Head part member, tube container and tube container with cap

A tube container with a head member made of polyethylene, ethylene-vinyl alcohol copolymer, and a modifier addresses the need for high oxygen barrier properties without aluminum, reducing manufacturing steps and costs, and achieving low oxygen permeability.

JP2024143599APending Publication Date: 2024-10-11DAI NIPPON PRINTING CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023056361
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

There is a need for a tube container that does not use aluminum and maintains high oxygen barrier properties, while also reducing the number of manufacturing steps and costs.

Method used

A head member for a tube container composed of polyethylene, ethylene-vinyl alcohol copolymer, and a modifier, with specific weight and density ratios, and a thickness range for the shoulder portion, to enhance oxygen barrier properties.

Benefits of technology

The solution effectively improves oxygen barrier properties and reduces manufacturing complexity and costs by using a single-layer structure with optimized polyethylene and ethylene-vinyl alcohol copolymer content, achieving low oxygen permeability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143599000001_ABST
    Figure 2024143599000001_ABST
Patent Text Reader

Abstract

To provide a head part member, a tube container, and a tube container with a cap, which can easily improve oxygen barrier properties.SOLUTION: A head part member 40 for a tube container 10 contains polyethylene, ethylene-vinyl alcohol copolymer, and modifiers. The content of the polyethylene is 20 wt.% or more and 80 wt.% or less. The content of the ethylene-vinyl alcohol copolymer is 20 wt.% or more and 50 wt.% or less. The oxygen permeability is 0.010 cc / pkg day atm or more and 0.030 cc / pkg day atm or less.SELECTED DRAWING: Figure 1A
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a head member, a tube container, and a tube container with a cap. [Background technology]

[0002] Tube containers have been known as containers for filling with contents (for example, Patent Documents 1 and 2). Patent Document 1 discloses a tube container in which the head member of the tube container is provided with a metal foil layer, such as aluminum foil, to improve the gas barrier properties. Patent Document 2 discloses a tube container in which the head member has a multi-layer structure comprising an inner layer, an intermediate layer (gas barrier layer), and an outer layer. Such tube containers may require a high oxygen barrier to prevent oxidation, particularly when the contents include fruit or the like. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 5509551 [Patent Document 2] Patent No. 6976032 Summary of the Invention [Problem to be solved by the invention]

[0004] However, in recent years, with the growing demand for the creation of a recycling-oriented society, there is a demand for packaging materials that do not use aluminum. For this reason, there is a demand for tube containers that have high oxygen barrier properties without using aluminum. In addition, when the head member has a multi-layer structure, the number of manufacturing steps for the head member increases, which may increase the manufacturing cost of the tube container.

[0005] The present disclosure has been made in consideration of these points, and aims to provide a head member, a tube container, and a capped tube container that can easily improve oxygen barrier properties. [Means for solving the problem]

[0006] A first aspect of the present disclosure is a head member for a tube container, comprising polyethylene, an ethylene-vinyl alcohol copolymer, and a modifier, wherein the polyethylene content is 20% by weight or more and 80% by weight or less, the ethylene-vinyl alcohol copolymer content is 20% by weight or more and 50% by weight or less, and the oxygen permeability is 0.010 cc / pkg·day·atm or more and 0.030 cc / pkg·day·atm or less.

[0007] A second aspect of the present disclosure is the head member according to the first aspect described above, wherein the content of the polyethylene is 0.5 to 5 times the content of the ethylene-vinyl alcohol copolymer.

[0008] A third aspect of the present disclosure is the head member according to the first aspect or the second aspect, wherein the ethylene-vinyl alcohol copolymer has an ethylene content of 30 mol % or more and 45 mol % or less.

[0009] A fourth aspect of the present disclosure is a head member according to each of the first to third aspects described above, wherein the density of the polyethylene is 910 kg / m 3 More than 970kg / m 3 The melt flow rate of the polyethylene may be 0.5 g / 10 min or more and 15.0 g / 10 min or less.

[0010] A fifth aspect of the present disclosure is a head member according to each of the first to fourth aspects described above, wherein the head member may have a shoulder portion and a mouth portion connected to the shoulder portion, and the thickness of the shoulder portion may be 0.25 mm or more and 2.0 mm or less.

[0011] A sixth aspect of the present disclosure is a tube container comprising a body tube and a head member according to each of the first to fifth aspects described above joined to one end of the body tube.

[0012] A seventh aspect of the present disclosure is a tube container with a cap, comprising the tube container according to the sixth aspect described above, and a cap attached to the head member. Effect of the Invention

[0013] According to the present disclosure, the oxygen barrier property of the head member can be easily improved. [Brief description of the drawings]

[0014] [Figure 1A] FIG. 1A is a partial vertical cross-sectional view showing a tube container with a cap according to the present embodiment filled with contents. [Figure 1B] FIG. 1B is a schematic perspective view illustrating a method for measuring oxygen permeability. [Figure 1C] FIG. 1C is a schematic cross-sectional view (cross-sectional view taken along line IC-IC in FIG. 1B) illustrating a method for measuring oxygen permeability. [Diagram 2] FIG. 2 is a cross-sectional view showing an example of a layer structure of the laminate according to the present embodiment. [Diagram 3] FIG. 3 is a schematic diagram showing a method for producing a tube container according to this embodiment. [Figure 4] 4(a)-(b) are schematic diagrams showing a method for manufacturing a tube container according to this embodiment. [Diagram 5] FIG. 5 is a schematic diagram showing a method for producing a tube container according to this embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] An embodiment will be described below with reference to the drawings. FIGS. 1A to 5 are diagrams showing an embodiment. Each of the following diagrams is a schematic diagram. Therefore, the size and shape of each part are appropriately exaggerated to facilitate understanding. In addition, the present invention can be modified appropriately within the scope of the technical concept. In each of the following diagrams, the same parts are given the same reference numerals, and some detailed explanations may be omitted. In addition, the numerical values ​​such as dimensions of each member and the material names described in this specification are examples of the embodiment, and are not limited to these, and can be appropriately selected and used. In this specification, terms that specify shapes and geometric conditions, such as parallel, orthogonal, and vertical, are interpreted to include substantially the same state in addition to their strict meanings. In this specification, "upper" and "lower" refer to the upper and lower sides of the capped tube container 10A in an upright state (FIG. 1A), respectively.

[0016] First, a capped tube container 10A according to the present embodiment will be described with reference to FIG. 1A.

[0017] As shown in FIG. 1A, a capped tube container 10A according to this embodiment includes a tube container 10 and a cap 20 attached to a head member 40 of the tube container 10, which will be described later.

[0018] Of these, the tube container 10 includes a body tube 30 which is a laminated molded tube, and a head member 40 joined to one end 31 of the body tube 30 .

[0019] First, the head member 40 of the tube container 10 will be described.

[0020] As shown in FIG. 1A, the head member 40 has a shoulder portion 41 and a mouth portion 42 connected to the shoulder portion 41. The shoulder portion 41 includes a portion extending in the radial direction and a portion located radially outward of the portion and extending downward. The portion extending downward is a portion to which the body tube 30 is joined. The thickness T of the shoulder portion 41 is preferably 1.0 mm or more and 2.0 mm or less. When the thickness T of the shoulder portion 41 is 1.0 mm or more, the barrier property of the head member 40 can be effectively improved. Furthermore, when the thickness T of the shoulder portion 41 is 1.0 mm or more, the strength of the head member 40 can be maintained and the moldability of the head member 40 can be improved. Furthermore, when the thickness T of the shoulder portion 41 is 2.0 mm or less, the moldability of the head member 40 can be improved. The thickness T of the shoulder portion 41 is the thickness of the portion extending in the radial direction. The thickness T of the shoulder portion 41 is a value measured in a region extending from the outer edge of the head member 40 radially inwardly and from 1 mm to 10 mm.

[0021] The mouth portion 42 is a portion that extends upward from the shoulder portion 41. In addition, the mouth portion 42 is configured so that the cap 20 can be attached thereto.

[0022] In this embodiment, the head member 40 is a single layer. The head member 40 contains polyethylene (PE), ethylene-vinyl alcohol copolymer (EVOH), and a modifier. Among these, the polyethylene may be, for example, low density polyethylene (LDPE), medium density polyethylene (MDPE), high density polyethylene (HDPE), or linear low density polyethylene (LLDPE). The polyethylene may also contain a biomass-derived component.

[0023] Low density polyethylene has a density of 910 kg / m 3 More than 930kg / m 3 Medium density polyethylene has a density of 930 kg / m 3 More than 942kg / m 3 The following polyethylenes are used: High density polyethylene has a density of 942 kg / m 3The low-density polyethylene is obtained, for example, by polymerizing ethylene at a high pressure of 1,000 atm or more and less than 2,000 atm. The medium-density polyethylene and high-density polyethylene are obtained, for example, by polymerizing ethylene at a medium or low pressure of 1 atm or more and less than 1,000 atm.

[0024] Linear low density polyethylene is obtained by copolymerizing an α-olefin into a linear polymer obtained by polymerizing ethylene at medium or low pressure to introduce short chain branches. Examples of α-olefins include 1-butene (C 4 ), 1-hexene (C 6 ), 4-methylpentene (C 6 ), 1-octene (C 8 The density of linear low density polyethylene is, for example, 915 kg / m 3 More than 945kg / m 3 The following is the result.

[0025] The density of the polyethylene contained in the head member 40 is 910 kg / m 3 More than 970kg / m 3 It is preferable that the density of polyethylene is 910 kg / m or less. 3 More than 970kg / m 3 By satisfying the density below 100%, it is possible to easily mold the multiple resins into a desired shape while mixing them. Note that a lower density of polyethylene tends to increase the adhesive strength between the body tube 30 and the resin constituting the head member 40. Also, a higher density of polyethylene tends to enhance the water vapor barrier of the head member 40. The density of polyethylene is measured by the JIS K7112B method (He gas replacement method). In the He gas replacement method, first, one head member 40 is placed in a 10 cm 3 The head member 40 was cut into a size that could fit into a measuring container. Next, all of the cut head member 40 was placed in the measuring container, and the density of the polyethylene was measured. The measurement was repeated five times, and the average value was taken as the density of the polyethylene contained in the head member 40.

[0026] The polyethylene preferably has a melt flow rate (MFR) of 0.5 g / 10 min or more and 15.0 g / 10 min or less. When the polyethylene has a melt flow rate of 0.5 g / 10 min or more, the fluidity of the resin constituting the head member 40 can be ensured when the head member 40 is compression molded. When the polyethylene has a melt flow rate of 15.0 g / 10 min or less, the moldability of the head member 40 can be ensured when the head member 40 is compression molded. The polyethylene melt flow rate is measured in accordance with JIS K6922-2:2018 "Plastics - Polyethylene materials for molding and extrusion - Part 2: Methods for preparing test pieces and determining properties".

[0027] The polyethylene content in the head member 40 is 20% by weight or more and 80% by weight or less. When the polyethylene content is 20% by weight or more, the bondability between the head member 40 and the body tube 30 can be improved. Furthermore, when the polyethylene content is 80% by weight or less, the content of the modifier in the head member 40 can be prevented from becoming too small. This makes it easier to make the polyethylene and the ethylene-vinyl alcohol copolymer compatible.

[0028] In the head member 40, the polyethylene content is preferably 0.5 to 5 times the ethylene-vinyl alcohol copolymer content. When the polyethylene content is 0.5 or more times the ethylene-vinyl alcohol copolymer content, the bondability between the head member 40 and the body tube 30 can be effectively improved. Furthermore, when the polyethylene content is 5 or less times the ethylene-vinyl alcohol copolymer content, the oxygen barrier property of the head member 40 can be improved.

[0029] In the head member 40, the content of the ethylene-vinyl alcohol copolymer is 20% by weight or more and 50% by weight or less. When the content of the ethylene-vinyl alcohol copolymer is 20% by weight or more, the barrier property of the head member 40 can be effectively improved. Furthermore, when the content of the ethylene-vinyl alcohol copolymer is 50% by weight or less, the content of the modifier in the head member 40 can be prevented from becoming too small. This makes it easier to make the polyethylene and the ethylene-vinyl alcohol copolymer compatible.

[0030] In the ethylene-vinyl alcohol copolymer, the ethylene content is preferably 30 mol % or more and 45 mol % or less. When the ethylene content is 30 mol % or more, the oxygen barrier of the head member 40 can be improved. Furthermore, when the ethylene content is 45 mol % or less, the mixability of the ethylene-vinyl alcohol copolymer and polyethylene can be improved. Therefore, the polyethylene and the ethylene-vinyl alcohol copolymer can be uniformly dispersed in the resin constituting the head member 40. As a result, the bondability between the head member 40 and the body tube 30 can be improved. Furthermore, the barrier property of the tube container 10 can be ensured by improving the bondability between the head member 40 and the body tube 30.

[0031] The oxygen permeability of the head member 40 is 0.010 cc / pkg·day·atm or more and 0.030 cc / pkg·day·atm or less. Here, the oxygen permeability of the head member 40 is measured as follows. First, a flattened portion (a portion extending in the radial direction) of the shoulder portion 41 of the head member 40 is hollowed out to prepare five test pieces S (see Figs. 1B and 1C). The shape of the test pieces S is a cylinder. At this time, the test pieces S are prepared so that the thickness direction of the shoulder portion 41 is the height direction of the cylinder. When the thickness T of the shoulder portion 41 is thicker than 1.0 mm, the test pieces S are prepared so that the height of the cylinder is 1.0 mm. The diameter of the bottom surface of the cylinder is 8.0 mm.

[0032] Next, a stainless steel plate (thickness 1.0 mm) 90 having a square shape (100 mm x 100 mm) in plan view is prepared. Five through holes 90a are formed in this stainless steel plate 90, penetrating the stainless steel plate 90 in the thickness direction. One of the five through holes 90a is formed in the center of the stainless steel plate 90. The remaining four are formed in the four corners of the stainless steel plate 90. The shape of each through hole 90a is a circle in plan view. The diameter of this circle is 8.0 mm.

[0033] Next, an adhesive is applied to the inner surface of each through hole 90a. A two-part epoxy adhesive (Bond Quick 5 (Konishi)) is used as the adhesive. The two-part epoxy adhesive is mixed just before being applied to the inner surface of the through hole 90a. At this time, after mixing the two-part epoxy adhesive, it is applied to the inner surface of the through hole 90a within 10 seconds. Then, the test piece S is fixed to the stainless steel plate 90 by inserting the test piece S into each through hole 90a.

[0034] Next, as shown in FIG. 1B and FIG. 1C, the stainless steel plate 90 to which the test piece S is fixed is attached to the measuring device 91. At this time, the stainless steel plate 90 is attached to the measuring device 91 with an adhesive. As the adhesive, a two-part epoxy adhesive (Bond Quick 5 (Konishi)) is used. The two-part epoxy adhesive is mixed just before being applied to the inner surface of the through hole 90a. At this time, after mixing the two-part epoxy adhesive, it is applied to the inner surface of the through hole 90a within 10 seconds. In this way, the stainless steel plate 90 is attached to the measuring device 91 with the adhesive, and a space 95 surrounded by the stainless steel plate 90 and the measuring device 91 is formed. As such a measuring device 91, an oxygen barrier measuring device (OX-TRAN2 / 61) manufactured by MOCON is used. This measuring device 91 has a nitrogen supply unit 92 and an oxygen measuring unit 93.

[0035] Next, the oxygen permeability of the head member 40 is measured. At this time, the room temperature is kept at 23°C, and the humidity is kept at 40% RH. In the measurement, first, nitrogen is supplied from the nitrogen supply unit 92 into the space 95 to make the nitrogen concentration in the space 95 100%. After that, it is left for one day, and the amount of oxygen that has permeated the test piece S is measured. That is, the concentration of oxygen that has entered the space 95 is measured. At this time, the oxygen measurement unit 93 measures the oxygen concentration in the space 95. Here, the oxygen that permeates the test piece S is oxygen in the air. The concentration of oxygen in the air is about 20%. Therefore, in order to convert it to a case where the oxygen concentration is 100%, the obtained measurement value is multiplied by 5. Then, the value obtained by multiplying the measurement value by 5 is set as the oxygen permeability of the head member 40. In the following description, the above-mentioned method for measuring oxygen permeability using the test piece S is also simply referred to as a permeability measurement method.

[0036] The water vapor transmission rate of the tube container 10 is preferably 0.001 g / pkg·day or more and 0.008 g / pkg·day or less. The water vapor transmission rate of the tube container 10 is measured as follows. First, the tube container 10 is filled with calcium chloride to about 70% of its capacity, and stored for 7 days or more under an environment of a temperature of 40°C and a humidity of 90% RH. Next, the weight change of the tube container 10 is measured. The measured weight change is then divided by the number of days of storage to calculate the weight change per day, and this weight change per day is defined as the water vapor transmission rate of the tube container 10.

[0037] The modifier plays a role of changing the phase structure of polyethylene and ethylene-vinyl alcohol copolymer (hereinafter, also simply referred to as EVOH) according to the purpose of modification. That is, the modifier functions as a compatibilizer of polyethylene and EVOH. The modifier may be a saponified ethylene-vinyl acetate copolymer. In this case, the interaction between the modifier and the ethylene-vinyl alcohol copolymer can be controlled by adjusting the amount of vinyl acetate and vinyl alcohol in the modifier. In addition, when the modifier is a saponified ethylene-vinyl acetate copolymer, the interaction between the modifier and EVOH is mainly due to hydrogen bonding. Therefore, even if the modifier and EVOH interact with each other when the modifier and EVOH are melt-mixed, the modifier does not react or gel. And, since the modifier changes the phase structure of the polyethylene and ethylene-vinyl alcohol copolymer according to the purpose of modification, the polyethylene and the ethylene-vinyl alcohol copolymer can be easily mixed when preparing the resin constituting the head member 40.

[0038] Here, the resin constituting the head member 40 may have a sea-island structure. The sea-island structure refers to a structure in which an ethylene-vinyl alcohol copolymer is discontinuously dispersed in a region in which polyethylene is continuous. In this way, when the resin constituting the head member 40 has a sea-island structure, the ethylene-vinyl alcohol copolymer can be uniformly dispersed in the resin constituting the head member 40. Therefore, the barrier property of the head member 40 can be effectively improved.

[0039] Such a head member 40 is molded, for example, by compression molding, as described below.

[0040] Next, the body tube 30 of the tube container 10 will be described. The body tube 30 shown in FIG. 1A has a generally cylindrical shape. This body tube 30 is composed of a laminated laminate 50 (see FIG. 2). The body tube 30 has a body seal portion (joint portion) 32 in which opposing ends 35 (see FIG. 3) of the laminate 50 are overlapped and joined to each other. This body seal portion 32 is formed along the longitudinal direction of the body tube 30. Such a body tube 30 is obtained by rolling the laminate 50 into a cylindrical shape, overlapping the opposing ends 35, and joining them to each other by, for example, heat sealing.

[0041] The body tube 30 also has a bottom seal 34 that joins the laminates 50 together. This bottom seal 34 is formed by joining the laminates 50 together near an opening 50B (see Figs. 3 and 5) formed at the other end 33 of the body tube 30 after a suitable amount of content C, such as an alcohol-containing cleansing agent, sunscreen, toothpaste, treatment, body cream, hair styling product (so-called hair wax), or other content C, is filled into the opening 50B.

[0042] Next, a description will be given of the layer structure of the laminate 50. Fig. 2 shows an example of the layer structure of the laminate 50 constituting the body tube 30. As shown in Fig. 2, the laminate 50 includes a first sealant layer 51, a first adhesive layer 54a, a base layer 52, a second adhesive layer 54b, and a second sealant layer 53, which are arranged in this order from an outer surface 501 to an inner surface 502.

[0043] 2, the laminate 50 includes, in this order from an outer surface 501 to an inner surface 502, a first sealant layer 51, a first adhesive layer 54a, a barrier layer 55, a base material layer 52, a printed layer 56, a second adhesive layer 54b, and a second sealant layer 53. In the example shown in FIG. 2, the first sealant layer 51 forms the outer surface of the body tube 30, and the second sealant layer 53 forms the inner surface of the body tube 30.

[0044] Each layer of the laminate 50 will now be described.

[0045] (First sealant layer) The first sealant layer 51 is a layer for bonding the laminates 50 together. A material that melts and fuses by heat is used as a material constituting the first sealant layer 51. For example, polyolefin is used for the first sealant layer 51. More specifically, for example, the first sealant layer 51 may be made of a resin consisting of one or more of acid-modified polyolefin resins obtained by modifying polyolefin resins such as low-density polyethylene (LDPE), medium-density polyethylene (MDPE), high-density polyethylene (HDPE), linear low-density polyethylene (LLDPE), polypropylene, polyethylene, or polypropylene with acrylic acid, methacrylic acid, maleic acid, maleic anhydride, fumaric acid, itaconic acid, or other unsaturated carboxylic acid, polyvinyl acetate resins, polyester resins, polystyrene resins, polyacrylonitrile, saturated polyester, or polyvinyl alcohol. When the first sealant layer 51 contains polyethylene, the polyethylene may contain a biomass-derived component.

[0046] In the present embodiment, when preparing the first sealant layer 51, for example, first, a desired additive may be added to a resin composition mainly composed of one or more of the above resins. In this manner, a desired resin composition is prepared. Next, a film or sheet as the first sealant layer 51 is formed using the resin composition prepared above, for example, by an inflation method or other molding method.

[0047] The material for the first sealant layer 51 may be a material to which, for example, an antiblocking agent, a lubricant (fatty acid amide, etc.), a flame retardant, an inorganic or organic filler, etc. are optionally added.

[0048] In the present embodiment, the thickness of the first sealant layer 51 is preferably not less than 50 μm and not more than 250 μm.

[0049] (base material layer) The base layer 52 is, for example, a layer for supporting the first sealant layer 51 and the second sealant layer 53 and for increasing the strength of the entire laminate 50. Examples of materials that can be used for the base layer 52 include films or sheets of polyester resins, polyamide resins, polyaramid resins, polyolefin resins, polycarbonate resins, polyacetal resins, fluorine resins, and other tough resins. As an example, the base layer 52 may contain polyethylene terephthalate. When the base layer 52 contains polyethylene terephthalate, the polyethylene terephthalate may contain a biomass-derived component.

[0050] As the above-mentioned resin film or sheet, any of unstretched films, uniaxially or biaxially stretched films, etc. can be used. Among them, in the present embodiment, a biaxially stretched polyester resin film is preferred because of its excellent printability.

[0051] In the present embodiment, the thickness of the base layer 52 is preferably not less than 10 μm and not more than 25 μm.

[0052] (Second sealant layer) The second sealant layer 53 is a layer for bonding the laminates 50 together, and as a material constituting the second sealant layer 53, for example, the same material as that of the first sealant layer 51 described above can be used.

[0053] In the present embodiment, the thickness of the second sealant layer 53 is preferably not less than 50 μm and not more than 250 μm.

[0054] (First adhesive layer and second adhesive layer) The adhesive layers such as the first adhesive layer 54a and the second adhesive layer 54b are layers for bonding the first sealant layer 51, the base material layer 52, the second sealant layer 53, etc. to one another. The material constituting the adhesive layer can be appropriately selected depending on the resin constituting the layer to be bonded.

[0055] The adhesive layer may be, for example, an anchor coating agent such as an isocyanate (urethane), polyethyleneimine, polybutadiene, or organic titanium. The adhesive layer may be, for example, a polyurethane, polyacrylic, polyester, epoxy, polyvinyl acetate, cellulose, or other laminating adhesive.

[0056] As materials constituting the adhesive layer, for example, polyethylene, polypropylene, ethylene-vinyl alcohol, ethylene-methacrylic acid copolymer (EMAA), ethylene-acrylic acid copolymer, ionomer, maleic anhydride modified polyolefin resin, etc. can be suitably used.

[0057] In the present embodiment, the thickness of each adhesive layer is preferably not less than 3 μm and not more than 60 μm.

[0058] The method for laminating the first sealant layer 51, the base layer 52, the second sealant layer 53, etc., may be, for example, a wet lamination method, a dry lamination method, a solventless dry lamination method, an extrusion lamination method, a co-extrusion lamination method, an inflation method, or any other method. When carrying out the above-mentioned lamination, the film may be subjected to a pretreatment such as a corona treatment or an ozone treatment.

[0059] (Printing layer) The printed layer is a layer on which a pattern or the like is printed, and is a layer for improving the design of the laminate 50. The printed layer can be an ink composition obtained by adjusting an ink composition by adding one or more of ordinary ink vehicles as the main component, optionally adding one or more of plasticizers, stabilizers, antioxidants, light stabilizers, ultraviolet absorbers, curing agents, crosslinking agents, lubricants, antistatic agents, fillers, and other additives as necessary, and further adding a colorant such as a dye or pigment, and thoroughly kneading with a solvent, a diluent, etc. Examples of such ink vehicles include linseed oil, tung oil, soybean oil, hydrocarbon oil, rosin, rosin ester, rosin-modified resin, shellac, alkyd resin, phenolic resin, maleic acid resin, natural resin, hydrocarbon resin, polyvinyl chloride resin, polyacetic acid resin, polystyrene resin, polyvinyl butyral resin, acrylic or methacrylic resin, polyamide resin, polyester resin, polyurethane resin, epoxy resin, urea resin, melamine resin, aminoalkyd resin, nitrocellulose, ethylcellulose, chlorinated rubber, cyclized rubber, and others, and one or more of these may be used in combination. The printing method may be gravure printing, letterpress printing, screen printing, transfer printing, flexographic printing, or other printing methods.

[0060] (Barrier layer) The barrier layer is a layer for suppressing the transmission of oxygen gas, water vapor, and the like. For example, a gas barrier material against oxygen gas, water vapor, and the like, a light-shielding material against sunlight, and a material having aroma retention for the contents can be used as the barrier layer. Specifically, for example, a thin metal deposition layer of tin, lead, copper, iron, nickel, or an alloy thereof, or aluminum, and the like can be used as the barrier layer. When aluminum foil is used as the barrier layer, the thickness of the barrier layer can be about 5 μm or more and 20 μm or less. By using aluminum foil as the barrier layer, the laminate 50 can be easily produced.

[0061] Furthermore, when using a vapor-deposited layer of a metal such as aluminum as the barrier layer, a vapor-deposited thin film of a metal such as aluminum can be formed on intermediate layer 57 by using a physical vapor deposition method (PVD method) such as vacuum deposition, sputtering, ion plating, or cluster ion beam method.

[0062] When a metal vapor-deposited aluminum layer is used as the barrier layer, the thickness of the barrier layer is usually preferably about 50 Å to 3000 Å, and particularly preferably about 100 Å to 2000 Å. The surface of the intermediate layer 57 supporting the vapor-deposited aluminum thin film can be coated in advance with, for example, a vapor deposition primer in order to improve the adhesion of the vapor-deposited film, and other pretreatments as required can be optionally performed.

[0063] The barrier layer may be a transparent vapor deposition layer and a gas barrier layer that can be formed by a conventionally known method. The barrier layer may be a transparent vapor deposition layer and a gas barrier layer, so that the laminate 50 can be made transparent. In this case, the transparent vapor deposition layer of the barrier layer may be a transparent vapor deposition layer made of an inorganic oxide vapor deposition layer.

[0064] The transparent deposition layer may be, for example, a deposition layer of an oxide of silicon (Si), aluminum (Al), magnesium (Mg), calcium (Ca), potassium (K), tin (Sn), sodium (Na), boron (B), titanium (Ti), lead (Pb), zirconium (Zr), yttrium (Y), etc. In particular, for a tube container, it is preferable to have a deposition layer of aluminum oxide or silicon oxide.

[0065] Inorganic oxides are expressed as, for example, SiO X , AlO X MO X(wherein, M represents an inorganic element, and the range of the value of X varies depending on the inorganic element). The range of the value of X is as follows: silicon (Si) is 0-2, aluminum (Al) is 0-1.5, magnesium (Mg) is 0-1, calcium (Ca) is 0-1, potassium (K) is 0-0.5, tin (Sn) is 0-2, sodium (Na) is 0-0.5, boron (B) is 0-1.5, titanium (Ti) is 0-2, lead (Pb) is 0-2, zirconium (Zr) is 0-2, and yttrium (Y) is 0-1.5. In the above, when X=0, it is a completely inorganic element (pure substance) and is not transparent, and the upper limit of the range of X is the value when it is completely oxidized. Silicon (Si) and aluminum (Al) are preferably used for the packaging material, and silicon (Si) with a value in the range of 1.0 to 2.0 and aluminum (Al) with a value in the range of 0.5 to 1.5 can be used.

[0066] The thickness of the transparent vapor deposition layer varies depending on the type of inorganic oxide used, but is desirably selected from the range of, for example, 50 Å to 2000 Å, preferably 100 Å to 1000 Å. For example, in the case of a vapor deposition layer of aluminum oxide or silicon oxide, the thickness is desirably 50 Å to 500 Å, more preferably 100 Å to 300 Å.

[0067] The transparent deposition layer can be formed on the intermediate layer 57 by using the following formation method. Examples of the method for forming the deposition layer include physical vapor deposition methods (PVD methods) such as vacuum deposition, sputtering, and ion plating, and chemical vapor deposition methods (CVD methods) such as plasma chemical vapor deposition, thermal chemical vapor deposition, and photochemical vapor deposition. Specifically, the deposition layer can be formed on a molding roller using a roller-type deposition layer forming device.

[0068] (Other layers) Although not shown, the laminate 50 may include other layers, such as an intermediate layer, for example, for increasing the strength of the entire laminate 50.

[0069] Next, a method for manufacturing the capped tube container 10A will be described with reference to FIGS.

[0070] First, for example, a laminate 50 shown in FIG. 2 is prepared.

[0071] 3, the laminate 50 is rolled into a cylindrical shape, so that the ends 35 are overlapped. Then, the outer surface 501 and the inner surface 502 of the laminate 50 are heat-sealed at the ends 35 to produce the body tube 30.

[0072] In this case, the first sealant layer 51 (see FIG. 2) provided on the outer surface 501 side of the laminate 50 and the second sealant layer 53 (see FIG. 2) provided on the inner surface 502 side are melted and joined to obtain the body tube 30.

[0073] Next, the above-mentioned tube container 10 is manufactured by compression molding. At this time, as shown in Fig. 4(a), the cylindrical laminate 50 (body tube 30) is wound around a mandrel 72, and a die 71 for compression molding the head member 40 is attached to one end of the mandrel 72. That is, the laminate 50 (body tube 30) previously molded into a cylindrical shape is inserted into the mandrel 72, the tip of which serves as a core for compression molding the head member 40, and is then advanced to a predetermined position into the cavity of the die 71 for molding the head member 40.

[0074] Next, molten resin is supplied from a resin supply device (not shown) into the metal mold 71, thereby compression molding the head member 40 at one opening 50A (see FIG. 3) of the body tube 30. In this case, the head member 40 is molded and at the same time, the body tube 30 is fused integrally to the head member 40. Thereafter, the integrated head member 40 and body tube 30 are removed from the metal mold 71 and mandrel 72, thereby obtaining the tube container 10 (see FIG. 4(b)).

[0075] In manufacturing the capped tube container 10A, the cap 20 is prepared in parallel with the production of the tube container 10. In this case, the cap 20 is produced by injection molding using, for example, an injection molding machine (not shown). Then, the cap 20 is screwed onto the mouth of the head member 40 of the tube container 10, thereby obtaining the capped tube container 10A as shown in FIG.

[0076] Thereafter, an appropriate amount of the contents C is filled through the opening 50B (see FIG. 5) of the body tube 30. The opening 50B is then welded to form the bottom seal portion 34 (see FIG. 1A). In this manner, a tube container 10A with a cap filled and packaged with the contents C is obtained.

[0077] As described above, according to this embodiment, the head member 40 contains polyethylene, an ethylene-vinyl alcohol copolymer, and a modifier. The head member 40 has a polyethylene content of 20% by weight or more and 80% by weight or less, and an ethylene-vinyl alcohol copolymer content of 20% by weight or more and 50% by weight or less. The head member 40 has an oxygen permeability of 0.010 cc / pkg·day·atm or more and 0.030 cc / pkg·day·atm or less. This can improve the barrier properties of the head member 40. The fact that the barrier properties of the head member 40 can be improved will be explained by examples described later.

[0078] In the present embodiment, the head member 40 is a single layer. In the single layer head member 40, polyethylene, an ethylene-vinyl alcohol copolymer, and a modifier are mixed. In this case, the head member 40 can be easily produced compared to a case where the head member is a multi-layered member. Therefore, the barrier property of the head member 40 can be easily improved. EXAMPLES

[0079] Next, a specific example of the above embodiment will be described.

[0080] Example 1 (1) Formability evaluation First, a laminate 50 shown in Fig. 2 was produced. In this process, a polyethylene film (thickness: 130 µm) having an antistatic function was first prepared as a first sealant layer 51.

[0081] Also, a polyethylene terephthalate film (thickness 12 μm) provided with an aluminum oxide deposition layer and a gas barrier layer (barrier layer 55) was prepared as the base layer 52. Subsequently, a print layer 56 was formed on the polyethylene terephthalate film.

[0082] Furthermore, as the second sealant layer 53, a milky white polyethylene film (thickness: 130 μm) was prepared.

[0083] Next, a polyethylene film for the first sealant layer 51, a polyethylene terephthalate film for the base layer 52, and a polyethylene film for the second sealant layer 53 were bonded by a dry lamination method to produce a laminate 50. The layer structure of the obtained laminate 50 is as follows. PE / DL / Barrier / PET / Printed / DL / PE In the above, "PE" means polyethylene film. "DL" means adhesive layer by dry lamination method. "PET" means polyethylene terephthalate film. "Mark" means printing layer (same below).

[0084] The obtained laminate 50 was used to produce the tube container 10 shown in FIG. 1A. The resin constituting the head member 40 was polyethylene (density 913 kg / m 3 , melt flow rate 8.0g / 10min) and ethylene-vinyl alcohol copolymer (density 1180kg / m 3 The resin used was a mixture of a saponified ethylene-vinyl acetate copolymer (made by Tosoh Corporation, product name: Mersen H3029A) and a polymer with a melt flow rate of 8.5 g / 10 min and an ethylene content of 35 mol%.

[0085] In the head member 40, the polyethylene content was 36% by weight, the ethylene-vinyl alcohol copolymer content was 40% by weight, and the modifier content was 24% by weight.

[0086] (2) Barrier property evaluation test The barrier properties of the head member 40 were evaluated by measuring the oxygen permeability of the head member 40. At this time, the oxygen permeability of the head member 40 was measured by the permeability measurement method described above.

[0087] Example 2 Moldability evaluation and barrier property evaluation tests were performed in the same manner as in Example 1, except that in the head member 40, the polyethylene content was 40% by weight, the ethylene-vinyl alcohol copolymer content was 30% by weight, and the modifier content was 30% by weight.

[0088] Example 3 The resin used to compose the head member 40 is polyethylene with a density of 911 kg / m 3 The moldability evaluation and barrier property evaluation tests were performed in the same manner as in Example 1, except that polyethylene having a melt flow rate of 12.0 g / 10 min was used, and in the head member 40, the polyethylene content was 40 wt %, the ethylene-vinyl alcohol copolymer content was 30 wt %, and the modifier content was 30 wt %.

[0089] Example 4 The resin used to compose the head member 40 is polyethylene with a density of 955 kg / m 3 The moldability evaluation and barrier property evaluation tests were performed in the same manner as in Example 1, except that polyethylene having a melt flow rate of 2.3 g / 10 min was used, and that in the head member 40, the polyethylene content was 40 wt %, the ethylene-vinyl alcohol copolymer content was 30 wt %, and the modifier content was 30 wt %. Example 5 The resin used to compose the head member 40 is polyethylene with a density of 925 kg / m 3 The moldability evaluation and barrier property evaluation tests were performed in the same manner as in Example 1, except that polyethylene with a melt flow rate of 8.0 g / 10 min was used, the head member 40 had a polyethylene content of 30 wt%, an ethylene-vinyl alcohol copolymer content of 40 wt%, and a modifier content of 30 wt%, and the modifier used was Mersen H4031A (product name) (saponified ethylene-vinyl acetate copolymer, manufactured by Tosoh Corporation). Example 6 The resin used to compose the head member 40 is polyethylene with a density of 925 kg / m 3 The moldability evaluation and barrier property evaluation tests were performed in the same manner as in Example 1, except that polyethylene with a melt flow rate of 8.0 g / 10 min was used, the head member 40 had a polyethylene content of 40 wt %, an ethylene-vinyl alcohol copolymer content of 30 wt %, and a modifier content of 30 wt %, and the modifier used was Mersen H4031A (product name) (saponified ethylene-vinyl acetate copolymer, manufactured by Tosoh Corporation).

[0090] Comparative Example 1 Moldability evaluation and barrier property evaluation tests were carried out in the same manner as in Example 1, except that the polyethylene content in the head member was 100% by weight.

[0091] Comparative Example 2 The polyethylene used in the resin that makes up the head part has a density of 911 kg / m 3 The moldability evaluation and barrier property evaluation tests were carried out in the same manner as in Example 1, except that polyethylene having a melt flow rate of 12.0 g / 10 min was used and the polyethylene content in the head member was 100% by weight.

[0092] Comparative Example 3 The polyethylene used in the resin that makes up the head part has a density of 955 kg / m3 The moldability evaluation and barrier property evaluation tests were carried out in the same manner as in Example 1, except that polyethylene having a melt flow rate of 2.3 g / 10 min was used and the polyethylene content in the head member was 100% by weight.

[0093] Comparative Example 4 The polyethylene used in the resin that makes up the head part has a density of 955 kg / m 3 The moldability evaluation and barrier property evaluation tests were carried out in the same manner as in Example 1, except that polyethylene having a melt flow rate of 2.3 g / 10 min was used, the polyethylene content in the head member was 100% by weight, and a laminate having gas barrier properties was attached to the inner surface of the head member. The layer structure of the laminate having a gas barrier layer is as follows. PE (thickness 150 μm) / DL / ALM (thickness 15 μm) / DL / PE (thickness 150 μm) In the above, "ALM" means aluminum foil.

[0094] The above results are shown in Tables 1 and 2. Table 1 shows the types and mixing ratios of polyethylene (PE), ethylene-vinyl alcohol copolymer (EVOH) and modifier in the resin constituting the head member 40 according to Examples 1 to 6. Table 1 also shows the type of polyethylene (PE) in the resin constituting the head member according to Comparative Examples 1 to 4. Table 2 shows the results of the moldability evaluation and barrier property evaluation tests.

[0095] [Table 1]

[0096] In the "PE" column of Table 1 above, "A" indicates a density of 913 kg / m 3 In the "PE" column of Table 1, "B" means polyethylene with a density of 911 kg / m 3In the "PE" column of Table 1, "C" means polyethylene with a density of 955 kg / m 3 In the "PE" column of Table 1, "D" means a polyethylene having a density of 925 kg / m 3 , refers to polyethylene having a melt flow rate of 8.0 g / 10 min.

[0097] [Table 2]

[0098] In the "Moldability" column of Table 2, "○" means that the head member was molded without any problems. In the "Barrier Properties" column of Table 2, "◎" means that the oxygen permeability was less than 0.030cc / pkg·day·atm. In the "Barrier Properties" column of Table 2, "○" means that the oxygen permeability was 0.030cc / pkg·day·atm or more and less than 0.035cc / pkg·day·atm. In the "Barrier Properties" column of Table 2, "×" means that the oxygen permeability was 0.035cc / pkg·day·atm or more.

[0099] As a result, the oxygen permeability of the tube containers according to Comparative Examples 1 to 3 was 0.051 cc / pkg·day·atm. In contrast, the oxygen permeability of the tube containers 10 according to Examples 1 to 6 was 0.030 cc / pkg·day·atm or less. In particular, the oxygen permeability of the tube containers 10 according to Examples 1, 5, and 6 was 0.023 cc / pkg·day·atm or less. Thus, the oxygen permeability of the tube containers 10 according to Examples 1 to 6 was smaller than that of a conventional tube container (the tube container according to Comparative Example 4 (oxygen permeability of 0.033 cc / pkg·day·atm)) in which a laminate having gas barrier properties was attached to the inner surface of the head member.

[0100] Thus, it was found that, according to this embodiment, the gas barrier property (oxygen barrier property) of the head member 40 can be easily improved.

[0101] It is also possible to combine the multiple components disclosed in the above embodiments as necessary, or to delete some of the components disclosed in the above embodiments. [Explanation of symbols]

[0102] 10 Tube container 10A Tube container with cap 20 Cap 30 Body tube 31 one end 32 Body seal 35 End 40 Head Component 50 Laminate 501 Exterior 502 Inside 51 First sealant layer 52 Base material layer 53 Second sealant layer 54a 1st adhesive layer 54b 2nd adhesive layer 55 Barrier Layer 56 Printing layer

Claims

1. A head member for a tube container, Polyethylene and an ethylene-vinyl alcohol copolymer; and a modifier, The content of the polyethylene is 20% by weight or more and 80% by weight or less, The content of the ethylene-vinyl alcohol copolymer is 20% by weight or more and 50% by weight or less, The head member has an oxygen permeability of 0.010 cc / pkg·day·atm or more and 0.030 cc / pkg·day·atm or less.

2. 2. The head member according to claim 1, wherein the content of said polyethylene is 0.5 to 5 times the content of said ethylene-vinyl alcohol copolymer.

3. 2. The head member according to claim 1, wherein the ethylene-vinyl alcohol copolymer has an ethylene content of 30 mol % or more and 45 mol % or less.

4. The density of the polyethylene is 910 kg / m 3 More than 970kg / m 3 2. The head member according to claim 1, wherein the polyethylene has a melt flow rate of 0.5 g / 10 min or more and 15.0 g / 10 min or less.

5. 2. The head member according to claim 1, further comprising a shoulder portion and a mouth portion connected to said shoulder portion, said shoulder portion having a thickness of 0.25 mm or more and 2.0 mm or less.

6. A body tube; A tube container comprising: a head member according to claim 1 joined to one end of the body tube.

7. The tube container according to claim 6 , A capped tube container comprising: a cap attached to the head member.

Citation Information

Patent Citations

  • Photo resist film comprising forming required image by active light shielding material

    JP1980009551A

  • Tube container

    JP6976032B2