flux.

Benefits of technology

The formulation effectively suppresses voids and cracks, maintaining the applied shape and ensuring reliable coating, suitable for BGA/CSP mounting and repair.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143495000001_ABST
    Figure 2024143495000001_ABST
Patent Text Reader

Abstract

To provide a flux that prevents generation of voids and cracks and retains its applied shape, and also to provide a cartridge.SOLUTION: A flux for BGA / CSP mounting and repair in the present invention includes a rosin component, a thixotropic component, and a solvent component. The thixotropic component includes a bisamide compound. The content of the rosin component is 40.0 mass% or more and 70.0 mass% or less relative to the total flux. The rosin component has an acid value of 80 mgKOH / g or more and 210 mgKOH / g or less. The content of the bisamide compound is 2.0 mass% or more and 9.0 mass% or less relative to the total flux.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a flux and a cartridge. [Background technology]

[0002] Solder materials used for joining electronic components and the like contain a solder alloy and a flux. The flux is formulated to improve solderability and contains various components such as a resin component, an activator component, a solvent component, an antioxidant component, and a thixotropic component (a thixotropic agent component).

[0003] For example, in mounting a BGA (Ball Grid Array) or the like, when solder bumps are bonded to a substrate or electronic component, the flux may be supplied to the substrate or electronic component by itself. For example, Patent Documents 1 and 2 disclose methods for transferring flux to solder bumps of an electronic component. In such a transfer method, a squeegee is used to spread the flux on the surface of a transfer stage to form a flux coating, and then the solder bumps provided on the electronic component are landed on the flux coating to transfer the flux.

[0004] As an example of the above-mentioned flux, Patent Document 3 discloses a flux for semiconductors containing a polyamide component having a base resin, a solvent, an activator, and a thixotropic agent, in which the thixotropic agent contains a polyamide compound of an aliphatic diamine having 2 to 10 carbon atoms and / or an aromatic primary diamine having 6 to 10 carbon atoms, and a polyvalent carboxylic acid having 12 to 36 carbon atoms and / or an unsubstituted or hydroxy-substituted aliphatic monocarboxylic acid having 12 to 30 carbon atoms.

[0005] Moreover, Patent Document 4 discloses a flux applicable to a tack flux, which contains at least one selected from N-acetylimidazole, N-acetylphthalimide, and tetraacetylethylenediamine as an activator. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2011-139085 A [Patent Document 2] JP 2007-103866 A [Patent Document 3] JP 2022-80429 A [Patent Document 4] JP 2018-24023 A Summary of the Invention [Problem to be solved by the invention]

[0007] The fluxes described in Patent Documents 3 and 4 may be filled in a syringe-shaped container and delivered to a customer, and may be cooled for storage. However, when the flux filled in the syringe-shaped container is cooled, there is a risk that voids (so-called shrinkage cavities), cracks, etc. may occur in the solidified flux. Flux with voids or cracks is one of the causes of defects such as poor application, so it cannot be shipped and must be discarded. In particular, in recent years, the number of mounted components has increased, and three-dimensional mounting such as PoP mounting (Package on Package mounting) has been performed. In such three-dimensional mounting, even small voids and cracks may cause defects, so there is a need to further suppress the occurrence of voids and cracks.

[0008] In addition, there is a demand for a flux that can maintain its applied shape when filled in a syringe-shaped container and applied with a dispenser.

[0009] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a flux and a cartridge that can suppress the occurrence of voids and cracks and can maintain the applied shape. [Means for solving the problem]

[0010] The flux according to the present invention is a flux for mounting and repairing BGA / CSP, comprising a rosin component, a thixotropic component, and a solvent component, wherein the thixotropic component comprises a bisamide compound, the content of the rosin component is 40.0% by mass or more and 70.0% by mass or less with respect to the entire flux, the acid value of the rosin component is 80 mgKOH / g or more and 210 mgKOH / g or less, and the content of the bisamide compound is 2.0% by mass or more and 9.0% by mass or less with respect to the entire flux.

[0011] The cartridge according to the present invention is a syringe-shaped cartridge including a flux and a container for containing the flux, the flux being the above-mentioned flux. Effect of the Invention

[0012] According to the present invention, it is possible to provide a flux and a cartridge which are capable of suppressing the occurrence of voids and cracks and also capable of maintaining the applied shape. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a plan view of a cartridge 1 according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, a flux and a cartridge according to an embodiment of the present invention will be described.

[0015] <Flux> The flux according to the present embodiment contains a rosin component, a thixotropic component, and a solvent component.

[0016] (rosin component) The rosin component includes a rosin-based resin. Examples of the rosin-based resin include rosin and rosin derivatives. Examples of the rosin derivatives include hydrogenated rosin, polymerized rosin, disproportionated rosin, acid-modified rosin (e.g., maleic acid-modified rosin, acrylic acid-modified rosin, etc.), acid-modified hydrogenated rosin (e.g., maleic acid-modified hydrogenated rosin, acrylic acid-modified hydrogenated rosin, etc.), rosin ester, pentaerythritol ester, etc. The rosin-based resins may be used alone or in combination of two or more.

[0017] The acid value of the rosin component is 80 mgKOH / g or more and 210 mgKOH / g or less. From the viewpoint of imparting sufficient wettability to the solder, the acid value of the rosin component is preferably 120 mgKOH / g or more, and more preferably 140 mgKOH / g or more. From the viewpoint of maintaining the shape retention of the flux, the acid value of the rosin component is preferably 180 mgKOH / g or less, and more preferably 160 mgKOH / g or less. The acid value of the rosin component is obtained by multiplying the acid value of the rosin resin by the content (mass%) of the rosin resin in the entire flux (when the rosin resins are used in combination, the sum of the values ​​obtained by multiplying the acid value of each rosin resin by the content (mass%) of each rosin resin in the entire flux) by the content (mass%) of the rosin component in the entire flux. Here, the acid value represents the number of mg of potassium hydroxide required to neutralize the acidic components contained in 1 g of the sample. The acid value of the rosin-based resin is measured in accordance with the potentiometric titration method of JIS K 2501:2003.

[0018] The content of the rosin component is 40.0% by mass or more and 70.0% by mass or less with respect to the entire flux. From the viewpoint of maintaining the shape retention of the flux, the content of the rosin component is preferably 45.0% by mass or more and more preferably 50.0% by mass or more with respect to the entire flux. Moreover, from the viewpoint of ensuring the printability of the flux, the content of the rosin component is preferably 67.0% by mass or less and more preferably 65.0% by mass or less with respect to the entire flux. Note that when the rosin component contains two or more kinds of the rosin-based resins, the content is the total content of the rosin-based resins.

[0019] From the viewpoint of imparting heat resistance to the flux, the rosin component preferably contains a high softening point rosin having a softening point of 110° C. or more. Examples of high softening point rosins include polymerized rosin, acid-modified rosin, rosin-modified maleic acid resin, polymerized rosin ester, etc. The high softening point rosins may be used alone or in combination of two or more.

[0020] The softening point of the rosin-based resin is measured by the softening point test method (ring and ball method) specified in JIS K 2207:2006.

[0021] The content of the high softening point rosin is preferably 10.0% by mass or more, more preferably 30.0% by mass or more, and particularly preferably 40.0% by mass or more, based on the rosin component, from the viewpoint of improving the heat sagging property of the flux. Also, the content of the high softening point rosin is preferably 70.0% by mass or less, more preferably 65.0% by mass or less, and particularly preferably 62.0% by mass or less, based on the rosin component, from the viewpoint of ensuring the printability of the flux. When two or more types of high softening point rosins are included, the above content is the total content.

[0022] (thixotropic component) The thixotropic component includes a bisamide compound. Examples of the bisamide compound include methylene bisstearic acid amide, ethylene biscapric acid amide, ethylene bislauric acid amide, ethylene bisstearic acid amide, ethylene bishydroxystearic acid amide, ethylene bisbehenic acid amide, hexamethylene bisstearic acid amide, hexamethylene bisbehenic acid amide, hexamethylene bis-12-hydroxystearic acid amide, N,N'-distearyl adipic acid amide, and N,N'-xylylene bis-12-hydroxystearyl amide. The bisamide compound may be used alone or in combination of two or more.

[0023] The bisamide compound is preferably a bisamide compound in which one or more endothermic peaks obtained by differential thermal analysis are all observed in the range of 120° C. to 150° C. By using the bisamide compound in which one or more endothermic peaks obtained by differential thermal analysis are all observed in the range of 120° C. to 150° C., the flux can maintain its shape retention and spread over the solder before the solder melts. Examples of bisamide compounds in which one or more endothermic peaks obtained by differential thermal analysis are observed in the range of 120°C to 150°C include methylene bisstearic acid amide, ethylene bisstearic acid amide, ethylene bis12-hydroxystearic acid amide, ethylene bisbehenic acid amide, hexamethylene bisstearic acid amide, hexamethylene behenic acid amide, hexamethylene bis12-hydroxystearic acid amide, N,N'-distearyl adipamide, N,N'-distearyl sebacic acid amide, and xylene bis12-hydroxystearyl amide. In this specification, the endothermic peak refers to a peak with an endothermic amount of 10 J / g or more. Differential thermal analysis can be performed using a differential scanning calorimeter (Thermo plus DSC 8230, manufactured by Rigaku Corporation) under the following conditions.

[0024] Measurement temperature range: 30~300℃ Heating rate: 10℃ / min Measurement atmosphere: Nitrogen atmosphere, flow rate 30mL / min Sample size: 10mg

[0025] The content of the bisamide compound is 2.0% by mass or more and 9.0% by mass or less with respect to the entire flux. From the viewpoint of imparting shape retention to the flux, the content of the bisamide compound is preferably 3.0% by mass or more and more preferably 4.0% by mass or more with respect to the entire flux. Moreover, from the viewpoint of preventing shrinkage cavities and cracks in the flux and preventing deterioration of printability, the content of the bisamide compound is preferably 8.0% by mass or less and more preferably 7.0% by mass or less with respect to the entire flux.

[0026] The thixotropic component may contain other compounds other than the bisamide compound. Examples of the other compounds include castor hardened oil, monoamide compounds, polyamide compounds, kaolin, colloidal silica, organic bentonite, glass frit, etc. Examples of the monoamide compounds include caproic acid amide, caprylic acid amide, lauric acid amide, myristic acid amide, palmitic acid amide, stearic acid amide, arachidic acid amide, behenic acid amide, palmitoleic acid amide, oleic acid amide, eicosenoic acid amide, erucic acid amide, elaidic acid amide, linoleic acid amide, linolenic acid amide, ricinoleic acid amide, etc. Examples of the polyamide compound include aliphatic polyamide compounds such as TALEN VA-79, AMX-6096A, WH-215, WH-255, EMSOLDER (all manufactured by Kyoeisha Chemical Co., Ltd.), SP-10, SP-500 (all manufactured by Toray Industries, Inc.), Grilamid L20G, Grilamid TR55 (all manufactured by Ems Chem Japan Co., Ltd.), and aromatic polyamide compounds (semi-aromatic polyamide compounds or fully aromatic polyamide compounds) containing cyclic compounds such as benzene rings and naphthalene rings in the main chain, such as JH-180 (manufactured by Ito Oil Mills, Ltd.). The other compounds may be used alone or in combination of two or more.

[0027] From the viewpoint of improving the application property of the flux and the wettability of the solder, the content of the other compounds is preferably 50.0 mass % or less, more preferably 30.0 mass % or less, based on the thixotropic component. When two or more kinds of the other compounds are contained, the above content is the total content.

[0028] (Solvent component) The solvent component includes, for example, glycol ethers such as diethylene glycol monohexyl ether (hexyl diglycol), diethylene glycol dibutyl ether (dibutyl diglycol), diethylene glycol mono 2-ethylhexyl ether (2 ethylhexyl diglycol), diethylene glycol monobutyl ether (butyl diglycol), triethylene glycol monobutyl ether (butyl triglycol), polyethylene glycol dimethyl ether, and tripropylene glycol n-butyl ether; aliphatic compounds such as n-hexane, isohexane, and n-heptane; esters such as isopropyl acetate, methyl propionate, and ethyl propionate; ketones such as methyl ethyl ketone, methyl-n-propyl ketone, and diethyl ketone; and alcohols such as ethanol, n-propanol, isopropanol, and isobutanol. The solvents may be used alone or in combination of two or more.

[0029] The content of the solvent component is preferably 15.0% by mass or more, more preferably 20.0% by mass or more, and particularly preferably 25.0% by mass or more, based on the entire flux, from the viewpoint of improving the application property of the flux. Also, the content of the solvent component is preferably 50.0% by mass or less, more preferably 45.0% by mass or less, and particularly preferably 40.0% by mass or less, based on the entire flux, from the viewpoint of improving the wettability of the solder and the shape retention of the flux. When the solvent component contains two or more of the solvents, the content is the total content.

[0030] (Other resin components) The flux according to the present embodiment may contain other resin components in addition to the rosin component. The other resin components include, for example, terpene phenol resin, phenol resin, polyvinyl acetate resin, ethylene-vinyl acetate copolymer, polylactic acid, polystyrene, and other resins. The resins may be used alone or in combination of two or more.

[0031] The content of the other resin components is preferably 5.0% by mass or more, and more preferably 10.0% by mass or more, based on the entire flux, from the viewpoint of improving the shape retention of the flux. Also, the content of the other resin components is preferably 20.0% by mass or less, and more preferably 15.0% by mass or less, based on the entire flux, from the viewpoint of improving the wettability of the solder. Note that when the other resin components include two or more kinds of the resins, the above content is the total content.

[0032] (Active ingredient) The flux according to the present embodiment may contain an activator component. The activator component may include, for example, an organic acid activator, an amine compound, an amino acid, a halogen activator, or the like. The activator may be used alone or in combination of two or more kinds.

[0033] Examples of organic acid surfactants include monocarboxylic acids such as formic acid, acetic acid, propionic acid, butyric acid, caproic acid, enanthic acid, capric acid, lauric acid, pentadecylic acid, myristic acid, palmitic acid, margaric acid, stearic acid, tuberculostearic acid, arachidic acid, behenic acid, lignoceric acid, and glycolic acid; dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, methylsuccinic acid, phenylsuccinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, fumaric acid, maleic acid, tartaric acid, and diglycolic acid; and other organic acids such as dimer acid, levulinic acid, lactic acid, acrylic acid, benzoic acid, salicylic acid, anisic acid, citric acid, and picolinic acid.

[0034] Examples of the amine compounds include imidazole compounds and triazole compounds. Examples of the imidazole compounds include benzimidazole, 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole (2E4MZ), 2-heptadecylimidazole, 2-undecylimidazole, 1-(4,6-diamino-s-triazin-2-yl)ethyl-2-undecylimidazole, 1-butylimidazole, 2-phenylimidazole, and 4-methyl-2-phenylimidazole. Examples of the triazole compounds include benzotriazole, 1H-benzotriazole-1-methanol, and 1-methyl-1H-benzotriazole. Other amine compounds include, for example, cetylamine, erucic acid amide, 3-(dimethylamino)-1,2-propanediol, 3,5-dimethylpyrazole, dimethylurea, hexahydro-1,3,5-triphenyl-1,3,5-triazine, pyrazinamide, N-phenylglycine, 3-methyl-5-pyrazolone, N-lauroylsarcosine, and 1,3-diphenylguanidine.

[0035] Examples of amino acids include N-acetylphenylalanine (N-acetyl-L-phenylalanine, N-acetyl-DL-phenylalanine, N-acetyl-D-phenylalanine), N-acetylglutamic acid (N-acetyl-L-glutamic acid), N-acetylglycine, N-acetylleucine (N-acetyl-L-leucine, N-acetyl-DL-leucine, N-acetyl-D-leucine), and N-acetylphenylglycine (N-acetyl-N-phenylglycine, N-acetyl-L-phenylglycine, N-acetyl-DL-phenylglycine).

[0036] Examples of halogen-based activators include amine halogen salts and halogen compounds. Examples of amines in amine halogen salts include diethylamine, dibutylamine, tributylamine, diphenylguanidine, and cyclohexylamine. Examples of halogens in amine halogen salts include fluorine, chlorine, bromine, and iodine. Examples of halogen compounds include tris(2,3-dibromopropyl)isocyanurate, 2,3-dibromo-2-butene-1,4-diol, 2-bromo-3-iodo-2-butene-1,4-diol, TBA-bis(2,3-dibromopropyl ether), and 4,4'-diiodobiphenyl.

[0037] The content of the activator component is preferably 20.0 mass % or less, more preferably 10.0 mass % or less, based on the total flux, from the viewpoint of preventing an increase in the viscosity and adhesive strength of the flux. Moreover, it is particularly preferable that the flux according to the present embodiment does not contain an activator component from the viewpoint of improving cleaning properties. Note that, when the activator component contains two or more types of the activators, the content is the total content.

[0038] The flux according to the present embodiment may contain other additive components. The other additive components include, for example, additives such as stabilizers, surfactants, defoamers, antioxidants, and pigments. From the viewpoint of improving the visibility of the flux, the pigment is preferably, for example, a black pigment, a blue pigment, a red pigment, a green pigment, or the like. The additives may be used alone or in combination of two or more kinds.

[0039] The content of the other additive components may be, for example, 5.0 mass % or less based on the total amount of the flux. When the other additive components include two or more of the additives, the above content is the total content.

[0040] The flux according to the present embodiment can be suitably used as a flux for BGA / CSP mounting and repair. Specifically, it can be used as a soldering flux for semiconductor package parts such as ball grid arrays (BGA) and CSP parts in PoP mounting, a repair flux, etc. In addition, the flux is applied to the soldering part by discharging from a cartridge, transferring, or printing.

[0041] The flux according to the present embodiment is a flux for mounting and repairing BGA / CSP, which contains a rosin component, a thixotropic component, and a solvent component, and the thixotropic component contains a bisamide compound, the rosin component has a content of 40.0% by mass to 70.0% by mass with respect to the entire flux, the acid value of the rosin component is 80 mgKOH / g to 210 mgKOH / g, and the bisamide compound has a content of 2.0% by mass to 9.0% by mass with respect to the entire flux, thereby suppressing the occurrence of voids and cracks and maintaining the applied shape, and also preventing the flux from dripping from the solder bumps after the flux is transferred to the solder bumps.

[0042] In the flux according to the present embodiment, the rosin component contains high softening point rosin having a softening point of 110°C or more, and the content of the high softening point rosin is 10.0 mass% or more relative to the rosin component, thereby suppressing the occurrence of voids and cracks and better maintaining the applied shape.

[0043] <Cartridge> Hereinafter, the cartridge 1 according to this embodiment will be described with reference to the drawings. Fig. 1 is a plan view of the cartridge 1 according to the embodiment of the present invention. The cartridge 1 according to this embodiment is a syringe-shaped cartridge including a flux 2 and a container 3 for storing the flux 2.

[0044] The container 3 configured to accommodate the flux 2 includes a cylindrical body 31, a sealing member 32 fitted into one axial end of the cylindrical body 31, and a lid member 33 fitted into the other axial end of the cylindrical body 31.

[0045] The container 3 is configured such that the flux 2 can be filled into the cylindrical body 31 from the other end side in the axial direction of the cylindrical body 31 by removing the lid member 33. Also, the cylindrical body 31 has a tapered shape at one end side in the axial direction. As a result, the container 3 is configured such that the flux 2 can be discharged from the one end side in the axial direction of the cylindrical body 31 by removing the sealing member 32.

[0046] With the sealing member 32 attached, the cylindrical body 31 is filled with the liquid flux 2 from the other end side in the axial direction. Thereafter, the lid member 33 is attached to the cylindrical body 31, thereby manufacturing the cartridge 1. The flux 2 is the flux described above.

[0047] The cartridge 1 can be attached to a dispenser for use. Specifically, the syringe-shaped cartridge 1 is attached to a fixture for the cartridge 1, and the flux filled in the cartridge 1 is discharged by applying pressure or force to the inside of the cartridge 1. Discharge methods include the air pulse method and JET method using compressed air, and the screw method in which discharge is performed by rotating a screw-shaped rod. The discharge amount can be controlled by changing the flow rate or outflow time of the compressed air with a controller, or by changing the temperature of the flux inside the cartridge 1 with a temperature regulator attached to the fixture for the cartridge 1.

[0048] The cartridge 1 of this embodiment is a syringe-shaped cartridge 1 including a flux 2 and a container 3 for containing the flux 2. Since the flux 2 is the above-mentioned flux, it is possible to prevent voids and cracks from occurring in the flux and to maintain the applied shape of the flux.

[0049] The present invention includes the following aspects. [1] A flux for mounting and repairing BGA / CSP, comprising a rosin component, a thixotropic component, and a solvent component, the thixotropic component comprises a bisamide compound, The content of the rosin component is 40.0 mass% or more and 70.0 mass% or less with respect to the entire flux, The acid value of the rosin component is 80 mgKOH / g or more and 210 mgKOH / g or less, A flux, wherein the content of the bisamide compound is 2.0 mass % or more and 9.0 mass % or less with respect to the entire flux. [2] The rosin component contains a high-softening point rosin having a softening point of 110°C or higher, The flux according to [1], wherein the content of the high softening point rosin is 10.0 mass% or more with respect to the rosin component. [3] A syringe-shaped cartridge including a flux and a container for storing the flux, The flux is the flux according to [1] or [2]. EXAMPLES

[0050] Examples of the present invention will be described below, but the present invention is not limited to the following examples.

[0051] <Preparation of flux> The materials in the amounts shown in Tables 1 to 3 were placed in a heating vessel and heated to 180°C to dissolve all of the materials. The materials were then cooled to room temperature to obtain uniformly dispersed fluxes of each Example and Comparative Example. The amounts shown in Tables 1 to 3 are equal to the contents of each component in the flux.

[0052] <Making Cartridges> The flux of each Example and Comparative Example that had been cooled to room temperature was left to stand for 16 hours, and then heated to 130°C to dissolve it. 30 g of the flux was filled into a syringe-shaped container and cooled to room temperature to obtain a cartridge of each Example and Comparative Example.

[0053] [Table 1]

[0054] [Table 2]

[0055] [Table 3]

[0056] Table 4 shows details of each material contained in the flux shown in Tables 1 to 3.

[0057] [Table 4]

[0058] <Acid value and softening point measurement> The acid value of the rosin-based resin was measured by the potentiometric titration method of JIS K 2501: 2003. The softening point of the rosin-based resin was measured by the softening point test method (ring and ball method) specified in JIS K 2207: 2006. The measurement results are shown in Table 5.

[0059] [Table 5]

[0060] <Measurement of endothermic peak temperature> The endothermic peak temperature of each thixotropic component was measured by differential thermal analysis. Specifically, the measurement was performed under the following conditions using a differential scanning calorimeter (Thermo plus DSC 8230, manufactured by Rigaku Corporation). The endothermic peak temperatures with endothermic amounts of 10 J / g or more obtained by differential thermal analysis are shown in Table 6.

[0061] (Measurement conditions) Measurement temperature range: 30~300℃ Heating rate: 10℃ / min Measurement atmosphere: Nitrogen atmosphere, flow rate 30mL / min Sample size: 10mg

[0062] [Table 6]

[0063] <Appearance evaluation> The produced cartridges of each Example and Comparative Example were left to stand at room temperature for 3 days, and then the appearance of the flux was visually observed. The appearance was evaluated as "good" when no voids or cracks were generated in the flux, and as "poor" when voids or cracks were generated in the flux. The evaluation results are shown in Tables 1 to 3.

[0064] <Evaluation of printability> The printability was evaluated by carrying out a room temperature static test of IPC TM-650 2.4.35 Solder Paste Slump Test. More specifically, a metal mask IPC-A-21 was placed on an alumina substrate, and about 5 g of the flux of each example and comparative example was placed on the metal mask, and hand printing was performed using a metal squeegee.

[0065] (Printing conditions) Pad shape: Square (0.33mm x 2.03mm) Pad material: OSP treated copper

[0066] After printing the flux of each Example and Comparative Example, the metal mask was removed and the specimen was left to stand for 10 minutes in an environment with a room temperature of 25±5°C and a humidity of 50±10%RH. Then, the spaces between the printed fluxes (7 locations of 0.45, 0.40, 0.35, 0.30, 0.25, 0.20, and 0.15 mm) were visually observed, and the locations where bridges occurred were recorded. The printability was evaluated as "good" when no bridges occurred in any of the spaces, as "△" when bridges occurred but no bridges occurred in the spaces of 0.45 to 0.30 mm, and as "x" when bridges occurred in the spaces of 0.45 to 0.30 mm or the flux could not be printed. The evaluation results are shown in Tables 1 to 3.

[0067] <Overall rating> When the appearance and printability were both evaluated as "good", it was judged as "A", and when the appearance was evaluated as "good" and the printability was evaluated as "△", it was judged as "B". When the evaluation results were "A" and "B", the overall evaluation was "pass". When the appearance was evaluated as "good" and the printability was evaluated as "x", it was judged as "C", when the appearance was evaluated as "x" and the printability was evaluated as "good", it was judged as "D", when the appearance was evaluated as "x" and the printability was evaluated as "△", it was judged as "E", and when the appearance and printability were both evaluated as "x", it was judged as "F". When the evaluation results were "C", "D", "E", or "F", the overall evaluation was "fail".

[0068] From the results of Tables 1 to 3, it can be said that the flux of each Example that satisfies all the requirements of the present invention can suppress the occurrence of voids and cracks because no voids or cracks occurred in the flux in the appearance evaluation. Also, it can be said that the flux of each Example that satisfies all the requirements of the present invention can maintain the coating shape because no bridges occurred in spaces of at least 0.45 to 0.30 mm in the printability evaluation. In other words, the flux and cartridge of each Example that satisfies all the requirements of the present invention can suppress the occurrence of voids and cracks and can maintain the coating shape. [Explanation of symbols]

[0069] 1 Cartridge 2. Flux 3 Flux container

Claims

1. A flux for BGA / CSP mounting and repair, comprising a rosin component, a thixotropic component, and a solvent component, the thixotropic component comprises a bisamide compound, The content of the rosin component is 40.0 mass% or more and 70.0 mass% or less with respect to the entire flux, The acid value of the rosin component is 80 mgKOH / g or more and 210 mgKOH / g or less, A flux, wherein the content of the bisamide compound is 2.0 mass % or more and 9.0 mass % or less with respect to the entire flux.

2. The rosin component contains a high-softening point rosin having a softening point of 110° C. or more, 2. The flux according to claim 1, wherein the content of the high softening point rosin is 10.0 mass% or more based on the rosin component.

3. A syringe-like cartridge including a flux and a container for containing the flux, A cartridge, wherein the flux is the flux according to claim 1 or 2.

Citation Information

Patent Citations

  • Device for transferring flux in electronic component packaging equipment

    JP2007103866A

  • Flux transfer device

    JP2011139085A

  • Flux and solder composition

    JP2018024023A

  • Flux and solder paste with use thereof

    JP2022080429A