Method for manufacturing conductive paste and electronic component
An emulsified conductive paste is prepared using specific material interactions to stabilize the silicone resin dispersion, addressing sheet attack and ensuring strong adhesion to silicone substrates, thereby enhancing conductivity and flexibility.
Patent Information
- Application Number
- JP2023056286
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Conductive pastes containing silicone resins face issues with organic solvents penetrating into silicone substrates, causing sheet attack such as swelling and deformation, while maintaining fixability to the substrate is challenging.
A method for preparing an emulsified conductive paste by uniformly dispersing a silicone resin in a liquid phase that is difficult to penetrate into a silicone substrate, using specific material interactions and solubility parameters to stabilize the emulsified state, ensuring a uniform contact area between the silicone resin and the substrate.
The method effectively suppresses sheet attack while ensuring strong adhesion of the conductive film to the silicone substrate, maintaining both conductivity and flexibility.
Smart Images

Figure 2024143551000010 
Figure 2024143551000011 
Figure 2024143551000012
Abstract
Description
[Technical field]
[0001] The technology disclosed herein relates to a method for producing a conductive paste and an electronic component. [Background technology]
[0002] With the progress of development of flexible devices, there is an increasing demand for electronic components in which conductive films such as electrodes and wiring are formed on the surface of a flexible resin substrate such as plastic or rubber. Such flexible electronic components are manufactured, for example, by applying a conductive paste to the surface of a substrate and curing the conductive paste. The conductive paste contains, for example, a conductive material, a binder resin, and an organic solvent. The binder resin is a curable resin that is cured by heat or light and fixed to the insulating substrate.
[0003] Silicone substrates are widely used as insulating substrates for this type of electronic component. Silicone substrates are excellent in chemical durability, high heat resistance, biosafety, low dielectric constant, high insulation, etc., and can contribute to improving the quality of electronic components. On the other hand, silicone substrates have low surface energy, so the binder resin tends not to adhere well after curing. For this reason, silicone resin, which is the same type of resin material as the insulating substrate, is used as the binder resin for conductive pastes for silicone substrates. For example, Patent Document 1 discloses an example of a conductive paste containing silicone resin. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent Publication No. 2021-193165 Summary of the Invention [Problem to be solved by the invention]
[0005] However, conductive pastes containing silicone resins use organic solvents capable of dissolving the silicone resins. Such organic solvents penetrate into the silicone substrate to which they are applied, causing sheet attacks such as swelling and deformation of the substrate. For this reason, there is a demand for conductive pastes for silicone substrates that can suppress sheet attacks while ensuring adhesion to the substrate.
[0006] In response to this, the present inventors came up with the idea of preparing an emulsified conductive paste in which a liquid phase containing a silicone resin is uniformly dispersed in a liquid phase that is difficult to penetrate into a silicone substrate. Although such an emulsified conductive paste is difficult to penetrate into a silicone substrate, it is possible to ensure the contact area between the silicone resin and the silicone substrate. In other words, if an emulsified conductive paste can be realized, it is expected that sheet attack can be suppressed while ensuring adhesion to the substrate. The present inventors then investigated a method for realizing an emulsified conductive paste. [Means for solving the problem]
[0007] The manufacturing method disclosed herein includes a preparation step of preparing raw materials including a conductive material A, a polyol B, a silicone resin C, an organic solvent D, and a silicone oil E, and a mixing step of mixing the prepared raw materials to prepare a paste. This manufacturing method is characterized in that in the preparation step, each raw material is prepared so as to satisfy the following conditions (1) to (4): (1) HSP distance Ra between polyol B and silicone resin C B-C is the interaction radius R of silicone resin C 0C The first relative energy difference RED is the value divided by BC (2) The HSP distance Ra between the silicone resin C and the silicone oil E is 1.0 or more and 2.0 or less. C-E The interaction radius R of the silicone oil E 0E The second relative energy difference RED is the value divided by CE (3) The HSP distance Ra between the polyol B and the silicone oil E is less than 1.0. B-E The interaction radius R of the silicone oil E0E The third relative energy difference RED is the value divided by BE (4) The polarity term ΔP of organic solvent D is 1.5 MPa. 0.5 More than 15MPa 0.5 The following is the result.
[0008] The condition (1) of the manufacturing method having the above configuration means that each material is selected so that the polyol B and the silicone resin C are not compatible with each other. The condition (2) means that each material is selected so that the silicone resin C dissolves in the silicone oil E. The condition (3) means that each material is selected so that the polyol B and the silicone oil E are appropriately compatible with each other. The condition (4) means that an organic solvent D is selected that can sufficiently dissolve the polyol B and maintain a stable emulsified state. By satisfying these conditions (1) to (4), a conductive paste can be prepared in which a liquid phase (silicone phase) mainly containing the silicone resin C and the silicone oil E is emulsified and dispersed in a liquid phase (polyol phase) mainly containing the polyol B and the organic solvent D.
[0009] As another aspect of the technology disclosed herein, an electronic component is provided. The electronic component disclosed herein includes a silicone substrate and a conductive film formed on the surface of the substrate and containing a conductive material. The conductive film includes a urethane region mainly made of urethane resin and a silicone region mainly made of silicone resin. In the electronic component disclosed herein, the number of silicone regions per 1 μm of the length of the contact interface between the substrate and the conductive film in a cross-sectional view is 1 to 20.
[0010] The electronic component disclosed herein is manufactured using the emulsified conductive paste obtained by the manufacturing method configured as above. Specifically, when the conductive paste having a polyol phase and a silicone phase is cured, a urethane region is formed by the curing of the polyol phase, and a silicone region is formed by the curing of the silicone phase. At this time, if the silicone phase is uniformly dispersed until the conductive paste is in an emulsified state, the number of silicone regions present per 1 μm length of the contact interface between the substrate and the conductive film in the cross-sectional view of the cured electronic component is 1 to 20. This makes it possible to suitably fix the conductive film to the substrate while suppressing sheet attack. [Brief description of the drawings]
[0011] [Figure 1] FIG. 2 is a schematic diagram showing a conductive paste prepared by the manufacturing method disclosed herein. [Diagram 2] 1 is an optical microscope photograph (500x) showing an example of a conductive paste prepared by the manufacturing method disclosed herein. [Diagram 3] 4 is an optical microscope photograph (500x) showing another example of a conductive paste prepared by the manufacturing method disclosed herein. [Figure 4] 3 is an enlarged photograph (1080x) of the conductive paste shown in FIG. 2. [Diagram 5] 1 is a cross-sectional view that diagrammatically illustrates an electronic component disclosed herein. [Figure 6] 1 is a FE-SEM photograph of the electronic component of Example 1. [Figure 7] 1 is a photograph showing the distribution of Si elements by EDX mapping of the electronic component of Example 1. [Figure 8] 1 is a FE-SEM photograph of the electronic component of Example 18. [Figure 9] 1 is a photograph showing the distribution of Si elements by EDX mapping of the electronic component of Example 18. [Figure 10] 1 is a graph showing the results of line analysis in the first field of view in Example 1. [Figure 11] 1 is a graph showing the results of line analysis in the second field of view of Example 1. [Figure 12] 1 is a graph showing the results of line analysis in the first field of view of Example 18. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, one embodiment of the technology disclosed herein will be described. Note that matters other than those specifically mentioned in this specification and necessary for implementing the technology disclosed herein can be implemented based on the technical content taught by this specification and the general technical common sense of a person skilled in the art. The technology disclosed herein can be implemented based on the contents disclosed in this specification and the technical common sense of a person skilled in the art.
[0013] In this specification, the expression "A to B (A and B are arbitrary values)" indicating a numerical range includes the meaning of "A or more and B or less", as well as "preferably larger than A" and "preferably smaller than B".
[0014] <Method of manufacturing conductive paste> The method for producing a conductive paste disclosed herein includes at least a preparation step and a mixing step. Each step will be described below.
[0015] 1.Preparation process In this step, there is prepared a raw material containing a conductive material A, a polyol B, a silicone resin C, an organic solvent D, and a silicone oil E. The raw materials of the conductive paste will be described below.
[0016] (1) Conductive material A The conductive material A is a component that imparts electrical conductivity to the conductive film after curing. The type of the conductive material A is not particularly limited, and one or more types can be appropriately selected from conventionally known materials having electrical conductivity. Examples of the conductive material A include simple conductive metals such as gold (Au), silver (Ag), copper (Cu), platinum (Pt), palladium (Pd), nickel (Ni), rhodium (Rh), ruthenium (Ru), iridium (Ir), and osmium (Os), as well as mixtures and alloys thereof. The conductive material A may also be a carbon material having electrical conductivity (e.g., graphite, carbon nanotubes, etc.). Among the above-mentioned materials, gold, silver, copper, platinum, palladium, nickel, rhodium, and carbon are particularly preferable because they can form a conductive film with excellent electrical conductivity at low cost.
[0017] In addition, the shape of the conductive material A is preferably non-spherical. When the conductive paste obtained by the manufacturing method disclosed herein is cured, the conductive material A is likely to aggregate inside the silicone region, as will be described in detail later. In this case, if a non-spherical (high aspect ratio) conductive material A is used, a part of the conductive material A is likely to protrude outside the silicone region. This makes it easier to generate a conductive path in the conductive film, so that a conductive film with low resistance can be formed. For example, the average aspect ratio of the conductive material A is preferably 1.2 or more, more preferably 1.5 or more, even more preferably 2 or more, and particularly preferably 2.5 or more. On the other hand, the upper limit of the average aspect ratio of the conductive material A is not particularly limited, and may be 20 or less, 15 or less, 10 or less, or 5 or less. In addition, specific shapes of the conductive material A include dendritic, plate-like, needle-like, fibrous, etc. By using these non-spherical conductive materials A, a network of suitable conductive paths can be formed in the conductive film after curing. In addition, the "average aspect ratio" in this specification can be obtained by observing multiple (e.g., 100) conductive materials A with an electron microscope and calculating the arithmetic average value of the aspect ratio (long side / short side) of each conductive material A.
[0018] The specific surface area of conductive material A is 0.5 m 2 / g or more is preferable, and 1.5m 2 / g or more is more preferable, and 2m2 / g or more is more preferable, and 3m 2 / g or more is particularly preferred. As the specific surface area of the conductive material A increases, the chances of the conductive material A coming into contact with itself increases. This improves the conductivity of the conductive film after curing. On the other hand, the upper limit of the specific surface area of the conductive material A is not particularly limited, and is preferably 20 m 2 / g or less, 10m 2 / g or less. If the specific surface area of the conductive material A becomes too large, the dispersibility of the conductive material A and the printability of the conductive paste tend to decrease. From this viewpoint, the specific surface area of the conductive material A is set to 8 m 2 / g or less is preferable, and 7m 2 / g or less is more preferable, and 6m 2 / g or less is more preferable, and 5m 2 / g or less is particularly preferred.
[0019] The tap density of conductive material A is 5 g / cm 3 Less than 2.5 g / cm is preferred. 3 Less than 1.5 g / cm is more preferable. 3 More preferably, 1 g / cm 3 The following is particularly preferred. This allows the conductive film to maintain its flexibility after curing while easily forming a conductive path in the conductive film. On the other hand, from the viewpoint of increasing the conductivity, the tap density of the conductive material A is preferably 0.01 g / cm 3 More than 0.05 g / cm is preferable. 3 More preferably, 0.1 g / cm 3 More preferably, 0.2 g / cm 3 The above is particularly preferred.
[0020] The weight of conductive material A when the total weight of the conductive paste is 100 wt% is W A is more preferably 75 wt% or less, more preferably 72 wt% or less, even more preferably 70 wt% or less, and particularly preferably 65 wt% or less. This allows the addition of a sufficient amount of other components (e.g., polyol B, silicone resin C), thereby further improving the fixation to the silicone substrate. On the other hand, when the conductivity of the conductive film after curing is taken into consideration, the weight W of conductive material A is Ais preferably 15 wt% or more, more preferably 20 wt% or more, even more preferably 23 wt% or more, and particularly preferably 25 wt% or more.
[0021] In addition, it is more preferable to adjust the amount of conductive material A based on the weight ratio when the weight of the conductive paste excluding the organic solvent D is taken as 100 wt%. This allows more accurate control of the performance (fixation and conductivity) of the conductive film after curing. For example, the amount of conductive material A excluding the organic solvent D is preferably 85 wt% or less, more preferably 82 wt% or less, even more preferably 80 wt% or less, and particularly preferably 77 wt% or less. This increases the contact area between the binder resin and the substrate in the electronic component after manufacture, thereby further improving the fixation of the conductive film. On the other hand, the amount of conductive material A excluding the organic solvent D is preferably 10 wt% or more, more preferably 15 wt% or more, even more preferably 20 wt% or more, and particularly preferably 25 wt% or more. This allows more accurate improvement of the conductivity of the conductive film.
[0022] (2) Polyol B Polyol B is a binder resin that forms a urethane region, which will be described later. The type of polyol B is not particularly limited, and one or more types can be appropriately selected from conventionally known materials that can be used to form a urethane resin according to the application. Specifically, polyol B is an organic compound having two or more hydroxyl groups (-OH). Such polyol B reacts with isocyanate F to produce a urethane resin and harden. An example of such polyol B is a polyether polyol obtained by adding an alkylene oxide such as ethylene oxide (EO) or propylene oxide (PO) to a polyhydric alcohol such as ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, butylene glycol, neopentyl glycol, 3-methyl-pentanediol, hexanediol, heptanediol, octanediol, nonanediol, glycerin, pentaerythritol, trimethylolpropane, sorbitol, or sucrose, and polymerizing the result. Further examples include polyester polyols obtained by polycondensation of an aliphatic carboxylic acid such as malonic acid, succinic acid, adipic acid, etc., an aromatic carboxylic acid such as phthalic acid, etc., and an aliphatic glycol such as ethylene glycol, diethylene glycol, propylene glycol, etc. Other examples include polycarbonate polyols, polyurethane polyols, epoxy polyols, vegetable oil polyols, polyolefin polyols, acrylic polyols, fluorine polyols, vinyl monomer modified polyols, etc.
[0023] It is preferable that polyol B has three or more hydroxyl groups. This provides the urethane resin (urethane region) after curing with restorability against deformation, and can suppress damage to the conductive film when the electronic component is folded. The upper limit of the number of hydroxyl groups in polyol B is not particularly limited, and may be six or less, or may be five or less.
[0024] The molecular weight of polyol B is preferably 1000 or more, more preferably 1300 or more, even more preferably 1700 or more, and particularly preferably 2000 or more. As the molecular weight of polyol B increases, the urethane resin after curing (the urethane region described below) becomes softer, so that the flexibility of the conductive film tends to improve. On the other hand, the upper limit of the molecular weight of polyol B is preferably 50000 or less, more preferably 25000 or less, even more preferably 10000 or less, and particularly preferably 6000 or less. As the molecular weight of polyol B decreases, the strength of the urethane resin tends to increase.
[0025] In addition, the weight W of polyol B when the total weight of the conductive paste is 100 wt% B is preferably 1 wt% or more, more preferably 3.5 wt% or more, further preferably 5 wt% or more, and particularly preferably 7 wt% or more. B As the weight W of polyol B increases, the amount of polyol phase in the paste increases relatively, so that sheet attack tends to be suppressed. B The upper limit of the weight W of polyol B is preferably 35 wt % or less, more preferably 30 wt % or less, further preferably 25 wt % or less, and particularly preferably 20 wt % or less. B As the value of α becomes smaller, the silicone phase becomes relatively more abundant, and the adhesion of the conductive film tends to improve.
[0026] (3) Silicone resin C Silicone resin C is a binder resin that forms a silicone region. The type of silicone resin C is not particularly limited, and one or more types can be appropriately selected from materials that have been conventionally used as thermosetting silicone resins according to the application. Specifically, silicone resin C is an organic compound having a plurality of unit structures having Si-O-Si bonds (siloxane bonds). Examples of unit structures of such silicone resin C include silicone oligomers, organosiloxanes, diorganosiloxanes, organopolysiloxanes, diorganopolysiloxanes, etc. The skeleton of silicone resin C may be linear or branched. Examples of thermosetting silicone resin C include addition-curing silicone resins in which Si-H groups and vinyl groups are bonded and cured by hydrosilylation reaction, and condensation-curing silicone resins in which silanol groups are cured by dehydration condensation reaction. Among these, addition-curing silicone resins are more preferable. The addition curing type silicone resin can prevent the formation of bubbles or cracks in the conductive film after curing because the generation of by-products during curing is suppressed. The silicone resin may have a reactive functional group such as an epoxy group, an isocyanate group, a hydroxyl group, or a carboxyl group. These reactive functional groups can crosslink silicone resins with each other or bond urethane resins to silicone resins. The number of reactive functional groups imparted to such a unit structure is not particularly limited and may be 1 to 5 or 2 to 4.
[0027] The molecular weight of silicone resin C is preferably 1000 or more, more preferably 2000 or more, even more preferably 3000 or more, and particularly preferably 4000 or more. As the molecular weight of silicone resin C increases, the viscosity increases, and the compatibility with silicone oil (E) described later tends to decrease. On the other hand, the upper limit of the molecular weight of silicone resin C is preferably 500000 or less, more preferably 200000 or less, even more preferably 100000 or less, and particularly preferably 80000 or less. As the molecular weight of silicone resin C decreases, the viscosity decreases, and the compatibility with silicone oil (E) tends to improve.
[0028] In addition, the weight W of silicone resin C when the total weight of the conductive paste is 100 wt% C is preferably 1 wt% or more, more preferably 2 wt% or more, even more preferably 5 wt% or more, and particularly preferably 7 wt% or more. C As the weight W of silicone resin C increases, the silicone phase becomes relatively more abundant, and the adhesion of the conductive film tends to improve. C The upper limit of the weight W of the silicone resin C is preferably 30 wt % or less, more preferably 20 wt % or less, further preferably 16 wt % or less, and particularly preferably 10 wt % or less. C As the ratio becomes smaller, the polyol phase becomes relatively larger, and sheet attack tends to be easily suppressed.
[0029] (4) Organic solvent D As described in detail below, the organic solvent D used in the manufacturing method disclosed herein is a solvent that can stably maintain the emulsified state of polyol B and silicone resin C. That is, in the manufacturing method disclosed herein, a solvent that satisfies the condition (4) described below is selected. The organic solvent D may be an organic solvent that can penetrate into a silicone substrate when used alone. Specifically, the HSP value of the organic solvent D is not particularly limited as long as the HSP value is such that the organic solvent D does not easily penetrate into a silicone substrate in the state of a polyol phase in which polyol B is dissolved. In other words, the organic solvent D can be appropriately selected from one or more conventionally known organic solvents that can be used to prepare a conductive paste, as long as the effect of the technology disclosed herein is not significantly impaired. For example, in the technology disclosed herein, under the criterion of satisfying the condition (4) described below, 2-octanone, 2-nonanone, 2-heptanone, 3-heptanone, 4-heptanone, 2-hexanone, 3-hexanone, diisobutyl ketone, methylcyclohexanone, acetophenone, methylacetophenone, ethylene glycol, propylene glycol, terpineol, texanol, dihydroterpineol, diglyme, triglyme, methyl acetate, ethyl acetate, propyl acetate, butyl acetate, isobutyl acetate, amyl acetate, butenyl acetate, isoamyl acetate, isobornyl acetate, propyl formate, butyl formate, isoformate, An appropriate solvent can be appropriately selected from butyl, amyl formate, isoamyl formate, methyl valerate, methyl pentenoate, methyl crotonate, ethyl crotonate, methyl lactate, ethyl lactate, propyl lactate, butyl lactate, isobutyl lactate, amyl lactate, isoamyl lactate, methyl 2-hydroxyisobutyrate, ethyl 2-hydroxyisobutyrate, methyl benzoate, ethyl benzoate, phenyl acetate, benzyl acetate, methyl phenylacetate, benzyl formate, phenylethyl formate, methyl 3-phenylpropionate, benzyl propionate, ethyl phenylacetate, 2-phenylethyl acetate, toluene, xylene, and solvent naphtha.
[0030] The content of the organic solvent D can be appropriately changed from the viewpoint of adjusting the viscosity of the conductive paste to an appropriate state, and does not limit the technology disclosed herein. As an example, the weight W of the organic solvent D when the total weight of the conductive paste is 100 wt % is D is preferably 5 wt% or more, more preferably 7.5 wt% or more, and particularly preferably 10 wt% or more. This tends to reduce the viscosity of the conductive paste. On the other hand, the weight W of the organic solvent D D is preferably 17.5 wt% or less, more preferably 15 wt% or less, and particularly preferably 12.5 wt% or less. D As the amount of the conductive paste decreases, the viscosity of the conductive paste tends to increase.
[0031] (5) Silicone Oil E Silicone oil E is an oil agent that dissolves silicone resin. The type of silicone oil E is not particularly limited, and one or more types can be appropriately selected from materials that have been conventionally used as silicone oils that can dissolve silicone resin, depending on the application. Specifically, silicone oil E refers to organic compounds that have a plurality of unit structures having Si-O-Si bonds (siloxane bonds) and are liquid at room temperature. Examples of such silicone oil E include dimethylpolysiloxane, decamethylcyclopentasiloxane, dodecamethylcyclohexasiloxane, disiloxane, trisiloxane, methyltrimethicone, caprylylmethicone, methylphenylpolysiloxane, methylhexylpolysiloxane, and methylhydrogenpolysiloxane. In addition, an alkyl group, a phenyl group, or the like is present at the end of the main chain (siloxane skeleton) of the above-mentioned silicone oil E. The ends of these silicone oils E may be substituted with a predetermined functional group (hydroxyl group, isocyanate group, carboxyl group, etc.). Among these substituents, hydroxyl groups, isocyanate groups, carboxyl groups, etc. are particularly preferred. When silicone oil E having these functional groups is contained in the silicone phase, the composite property of the silicone phase and the polyol phase is improved. This can improve the extensibility of the conductive film after curing.
[0032] In addition, the weight of silicone oil E when the total weight of the conductive paste is 100 wt% is W E is preferably 1 wt% or more, more preferably 1.5 wt% or more, and particularly preferably 1.9 wt% or more. E As the weight W of silicone oil E increases, the silicone phase becomes relatively more abundant, and the adhesion of the conductive film tends to improve. E The weight W of the silicone oil E is preferably 15 wt% or less, more preferably 14 wt% or less, and particularly preferably 13 wt% or less. E As the amount of the polyol phase decreases, the amount of the polyol phase relatively increases, so that the sheet attack tends to be easily suppressed.
[0033] (6) Isocyanate F In addition, in the technology disclosed herein, it is preferable to add isocyanate F as a raw material for the conductive paste. Isocyanate F is an organic compound having one or more isocyanate groups (-N=C=O). This isocyanate F forms a urethane bond with the hydroxyl group of polyol B to produce a urethane resin. Also, isocyanate F may be a diisocyanate having two isocyanate groups, or a polyisocyanate having three or more isocyanate groups.
[0034] In addition, the weight W of isocyanate F when the total weight of the conductive paste is 100 wt% F is preferably 1 wt% or more, more preferably 2 wt% or more, and particularly preferably 2.5 wt% or more. F As the weight W of isocyanate F increases, the urethane region is more likely to form in the cured conductive film. F is preferably 20 wt % or less, more preferably 17 wt % or less, and particularly preferably 14 wt % or less, whereby the contents of other raw materials in the conductive paste can be sufficiently ensured.
[0035] (7) Other additives In addition, the manufacturing method disclosed herein can use additives used as raw materials for the conductive paste without any particular restrictions, so long as they do not significantly impair the effects of the technology disclosed herein. Examples of such additives include dispersants, surface tension regulators, surfactants, adhesion promoters, and strength enhancers (fillers). The content of these additives is also appropriately adjusted within a range that does not significantly impair the effects of the technology disclosed herein.
[0036] 2.Mixing process In this step, the prepared raw materials are mixed to prepare a paste. Specifically, in the mixing step, the raw materials prepared and weighed in the preparation step are homogeneously stirred and mixed. This allows the preparation of a conductive paste. For the stirring and mixing in this step, a conventionally known stirring and mixing device can be used. Examples of such stirring and mixing devices include a planetary mixer, a rotary orbital mill, a roll mill, a magnetic stirrer, a planetary mixer, a disperser, and the like.
[0037] 3.Dispersion conditions In the manufacturing method disclosed herein, in the preparation step, the raw materials are prepared so that the following conditions (1) to (4) are controlled within predetermined ranges, thereby making it possible to prepare a conductive paste in which a silicone phase is emulsified and dispersed in a polyol phase.
[0038] (1) First relative energy difference RED BC First, in the production method disclosed herein, the HSP distance Ra between polyol B and silicone resin C is B-C is the interaction radius R of silicone resin C 0C The first relative energy difference RED is the value divided by BC is controlled to be 1.0 or more and 2.0 or less. This makes it possible to prevent compatibility between the polyol B and the silicone resin C. This will be specifically explained below.
[0039] First, the "HSP distance Ra" is the difference between the Hansen solubility parameters (HSP) of two substances. Specifically, the HSP is expressed by a coordinate position in a three-dimensional space (Hansen space) consisting of a dispersion term δD, a polar term δP, and a hydrogen bond term δH. The HSP distance Ra is the distance between two substances in the Hansen space. The smaller the HSP distance Ra, the more similar the solubilities of the two substances can be considered to be. Next, the "interaction radius R0" is the radius of a sphere (Hansen sphere) in the Hansen space centered on the target substance. The radius of this Hansen sphere (interaction radius R0) is set so as to include the coordinates of a substance that can dissolve the target substance. Here, whether or not two given substances are compatible with each other is determined by the ratio (Ra / R0) of the HSP distance Ra of the two substances to the interaction radius R0 of one substance. In general, this ratio Ra / R0 is called the "relative energy difference RED." When this relative energy difference RED becomes large, the interface between the two target substances repels each other, making them more likely to separate in the paste. On the other hand, when the relative energy difference RED becomes small, the interface between the two substances becomes more compatible, making them more likely to disperse uniformly in the paste. Furthermore, when the relative energy difference RED becomes even smaller and becomes less than 1, the two substances become compatible.
[0040] In the production method disclosed herein, the relative energy difference RED between polyol B and silicone resin C (first relative energy difference RED BC ) is set to 1.0 or more. By selecting polyol B and silicone resin C so as to satisfy this condition, it is possible to prevent polyol B and silicone resin C from becoming miscible with each other in the conductive paste. BC The lower limit of is preferably 1.2 or more, more preferably 1.4 or more, further preferably 1.6 or more, and particularly preferably 1.8 or more. This allows the polyol B and the silicone resin C to be suitably separated.
[0041] On the other hand, according to an experiment conducted by the present inventor, the first relative energy difference REDBC It has been confirmed that when the first relative energy difference RED exceeds 2.0, the adhesion of the cured conductive film is significantly reduced. BC The upper limit of the first relative energy difference RED is set to 2.0 or less. BC The upper limit of is preferably 1.98 or less, more preferably 1.96 or less, even more preferably 1.94 or less, and particularly preferably 1.92 or less, whereby the deterioration of the fixing property of the conductive film can be more suitably prevented.
[0042] (2) Second relative energy difference RED CE Next, in the manufacturing method disclosed herein, the HSP distance Ra between the silicone resin C and the silicone oil E is C-E The interaction radius R of the silicone oil E 0E (Second relative energy difference RED CE ) is controlled to be less than 1.0. By selecting the silicone resin C and the silicone oil E so as to satisfy this condition, it is possible to dissolve the silicone resin C in the silicone oil E. As a result, in the manufactured conductive paste, a silicone phase containing the silicone resin C and the silicone oil E is easily generated. Note that the second relative energy difference RED CE is preferably 0.9 or less, more preferably 0.8 or less, even more preferably 0.6 or less, and particularly preferably 0.5 or less. This allows the silicone phase to be generated more appropriately. On the other hand, the second relative energy difference RED CE The lower limit of is not particularly limited, and may be 0 or more, 0.01 or more, 0.05 or more, or 0.1 or more.
[0043] (3) 3rd relative energy difference RED BE Next, in the production method disclosed herein, the HSP distance Ra between the polyol B and the silicone oil E is B-E The interaction radius R of the silicone oil E 0E The third relative energy difference RED is the value divided by BEis controlled to 1.0 or more. By selecting polyol B and silicone oil E so as to satisfy this condition, polyol B becomes less soluble in silicone oil E. As a result, the conductive paste after preparation is more likely to have both a liquid phase containing polyol B (polyol phase) and a liquid phase containing silicone resin C (silicone phase). Note that the third relative energy difference RED BE The lower limit value of is preferably 1.02 or more, more preferably 1.04 or more, and particularly preferably 1.06 or more. This makes it more difficult for the polyol phase and the silicone phase to become miscible with each other.
[0044] On the other hand, in the manufacturing method disclosed herein, the third relative energy difference RED BE The upper limit of the third relative energy difference RED is controlled to 1.5 or less. This makes the interface between the polyol B and the silicone oil E more compatible. As a result, the polyol phase and the silicone phase tend to be more easily emulsified and dispersed uniformly. BE The upper limit of is preferably 1.41 or less, more preferably 1.3 or less, and particularly preferably 1.2 or less. This makes it easier to prepare an emulsified conductive paste.
[0045] (4) Polarity term δP of organic solvent D In the manufacturing method disclosed herein, the polarity term ΔP of the Hansen solubility parameter of organic solvent D is appropriately set from the viewpoint of maintaining a stable emulsified state between the polyol phase and the silicone phase. Specifically, the upper limit of the polarity term ΔP of organic solvent D is set to 15 MPa. 0.5 Less than or equal to 14MPa 0.5 Less than 13MPa, more preferably 13MPa 0.5 More preferably, 12 MPa or less. 0.5 Below 11MPa, particularly preferably 0.5 On the other hand, the lower limit of the polarity term ΔP of organic solvent D is set to 1.5 MPa. 0.5 or more (preferably 1.6MPa 0.5 More preferably, 1.7 MPa 0.5 More preferably, 1.8 MPa 0.5 More preferably, 1.9 MPa or more 0.5(or more).
[0046] (5) Summary As described above, in the manufacturing method disclosed herein, a plurality of liquid phases including a polyol phase containing polyol B and a silicone phase containing silicone resin C are generated, and the relative solubility of each raw material is set so that the interface between the polyol phase and the silicone phase is compatible to a certain extent. This makes it possible to prepare a conductive paste in which the silicone phase is emulsified and dispersed in the polyol phase. In addition, in the manufacturing method disclosed herein, the polarity term ΔP of the organic solvent D is set so that the emulsified state between the polyol phase and the silicone phase is stabilized.
[0047] (6) Other conditions An example of the conditions for the manufacturing method disclosed herein has been described above. Note that the manufacturing method disclosed herein may be set to conditions other than the above-mentioned conditions (1) to (4).
[0048] (6-1) Relative Energy Difference RED for Isocyanates For example, in the manufacturing method disclosed herein, the relative energy difference of other raw materials may be adjusted. An example of the relative energy difference regarding isocyanate F will be described below. The emulsified conductive paste can be realized if the above conditions (1) to (4) are satisfied. The following conditions are for more easily preparing the emulsified conductive paste, and are not intended to limit the technology disclosed herein.
[0049] As described above, in the manufacturing method disclosed herein, isocyanate F may be added. It is preferable that the relative energy difference of this isocyanate F with respect to other raw materials is set so that it is mainly present in the polyol phase of the conductive paste after preparation. For example, the HSP distance Ra between isocyanate F and polyol B is F-B is the interaction radius R of isocyanate F 0F The fifth relative energy difference RED is the value divided by FBis preferably less than 1.0 (more preferably 0.8 or less, even more preferably 0.6 or less, and particularly preferably 0.5 or less). This allows the formation of a polyol phase containing polyol B and isocyanate F. FD The lower limit value is not particularly limited, and may be 0 or more, 0.01 or more, or 0.05 or more.
[0050] On the other hand, the HSP distance Ra between silicone resin C and isocyanate F C-F is the interaction radius R of silicone resin C 0C The sixth relative energy difference RED is the value divided by CF is preferably 1.0 or more (more preferably 1.1 or more, even more preferably 1.15 or more, and particularly preferably 1.2 or more). This makes it possible to prevent compatibility between the isocyanate F and the silicone resin C. In addition, the sixth relative energy difference RED CF By increasing the relative energy difference RED, the sheet attack by isocyanate F can be suppressed. CF The upper limit of is preferably 1.5 or less, more preferably 1.4 or less, and particularly preferably 1.3 or less. This allows the polyol phase and the silicone phase to blend more easily, making it easier to prepare an emulsified conductive paste.
[0051] (6-2) Mixing ratio of each ingredient In the manufacturing method disclosed herein, it is preferable to adjust not only the solubility of each raw material but also the blending ratio within a predetermined range. Note that the blending ratio described below can be appropriately changed depending on the composition of the object (substrate) to which the paste is applied and the performance (conductivity, elasticity, etc.) required for the conductive film after curing, and is not intended to limit the technology disclosed herein.
[0052] (a) Weight ratio W of silicone resin C to polyol B B / W C For example, the weight W of silicone resin C C Weight W of polyol B B Ratio of W B / WC is preferably set to 0.6 or more (more preferably 0.8 or more, even more preferably 1.0 or more, and particularly preferably 1.2 or more). This increases the contact area between the polyol phase and the substrate, making it possible to more suitably suppress sheet attack. On the other hand, the ratio W B / W C The upper limit is preferably set to 4.0 or less (more preferably 3.6 or less, even more preferably 3 or less, and particularly preferably 2.5 or less), which increases the contact area between the silicone phase and the substrate, thereby more preferably improving the fixation of the conductive film after curing.
[0053] (b) Weight ratio W of silicone resin C to silicone oil E E / W C In addition, the weight W of silicone resin C C Weight W of silicone oil E E Ratio of W E / W C is preferably set to 0.35 or more (more preferably 0.4 or more, even more preferably 0.5 or more, and particularly preferably 0.7 or more). This allows the polyol phase and the silicone phase to be sufficiently blended together. On the other hand, the above ratio W E / W C The upper limit is preferably set to 2.0 or less (more preferably 1.9 or less, even more preferably 1.8 or less, and particularly preferably 1.7 or less). This makes it possible to prevent inhibition of curing of silicone resin C, thereby imparting sufficient strength to the cured film and ensuring adhesion to the substrate.
[0054] <Conductive paste> Next, a conductive paste produced by the manufacturing method having the above configuration will be described. FIG. 1 is a schematic diagram showing a conductive paste obtained by the manufacturing method disclosed herein. FIG. 2 is an optical microscope photograph (500x) showing an example of a conductive paste obtained by the manufacturing method disclosed herein. FIG. 3 is an optical microscope photograph (500x) showing another example of a conductive paste obtained by the manufacturing method disclosed herein. FIG. 4 is an enlarged photograph (1080x) of the conductive paste shown in FIG. 2. Note that FIG. 3 is an optical microscope photograph of a conductive paste in which the amount of conductive material is reduced compared to the example shown in FIG. 2.
[0055] First, this conductive paste contains at least a conductive material A, a polyol B, a silicone resin C, an organic solvent D, and a silicone oil E. The details of these raw materials have already been described, so a duplicated description will be omitted.
[0056] 1 to 4 is a two-phase paste having a polyol phase 1 and a silicone phase 2. In this conductive paste, the silicone phase 2 is emulsified and dispersed in the polyol phase 1.
[0057] The term "polyol phase" as used herein refers to a liquid phase mainly containing polyol B and organic solvent D. The term "mainly containing" as used herein means that most of the polyol phase 1 is polyol B and organic solvent D, and does not intend to exclude the inclusion of other components. For example, when isocyanate F is added as a curing agent for polyol B, it is preferable that the isocyanate F is also contained in the polyol phase 1. More specifically, the term "polyol phase" as used herein refers to a liquid phase in which the total amount of polyol B, organic solvent D, and isocyanate F is 20 wt% or more (preferably 25 wt% or more, more preferably 30 wt% or more, and particularly preferably 35 wt% or more) relative to the total amount of the liquid phase (100 wt%).
[0058] On the other hand, the term "silicone phase" refers to a liquid phase mainly containing silicone resin C and silicone oil E. As with the polyol phase, the term "mainly containing" here means that the majority of the silicone phase is silicone resin C and silicone oil E, and does not intend to exclude the inclusion of other components. For example, the term "silicone phase" in this specification refers to a liquid phase in which the total amount of silicone resin C and silicone oil E is 20 wt% or more (preferably 25 wt% or more, more preferably 30 wt% or more, and particularly preferably 35 wt% or more) relative to the total amount of the liquid phase (100 wt%). In addition, as shown in Figs. 3 and 4, in the prepared conductive paste 1, the conductive material A is easily held inside the silicone phase 3. This is presumably because the conductive material A, which has a hydrophobic surface, is easily compatible with the hydrophobic silicone resin.
[0059] In addition, the term "emulsion dispersion" in this specification is a concept that includes emulsion, microemulsion, and bicontinuous emulsion. The term "emulsion" here refers to a state in which a substantially spherical silicone phase of about 1 to 1000 μm is uniformly dispersed in a polyol phase. The term "microemulsion" refers to a state in which a substantially spherical silicone phase of 1 μm or less is uniformly dispersed in a polyol phase. The term "bicontinuous emulsion" refers to a state in which both the silicone phase and the polyol phase have a continuous structure. Although this does not limit the technology disclosed herein, the conductive paste obtained by the manufacturing method of the above configuration maintains an emulsification dispersion even after being left at 25° C. for one day or more (preferably five days or more, more preferably ten days or more, even more preferably fifteen days or more, and particularly preferably twenty days or more) after preparation. As described above, the manufacturing method disclosed herein appropriately controls the relative energy difference between each material, and therefore, separation between the silicone phase and the polyol phase can be prevented in the conductive paste after preparation.
[0060] <Electronic components> Next, an electronic component manufactured using the conductive paste having the above-mentioned structure will be described. Fig. 5 is a cross-sectional view showing a schematic example of an electronic component.
[0061] In forming the electronic component disclosed herein, first, the conductive paste having the above-mentioned configuration is applied to the surface of a substrate, and then heated at a predetermined temperature. This causes the binder resins (polyol B, silicone resin C) in the conductive paste to thermally cure. As a result, an electronic component 100 having the configuration shown in FIG. 5 is manufactured. The electronic component 100 includes a substrate 10 made of silicone and a conductive film 20 formed on the surface of the substrate 10.
[0062] (1) Base material The substrate 10 of the electronic component 100 disclosed herein is an insulating substrate made of silicone. The specific material and structure of the substrate 10 are not particularly limited, and any conventionally known substrate that can be used as a substrate for this type of electronic component can be used without particular limitation.
[0063] (2) Conductive film As shown in FIG. 5, the conductive film 20 includes a urethane region 22 and a silicone region 24. The urethane region 22 is a region where the polyol phase 2 of the conductive paste shown in FIG. 1 is thermally cured. Therefore, the urethane region 22 contains, as a main component, a urethane resin in which polyol is urethane-bonded. Here, "containing a urethane resin as a main component" refers to 50% or more (preferably 55% or more, more preferably 60% or more, and particularly preferably 65% or more) of the organic compound contained in the urethane region 22 being a urethane resin. The upper limit of the urethane resin in the urethane region 22 is not particularly limited, and may be 100%, 95% or less, or 90% or less.
[0064] Next, the silicone region 24 is a region where the silicone phase 3 of the conductive paste 1 shown in FIG. 1 has been thermally cured. Therefore, the silicone region 24 contains, as a main component, a silicone resin cured by a dehydration condensation reaction caused by heating. Here, "containing a silicone resin as a main component" refers to 50% or more (preferably 55% or more, more preferably 60% or more, and particularly preferably 65% or more) of the organic compound contained in the silicone region 24 being silicone resin. The upper limit of the silicone resin in the silicone region 24 is not particularly limited, and may be 100%, 95% or less, or 90% or less.
[0065] In the conductive paste before curing, the silicone phase 2 is dispersed in the polyol phase 1. Therefore, in the conductive film 20 after curing, a urethane region 22 derived from the polyol phase 1 and a silicone phase 2 derived from the silicone phase 2 are formed. At this time, when the conductive paste in which the silicone phase 2 is dispersed until it becomes an emulsified state is thermally cured, the number of silicone regions 24 present per 1 μm length of the contact interface between the substrate 10 and the conductive film 20 in the cross-sectional view shown in FIG. 5 is 1 to 20. This makes it possible to sufficiently ensure the adhesion between the substrate 10 and the conductive film 20 while suppressing sheet attack on the substrate 10.
[0066] The "number of silicone regions per 1 μm of the length of the contact interface between the substrate and the conductive film" can be measured by line analysis using EDX (Energy Dispersive X-ray). The "number of silicone regions per 1 μm" was measured by the following procedure. First, a cross-sectional photograph of the electronic component is taken using FE-SEM. The sample for FE-SEM photography is prepared by polishing the resin member in which the electronic component is embedded by ion milling, and then evaporating carbon onto the exposed cross-section (photographed surface). Next, a measurement line parallel to the upper surface of the substrate is drawn on the conductive film in the acquired FE-SEM image. At this time, the region in which the measurement line is drawn is set to a region within 500 nm from the upper surface of the substrate. Then, a line scan EDX measurement is performed along this measurement line. Then, the obtained line scan image is used to quantify the number of Si elements present on the measurement line using image analysis software (such as Web Plot Digitizer Version 4.6). In addition, in the measurement of the number of Si elements, it is preferable to evaluate in a field where the absolute value of the skewness is 0.35 or more. This can suppress the inclusion of noise in the measurement results. In addition, from the viewpoint of obtaining more accurate measurement results, it is preferable that the magnification of the FE-SEM image of the measurement target is about 3000 to 5000 times (the length of the measurement line is 2 to 4 μm). In this case, in order to eliminate errors due to the presence of aggregates, voids, etc., line analysis is performed in multiple (3 to 10) fields of view. Then, after calculating the deviation of the Si count number in each field of view (individual value-average value), the deviation is divided by the average value. Then, the region where the value obtained by dividing this deviation by the average value is a positive value is regarded as a "silicone region", and the "number of silicone regions present per 1 μm" can be obtained by dividing the number of silicone regions present by the length of the measurement line.
[0067] The "number of silicone regions per 1 μm" is preferably 18 or less, more preferably 16 or less, even more preferably 14 or less, and particularly preferably 10 or less. This makes it possible to more suitably suppress sheet attack on the substrate 10 by the silicone regions 24 (silicone phase). On the other hand, the lower limit of the "number of silicone regions per 1 μm" is preferably 2 or more, more preferably 3 or more, and particularly preferably 4 or more. This makes it possible to further improve the adhesion between the substrate 10 and the conductive film 20.
[0068] As shown in Figs. 1 to 3, in the conductive paste before curing, the conductive material A is mainly present in the silicone phase 2. Therefore, in the conductive film 20 after curing, the conductive material A aggregates inside each of the plurality of silicone regions 24 as shown in Fig. 5. In the conductive film 20 of the electronic component 100 disclosed herein, the silicone regions 24 are in contact with each other. As a result, the conductive materials A in the plurality of silicone regions 24 are connected to each other, and a conductive path is formed inside the conductive film 20. Note that this form is not intended to limit the electronic component disclosed herein. For example, as shown in Fig. 5, the conductive material A2 present in the silicone region 24 may be connected via the conductive material A1 present in the urethane region 22. Even in such a case, an appropriate conductive path can be formed inside the conductive film 20.
[0069] The tensile modulus of the silicone region 24 is preferably 0.1 MPa or more, more preferably 0.3 MPa or more, even more preferably 0.5 MPa or more, and particularly preferably 0.7 MPa or more. This allows the conductive film 20 to be formed with a certain level of strength or more. On the other hand, the tensile modulus of the silicone region 24 is preferably 10.0 MPa or less, preferably 7.5 MPa or less, preferably 5 MPa or less, and particularly preferably 3.4 MPa or less. This allows the stretchability of the conductive film 20 to be improved.
[0070] [Test example] Hereinafter, some test examples related to the technology disclosed herein will be described. Note that the following descriptions of the test examples are not intended to limit the technology disclosed herein.
[0071] [Preparation of conductive composition] First, conductive material A, polyol B, silicone resin C, organic solvent D, and silicone oil E shown in Tables 1 to 5 were prepared. Then, the Hansen solubility parameters of polyol B, silicone resin C, organic solvent D, and silicone oil E were measured. Details of each material are shown in Tables 2 to 5.
[0072] [Table 1]
[0073] [Table 2]
[0074] [Table 3]
[0075] [Table 4]
[0076] [Table 5]
[0077] The procedure for measuring the Hansen solubility parameters in this test is as follows. First, 10 mg of the measurement target (polyol B, silicone resin C, silicone oil E) was weighed. Then, the measurement target was added to a solvent (10 ml) and kept in a sealed container at 25°C for 24 hours. Then, it was determined whether the measurement target was completely dissolved or not. Next, two types of silicone substrates were cut into 5 mm square test pieces, and the test pieces were immersed in each of the solvents (2 ml). The silicone substrates used here were a silicone rubber sponge sheet with a skin layer (δD=15.9, δP=2.5, δH=3.4, R0=4.7) and a low-hardness silicone rubber sheet (δD=16.4, δP=4.2, δH=2.5, R0=5.8). Then, 5 hours after immersion, the test pieces were taken out, and the organic solvent D attached to the surface was wiped off, and the swelling degree was measured. The degree of swelling here is the value obtained by dividing the "difference in weight before and after immersion" by the "weight before immersion." If the degree of swelling was 0.3 or more, it was determined that swelling had occurred in the test piece. The results of judging the "solubility of the resin" and the "swellability of the substrate" on a two-level scale of good / bad were then entered into the software HSPiP (Hansen Solubility Parameters in Practice) to calculate δD, δP, δH, and R0. The solubility and swelling tests were conducted using pure and mixed solvents.
[0078] Next, 19 kinds of conductive pastes were prepared (Examples 1 to 19) by mixing the materials shown in Tables 1 to 5 in the weight ratios (wt%) shown in Tables 6 and 7. In addition, in the preparation of the conductive pastes, a stirring and degassing device with a vacuum device (Mazerustar KK-VT300, manufactured by Kurabo Industries, Ltd.) was used to uniformly stir and mix. In this test, polyisocyanate (Takenate B-820NP, manufactured by Mitsui Chemicals, Inc.) was added as isocyanate F, and titanium ethyl acetoacetate (TC-750, manufactured by Matsumoto Fine Chemical Co., Ltd.) was added as a curing catalyst. The contents of these additives are also shown in Tables 6 and 7. In addition, silicone resins (c-1) and (c-3) contained silica as impurities, and silicone resin (c-3) contained iron oxide. The contents of these impurities are also shown in Tables 6 and 7.
[0079] [Table 6]
[0080] [Table 7]
[0081] 1. Evaluation test (1) Preparation of test specimens A conductive paste was applied to the surface of each of the two types of silicone base materials by printing using a metal mask (opening size: 10 mm x 10 mm, thickness: 0.05 mm). The conductive paste was then thermally cured by performing a heat treatment at 100°C for 3 hours. In this manner, a test piece was produced in which a conductive film was formed on the surface of the silicone base material. In this test example, an evaluation test was performed on two types of silicone base materials. The results of the evaluation test below are based on the average value of the two silicone base materials.
[0082] (2) Cross-sectional observation In this test, cross-sectional observation was performed on the test pieces of Example 1 and Example 18. Specifically, first, the test pieces embedded in resin were sliced, and FE-SEM images were obtained. In addition, EDX element mapping was performed on the obtained FE-SEM images to examine the distribution of Si elements. The FE-SEM photograph of Example 1 is shown in FIG. 6, and the EDX mapping of Si elements is shown in FIG. 7. The FE-SEM photograph of Example 18 is shown in FIG. 8, and the EDX mapping of Si elements is shown in FIG. 9. The EDX measurement was performed under the following conditions.
[0083] [EDX measurement conditions] FE-SEM equipment: Hitachi High-Technologies Corporation, SU-8200 EDX analyzer: Horiba, X-Max80 Analysis software: EMAX ENERGY version 2.04
[0084] [EDX detection conditions] Applied voltage: 15.0 kV Emission current: 10 μA Extraction voltage: 4.2 kV Probe current setting: High Condenser lens 1: 4.0 Working distance: 15.0 ± 0.5 mm
[0085] In this test, according to the above-described procedure, for Example 1 and Example 18, the "number of silicone regions per 1 μm length of the contact interface between the substrate and the conductive film" was measured. In this test, line analysis was performed in three fields of view. The analysis results in the first field of view of Example 1 are shown in FIG. 10, and the analysis results in the second field of view are shown in FIG. 11. On the other hand, the analysis results in the first field of view of Example 18 are shown in FIG. 12. In the second to third fields of view of Example 18, since the skewness of the Si count number became 0 or less, they were excluded from the measurement targets. In FIGS. 10 to 12, the horizontal axis indicates the "distance of line scan (length of measurement line)", and the vertical axis indicates the "count number of line scan (number of Si elements)". The conditions in this line analysis are as follows.
[0086] [Line scan conditions] Number of frames: 5 Dwell time: 50000 s
[0087] <WebPlotDigitizer analysis conditions> Algorithm: ΔX step w / Interpolation ΔX step: 0.05 units Smoothing: 50% of ΔX
[0088] (3) Volume resistivity The volume resistivity of the conductive film of each test piece was measured using a resistivity meter (manufactured by Mitsubishi Chemical Analytech Co., Ltd., model: Loresta GP MCP-T610). The measurement results are shown in Tables 8 and 9. In the table, "OL" means that the measurement exceeded the upper limit value.
[0089] (4) Fixing property test A cross-cut test was performed by cutting each test piece into a lattice shape with a width of 2 mm to prepare 25 micro-pieces. Each micro-piece was then observed to see whether or not damage (peeling) had occurred at the interface between the substrate and the conductive film. In this test, if there were 23 or more micro-pieces that were not damaged, the test was judged as "○", and if there were less than 23 micro-pieces, the test was judged as "×". The evaluation results are shown in Tables 8 and 9.
[0090] (5) Sheet attack test The interface between the substrate and the conductive film of each test piece was observed from the horizontal direction. Test pieces in which warping due to swelling of the substrate was confirmed were rated as "x", and test pieces in which warping was not confirmed were rated as "○". The evaluation results are shown in Tables 8 and 9.
[0091] [Table 8]
[0092] [Table 9]
[0093] As shown in Figs. 6 and 7, in the electronic component manufactured using the conductive paste of Example 1, the contact area between the silicone region (the region in Fig. 7 where the Si element is confirmed) and the substrate was controlled to a certain range. Specifically, as shown in Figs. 10 and 11, in Example 1, in the line analysis along the interface between the substrate and the conductive film, the region (silicone region) with a high count of Si element was present at a rate of about 1.75 pieces / μm (about 7 pieces / 4 μm). When the conductive paste of Example 1 was observed with an optical microscope, the silicone phase was emulsified and dispersed in the polyol phase, as shown in Figs. 2 and 4. This explains why Example 1 achieved both high levels of fixation and sheet attack suppression performance. On the other hand, as shown in Figs. 8 and 9, in the electronic component manufactured using the conductive paste of Example 18, the contact area between the silicone region and the substrate was not fully secured. Specifically, as shown in Fig. 12, in Example 18, the number of silicone regions present in the line analysis was about 0.5 pieces (2 pieces / 4 μm). This is believed to be the reason why the fixation of Example 18 was reduced.
[0094] Considering the above, (1) First relative energy difference RED BC is 1.0 or more and 2.0 or less, and (2) the second relative energy difference RED CE is less than 1.0, and (3) the third relative energy difference RED BE is 1.0 or more and 1.5 or less, and (4) the polarity term ΔP of organic solvent D is 1.5 MPa 0.5 More than 15MPa 0.5 It was found that a conductive paste in which a silicone phase is emulsified and dispersed in a polyol phase can be prepared by satisfying the following four conditions. It was also found that when electronic components are manufactured using this emulsified conductive paste, it is possible to suitably improve each of the conductivity, adhesion, and sheet attack suppression performance.
[0095] Although the specific examples of the present invention have been described in detail above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and alterations of the specific examples exemplified above. [Explanation of symbols]
[0096] 1 Polyol phase 2 Silicone phase 10 Base material 20 Conductive Film 22 Urethane area 24 Silicone Area 100 Electronic Components A Conductive material
Claims
1. A preparation step of preparing a raw material including a conductive material A, a polyol B, a silicone resin C, an organic solvent D, and a silicone oil E; A mixing process in which the prepared raw materials are mixed to prepare a paste; Including, In the preparation step, the following conditions (1) to (4): (1) HSP distance Ra between the polyol B and the silicone resin C B-C The interaction radius R of the silicone resin C 0C The first relative energy difference RED is the value obtained by dividing BC is 1.0 or more and 2.0 or less; (2) HSP distance Ra between the silicone resin C and the silicone oil E C-E The interaction radius R of the silicone oil E 0E The second relative energy difference RED is the value obtained by dividing CE is less than 1.0; (3) HSP distance Ra between the polyol B and the silicone oil E B-E The interaction radius R of the silicone oil E 0E The third relative energy difference RED is the value obtained by dividing BE is 1.0 or more and 1.5 or less; (4) The polarity term δP of the organic solvent D is 1.5 MPa. 0.5 More than 15MPa 0.5 Below is the and preparing each of the raw materials so as to satisfy the above.
2. The method according to claim 1 , wherein the raw material further comprises an isocyanate F.
3. The method according to claim 1 or 2, wherein the conductive material A has at least one shape selected from the group consisting of dendritic, plate-like, needle-like and fibrous.
4. The specific surface area of the conductive material A is 0.5 m 2 The method according to claim 3, wherein the molecular weight of the polymer is 1 / g or more.
5. The tap density of the conductive material A is 5 g / cm 3 The method of claim 3, wherein:
6. The method according to claim 1 or 2, wherein the conductive material A is at least one selected from the group consisting of gold, silver, copper, platinum, palladium, nickel, rhodium, and carbon.
7. The weight W of the silicone resin C C The weight W of the polyol B relative to B The ratio W B / W C The method according to claim 1 or 2, wherein the m is 0.6 or more and 4.0 or less.
8. The weight W of the silicone resin C C The weight W of the silicone oil E relative to E The ratio W E / W C The method according to claim 1 or 2, wherein the ratio is 0.35 or more and 2.0 or less.
9. 3. The method according to claim 1, wherein a weight of said conductive material A is set to 25 wt % or more and 85 wt % or less when a weight excluding said organic solvent D from a total weight of said conductive paste is taken as 100 wt %.
10. 3. The method according to claim 1, wherein the silicone oil E has at least one functional group selected from the group consisting of a hydroxyl group, an isocyanate group, and a carboxyl group.
11. The method according to claim 1 or 2, wherein the polyol B has three or more hydroxyl groups.
12. The method according to claim 1 or 2, wherein the polyol B has a molecular weight of 1,000 or more and 50,000 or less.
13. A silicone substrate; a conductive film formed on a surface of the substrate and including a conductive material; Equipped with The conductive film is A urethane region mainly composed of urethane resin; Silicone region, which is mainly composed of silicone resin Equipped with an electronic component in which the number of silicone regions per 1 μm of length of the contact interface between the substrate and the conductive film in a cross-sectional view is 1 to 20;
14. The electronic component of claim 13 , wherein the conductive material is aggregated within each of a plurality of the silicone regions, the silicone regions contacting each other.
15. The electronic component according to claim 13 or 14, wherein the silicone region has a tensile modulus of elasticity of 0.1 MPa or more and 10.0 MPa or less.
Citation Information
Patent Citations
Conductive paste and conductive film formed using the same
JP2017147163A
Silver coating elastomer particle and flexible conductive material and conductive paste therewith
JP2019185936A
Conductive composition and composite using the same
JP2021193165A
Pasty resin composition, high heat-conductive material, and semiconductor device
JP2022018051A
Electrically conductive paste and electrically conductive film formed by using same
US20190043638A1